Positive plate and preparation method thereof

By designing the active layer, reaction balance layer and ion transport layer with gradient pore structure in the positive electrode sheet of the lithium-ion battery, the polarization problem caused by the high conductivity of the positive electrode sheet of the existing battery is solved, and the fast charging performance of the battery is improved.

CN118919644APending Publication Date: 2024-11-08QILU ZHONGKE ELECTRICAL ADVANCED ELECTROMAGNETIC DRIVE TECH RES INST +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192729.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The positive electrode sheet of existing lithium-ion batteries has a high conductivity, which leads to severe polarization during charging and discharging, affecting battery performance.

Method used

A positive electrode sheet structure is designed, including an active layer, a reaction equilibrium layer and an ion transport layer arranged in sequence, with the porosity increasing in a step-like manner to form a gradient distribution structure to improve the wettability of the electrolyte and reduce the polarization of the battery.

Benefits of technology

Through the gradient pore structure, the battery's electrolyte wetting and conductivity are improved, the polarization during the charging and discharging process is reduced, and the battery's fast charging rate performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015529530000211
    Figure BDA0005015529530000211
  • Figure HDA0005015529550000011
    Figure HDA0005015529550000011
Patent Text Reader

Abstract

The invention relates to the technical field of pole pieces, particularly provides a positive pole piece and a preparation method thereof, and aims to solve the problems that an existing pole piece is relatively high in conductivity, and polarization is relatively serious in a battery charging and discharging process. In order to achieve the purpose, the positive plate comprises an active layer, a reaction balance layer and an ion transmission layer which are sequentially arranged, the porosity of the active layer, the porosity of the reaction balance layer and the porosity of the ion transmission layer are sequentially increased, namely gradient change is presented, and therefore sufficient infiltration of an electrolyte on a positive material layer is achieved, and the electrolyte wettability of the pole plate is improved; the active layer, the reaction balance layer and the ion transport layer form a gradient distribution structure on two sides of the electrode, so that the conductivity of the pole piece is reduced, and the polarization of the battery in the charge-discharge process is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of pole pieces, and specifically provides a positive pole piece and a preparation method thereof. Background Art

[0002] With the rapid development of electric vehicles and consumer electronics, it is crucial to develop batteries with high energy density and fast charging capabilities. The energy density of lithium-ion batteries (LIBs) with embedded cathodes, liquid electrolytes, and graphite anodes has reached its limit, so it is necessary to explore new electrode materials with higher specific capacity or construct advanced electrode structures with higher active material ratios and excellent electrochemical properties to improve battery performance.

[0003] Charge transport in batteries includes the transport of metal ions in the electrolyte, charge transport at the electrolyte / electrode interface, solid-state diffusion inside the electrode, and the transport of electrons along the conductive pathway. At low current density, the charge transfer process is dominated by electrochemical kinetics. As the current density increases, ion diffusion in the electrolyte plays a major role. At present, due to the excessive pursuit of battery energy density, the demand for high-area density battery electrodes continues to increase. However, at a certain charge rate, the reaction polarization increases in direct proportion to the increase in electrode thickness due to the extension of the diffusion path inside the electrode. Therefore, it is crucial to design electrodes with reasonable structures to regulate charge transport.

[0004] Therefore, there is an urgent need for a positive electrode sheet and a preparation method thereof to solve the above technical problems. Summary of the invention

[0005] The present invention aims to solve the above technical problem, that is, to solve the problem that the existing pole piece has high conductivity and the polarization is serious during the battery charging and discharging process.

[0006] In a first aspect, the present invention provides a positive electrode sheet, which includes an active layer, a reaction balance layer and an ion transport layer arranged in sequence.

[0007] The porosities of the active layer, the reaction balance layer and the ion transport layer increase in sequence.

[0008] In the specific embodiment of the above positive electrode sheet, the porosity of the active layer is 5-15%; and / or

[0009] The porosity of the reaction balance layer is 15-25%; and / or

[0010] The porosity of the ion transport layer is 25-35%; and / or

[0011] The thickness of the carbon-based layer is 1-10 um; preferably, the thickness of the carbon-based layer is 2-5 um;

[0012] The positive electrode sheet further includes a carbon-based layer, and the active layer is arranged on the carbon-based layer.

[0013] In a second aspect, the present invention provides a method for preparing the positive electrode sheet as described above, characterized in that it comprises the following steps:

[0014] Preparing a first positive electrode slurry, and using the first positive electrode slurry to prepare an active layer;

[0015] preparing a second positive electrode slurry, and using the second positive electrode slurry to form a reaction balance layer on the surface of the active layer;

[0016] A third positive electrode slurry is prepared, and the third positive electrode slurry is used to form an ion transport layer on the surface of the reaction balance layer.

[0017] In a specific embodiment of the above-mentioned positive electrode sheet preparation method, the first positive electrode slurry comprises component S1, component S2 and nitrogen methyl pyrrolidone solvent; and / or

[0018] The component S1 comprises a conductive agent and a binder; and / or

[0019] The conductive agent and the binder are ball-milled in a ball mill for a second preset time to obtain component S1; and / or

[0020] The conductive agent comprises at least one of carbon nanotubes, conductive carbon black, graphene, carbon nanotubes, conductive graphite and carbon fiber; and / or

[0021] The particle size of the conductive agent is 15nm-5000nm; and / or

[0022] The particle size of the binder is 3000-6000nm; and / or

[0023] The particle size of the component S1 is 1000-5000 nm; and / or

[0024] The component S2 includes lithium iron phosphate; and / or

[0025] The particle size of the component S2 is 1000-3000 nm.

[0026] In the specific embodiment of the above-mentioned positive electrode sheet preparation method, the density of component S1 is ρ S1 , the density of the component S2 is ρ S2 ; Among them, 0.92<ρ S2 / ρ S1 <2.24;

[0027] 2.8mg / cm 3 <ρ S2 <3.0mg / cm3 ;

[0028] 1.25mg / cm 3 <ρ S1 <3.26mg / cm 3 .

[0029] In a specific embodiment of the above-mentioned positive electrode sheet preparation method, the second positive electrode slurry includes component S3, component S4 and the nitrogen methyl pyrrolidone solvent; and / or

[0030] The component S3 includes the conductive agent and the binder; and / or

[0031] The component S4 includes lithium iron phosphate; and / or

[0032] The particle size of the component S4 is 4000-10000 nm.

[0033] In the specific embodiment of the above-mentioned positive electrode sheet preparation method, the density of component S3 is p S3 , the density of the component S4 is ρ S4 ; Among them, 2.24<ρ S4 / ρ S3 <2.98; 3.1mg / cm 3 <ρ S4 <3.3mg / cm 3 ,1.04mg / cm 3 <ρ S3 <1.47mg / cm 3 ;.

[0034] In a specific embodiment of the above-mentioned positive electrode sheet preparation method, the third positive electrode slurry includes component S5, component S6 and the nitrogen methyl pyrrolidone solvent; and / or

[0035] The component S5 includes the conductive agent and the binder; and / or

[0036] The component S6 includes lithium iron phosphate; and / or

[0037] The particle size of the component S6 is 11-20 μm.

[0038] In the specific embodiment of the above-mentioned positive electrode sheet preparation method, the density of component S5 is p S5 , the density of the component S6 is ρ S6 ; Among them, 4.34<ρ S6 / ρ S5 <6.53;

[0039] 3.4mg / cm 3 <ρ S6<3.6mg / cm 3 ;

[0040] 0.52mg / cm 3 <ρ S5 <0.82mg / cm 3 .

[0041] In a specific embodiment of the above-mentioned positive electrode sheet preparation method, before preparing the carbon-based layer, a fourth positive electrode slurry is prepared, and the fourth positive electrode slurry is used to prepare the carbon-based layer;

[0042] The fourth positive electrode slurry includes the conductive agent, the binder, and the nitrogen methyl pyrrolidone solvent.

[0043] When the above technical solution is adopted, the positive electrode sheet of the present invention includes an active layer, a reaction balance layer and an ion transport layer arranged in sequence. The porosity of the active layer, the reaction balance layer and the ion transport layer increases in sequence, that is, they show a gradient change, thereby achieving sufficient infiltration of the electrolyte into the positive electrode material layer to improve the electrolyte wettability of the electrode sheet. The active layer, the reaction balance layer and the ion transport layer form a gradient distribution structure on both sides of the electrode, so that the conductivity of the electrode sheet is reduced, thereby reducing the polarization of the battery charging and discharging process. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings, in which:

[0045] Figure 1 It is a schematic diagram of the structure of the positive electrode sheet provided by the present invention.

[0046] List of reference numerals:

[0047] 1. Current collector; 2. Carbon-based layer; 3. Active layer; 4. Reaction balance layer; 5. Ion transport layer. DETAILED DESCRIPTION

[0048] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0049] It should be noted that in the description of the present invention, the terms "upper", "lower", "left", "right", "inner", "outer" and the like indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings, which are only for the convenience of description, and do not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.

[0050] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installation", "setting", and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, an indirect connection through an intermediate medium, or the internal connection of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0051] like Figure 1 As shown, the present invention discloses a positive electrode sheet, which includes an active layer 3, a reaction balance layer 4 and an ion transport layer 5 arranged in sequence, and the porosity of the active layer 3, the reaction balance layer 4 and the ion transport layer 5 increases in sequence; specifically, they gradually increase in a step-like manner. The active layer 3 is arranged on a carbon-based layer 2, and the carbon-based layer 2 is arranged on a current collector 1. The active layer 3 and the carbon-based layer 2 together form an electron transport layer.

[0052] The porosity of the active layer 3 is 5-15%, the porosity of the reaction balance layer 4 is 15-25%, and the porosity of the ion transport layer 5 is 25-35%.

[0053] The thickness of the carbon-based layer 2 is 1-10 um; the thickness of the carbon-based layer 2 is preferably 2-5 um.

[0054] The present invention also discloses a method for preparing the positive electrode sheet, which comprises the following steps:

[0055] Step S1, preparing a first positive electrode slurry and forming an active layer 3;

[0056] Step S2, preparing a second positive electrode slurry and forming a reaction balance layer 4 on the surface of the active layer 3;

[0057] Step S3 , preparing a third positive electrode slurry, and forming an ion transport layer 5 on the surface of the reaction balance layer 4 .

[0058] The preparation method also includes correcting S0; step S0, preparing a fourth positive electrode slurry, and forming a carbon-based layer 2 on the surface of the current collector 1; specifically, coating the fourth positive electrode slurry on the surface of the current collector 1, and then drying and rolling to obtain the carbon-based layer 2. The drying and rolling temperature is 90° C. to 120° C. The current collector 1 is specifically aluminum foil, copper foil or metal alloy foil.

[0059] The fourth positive electrode slurry includes the conductive agent, the binder and the nitrogen methyl pyrrolidone solvent. The conductive agent in the conductive slurry includes at least one of carbon nanotubes, conductive carbon black, graphene, carbon nanotubes, conductive graphite and carbon fiber. The binder includes at least one of PVP (polyvinyl pyrrolidone) and PVDF (polyvinylidene fluoride), polyacrylic acid, polyvinyl alcohol, carboxymethyl cellulose, hydroxyethyl cellulose, styrene-butadiene rubber and polytetrafluoroethylene.

[0060] Specifically, a conductive agent and a binder are added to a solvent of nitrogen methyl pyrrolidone (NMP) in a certain proportion, and stirred for a first preset time in a vacuum environment to obtain a fourth positive electrode conductive slurry with a certain viscosity; wherein the first preset time is preferably 3 hours. Long-term stirring can provide different shear forces to reduce its viscosity and make it mixed evenly, thereby ensuring the stable performance of the carbon-based layer 2.

[0061] It should be noted that the first preset time length is 3 hours in this embodiment, but this is not a limitation of the present invention. Without departing from the principle of the present invention, in other embodiments, those skilled in the art may also select it to be 4 hours or 5 hours, etc., which is specifically determined according to the required characteristics of the fourth positive electrode slurry. This does not deviate from the basic principles of the present invention and will fall within the scope of protection of the present invention.

[0062] The step S1 specifically includes coating the first positive electrode slurry on the surface of the carbon-based layer 2, and then drying and rolling to obtain the active layer 3. The drying and rolling temperature is 90°C to 120°C.

[0063] The step S1 specifically includes coating the second positive electrode slurry on the surface of the active layer 3, and then drying and rolling to obtain the reaction balance layer 4. The drying and rolling temperature is 90°C to 120°C.

[0064] The step S1 specifically includes coating the third positive electrode slurry on the surface of the reaction balance layer 4, and then drying and rolling to obtain the ion transport layer 5. The drying and rolling temperature is 90°C to 120°C.

[0065] Specifically, the first positive electrode slurry includes component S1, component S2 and nitrogen methyl pyrrolidone solvent.

[0066] Specifically, component S1 includes a conductive agent and a binder; the conductive agent and the binder are ball-milled in a ball mill for a second preset time to obtain component S1; wherein the second preset time is preferably 4 hours.

[0067] It should be noted that the second preset time length is 4 hours in this embodiment, but this is not a limitation of the present invention. Without departing from the principle of the present invention, in other embodiments, those skilled in the art may also select it to be 5 hours or 3 hours, etc., specifically determined according to the required characteristics of component S1 (specifically according to the particle size of component S1). This does not deviate from the basic principles of the present invention and will fall within the scope of protection of the present invention.

[0068] The conductive agent includes at least one of carbon nanotubes, conductive carbon black, graphene, carbon nanotubes, conductive graphite and carbon fiber; and the particle size of the conductive agent is 15nm-5000nm.

[0069] The binder includes at least one of PVP (polyvinyl pyrrolidone), PVDF (polyvinylidene fluoride), polyacrylic acid, polyvinyl alcohol, carboxymethyl cellulose, hydroxyethyl cellulose, styrene-butadiene rubber and polytetrafluoroethylene. The particle size of the binder is 3000-6000nm.

[0070] The particle size of component S1 is 1000-5000nm;

[0071] Component S2 includes lithium iron phosphate; its particle size is specifically 1000-3000 nm.

[0072] The density of component S1 is ρ S1 , the density of component S2 is ρ S2 ; Among them, 0.92<ρ S2 / ρ S1 <2.24;2.8mg / cm 3 <ρ S2 <3.0mg / cm 3 ; 1.25mg / cm 3 <ρ S1 <3.26mg / cm 3 .

[0073] For component S1, the particle size of component S1 can be changed by adjusting the ratio of each component of the conductive agent and each component of the binder of component S1, controlling the ball milling time and performing screening, thereby changing the density of component S1. For component S2, the particle size of component S2 can be changed by selecting lithium iron phosphate prepared by different synthesis methods, controlling the ball milling time and performing screening, thereby changing the density of component S2.

[0074] The second positive electrode slurry includes component S3, component S4 and nitrogen methyl pyrrolidone solvent; component S3 includes a conductive agent and a binder; the conductive agent and the binder are ball milled in a ball mill for a third preset time to obtain component S3; wherein the third preset time is preferably 3.5h.

[0075] It should be noted that, although the third preset time length in this embodiment is 3.5h, this is not a limitation of the present invention. Without departing from the principle of the present invention, in other embodiments, those skilled in the art may also select it to be 5h or 3h, etc., specifically determined according to the required characteristics of component S3 (specifically according to the particle size of component S3). This does not deviate from the basic principles of the present invention and will fall within the scope of protection of the present invention.

[0076] The conductive agent includes at least one of carbon nanotubes, conductive carbon black, graphene, carbon nanotubes, conductive graphite and carbon fiber; and the particle size of the conductive agent is 15nm-5000nm.

[0077] The binder includes at least one of PVP (polyvinyl pyrrolidone) and PVDF (polyvinylidene fluoride), polyacrylic acid, polyvinyl alcohol, carboxymethyl cellulose, hydroxyethyl cellulose, styrene-butadiene rubber, and polytetrafluoroethylene. The particle size of the binder is 3000-6000nm. The particle size of component S3 is 1000-5000nm.

[0078] Component S4 includes lithium iron phosphate, and its particle size is 4000-10000 nm.

[0079] The density of component S3 is ρ S3 , the density of component S4 is ρ S4 ; Among them, 2.24<ρ S4 / ρ S3 <2.98; 3.1mg / cm 3 <ρ S4 <3.3mg / cm 3 ,1.04mg / cm 3 <ρ S3 <1.47mg / cm 3 .

[0080] For component S3, the particle size of component S3 can be changed by adjusting the ratio of each component of the conductive agent and each component of the binder of component S3, controlling the ball milling time and performing screening, thereby changing the density of component S3. For component S4, the particle size of component S4 can be changed by selecting lithium iron phosphate prepared by different synthesis methods, controlling the ball milling time and performing screening, thereby changing the density of component S4.

[0081] The third positive electrode slurry includes component S5, component S6 and nitrogen methyl pyrrolidone solvent; component S5 includes a conductive agent and a binder; the conductive agent and the binder are ball-milled in a ball mill for a fourth preset time to obtain component S5; wherein the fourth preset time is preferably 3h.

[0082] It should be noted that, although the third preset time length is 3 hours in the present embodiment, this is not a limitation of the present invention. Without departing from the principle of the present invention, in other embodiments, those skilled in the art may also select it to be 5 hours or 3 hours, etc., specifically determined according to the required characteristics of component S5 (specifically according to the particle size of component S5). This does not deviate from the basic principles of the present invention and will fall within the scope of protection of the present invention.

[0083] The conductive agent includes at least one of carbon nanotubes, conductive carbon black, graphene, carbon nanotubes, conductive graphite and carbon fiber; and the particle size of the conductive agent is 15nm-5000nm.

[0084] The binder includes at least one of PVP (polyvinyl pyrrolidone) and PVDF (polyvinylidene fluoride), polyacrylic acid, polyvinyl alcohol, carboxymethyl cellulose, hydroxyethyl cellulose, styrene-butadiene rubber, and polytetrafluoroethylene. The particle size of the binder is 3000-6000nm. The particle size of component S5 is 1000-5000nm. Component S6 includes lithium iron phosphate; its particle size is 11-20μm.

[0085] The density of component S5 is ρ S6 , the density of component S6 is ρ S6 ; Among them, 4.34<ρ S6 / ρ S5 <6.53;3.4mg / cm 3 <ρ S6 <3.6mg / cm 3 ; 0.52mg / cm 3 <ρ S5 <0.82mg / cm 3 .

[0086] For component S5, the particle size of component S5 can be changed by adjusting the ratio of each component of the conductive agent and each component of the binder of component S5, controlling the ball milling time and performing screening, thereby changing the density of component S5. For component S6, the particle size of component S6 can be changed by selecting lithium iron phosphate prepared by different synthesis methods, controlling the ball milling time and performing screening, thereby changing the density of component S6.

[0087] The positive electrode sheet and the preparation method thereof of the present invention will be described in detail below with reference to several embodiments and comparative examples.

[0088] Example 1

[0089] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After being stirred evenly by a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained; that is, the fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and a carbon-based layer 2 with a coating thickness of 2μm is obtained after drying and rolling at 120°C.

[0090] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), methyl cellulose and styrene-butadiene rubber.

[0091] The carbon fiber, the conductive graphite and the conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain a conductive agent;

[0092] The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, the particle size of component S1 is 3000nm, and the particle size of component S1 is 3000nm. S1 1.83 mg / cm 3 .

[0093] The particle size is 2000nm, ρ S2 2.9 mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0094] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0095] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber.

[0096] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.75:1.25 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 1:1 to obtain component S3, with a particle size (D50) of 800 nm and a particle size of ρ S3 1.2mg / cm 3 . Take the particle size as 6um, ρ S43.2mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained.

[0097] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0098] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber.

[0099] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.25:1.75 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 3:2 to obtain component S5, with a particle size (D50) of 200 nm and a particle size of ρ S5 0.63mg / cm 3 ; Take the particle size as 15nm, ρ S6 3.5mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0100] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and roller pressing, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 30%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0101] Embodiment 2:

[0102] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained, that is, the fourth positive electrode slurry is obtained. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 3μm is obtained;

[0103] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), methyl cellulose and styrene-butadiene rubber.

[0104] The carbon fiber, the conductive graphite and the conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain a conductive agent;

[0105] The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, the particle size of component S1 is 3000nm, and the particle size of component S1 is 3000nm. S1 1.83 mg / cm 3 .

[0106] The particle size is 2000nm, ρ S2 2.9 mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0107] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0108] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber.

[0109] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.75:1.25 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 1:1 to obtain component S3, with a particle size (D50) of 800 nm and a particle size of ρ S3 1.2mg / cm 3 . Take the particle size as 6um, ρ S4 3.2mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained.

[0110] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0111] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber.

[0112] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.25:1.75 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 3:2 to obtain component S5, with a particle size (D50) of 200 nm and a particle size of ρ S5 0.63mg / cm 3 ; Take the particle size as 15nm, ρ S6 3.5mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0113] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and roller pressing, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 30%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0114] Embodiment 3:

[0115] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained, that is, the fourth positive electrode slurry is obtained. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 5μm is obtained;

[0116] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), methyl cellulose and styrene-butadiene rubber.

[0117] The carbon fiber, the conductive graphite and the conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain a conductive agent;

[0118] The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, the particle size of component S1 is 3000nm, and the particle size of component S1 is 3000nm. S1 1.83 mg / cm 3 .

[0119] The particle size is 2000nm, ρ S2 2.9 mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0120] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0121] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber.

[0122] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.75:1.25 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 1:1 to obtain component S3, with a particle size (D50) of 800 nm and a particle size of ρ S3 1.2mg / cm 3 . Take the particle size as 6um, ρ S4 3.2mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained.

[0123] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0124] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber.

[0125] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.25:1.75 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 3:2 to obtain component S5, with a particle size (D50) of 200 nm and a particle size of ρ S5 0.63mg / cm 3 ; Take the particle size as 15nm, ρ S6 3.5mg / cm 3Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0126] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and roller pressing, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 30%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0127] Embodiment 4:

[0128] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0129] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, the particle size (D50) of S1 is 1200nm, and the particle size (D50) of S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0130] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%. The drying and rolling temperature is 100 degrees Celsius.

[0131] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0132] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.25:1.75 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 1:1 to obtain component S3, with a particle size (D50) of 800 nm and a particle size of ρ S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained.

[0133] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0134] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0135] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:1:1, and the mixed conductive agent and binder were mixed in a mass ratio of 3:2 to obtain component S5, the particle size (D50) of S5 was 100 nm, and the particle size (D50) of S5 was 100 nm. S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0136] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0137] Embodiment 5:

[0138] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained, that is, the fourth positive electrode slurry is obtained. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and a carbon-based layer 2 with a coating thickness of 2μm is obtained after drying and rolling at 120°C.

[0139] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0140] Carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 0.5:2:0.5 to obtain a conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1. The particle size (D50) of component S1 is 3000nm, and the particle size (D50) of component S1 is 3000nm. S1 3.26mg / cm 3 . Take the particle size as 3000nm, ρ S2 3.0mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0141] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 15%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0142] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, and the particle size (D50) of component S3 is 1500nm ... S3 1.47 mg / cm 3 ; Take the particle size as 10um, ρ S4 3.3mg / cm 3Component S4 (lithium iron phosphate) and component S1 are mixed at a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained.

[0143] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 25%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0144] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 400nm, and the particle size (D50) of component S5 is 1 ... S5 0.82mg / cm 3 ; Take the particle size as 20nm, ρ S6 3.6mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0145] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 35%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0146] Embodiment 6:

[0147] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0148] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0149] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.8:1.2 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 2:1 to obtain component S1. The particle size (D50) of component S1 was 1200nm, and the particle size (D50) of component S1 was 1200nm. S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0150] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 10%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0151] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0152] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.25:1.75 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 1:1 to obtain component S3, with a particle size (D50) of 800 nm and a particle size of ρ S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0153] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0154] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0155] The carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:1:1 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 3:2 to obtain component S5. The particle size (D50) of component S5 was 100 nm. S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S6 are mixed at a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000 mPa·S%, that is, a third positive electrode slurry is obtained.

[0156] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0157] Embodiment 7:

[0158] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0159] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, the particle size (D50) of S1 is 1200nm, and the particle size (D50) of S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0160] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 15%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0161] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0162] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.25:1.75 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 1:1 to obtain component S3, with a particle size (D50) of 800 nm and a particle size of ρ S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0163] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0164] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0165] Carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:1:1 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 3:2 to obtain component S5, S2 with a particle size (D50) of 100 nm, and ρ S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0166] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0167] Embodiment 8:

[0168] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0169] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0170] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0171] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0172] Carbon fiber, conductive graphite, and conductive carbon black are mixed and milled in a ratio of 1:0.25:1.75 to obtain a conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, and the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0173] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 20%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0174] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0175] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0176] Embodiment 9:

[0177] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0178] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the conductive fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0179] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0180] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0181] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 25%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0182] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:1:1, and the mixed conductive agent and binder are mixed in a mass ratio of 3:2 to obtain component S5, the particle size (D50) of component S5 is 100 nm, and the particle size (D50) of component S5 is 100 nm. S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0183] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0184] Embodiment 10:

[0185] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0186] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0187] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0188] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber;

[0189] The carbon fiber, conductive graphite and conductive carbon black were mixed and milled in a ratio of 1:0.25:1.75 to obtain a conductive agent. The conductive agent and the binder were mixed in a mass ratio of 1:1 to obtain component S3. The particle size (D50) of component S3 was 800 nm, and the particle size (D50) of component S3 was 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0190] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 20%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0191] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0192] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 30%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0193] Embodiment 11:

[0194] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0195] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber. The carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0196] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0197] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0198] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 20%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0199] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:1:1, and the mixed conductive agent and binder are mixed in a mass ratio of 3:2 to obtain component S5, the particle size (D50) of S5 is 100nm, and the particle size (D50) of S5 is 100nm. S5 0.52mg / cm 3 ;

[0200] The particle size is 11 nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0201] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 35%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0202] Comparative Example 1:

[0203] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and a carbon-based layer 2 with a coating thickness of 2μm is obtained after drying and rolling at 120°C.

[0204] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0205] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0206] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1.S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0207] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0208] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The mixed conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S1, and the particle size (D50) of component S1 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S6 are mixed at a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000 mPa·S%, that is, a third positive electrode slurry is obtained.

[0209] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0210] Comparative Example 2:

[0211] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After being stirred evenly by a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and a carbon-based layer 2 with a coating thickness of 2μm is obtained after drying and rolling at 120°C.

[0212] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0213] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 having a porosity of 20%; and a drying and rolling temperature of 100 degrees Celsius.

[0214] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0215] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 20%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0216] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; conductive fiber, conductive graphite and conductive carbon black of different particle sizes are mixed and ball-milled in a ratio of 1:1:1 to obtain a conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0217] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 20%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0218] Comparative Example 3:

[0219] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0220] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0221] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 30%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0222] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber. The carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, and the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0223] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 30%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0224] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0225] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 30%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0226] Comparative Example 4:

[0227] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0228] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0229] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 2%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0230] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber. The carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, and the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S31.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0231] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0232] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0233] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0234] Comparative Example 5:

[0235] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0236] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0237] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 20%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0238] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber. The carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, and the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0239] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0240] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0241] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0242] Comparative Example 6:

[0243] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0244] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0245] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0246] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber. The carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, and the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0247] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 10%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0248] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0249] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0250] Comparative Example 7:

[0251] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0252] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0253] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0254] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber. The carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, and the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S31.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0255] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 30%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0256] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0257] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0258] Comparative Example 8:

[0259] The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0260] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3 Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0261] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 2%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0262] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber. The carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, and the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0263] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0264] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0265] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 26%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0266] Comparative Example 9: The conductive agent of the fourth positive electrode slurry includes graphene, single-arm carbon nanotubes and conductive carbon black, and the binder of the fourth positive electrode slurry includes PVP and PVDF. Graphene, single-arm carbon nanotubes, conductive carbon black, PVP, and PVDF are mixed in a mass ratio of 1.5:0.5:0.5:1:1, and nitrogen methyl pyrrolidone is added as a solvent to prepare a slurry with a solid content of 4wt%. After stirring evenly with a vacuum mixer, a conductive slurry with a viscosity of 10000mPa·S is obtained to obtain a fourth positive electrode slurry. The fourth positive electrode slurry is evenly coated on one surface of an aluminum foil with a thickness of 12μm, and after drying and rolling at 120°C, a carbon-based layer 2 with a coating thickness of 2μm is obtained;

[0267] The conductive agent of the first positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the first positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and milled in a ratio of 1:0.8:1.2 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 2:1 to obtain component S1, and the particle size (D50) of component S1 is 1200nm, and the particle size (D50) of component S1 is ρ S1 1.25mg / cm 3 . Take the particle size as 1000nm, ρ S2 2.8mg / cm 3Component S2 (lithium iron phosphate) and component S1 are mixed in a mass ratio of 85:15, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 20000 mPa·S, that is, a first positive electrode slurry is obtained.

[0268] The first positive electrode slurry is coated on the carbon-based layer 2, and after drying and rolling, the compaction density is 2.4 mg / cm 3 , an active layer 3 with a porosity of 5%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0269] The conductive agent of the second positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the second positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber. The carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:0.25:1.75 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 1:1 to obtain component S3, and the particle size (D50) of component S3 is 800nm, and the particle size (D50) of component S3 is 1:1. S3 1.04mg / cm 3 ; Take the particle size as 11um, ρ S3 3.1mg / cm 3 Component S4 (lithium iron phosphate) and component S3 are mixed in a mass ratio of 90:10, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 10000 mPa·S, that is, a second positive electrode slurry is obtained;

[0270] The second positive electrode slurry was coated on the active layer 3, and after drying and roller pressing, the compaction density was 2.2 mg / cm 3 , a reaction balance layer 4 with a porosity of 16%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0271] The conductive agent of the third positive electrode slurry includes carbon fiber, conductive graphite and conductive carbon black; the binder of the third positive electrode slurry includes PVDF (polyvinylidene fluoride), carboxymethyl cellulose and styrene-butadiene rubber; the carbon fiber, conductive graphite and conductive carbon black are mixed and ball-milled in a ratio of 1:1:1 to obtain the conductive agent. The conductive agent and the binder are mixed in a mass ratio of 3:2 to obtain component S5, and the particle size (D50) of component S5 is 100nm ... S5 0.52mg / cm 3 ; Take the particle size as 11nm, ρ S6 3.4 mg / cm 3 Component S6 (lithium iron phosphate) and component S5 are mixed in a mass ratio of 95:5, and nitrogen methyl pyrrolidone is added as a solvent to prepare a positive electrode slurry with a viscosity of 6000mPa·S%, that is, a third positive electrode slurry is obtained.

[0272] The third positive electrode slurry is coated on the reaction balance layer 4, and after drying and rolling, a compaction density of 2.0 mg / cm 3 , an ion transport layer 5 with a porosity of 40%; wherein the drying and rolling temperature is 100 degrees Celsius.

[0273] Battery Assembly:

[0274] The prepared positive electrode sheet, separator, and negative electrode sheet are placed in order, the electrode assembly is placed in an aluminum-plastic film packaging bag, and the water is removed at 80°C, the electrolyte is injected, and the lithium-ion battery is obtained through vacuum packaging, standing, formation, degassing, trimming, etc. The formation upper limit voltage is 3.65V, the formation temperature is 70°C, and the formation standing time is 2h.

[0275] Test method:

[0276] The battery was charged to 3.65V at 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharged to 2.5V at 1C constant current for 3 cycles;

[0277] The battery was charged to 3.65V at 10C constant current and constant voltage, with a cut-off current of 0.05C, and then discharged to 2.5V at 1C constant current for 500 cycles;

[0278] Test results:

[0279] Table 1

[0280] As can be seen from Table 1, by comparing Examples 1-3, it is found that the lithium iron phosphate battery with a carbon layer thickness of 2 mm has the best initial discharge specific capacity, 10C discharge specific capacity and capacity retention rate after 500 cycles at a 10C charging rate, that is, the smaller the thickness of the carbon-based layer, the better the performance of the battery.

[0281] By comparing Example 4, Example 6, Example 7, Comparative Example 4 and Comparative Example 5, it can be seen that the porosity of the active layer is excellent between 5% and 15%, and as the porosity decreases within this range, its performance improves; however, when the porosity of the active layer is less than 5% and greater than 15%, its battery performance decreases significantly. Therefore, the porosity of the active layer is preferably 5% to 15%, and the most preferred porosity of the active layer is 5%.

[0282] By comparing Example 4, Example 8, Example 9, Comparative Example 6 and Comparative Example 7, it can be seen that the battery performance is better when the porosity of the reaction balance layer is between 15% and 25%, and the battery performance is optimal when the porosity of the reaction balance layer is 20%, that is, the performance is optimal at the intermediate value. When the porosity is less than 15% and greater than 25%, the battery performance is greatly reduced. Therefore, it is preferred that the porosity of the reaction balance layer is 15% to 25%, and most preferably 20%.

[0283] By comparing Example 8, Example 10, Example 11, Comparative Example 8 and Comparative Example 9, it can be seen that the battery performance is better when the porosity of the ion transport layer is 25%-35%, and the battery performance is optimal when the porosity of the ion transport layer is 30%, that is, the performance is optimal at the intermediate value. When the porosity is less than 25% and greater than 35%, the battery performance is greatly reduced. Therefore, it is preferred that the porosity of the ion transport layer is 25% to 35%, and most preferably 30%.

[0284] By comparing Example 1 with Comparative Example 1, comparing Example 8, Example 11 with Comparative Example 2, and comparing Example 10 with Comparative Example 3, it can be found that increasing the porosity of the active layer, the porosity of the reaction equilibrium layer, and the porosity of the ion transport layer in a step-like manner can exhibit better high-rate fast charging performance, indicating that the gradient pore electrode structure design has a practical effect on improving the fast charging rate performance of lithium iron phosphate batteries.

[0285] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. A positive electrode sheet, characterized in that: It includes an active layer, a reaction balance layer and an ion transport layer arranged in sequence. The porosities of the active layer, the reaction balance layer and the ion transport layer increase in sequence.

2. The positive electrode sheet according to claim 1, characterized in that: The porosity of the active layer is 5-15%; and / or The porosity of the reaction balance layer is 15-25%; and / or The porosity of the ion transport layer is 25-35%; and / or The thickness of the carbon-based layer is 1-10 um; preferably, the thickness of the carbon-based layer is 2-5 um; The positive electrode sheet further includes a carbon-based layer, and the active layer is arranged on the carbon-based layer.

3. A method for preparing a positive electrode sheet as claimed in claim 1 or 2, characterized in that: It includes the following steps: Preparing a first positive electrode slurry, and using the first positive electrode slurry to prepare an active layer; preparing a second positive electrode slurry, and using the second positive electrode slurry to form a reaction balance layer on the surface of the active layer; A third positive electrode slurry is prepared, and the third positive electrode slurry is used to form an ion transport layer on the surface of the reaction balance layer.

4. The preparation method according to claim 3, characterized in that: The first positive electrode slurry comprises component S1, component S2 and nitrogen methyl pyrrolidone solvent; and / or The component S1 comprises a conductive agent and a binder; and / or The conductive agent and the binder are ball-milled in a ball mill for a second preset time to obtain component S1; and / or The conductive agent comprises at least one of carbon nanotubes, conductive carbon black, graphene, carbon nanotubes, conductive graphite and carbon fiber; and / or The particle size of the conductive agent is 15nm-5000nm; and / or The particle size of the binder is 3000-6000nm; and / or The particle size of the component S1 is 1000-5000 nm; and / or The component S2 includes lithium iron phosphate; and / or The particle size of the component S2 is 1000-3000 nm.

5. The preparation method according to claim 4, characterized in that: The density of component S1 is ρ S1 , the density of the component S2 is ρ S2 ; Among them, 0.92<ρ S2 / ρ S1 <2.24; 2.8mg / cm 3 <ρ S2 <3.0mg / cm 3 ; 1.25mg / cm 3 <ρ S1 <3.26mg / cm 3 。 6. The preparation method according to claim 4, characterized in that: The second positive electrode slurry comprises component S3, component S4 and the nitrogen methyl pyrrolidone solvent; and / or The component S3 includes the conductive agent and the binder; and / or The component S4 includes lithium iron phosphate; and / or The particle size of the component S4 is 4000-10000 nm.

7. The preparation method according to claim 6, characterized in that: The density of component S3 is ρ S3 , the density of the component S4 is ρ S4 ; Among them, 2.24<ρ S4 / ρ S3 <2.98; 3.1mg / cm 3 <ρ S4 <3.3mg / cm 3 ,1.04mg / cm 3 <ρ S3 <1.47mg / cm 3 ;.

8. The preparation method according to claim 4, characterized in that: The third positive electrode slurry comprises component S5, component S6 and the nitrogen methyl pyrrolidone solvent; and / or The component S5 includes the conductive agent and the binder; and / or The component S6 includes lithium iron phosphate; and / or The particle size of the component S6 is 11-20 μm.

9. The preparation method according to claim 8, characterized in that: The density of component S5 is ρ S5 , the density of the component S6 is ρ S6 ; Among them, 4.34<ρ S6 / ρ S5 <6.53; 3.4mg / cm 3 <ρ S6 <3.6mg / cm 3 ; 0.52mg / cm 3 <ρ S5 <0.82mg / cm 3 。 10. The preparation method according to claim 4, characterized in that: Before preparing the carbon-based layer, preparing a fourth positive electrode slurry, and using the fourth positive electrode slurry to prepare a carbon-based layer; The fourth positive electrode slurry includes the conductive agent, the binder, and the nitrogen methyl pyrrolidone solvent.