Thermal-insulation flame-retardant photovoltaic backboard and preparation method thereof
By introducing aerogel material into the back plate of the photovoltaic module to form a thermally insulated and flame-retardant photovoltaic back plate with nanoporous structure, the problem of prone to fire on the back plate of the existing photovoltaic module is solved, and the flame retardancy and fire resistance are significantly improved. Improves the safety and service life of components.
Patent Information
- Application Number
- CN202410988569.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-08
AI Technical Summary
The back panel of existing photovoltaic modules is prone to fire during use and causes fire, with unsatisfactory flame retardant and fire-proofing effects, which affects the safety and service life of the components.
The aerogel material of silica or aluminum trioxide is introduced into the back plate of PET substrate to form an aerogel film layer and composite it with the PET substrate to prepare a back plate for thermal insulation and flame retardant photovoltaics, and limit heat conduction through nanoporous structures And fire resistance improves the overall flame retardancy of the backplane.
It effectively improves the flame retardancy and fire resistance of the backplane of the photovoltaic module, reduces the risk of fire spread, and improves the safety and service life of the module.
Smart Images

Figure CN118919592A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar photovoltaic module backboards, and in particular to a heat-insulating and flame-retardant photovoltaic backboard. Background Art
[0002] At present, the backplanes used in photovoltaic modules are mostly based on PET (ethylene terephthalate). This material has good insulation and strength and is a qualified backplane substrate, but its flame retardant and fireproof effects are not ideal. Fires caused by photovoltaic modules during use are not uncommon. The selection of flame-retardant photovoltaic materials will improve the safety of modules and reduce losses. Summary of the invention
[0003] The purpose of the present invention is to overcome and supplement the deficiencies in the prior art, and to provide a heat-insulating and flame-retardant photovoltaic backplane and a preparation method thereof. Aerogel material is introduced into the backplane of a PET substrate, mainly an inorganic aerogel material of silicon dioxide or aluminum oxide. Aerogel is a lightweight nanoporous material. Its nanoporous network structure and high porosity can effectively limit heat conduction, and it has high chemical stability, will not burn at high temperatures, and has excellent fireproof properties. The aerogel film is compounded with the PET substrate to improve the overall flame retardancy of the backplane.
[0004] The technical solution adopted by the present invention is:
[0005] A heat-insulating and flame-retardant photovoltaic back sheet, wherein the back sheet comprises, from bottom to top, a first fluorine coating, a PET substrate layer, an aerogel film layer and a second fluorine coating.
[0006] Preferably, in the heat-insulating and flame-retardant photovoltaic backsheet, the thickness of the first fluorine coating and the second fluorine coating are both 15-25 um; the thickness of the aerogel film layer is 0.05-0.12 mm, and the thickness of the PET substrate layer is 0.25-0.35 mm.
[0007] Preferably, in the heat-insulating and flame-retardant photovoltaic backsheet, the material of the aerogel film layer is selected from one of silicon dioxide and aluminum oxide.
[0008] The present invention also provides a method for preparing a heat-insulating flame-retardant photovoltaic backsheet, which comprises the following steps:
[0009] Step S1. providing a PET substrate, applying a fluorine-containing coating to a surface of the PET substrate layer after corona treatment, and then drying the fluorine-containing coating to form a first fluorine coating on the PET substrate layer;
[0010] Step S2. After corona treatment, the other surface of the PET substrate layer is coated with glue, and then the aerogel film layer is composited on the side coated with glue, and finally a aging treatment is performed;
[0011] Step S3. Coat a fluorine-containing coating on the side of the aerogel film layer that has been cured in step S2 and is away from the PET substrate layer, and then dry the fluorine-containing coating to form a second fluorine coating on the aerogel film layer to obtain a heat-insulating and flame-retardant photovoltaic backplane.
[0012] Preferably, in the method for preparing the heat-insulating flame-retardant photovoltaic backsheet, the temperature of the drying treatment in step S1 is 60-70° C., and the drying time is 20-40 min.
[0013] Preferably, in the method for preparing the heat-insulating flame-retardant photovoltaic backsheet, the temperature of the aging treatment in step S2 is 60-80° C., and the aging treatment time is 48-72 hours.
[0014] Preferably, in the method for preparing the heat-insulating flame-retardant photovoltaic backsheet, the temperature of the drying treatment in step S3 is 60-70° C., and the drying time is 20-40 min.
[0015] Advantages of the present invention:
[0016] The heat-insulating and flame-retardant photovoltaic backboard and preparation method thereof of the present invention introduce an aerogel film layer into a traditional PET-based backboard. Aerogel is a lightweight nanoporous material whose nanoporous network structure and high porosity can effectively limit heat conduction, and has high chemical stability, will not burn at high temperatures, and has excellent fireproof properties. The aerogel film layer is compounded with the PET substrate to improve the overall flame retardancy of the backboard. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic structural diagram of the heat-insulating and flame-retardant photovoltaic backsheet of the present invention. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with specific embodiments.
[0019] Example 1
[0020] like Figure 1 A heat-insulating and flame-retardant photovoltaic backplane, the backplane comprises, from bottom to top, a first fluorine coating 1, a PET substrate layer 2, an aerogel film layer 3 and a second fluorine coating 4, the thickness of the first fluorine coating 1 and the second fluorine coating 4 is 20 um; the thickness of the aerogel film layer 3 is 0.05 mm, and the thickness of the PET substrate layer 2 is 0.3 mm.
[0021] The method for preparing the heat-insulating flame-retardant photovoltaic backsheet of this embodiment comprises the following steps:
[0022] Step S1. providing a PET substrate 2, applying a fluorine-containing coating to a surface of the PET substrate layer 2 after corona treatment, and then drying the fluorine-containing coating at a temperature of 65° C. for 50 minutes, thereby forming a first fluorine coating 1 on the PET substrate layer 2;
[0023] Step S2. After corona treatment, the other surface of the PET substrate layer 2 is coated with polyurethane glue, and then the aerogel film layer 3 is composited on the glue-coated side, and finally a aging treatment is performed at a temperature of 70° C. for 60 hours;
[0024] Step S3. Coat the side of the aerogel film layer 3 that has been cured in step S2 away from the PET substrate layer 2 with a fluorine-containing coating, and then dry the fluorine-containing coating at a temperature of 60° C. for 40 minutes, thereby forming a second fluorine coating 4 on the aerogel film layer 3 to obtain a heat-insulating and flame-retardant photovoltaic backplane.
[0025] Example 2
[0026] like Figure 1 A heat-insulating and flame-retardant photovoltaic backplane, the backplane comprises, from bottom to top, a first fluorine coating 1, a PET substrate layer 2, an aerogel film layer 3 and a second fluorine coating 4, the thickness of the first fluorine coating 1 and the second fluorine coating 4 is 20 um; the thickness of the aerogel film layer 3 is 0.08 mm, and the thickness of the PET substrate layer 2 is 0.3 mm.
[0027] The method for preparing the heat-insulating flame-retardant photovoltaic backsheet of this embodiment comprises the following steps:
[0028] Step S1. providing a PET substrate 2, applying a fluorine-containing coating to a surface of the PET substrate layer 2 after corona treatment, and then drying the fluorine-containing coating at a temperature of 65° C. for 50 minutes, thereby forming a first fluorine coating 1 on the PET substrate layer 2;
[0029] Step S2. After corona treatment, the other surface of the PET substrate layer 2 is coated with polyurethane glue, and then the aerogel film layer 3 is composited on the glue-coated side, and finally a aging treatment is performed at a temperature of 70° C. for 60 hours;
[0030] Step S3. Coat the side of the aerogel film layer 3 that has been cured in step S2 away from the PET substrate layer 2 with a fluorine-containing coating, and then dry the fluorine-containing coating at a temperature of 60° C. for 40 minutes, thereby forming a second fluorine coating 4 on the aerogel film layer 3 to obtain a heat-insulating and flame-retardant photovoltaic backplane.
[0031] Example 3
[0032] like Figure 1 A heat-insulating and flame-retardant photovoltaic backplane, the backplane comprises, from bottom to top, a first fluorine coating 1, a PET substrate layer 2, an aerogel film layer 3 and a second fluorine coating 4, the thickness of the first fluorine coating 1 and the second fluorine coating 4 is 20 um; the thickness of the aerogel film layer 3 is 0.10 mm, and the thickness of the PET substrate layer 2 is 0.3 mm.
[0033] The method for preparing the heat-insulating flame-retardant photovoltaic backsheet of this embodiment comprises the following steps:
[0034] Step S1. providing a PET substrate 2, applying a fluorine-containing coating to a surface of the PET substrate layer 2 after corona treatment, and then drying the fluorine-containing coating at a temperature of 65° C. for 50 minutes, thereby forming a first fluorine coating 1 on the PET substrate layer 2;
[0035] Step S2. After corona treatment, the other surface of the PET substrate layer 2 is coated with polyurethane glue, and then the aerogel film layer 3 is composited on the glue-coated side, and finally a aging treatment is performed at a temperature of 70° C. for 60 hours;
[0036] Step S3. Coat the side of the aerogel film layer 3 that has been cured in step S2 away from the PET substrate layer 2 with a fluorine-containing coating, and then dry the fluorine-containing coating at a temperature of 60° C. for 40 minutes, thereby forming a second fluorine coating 4 on the aerogel film layer 3 to obtain a heat-insulating and flame-retardant photovoltaic backplane.
[0037] Example 4
[0038] like Figure 1 A heat-insulating and flame-retardant photovoltaic backplane, the backplane comprises, from bottom to top, a first fluorine coating 1, a PET substrate layer 2, an aerogel film layer 3 and a second fluorine coating 4, the thickness of the first fluorine coating 1 and the second fluorine coating 4 is 20 um; the thickness of the aerogel film layer 3 is 0.12 mm, and the thickness of the PET substrate layer 2 is 0.3 mm.
[0039] The method for preparing the heat-insulating flame-retardant photovoltaic backsheet of this embodiment comprises the following steps:
[0040] Step S1. providing a PET substrate 2, applying a fluorine-containing coating to a surface of the PET substrate layer 2 after corona treatment, and then drying the fluorine-containing coating at a temperature of 65° C. for 50 minutes, thereby forming a first fluorine coating 1 on the PET substrate layer 2;
[0041] Step S2. After corona treatment, the other surface of the PET substrate layer 2 is coated with polyurethane glue, and then the aerogel film layer 3 is composited on the glue-coated side, and finally a aging treatment is performed at a temperature of 70° C. for 60 hours;
[0042] Step S3. Coat the side of the aerogel film layer 3 that has been cured in step S2 away from the PET substrate layer 2 with a fluorine-containing coating, and then dry the fluorine-containing coating at a temperature of 60° C. for 40 minutes, thereby forming a second fluorine coating 4 on the aerogel film layer 3 to obtain a heat-insulating and flame-retardant photovoltaic backplane.
[0043] The heat-insulating flame-retardant photovoltaic backsheets of Example 1, Example 2, Example 3, and Example 4 were subjected to a flame spread test, and the test results are shown in Table 1 below.
[0044] Table 1
[0045]
[0046] It can be seen from Table 1 above that the heat-insulating and flame-retardant photovoltaic backsheets of Examples 1, 2, 3 and 4 of the present invention have obvious advantages in flame spread length compared with existing products.
[0047] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, ordinary technicians in the field should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A heat-insulating flame-retardant photovoltaic backsheet, characterized in that: The back plate comprises, from bottom to top, a first fluorine coating layer (1), a PET substrate layer (2), an aerogel film layer (3) and a second fluorine coating layer (4).
2. The heat-insulating flame-retardant photovoltaic backsheet according to claim 1, characterized in that: The thickness of the first fluorine coating (1) and the second fluorine coating (4) are both 15-25 um; the thickness of the aerogel film layer (3) is 0.05-0.12 mm; and the thickness of the PET substrate layer (2) is 0.25-0.35 mm.
3. The heat-insulating flame-retardant photovoltaic backsheet according to claim 1, characterized in that: The material of the aerogel film layer (3) is selected from one of silicon dioxide and aluminum oxide.
4. The method for preparing a heat-insulating flame-retardant photovoltaic backsheet according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step S1. providing a PET substrate (2), applying a fluorine-containing coating to a surface of the PET substrate layer (2) after corona treatment, and then drying the fluorine-containing coating to form a first fluorine coating (1) on the PET substrate layer (2); Step S2. Corona discharge the other surface of the PET substrate layer (2) and then apply glue, then laminate the aerogel film layer (3) on the side coated with glue, and finally perform a aging treatment; Step S3. A fluorine-containing coating is applied to the side of the aerogel film layer (3) that has been cured in step S2 and is away from the PET substrate layer (2), and then the fluorine-containing coating is dried to form a second fluorine coating (4) on the aerogel film layer (3), thereby obtaining a heat-insulating and flame-retardant photovoltaic backsheet.
5. The method for preparing the heat-insulating flame-retardant photovoltaic backsheet according to claim 4, characterized in that: The temperature of the drying treatment in step S1 is 60-70° C., and the drying time is 20-40 minutes.
6. The method for preparing the heat-insulating flame-retardant photovoltaic backsheet according to claim 4, characterized in that: The temperature of the aging treatment in step S2 is 60-80° C., and the aging treatment time is 48-72 hours.
7. The method for preparing the heat-insulating flame-retardant photovoltaic backsheet according to claim 4, characterized in that: The temperature of the drying treatment in step S3 is 60-70° C., and the drying time is 20-40 minutes.
Citation Information
Cited By
Light metal photovoltaic module and preparation method thereof
CN121310659A