Monolithic integrated wavelength tunable quantum dot chip and preparation method thereof

By using a combination of monolithic integrated structure and optical Stark effect in quantum dot chips, the problems of limited wavelength regulation range and complex preparation process in the existing technology are solved, and the wavelength range is widened and precise adjustment is achieved, and the cost is reduced. , adapt to diverse application scenarios.

CN118919630APending Publication Date: 2024-11-08QINGDAO YICHENLEISHUO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410996110.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The wavelength regulation range of existing quantum dot chips is limited and the preparation process is complex, resulting in high costs and low yield, making it difficult to achieve large-scale production.

Method used

Using a monolithic integrated structure, including substrate, buffer layer, Bragg reflective layer, quantum dot layer, cap layer and wavelength adjustment layer, the optical Stark effect is used by the combination of silicon dioxide film layer and tin doped indium oxide film layer. The localization characteristics of the light field of ENZ materials, combined with the rapid thermal annealing process, broaden the luminescence wavelength regulation range of quantum dots.

Benefits of technology

The wavelength range of quantum dot chips is expanded and precisely adjusted, reducing the difficulty and cost of preparation processes, improving the integration of chip structure, and adapting to diversified wavelength tuning application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919630A_ABST
    Figure CN118919630A_ABST
Patent Text Reader

Abstract

The invention relates to a monolithic integrated wavelength tunable quantum dot chip and a preparation method thereof. The chip comprises a substrate, a buffer layer, a Bragg reflection layer, a quantum dot layer, a cover layer and a wavelength adjustment layer which are sequentially arranged from bottom to top, wherein the wavelength adjusting layer comprises a silicon dioxide thin film layer and a tin-doped indium oxide thin film layer, the width of the silicon dioxide thin film layer and the width of the tin-doped indium oxide thin film layer are both smaller than one half of the width of the cover layer, and the silicon dioxide thin film layer and the tin-doped indium oxide thin film layer are arranged at the two ends of the cover layer respectively. On the basis of the structure, the wavelength range of the quantum dot chip can be widened, accurate adjustment of the quantum dot light-emitting wavelength can be achieved, meanwhile, the chip structure integration degree is high, and the preparation technology difficulty and cost are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a monolithic integrated wavelength tunable quantum dot chip and a preparation method thereof. Background Art

[0002] Chips with wavelength tunability have shown great application potential in a variety of fields. They can achieve dynamic wavelength allocation, accurately measure pollutant concentrations, provide higher imaging contrast, and achieve precise quantum manipulation and quantum entanglement. Semiconductor quantum dots are a type of nanoscale semiconductor material that exhibits size-dependent energy level spacing characteristics due to its quantum confinement effect. By adjusting the size of quantum dots, their electronic energy levels can be precisely controlled, thereby regulating the wavelength of light absorption and emission.

[0003] However, the wavelength control range of quantum dots is currently limited, and achieving wavelength tunability based on current methods often requires complex chip structures and complicated processing procedures, which increases manufacturing costs and affects yields, making it impossible to achieve large-scale production. Therefore, the wavelength control range of current wavelength tunable quantum dot chips is small, and the preparation process is difficult and costly. Summary of the invention

[0004] The embodiments of the present invention provide a monolithic integrated wavelength tunable quantum dot chip and a method for preparing the same, which at least solve the problems in the related art that the wavelength tunable quantum dot chip has a small wavelength control range and a high difficulty and cost in the preparation process.

[0005] According to a first aspect of an embodiment of the present invention, there is provided a monolithically integrated wavelength tunable quantum dot chip, comprising a substrate, a buffer layer, a Bragg reflection layer, a quantum dot layer, a cap layer and a wavelength adjustment layer arranged in sequence from bottom to top;

[0006] Among them, the wavelength adjustment layer includes a silicon dioxide thin film layer and a tin-doped indium oxide thin film layer, the widths of the silicon dioxide thin film layer and the tin-doped indium oxide thin film layer are both less than half of the width of the cover layer, and the silicon dioxide thin film layer and the tin-doped indium oxide thin film layer are respectively arranged at both ends of the cover layer.

[0007] Preferably, the thickness of the tin-doped indium oxide thin film layer gradually increases from the inside to the outside.

[0008] Preferably, the thickness of the silicon dioxide thin film layer is 10 nm to 500 nm, and the thickness of the tin-doped indium oxide thin film layer is 10 nm to 500 nm.

[0009] Preferably, the Bragg reflection layer comprises a multi-layer reflection layer group, and the number of the reflection layer group is 8 to 30 layers;

[0010] The multi-layer reflective layer group includes a first refractive film layer and a second refractive film layer, and the first refractive film layer and the second refractive film layer have different refractive indices;

[0011] The material of the first refractive film layer is GaAs, and the material of the second refractive film layer is AlGaAs; or, the material of the first refractive film layer is InP, and the material of the second refractive film layer is GaInAsP.

[0012] Preferably, the material of the quantum dot layer is a mixed material of InAs and GaAs, or a mixed material of InAs and InP.

[0013] Preferably, the material of the buffer layer is GaAs or InP, and the thickness is 30nm-200nm; the material of the cap layer is GaAs or InP, and the thickness is 30nm-300nm.

[0014] According to a second aspect of an embodiment of the present invention, there is provided a method for preparing a monolithically integrated wavelength tunable quantum dot chip, comprising:

[0015] epitaxially growing a buffer layer, a Bragg reflection layer, a quantum dot layer and a cap layer on the substrate in sequence;

[0016] preparing a silicon dioxide thin film layer on the cap layer by a plasma enhanced chemical vapor deposition method;

[0017] Performing a rapid thermal annealing process on the quantum dot layer region covered by the silicon dioxide thin film layer;

[0018] Preparing a tin-doped indium oxide thin film layer on the cap layer by a magnetron sputtering method or an electron beam evaporation method, so as to generate a wavelength adjustment layer of the monolithic integrated wavelength tunable quantum dot chip according to the silicon dioxide thin film layer and the tin-doped indium oxide thin film layer;

[0019] The widths of the silicon dioxide film layer and the tin-doped indium oxide film layer are both less than half of the width of the cover layer, and the silicon dioxide film layer and the tin-doped indium oxide film layer are respectively arranged at two ends of the cover layer.

[0020] Preferably, the thickness of the silicon dioxide thin film layer gradually increases from the inside to the outside, and the thickness of the tin-doped indium oxide thin film layer gradually increases from the inside to the outside.

[0021] Preferably, the material of the quantum dot layer is a mixed material of InAs and GaAs, or a mixed material of InAs and InP;

[0022] Wherein, when the material of the quantum dot layer is a mixed material of InAs and GaAs, when the quantum dot layer region covered by the silicon dioxide thin film layer is subjected to rapid thermal annealing, the annealing temperature is 400° C. to 900° C., and the annealing time is 10s to 180s;

[0023] In the case where the material of the quantum dot layer is a mixed material of InAs and InP, when the quantum dot layer region covered by the silicon dioxide thin film layer is subjected to rapid thermal annealing, the annealing temperature is 500° C. to 800° C., and the annealing time is 10s to 300s.

[0024] A monolithic integrated wavelength tunable quantum dot chip provided by an embodiment of the present invention can broaden the wavelength range of the quantum dot chip, and can realize the precise adjustment of the quantum dot emission wavelength, and at the same time, the chip structure has a high degree of integration, which reduces the difficulty and cost of the preparation process. Specifically, the monolithic integrated wavelength tunable quantum dot chip provided by an embodiment of the present invention includes a substrate, a buffer layer, a Bragg reflection layer, a quantum dot layer, a cover layer and a wavelength adjustment layer arranged in sequence from bottom to top. Among them, the wavelength adjustment layer includes a silicon dioxide film layer and a tin-doped indium oxide film layer, and the width of the silicon dioxide film layer and the tin-doped indium oxide film layer are both less than half of the width of the cover layer, and the silicon dioxide film layer and the tin-doped indium oxide film layer are respectively arranged at both ends of the cover layer. In practical applications, by performing rapid thermal annealing on the quantum dot layer area covered by the silicon dioxide film layer, and combining the silicon dioxide film layer and the tin-doped indium oxide film layer, the luminous range of the quantum dot can be broadened and the regulation effect of the quantum dot emission wavelength can be enhanced. At the same time, the chip structure integration and compactness are improved, and the difficulty and cost of the chip preparation process are reduced.

[0025] The details of one or more embodiments of the invention are set forth in the following drawings and description so that other features, objects, and advantages of the invention are more readily apparent. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art descriptions. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other embodiments can be obtained based on these drawings without creative work.

[0027] Figure 1 A schematic diagram of the structure of a monolithically integrated wavelength tunable quantum dot chip provided in an embodiment of the present application.

[0028] Figure 2 This is a normalized light intensity spectrum showing the effect of silicon dioxide film layer thickness on the emission wavelength of quantum dots provided in an embodiment of the present application.

[0029] Figure 3 This is a normalized light intensity spectrum showing the effect of the thickness of the tin-doped indium oxide thin film layer on the emission wavelength of quantum dots provided in an embodiment of the present application.

[0030] Figure 4 A flow chart of a method for preparing a monolithically integrated wavelength tunable quantum dot chip provided in an embodiment of the present application.

[0031] In the figure, 1, substrate; 2, buffer layer; 3, Bragg reflection layer; 4, quantum dot layer; 5, cover layer; 6, wavelength adjustment layer; 7, silicon dioxide thin film layer; 8, tin-doped indium oxide thin film layer. DETAILED DESCRIPTION

[0032] Embodiments of the present embodiment will be described in more detail below with reference to the accompanying drawings. Although certain embodiments of the present embodiment are shown in the accompanying drawings, it should be understood that the present embodiment can be implemented in various forms and should not be construed as being limited to the embodiments set forth herein, which are instead provided for a more thorough and complete understanding of the present embodiment. It should be understood that the drawings and embodiments of the present embodiment are only for exemplary purposes and are not intended to limit the scope of protection of the present embodiment.

[0033] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the case where there is no conflict between the embodiments, the following embodiments and the features in the embodiments can be combined with each other. In addition, the step sequence in the following method embodiments is only an example and not a strict limitation.

[0034] Chips with wavelength tunability have shown great application potential in many high-tech fields with their unique flexibility and high efficiency, and have become one of the important directions for promoting the development of future information technology and optoelectronic technology. In optical fiber communication systems, wavelength tunable chips realize dynamic wavelength allocation, enhance the flexibility and bandwidth management capabilities of the network; in environmental monitoring, tunable lasers accurately measure the concentration of pollutants in the air; in biomedical imaging technologies, such as fluorescence imaging and Raman imaging, wavelength tunable light sources provide fine control and high contrast, improve imaging quality and resolution, and have important application value in cell structure, tissue pathology research and drug screening; in the field of quantum computing and quantum communication, wavelength tunable light sources support precise quantum manipulation and quantum entanglement, and improve the stability and efficiency of quantum systems.

[0035] Semiconductor quantum dots are a type of nanoscale semiconductor material whose characteristic size is smaller than the de Broglie wavelength of electrons or the mean free path of electrons, resulting in the restriction of electron movement in three-dimensional space. Quantum dot materials exhibit a series of properties different from bulk materials and quantum well materials due to their unique quantum confinement effect. The energy level spacing of quantum dots is closely related to their size. Therefore, by adjusting the size of quantum dots, their electronic energy levels can be precisely controlled, and then the wavelength of light absorption and emission can be adjusted, showing a significant advantage of wavelength tunability. However, relying solely on epitaxial growth technology to expand the emission wavelength of quantum dots faces many challenges, including complex epitaxial processes, difficult-to-control quantum dot morphology, size and distribution uniformity, which severely limits the potential and feasibility of wavelength adjustment. In addition, achieving wavelength tunability usually requires the construction of complex chip structures and complex processing processes, which not only significantly increases manufacturing costs, but also affects the yield of chips, bringing challenges to large-scale commercial production.

[0036] To solve the above problems, the embodiments of the present application integrate the optical Stark effect of quantum dot materials, the light field localization characteristics of Epsilon-Near-Zero (ENZ) materials, and a precise selective area annealing process to provide a monolithic integrated wavelength tunable quantum dot chip.

[0037] In order to better understand the technical solution of the present application, the terms involved in the embodiments of the present application are first described in detail.

[0038] Optical Stark effect: The optical Stark effect is an inelastic light scattering phenomenon that usually occurs when a strong light field interacts with matter. When the light field intensity is high enough, it can directly disturb the electron energy levels inside the matter, causing a small shift in the energy levels. In quantum dots, due to the quantum confinement effect, the energy levels of electrons are quantized, and even a small change in energy can lead to a significant change in the spectrum. The optical Stark effect is therefore particularly significant in quantum dots, and has an important impact on the fields of optoelectronics and quantum optics.

[0039] Nearly zero dielectric constant materials (ENZ): Nearly zero dielectric constant materials refer to materials whose dielectric constant is very close to zero within a specific frequency range. At the interface between ENZ materials and non-ENZ materials, due to the sharp change in dielectric constant, a strong electromagnetic field localization phenomenon can be formed. This localization effect can significantly enhance the interaction between nonlinear media (such as quantum dots, dye molecules, etc.) around the material and light, providing new possibilities for optical regulation and sensor applications.

[0040] Bragg reflector (DBR): Bragg reflector is a periodic multilayer structure that can strongly reflect light in a specific wavelength band. Its working principle is based on the Bragg diffraction law. By adjusting the refractive index or thickness of the layer, the wavelength of the reflected light matches the Bragg condition. When the Bragg reflector is combined with the ENZ material, it can effectively suppress the propagation of light in the vertical direction, and at the same time significantly enhance the intensity of the light field by using the resonance effect, especially in the vicinity of the ENZ material, the localization effect of the light field is particularly significant.

[0041] Selective area annealing process: Selective area annealing process is an important material processing technology, which is usually used to adjust the optical and electrical properties of materials. This process adjusts the optical properties by controlling the annealing temperature and time to change the composition, morphology and size of the material. In quantum dot materials, the selective area annealing process is particularly critical because it can significantly affect the luminescence properties of quantum dots, including luminescence wavelength and luminescence intensity. In addition, the selection of suitable capping materials (such as SiO2) can further regulate the luminescence spectrum of quantum dots and enhance their application potential in optoelectronic devices.

[0042] Figure 1 This is a schematic diagram of the structure of a monolithic integrated wavelength tunable quantum dot chip provided in an embodiment of the present application. Figure 1 As shown, the monolithic integrated wavelength tunable quantum dot chip includes a substrate 1, a buffer layer 2, a Bragg reflection layer 3, a quantum dot layer 4, a cover layer 5 and a wavelength adjustment layer 6 which are arranged in sequence from bottom to top.

[0043] In this embodiment, substrate 1 is the base part of the entire chip. Substrate 1 can be made of gallium arsenide (GaAs) or other semiconductor materials to provide mechanical support and basic electronic properties; buffer layer 2 can be used to adjust the lattice matching; Bragg reflection layer 3 can be used for light wave reflection; quantum dot layer 4 is used to carry embedded quantum dots; cover layer 5 can be used to protect quantum dot layer 4 and provide an optical environment; wavelength adjustment layer 6 can be used to adjust the light emission wavelength of quantum dots.

[0044] Furthermore, the wavelength adjustment layer 6 includes a silicon dioxide thin film layer 7 and a tin-doped indium oxide thin film layer 8, the widths of the silicon dioxide thin film layer 7 and the tin-doped indium oxide thin film layer 8 are both less than half of the width of the cover layer 5, and the silicon dioxide thin film layer 7 and the tin-doped indium oxide thin film layer 8 are respectively arranged at both ends of the cover layer 5.

[0045] Based on the above structure, the monolithic integrated wavelength tunable quantum dot chip can be divided into three parts. Specifically, the first part is an area covered with a tin-doped indium oxide thin film layer 8 with a gradient thickness, and the red shift of the luminescence wavelength is achieved by utilizing the optical Stark effect of quantum dots and the light field localization characteristics of ENZ materials; the second part is an area covered with a silicon dioxide thin film layer 7 with a gradient thickness, which can achieve a blue shift of the luminescence wavelength after being treated by a rapid thermal annealing process; the third part is the area between the first and second parts, which can retain the luminescence characteristics of the quantum dots themselves. In addition, the Bragg reflection layer 3 can further optimize the light field localization effect of the ENZ material, and through the synergistic effect with the ENZ material, a resonant microstructure is formed to enhance the localization degree of the light field and promote the optical Stark effect. Based on the above structure, the wavelength tunable range of the quantum dot chip is expanded, the manufacturing process is greatly simplified, and the production cost is reduced, making it an ideal choice for adapting to a variety of wavelength tuning application scenarios, which helps to promote its large-scale commercial production and wide application.

[0046] In an optional embodiment, the buffer layer 2 is located on the substrate 1 to improve the lattice matching between the subsequent layer and the substrate 1 and reduce the strain caused by the lattice mismatch in the epitaxial growth. In practical applications, the material of the buffer layer 2 may include gallium arsenide (GaAs) or indium phosphide (InP), etc., and the thickness of the buffer layer 2 may be 30nm to 200nm.

[0047] By selecting the thickness and material of the buffer layer 2 accordingly, the lattice matching with the quantum dot layer 4 can be optimized, defects can be reduced, and high-quality optical performance can be ensured.

[0048] In an optional embodiment, the Bragg reflection layer 3 is composed of a multi-layer structure, which utilizes the Bragg reflection principle to strongly reflect light waves in a specific band, thereby enhancing the localization of the light field and improving the optical efficiency.

[0049] Specifically, the Bragg reflection layer 3 includes a multi-layer reflection layer group, and the number of the reflection layer groups is 8 to 30. The multi-layer reflection layer group includes a first refractive film layer and a second refractive film layer, and the first refractive film layer and the second refractive film layer have different refractive indices.

[0050] In practical applications, the material of the first refractive film layer may be GaAs, and the material of the second refractive film layer may be AlGaAs. Alternatively, the material of the first refractive film layer may be InP, and the material of the second refractive film layer may be GaInAsP.

[0051] In an optional embodiment, the quantum dot layer 4 is a layer embedded with quantum dots and is the core part of the chip. The quantum dots can be a mixed material of InAs (indium arsenide) and GaAs (gallium arsenide), or a mixed material of InAs (indium arsenide) and InP (indium phosphide), and precise light emission is achieved through composition and quantum confinement effects.

[0052] Based on the above materials, different electronic and optical properties can be provided in the quantum dot layer 4, and precise light emission and wavelength adjustment can be achieved through the quantum confinement effect.

[0053] In an optional embodiment, the cover layer 5 covers the quantum dot layer 4 to protect the quantum dots and provide a suitable optical environment. The material may include GaAs or InP, and the thickness may be 30nm to 300nm. Based on the above materials and according to actual needs, the thickness of the cover layer 5 can be adjusted to optimize the optical effect and mechanical protection.

[0054] In an optional embodiment, the wavelength adjustment layer 6 is located at the top layer of the monolithic integrated wavelength tunable quantum dot chip, and can be used to adjust the light emission wavelength of the quantum dots, including a silicon dioxide (SiO2) thin film layer and a tin-doped indium oxide (ITO) thin film layer.

[0055] In practical applications, the widths of the silicon dioxide thin film layer 7 and the tin-doped indium oxide thin film layer 8 are both less than half the width of the cover layer 5, and they are located at both ends of the cover layer 5, symmetrically arranged based on the center line of the cover layer 5 to ensure the uniformity and effect of wavelength adjustment.

[0056] Optionally, the thickness of the silicon dioxide film layer 7 gradually increases from the inside to the outside, and the gradually increasing thickness can regulate the size and shape of the quantum dots differently during the rapid thermal annealing process, which helps to cause a blue shift (shortening of the wavelength); the thickness of the tin-doped indium oxide film layer 8 gradually increases from the inside to the outside, which helps to form a different optical environment and promotes a red shift (longer wavelength).

[0057] Based on the above structure, it is helpful to optimize the effect of wavelength adjustment and ensure the stability and consistency of optical performance in the entire optical path.

[0058] Furthermore, in order to achieve accurate wavelength adjustment and optical performance optimization, the thickness range of the silicon dioxide film layer 7 and the thickness range of the tin-doped indium oxide film layer 8 are both 10nm to 500nm. It should be noted that the thickness of the silicon dioxide film layer 7 and the thickness of the tin-doped indium oxide film layer 8 can be arbitrarily set within the above range to optimize the optical performance and achieve accurate wavelength adjustment. The normalized light intensity spectrum of the effect of the thickness of the silicon dioxide film layer 7 on the wavelength of the quantum dot emission is shown in FIG. Figure 2 As shown, the normalized light intensity spectrum of the effect of the thickness of the tin-doped indium oxide film layer 8 on the wavelength of the quantum dot emission is as follows Figure 3 shown.

[0059] Based on the above-mentioned monolithically integrated wavelength tunable quantum dot chip, an embodiment of the present application also provides a method for preparing a monolithically integrated wavelength tunable quantum dot chip.

[0060] Figure 4 A flow chart of a method for preparing a monolithic integrated wavelength tunable quantum dot chip provided in an embodiment of the present application. Figure 4 As shown, the method includes the following steps.

[0061] Step S401, epitaxially growing a buffer layer, a Bragg reflection layer, a quantum dot layer and a cap layer in sequence on a substrate.

[0062] Step S402 , preparing a silicon dioxide thin film layer on the cap layer by plasma enhanced chemical vapor deposition method.

[0063] Step S403, performing a rapid thermal annealing process on the quantum dot layer region covered by the silicon dioxide thin film layer.

[0064] Step S404, preparing a tin-doped indium oxide thin film layer on the cover layer by magnetron sputtering or electron beam evaporation to generate a wavelength adjustment layer of a monolithic integrated wavelength tunable quantum dot chip based on the silicon dioxide thin film layer and the tin-doped indium oxide thin film layer.

[0065] First, a buffer layer, a Bragg reflection layer, a quantum dot layer and a cap layer are epitaxially grown in sequence on a substrate. In this embodiment, the above steps can be performed by a molecular beam epitaxy device.

[0066] In practical applications, the material of the substrate is first selected, and the substrate is cleaned and surface treated. In this embodiment, the material of the substrate may include silicon (Si), gallium arsenide (GaAs), indium phosphide (InP), etc. Impurities are removed by cleaning and surface treatment to ensure the quality of epitaxial growth. Optionally, a double-sided polished substrate can be used to improve the uniformity of epitaxial growth; an ion beam surface treatment technology can be used to enhance the activity of the substrate surface.

[0067] The growth temperature of the buffer layer may be 550°C to 630°C.

[0068] The Bragg reflector layer is composed of multiple layers of high refractive index materials (such as GaAs) and low refractive index materials (such as AlGaAs), and its growth temperature can be 550°C to 630°C. In practical applications, the thickness and material selection of the reflector layer can be adjusted according to the target wavelength; the reflection efficiency can be adjusted by the number of layers of the multilayer structure.

[0069] The material of the quantum dot layer may include a mixed material of InAs and GaAs, or a mixed material of InAs and InP, and the growth temperature may be 500° C. to 530° C. In practical applications, self-assembled quantum dot technology may be used to control the size and density of quantum dots by adjusting the growth rate and temperature; and strained layer technology may be used to enhance the optical properties of quantum dots.

[0070] The material of the cap layer may include GaAs or InP, and its thickness may range from 30nm to 300nm. In practical applications, the optical properties of quantum dots can be optimized by adjusting the thickness of the cap layer; at the same time, the use of a multi-layer cap layer structure can further improve device performance.

[0071] After epitaxially growing a buffer layer, a Bragg reflection layer, a quantum dot layer and a cap layer in sequence on a substrate, a silicon dioxide thin film layer can be prepared on the cap layer by a plasma enhanced chemical vapor deposition method.

[0072] Specifically, the deposition temperature, gas flow rate and plasma power can be controlled to ensure the uniformity and quality of the film. In practical applications, the following process parameters can be used when preparing a silicon dioxide film layer: silane flow rate of 12 sccm, N2O flow rate of 480 sccm, nitrogen flow rate of 240 sccm, pressure of 90 Pa, RF power of 50 W, heater temperature of 350 ° C, deposition time of 1 minute to 5 minutes, and sample tilt angle of 5 degrees to 45 degrees during deposition.

[0073] In practical applications, the thickness gradient of the SiO2 thin film layer can be controlled by adjusting the deposition parameters; doping elements can be introduced during the deposition process to improve the properties of the film.

[0074] Subsequently, the quantum dot layer region covered by the silicon dioxide film layer can be subjected to rapid thermal annealing. In practical applications, the quantum dot layer region can be subjected to overall rapid thermal annealing to indirectly achieve the effect of performing rapid thermal annealing on the quantum dot layer region covered by the silicon dioxide film layer.

[0075] In this embodiment, when the material of the quantum dot layer is a mixed material of InAs and GaAs, when the rapid thermal annealing treatment is performed on the quantum dot layer area covered by the silicon dioxide thin film layer, the annealing temperature is 400°C to 900°C, and the annealing time is 10s to 180s; when the material of the quantum dot layer is a mixed material of InAs and InP, when the rapid thermal annealing treatment is performed on the quantum dot layer area covered by the silicon dioxide thin film layer, the annealing temperature is 500°C to 800°C, and the annealing time is 10s to 300s.

[0076] In practical applications, a multi-step annealing process can also be used to optimize the optical properties of quantum dots by gradually increasing and decreasing the temperature; a gas protection environment (such as nitrogen or argon) can be introduced to reduce oxidation during the annealing process.

[0077] Subsequently, a tin-doped indium oxide thin film layer is prepared on the cap layer by a magnetron sputtering method or an electron beam evaporation method.

[0078] In this embodiment, the sputtering power, gas pressure and deposition time can be controlled according to the specific implementation needs to ensure the uniformity and optical properties of the film. Optionally, the doping concentration of the ITO film can be adjusted during the deposition process to optimize its conductivity and optical properties; at the same time, a multi-layer ITO structure can be used to further enhance its performance.

[0079] For example, taking the preparation of tin-doped indium oxide thin film layer by magnetron sputtering method as an example, the following process parameters can be adopted: argon gas flow rate is 60sccm, pressure is 0.3Pa, power supply power is 150W, sputtering time is 60s~300s, and sample tilt angle during deposition is 5 degrees to 45 degrees.

[0080] In this embodiment, the widths of the silicon dioxide film layer and the tin-doped indium oxide film layer are both less than half of the width of the cover layer, and the silicon dioxide film layer and the tin-doped indium oxide film layer are respectively disposed at both ends of the cover layer.

[0081] Optionally, the structure and material selection of the wavelength adjustment layer can be optimized by computer simulation to achieve a wider wavelength adjustment range; nanostructures can be introduced into the wavelength adjustment layer to enhance its optical properties.

[0082] It should be noted that the term "including" and its variations used in the embodiments of the present invention are open inclusions, that is, "including but not limited to". The term "based on" means "based at least in part on". The term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments". The modifications of "one" and "multiple" mentioned in the embodiments of the present invention are illustrative rather than restrictive. Those skilled in the art should understand that unless the context clearly indicates otherwise, it should be understood as "one or more".

[0083] The user information (including but not limited to user device information, user personal information, etc.) and data (including but not limited to data used for analysis, stored data, displayed data, etc.) involved in the embodiments of the present invention are all information and data authorized by the user or fully authorized by all parties, and the collection, use and processing of relevant data must comply with relevant laws, regulations and standards of relevant countries and regions, and provide corresponding operation entrances for users to choose to authorize or refuse.

[0084] The various steps described in the method implementation methods provided in the embodiments of the present invention may be performed in different orders and / or in parallel. In addition, the method implementation methods may include additional steps and / or omit the steps shown. The scope of protection of the present invention is not limited in this respect.

[0085] The term "embodiment" in this specification refers to specific features, structures or characteristics described in conjunction with the embodiment that can be included in at least one embodiment of the present invention. The appearance of this phrase in various places in the specification does not necessarily mean the same embodiment, nor does it mean that it is mutually exclusive with other embodiments and is independent or optional. The various embodiments in this specification are described in a related manner, and the same or similar parts between the various embodiments refer to each other. In particular, for the device, equipment, and system embodiments, since they are basically similar to the method embodiments, the description is relatively simple, and the relevant parts refer to the partial description of the method embodiment.

[0086] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of patent protection. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A monolithic integrated wavelength tunable quantum dot chip, characterized in that: It includes a substrate, a buffer layer, a Bragg reflection layer, a quantum dot layer, a cover layer and a wavelength adjustment layer which are arranged in sequence from bottom to top; Among them, the wavelength adjustment layer includes a silicon dioxide thin film layer and a tin-doped indium oxide thin film layer, the widths of the silicon dioxide thin film layer and the tin-doped indium oxide thin film layer are both less than half of the width of the cover layer, and the silicon dioxide thin film layer and the tin-doped indium oxide thin film layer are respectively arranged at both ends of the cover layer.

2. The thickness of the silicon dioxide thin film layer gradually increases from the inside to the outside, and the thickness of the tin-doped indium oxide thin film layer gradually increases from the inside to the outside.

3. The chip according to claim 2, characterized in that: The thickness of the silicon dioxide film layer is 10nm to 500nm, and the thickness of the tin-doped indium oxide film layer is 10nm to 500nm.

4. The chip according to claim 1, characterized in that: The Bragg reflection layer includes a multi-layer reflection layer group, and the number of the reflection layer group is 8 to 30 layers; The multi-layer reflective layer group includes a first refractive film layer and a second refractive film layer, and the first refractive film layer and the second refractive film layer have different refractive indices; The material of the first refractive thin film layer is GaAs, and the material of the second refractive thin film layer is AlGaAs; Alternatively, the material of the first refractive thin film layer is InP, and the material of the second refractive thin film layer is GaInAsP.

5. The chip according to claim 1, characterized in that: The material of the quantum dot layer is a mixed material of InAs and GaAs, or a mixed material of InAs and InP.

6. The chip according to claim 1, characterized in that: The material of the buffer layer is GaAs or InP, and the thickness is 30nm-200nm; the material of the cap layer is GaAs or InP, and the thickness is 30nm-300nm.

7. A method for preparing a monolithic integrated wavelength tunable quantum dot chip, characterized in that: include: epitaxially growing a buffer layer, a Bragg reflection layer, a quantum dot layer and a cap layer on the substrate in sequence; preparing a silicon dioxide thin film layer on the cap layer by a plasma enhanced chemical vapor deposition method; Performing a rapid thermal annealing process on the quantum dot layer region covered by the silicon dioxide thin film layer; Preparing a tin-doped indium oxide thin film layer on the cap layer by a magnetron sputtering method or an electron beam evaporation method, so as to generate a wavelength adjustment layer of the monolithic integrated wavelength tunable quantum dot chip according to the silicon dioxide thin film layer and the tin-doped indium oxide thin film layer; The widths of the silicon dioxide film layer and the tin-doped indium oxide film layer are both less than half of the width of the cover layer, and the silicon dioxide film layer and the tin-doped indium oxide film layer are respectively arranged at two ends of the cover layer.

8. The method according to claim 7, characterized in that The thickness of the silicon dioxide film layer gradually increases from the inside to the outside, and the thickness of the tin-doped indium oxide film layer gradually increases from the inside to the outside.

9. The method according to claim 7, characterized in that: The material of the quantum dot layer is a mixed material of InAs and GaAs, or a mixed material of InAs and InP; Wherein, when the material of the quantum dot layer is a mixed material of InAs and GaAs, when the quantum dot layer region covered by the silicon dioxide thin film layer is subjected to rapid thermal annealing, the annealing temperature is 400° C. to 900° C., and the annealing time is 10s to 180s; In the case where the material of the quantum dot layer is a mixed material of InAs and InP, when the quantum dot layer region covered by the silicon dioxide thin film layer is subjected to rapid thermal annealing, the annealing temperature is 500° C. to 800° C., and the annealing time is 10s to 300s.