Positive plate and lithium ion battery

By using emulsion homopolymer binder and suspension copolymer binder in the electrode layer of the positive electrode sheet of the lithium ion battery, combining lithium cobalt oxide and conductive agent, the problems of slurry instability and low peel strength are solved, and high pressure is achieved The solid density and stability improve the cell performance and energy density.

CN118919647APending Publication Date: 2024-11-08SHENZHEN HIGHPOWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411222373.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

After the existing lithium-ion battery positive electrode sheet increases the proportion of main material quality, it leads to unstable slurry, low peel strength of the electrode sheet, affecting processing stability and battery cell performance, and high compaction density will lead to brittle breakage and belt breakage. Anomaly.

Method used

The emulsion homopolymer binder and suspension copolymer binder are combined in the electrode layer. The molecular weight of the emulsion homopolymer binder is lower to improve flexibility, and the molecular weight of the suspension copolymer binder is larger to enhance the intermolecular force and ensure the slurry. Stability and peel strength, while using lithium cobalt oxide and conductive agent as main material and conductive material, the ratio of conductive agent is optimized to increase the compaction density of the electrode layer.

Benefits of technology

While achieving a high proportion of the main positive electrode material, the electrode layer slurry is stable, the electrode sheet peeling strength is high, and the processing stability is good, which avoids brittle breaking and belt breaking, and improves the cell performance and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005023400430000021
    Figure BDA0005023400430000021
  • Figure BDA0005023400430000101
    Figure BDA0005023400430000101
  • Figure BDA0005023400430000121
    Figure BDA0005023400430000121
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, in particular to a positive plate and a lithium ion battery. The positive plate comprises a current collector and an electrode layer coated on the current collector. The electrode layer comprises the following components in percentage by mass: 97.7%-98.5% of lithium cobalt oxide, 0.4%-1.2% of a conductive agent, 0.4%-1.0% of a first binder and 0.2%-0.6% of a second binder. Wherein the first binder is an emulsion homopolymerization binder, and the second binder is a suspension copolymerization binder. The first binder and the second binder are added into the electrode layer to realize the high mass ratio of the positive electrode main material of the positive plate, the electrode layer slurry is stable, the stripping strength of the electrode plate is high, the compaction density is high, brittle failure, belt breakage, main material particle breakage and other abnormalities are not easy to occur during rolling, the processing stability is high, and the battery cell performance is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, in particular to a positive electrode sheet and a lithium ion battery. Background Art

[0002] At present, the competition in the lithium-ion battery industry is becoming increasingly fierce, requiring lithium-ion batteries to store more electricity and provide longer use time, so it is necessary to improve the energy density of lithium-ion batteries. There are many ways to improve energy density, which are mainly divided into two directions: one is to improve mass energy density, and the other is to improve volume energy density. Among them, in order to improve volume energy density, it is required to release more electricity under a fixed battery cell volume. The solution in the industry is to increase the mass proportion of the positive electrode main material and increase the compaction density.

[0003] However, increasing the mass proportion of the positive electrode main material will reduce the amount of auxiliary materials (such as conductive agents and binders), which can easily lead to instability of the positive electrode slurry, easy sedimentation, affecting the coating quality, and low pole piece peeling strength. Increasing the compaction density will cause the positive electrode sheet to be easily broken during rolling, the belt is broken, and the main material particles are crushed. This not only affects the processing stability and battery performance, but also requires more manpower and material resources for slurry processing and pole piece rolling belt breaking, delaying production capacity and increasing R&D and production costs. Summary of the invention

[0004] The embodiments of the present invention provide a positive electrode sheet and a lithium-ion battery to solve the problems in the prior art of slurry instability caused by the high mass proportion of the positive electrode main material, low electrode sheet peeling strength, and high compaction density affecting processing stability and battery performance.

[0005] The present invention discloses a positive electrode sheet, comprising a current collector and an electrode layer coated on the current collector; in terms of mass percentage, the electrode layer comprises:

[0006]

[0007] The first binder is an emulsion homopolymer binder, and the second binder is a suspension copolymer binder.

[0008] Optionally, the molecular weight of the first binder is 80-95w, and the molecular weight of the second binder is 130-150w.

[0009] Optionally, the second binder is formed by suspension copolymerization of a first monomer, a second monomer and a third monomer; the first monomer is vinylidene fluoride, the second monomer is acrylonitrile, and the third monomer is one or two of vinyl acetate, methyl acrylate, ethyl acrylate, methyl methacrylate, isooctyl acrylate, and butyl acrylate.

[0010] Optionally, in the second binder, by mass percentage, the first monomer accounts for 91% to 96%, the second monomer accounts for 0.5% to 3.5%, and the third monomer accounts for 1% to 5.5%.

[0011] Optionally, the first binder is formed by homopolymerization of vinylidene fluoride monomer emulsion.

[0012] Optionally, the conductive agent is one or two of conductive carbon black, conductive graphite, carbon nanotubes, and graphene.

[0013] Optionally, the conductive agent is conductive carbon black and carbon nanotubes, with lithium cobalt oxide accounting for 97.7% to 98%, conductive carbon black accounting for 0.3% to 0.6%, carbon nanotubes accounting for 0.3% to 0.5%, the first binder accounting for 0.4% to 0.7%, and the second binder accounting for 0.4% to 0.6%.

[0014] Optionally, the conductive agent is conductive carbon black and carbon nanotubes, with lithium cobalt oxide accounting for 98% to 98.4%, conductive carbon black accounting for 0.5% to 0.6%, carbon nanotubes accounting for 0.2% to 0.5%, the first binder accounting for 0.4% to 0.5%, and the second binder accounting for 0.5% to 0.6%.

[0015] Optionally, the conductive agent is conductive carbon black and carbon nanotubes, lithium cobalt oxide accounts for 97.7% to 98%, conductive carbon black accounts for 0.3% to 0.6%, carbon nanotubes account for 0.3% to 0.5%, the first binder accounts for 0.6% to 1%, and the second binder accounts for 0.2% to 0.3%.

[0016] The invention also discloses a lithium ion battery, comprising the positive electrode sheet as described above.

[0017] Compared with the prior art, the positive electrode sheet provided by the embodiment of the present invention has the beneficial effect that: the electrode layer of the positive electrode sheet in the present invention includes lithium cobalt oxide and a conductive agent, lithium cobalt oxide is the active material of the electrode layer and is the main material of the electrode layer, and the conductive agent is the conductive material of the electrode layer. In addition, the electrode layer includes 0.4% to 1.0% of a first binder and 0.2% to 0.6% of a second binder, wherein the first binder is an emulsion homopolymer binder and the second binder is a suspension copolymer binder. The emulsion homopolymer binder has a lower molecular weight and is formed by homopolymerization of a monomer emulsion. The intermolecular force is smaller and the molecular chain is softer, which can improve the flexibility of the electrode sheet, improve compaction, avoid brittle fracture, belt breakage, and main material particle crushing during rolling, and can play a role in suspending and stabilizing the slurry and avoiding slurry sedimentation. The molecular weight of the suspension copolymer binder is larger, providing a higher intermolecular force, reducing the agglomeration of particles in the slurry system, and improving the slurry suspension stability and peeling strength. Therefore, the present invention achieves a high positive electrode main material mass proportion in the positive electrode sheet by adding the first binder and the second binder in the electrode layer. At the same time, the electrode layer slurry is stable, the electrode sheet has high peeling strength, high compaction density, and is not prone to abnormalities such as brittle fracture, belt breakage, and main material particle crushing during rolling. The processing stability is high and the battery cell performance is good. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The preferred embodiments of the present invention are now described in detail.

[0019] The embodiment of the present invention provides a positive electrode sheet. The positive electrode sheet includes a current collector and an electrode layer coated on the current collector. In terms of mass percentage, the electrode layer includes 97.7% to 98.5% of lithium cobalt oxide, 0.4% to 1.2% of a conductive agent, 0.4% to 1.0% of a first binder, and 0.2% to 0.6% of a second binder. The first binder is an emulsion homopolymer binder, and the second binder is a suspension copolymer binder.

[0020] The electrode layer of the positive electrode sheet in the present invention includes lithium cobalt oxide and a conductive agent. Lithium cobalt oxide is the active material of the electrode layer and is the main material of the electrode layer. The conductive agent is the conductive material of the electrode layer. In addition, the electrode layer includes 0.4% to 1.0% of a first binder and 0.2% to 0.6% of a second binder, wherein the first binder is an emulsion homopolymer binder and the second binder is a suspension copolymer binder. The emulsion homopolymer binder has a lower molecular weight and is formed by homopolymerization of a monomer emulsion. The intermolecular force is smaller and the molecular chain is softer. It can improve the flexibility of the electrode sheet and improve compaction, avoid brittle fracture, belt breakage, and main material particle crushing during rolling, and can play a role in suspending and stabilizing the slurry and avoiding slurry sedimentation. The molecular weight of the suspension copolymer binder is larger, providing a higher intermolecular force, reducing the agglomeration of particles in the slurry system, and improving the slurry suspension stability and peel strength. Therefore, the present invention achieves a high positive electrode main material mass proportion in the positive electrode sheet by adding the first binder and the second binder in the electrode layer. At the same time, the electrode layer slurry is stable, the electrode sheet has high peeling strength, high compaction density, and is not prone to abnormalities such as brittle fracture, belt breakage, and main material particle crushing during rolling. The processing stability is high and the battery cell performance is good.

[0021] Specifically, the proportion of lithium cobalt oxide can be, for example, any one of 97.7%, 97.8%, 97.9%, 98.0%, 98.1%, 98.2%, 98.3%, 98.4%, and 98.5%. The proportion of the conductive agent can be, for example, any one of 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, and 1.2%. The proportion of the first binder can be, for example, any one of 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, and 1.0%. The proportion of the second binder can be, for example, any one of 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, and 0.6%.

[0022] Specifically, the molecular weight of the first binder is 80-95w. The first binder is an emulsion homopolymer binder with a molecular weight controlled at 80-95w. The lower the molecular weight, the smaller the intermolecular force, the softer the molecular chain, and the better the flexibility of the electrode. The molecular weight of the second binder is 130w-150w. The second binder is a suspension copolymer binder with a molecular weight controlled at 130w-150w and a larger molecular weight. The molecular weight of the first binder may be, for example, any one of 80w, 81w, 82w, 83w, 84w, 85w, 86w, 87w, 88w, 89w, 90w, 91w, 92w, 93w, 94w, and 95w, and the molecular weight of the second binder may be, for example, any one of 130w, 131w, 132w, 133w, 134w, 135w, 136w, 137w, 138w, 139w, 140w, 141w, 142w, 143w, 144w, 145w, 146w, 147w, 148w, 149w, and 150w. In the present application, "w" in the molecular weight means ten thousand.

[0023] The second binder is formed by suspension copolymerization of the first monomer, the second monomer and the third monomer; the first monomer is vinylidene fluoride, the second monomer is acrylonitrile, and the third monomer is one or two of vinyl acetate, methyl acrylate, ethyl acrylate, methyl methacrylate, isooctyl acrylate, and butyl acrylate. The second monomer is acrylonitrile, which can provide higher intermolecular forces and improve the slurry stability and peel strength; the polarity of the substituent of the third monomer is weaker than that of the cyano group, and the group volume is larger, which can provide intermolecular steric hindrance, reduce the agglomeration of particles in the slurry system, and improve the slurry suspension stability.

[0024] Suspension copolymerization is a polymerization method in which two or more monomers (small molecule compounds) are chemically reacted in a suspended state to form a copolymer. The suspended state is that the monomers are dispersed but not dissolved in a medium (such as water or other solvent medium) to form small particles or droplets.

[0025] Specifically, in the second binder, the first monomer accounts for 91% to 96% by mass, for example, any one of 91.0%, 91.5%, 92.0%, 92.5%, 93.0%, 93.5%, 94.0%, 94.5%, 95.0%, 95.5%, and 96.0%. In the second binder, the second monomer accounts for 0.5% to 3.5% by mass, for example, any one of 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.3%, 2.5%, 2.8%, 3.0%, and 3.5%. In the second binder, the third monomer accounts for 1% to 5.5% by mass, for example, it can be any one of 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.5%, 4.0%, 4.3%, 4.5%, 5.0%, and 5.5%.

[0026] The first binder is a homopolymer binder of vinylidene fluoride monomer, which is formed by homopolymerization of vinylidene fluoride monomer emulsion. In this scheme, the first binder is formed by homopolymerization of vinylidene fluoride monomer emulsion, has a low molecular weight, and the force generated between molecules is weak, which can make the flexibility higher. The soft binder can better fill the gaps between the active materials, help increase the compaction density of the electrode layer, provide better fit and flexibility during the compaction process of electrode production, reduce the damage caused by mechanical stress during the electrode manufacturing process, prevent brittle fracture or belt breakage during rolling, winding, cutting or other mechanical processing, and improve the overall processing stability. At the same time, the soft binder can better fill the gaps between the active materials, help increase the compaction density of the electrode layer, so that the electrode sheet contains more active materials in a smaller volume, which may increase the energy density of the battery.

[0027] Specifically, the conductive agent is one or two of conductive carbon black, conductive graphite, carbon nanotubes, and graphene. Conductive carbon black is used to improve the overall conductivity of the electrode. It has good conductivity and structural stability, low cost, and is easy to disperse in the electrode slurry. Conductive carbon black can also be used as a porous material to increase the electrolyte permeability inside the electrode.

[0028] Conductive graphite is a layered carbon material with good electrical conductivity and thermal stability. It can form a stable conductive network in the electrode and provide higher electrical conductivity than carbon black. Conductive graphite also helps to improve the mechanical properties of the electrode and reduce volume changes during electrochemical reactions. Carbon nanotubes (CNTs) have the characteristics of special structure, light weight, high strength, and excellent electrical conductivity. They can form a three-dimensional conductive network and effectively improve the electronic conductivity of the electrode. Carbon nanotubes also help to improve the mechanical strength of the electrode, thereby resisting structural damage during the cycle process. Graphene is a two-dimensional carbon material with ultra-high conductivity and a particularly large specific surface area. The single-layer structure of graphene enables it to greatly increase the transmission rate of electrons and ions in electrode materials. The use of graphene can reduce the internal resistance of the battery, increase the charge and discharge rate, and is particularly important for improving the power density of the battery.

[0029] Optionally, the conductive agent is conductive carbon black and carbon nanotubes, with lithium cobalt oxide accounting for 97.7% to 98%, conductive carbon black accounting for 0.3% to 0.6%, carbon nanotubes accounting for 0.3% to 0.5%, the first binder accounting for 0.4% to 0.7%, and the second binder accounting for 0.4% to 0.6%.

[0030] Optionally, the conductive agent is conductive carbon black and carbon nanotubes, with lithium cobalt oxide accounting for 98% to 98.4%, conductive carbon black accounting for 0.5% to 0.6%, carbon nanotubes accounting for 0.2% to 0.5%, the first binder accounting for 0.4% to 0.5%, and the second binder accounting for 0.5% to 0.6%.

[0031] Optionally, the conductive agent is conductive carbon black and carbon nanotubes, lithium cobalt oxide accounts for 97.7% to 98%, conductive carbon black accounts for 0.3% to 0.6%, carbon nanotubes account for 0.3% to 0.5%, the first binder accounts for 0.6% to 1%, and the second binder accounts for 0.2% to 0.3%.

[0032] In a specific embodiment, the conductive agent is conductive carbon black and carbon nanotubes, lithium cobalt oxide accounts for 97.8%, conductive carbon black accounts for 0.7%, carbon nanotubes account for 0.5%, the first binder accounts for 0.4%, and the second binder accounts for 0.6%. Under the proportion in this scheme, the electrode slurry has moderate viscosity, the slurry does not settle after standing for 48 hours, the sedimentation stability is good, the pole piece has good flexibility, the pole piece peeling strength is large, and can reach 25N / m. The comprehensive evaluation of electrode processing (slurry state, and evaluation of brittle fracture or belt breakage during coating and rolling) can reach 3.5 points (out of 5 points).

[0033] In another specific embodiment, the conductive agent is conductive carbon black and carbon nanotubes, lithium cobalt oxide accounts for 97.8%, conductive carbon black accounts for 0.7%, carbon nanotubes account for 0.5%, the first binder accounts for 0.6%, and the second binder accounts for 0.4%. Under the proportions in this scheme, the electrode slurry has moderate viscosity, the slurry does not settle after standing for 48 hours, the sedimentation stability is good, the pole piece is soft and flexible, the pole piece peeling strength is large, which can reach 22N / m, and the comprehensive evaluation of electrode processing can reach 4 points (out of 5 points).

[0034] In another specific embodiment, the conductive agent is conductive carbon black and carbon nanotubes, lithium cobalt oxide accounts for 97.8%, conductive carbon black accounts for 0.7%, carbon nanotubes account for 0.5%, the first binder accounts for 0.8%, and the second binder accounts for 0.2%. Under the proportions in this scheme, the viscosity of the electrode slurry is moderate, the pole piece is soft in flexibility, and the comprehensive evaluation of electrode processing can reach 3.5 points (out of 5 points).

[0035] The slurry of the electrode layer of the positive electrode sheet of the present invention can be prepared by one of wet pulping, dry pulping and semi-dry pulping. Taking semi-dry pulping as an example, the process steps are: first, the first binder and the second binder are respectively prepared into a glue solution with a solid content of 5% to 9%, the main material lithium cobalt oxide and conductive carbon black are mixed and stirred at a low speed, and then the glue solution, carbon nanotubes and N-methylpyrrolidone (N-Methyl-2-pyrrolidone, NMP) are added for kneading and high-speed dispersion, and finally vacuum defoaming is performed to obtain a slurry. After the slurry is coated on the current collector, it is baked, rolled and cut to obtain a positive electrode sheet. The current collector is aluminum foil.

[0036] The present invention also discloses a lithium-ion battery, comprising the positive electrode sheet as described above. The lithium-ion battery also comprises a negative electrode sheet and a separator. The positive electrode sheet, the separator and the negative electrode sheet are sequentially stacked and wound into a winding core, which is then loaded into a battery housing and injected with electrolyte to seal.

[0037] The technical solution of the present invention is further described in detail below through specific embodiments.

[0038] Examples 1-26 and Comparative Examples 1-18

[0039] 1. According to the dosage of each component in Table 1 and Table 2 below, prepare the first binder and the second binder into a 7% solid content glue solution, let it stand for 12 hours to defoam;

[0040] 2. Mixing lithium cobalt oxide and conductive carbon black;

[0041] 3. Add glue, carbon nanotubes and NMP to mix and wet at a low speed, and knead to obtain a solid content of 72%;

[0042] 4. Add the remaining NMP and stir at high speed, and perform vacuum defoaming to obtain a slurry;

[0043] 5. The slurry is coated on aluminum foil, and then baked, rolled, and cut to obtain the positive electrode sheets of Examples 1-26 and Comparative Examples 1-18.

[0044] In Table 1 below, the first binder is a homopolymer binder of vinylidene fluoride monomer; in the second binder, the first monomer vinylidene fluoride accounts for 96%, the second monomer acrylonitrile accounts for 1.5%, and the third monomer isooctyl acrylate accounts for 2.5%.

[0045] Table 1

[0046]

[0047] The experimental results of the embodiments and comparative examples in Table 1 are shown in Table 3 below.

[0048] The viscosity of the slurry was tested by a rotational viscometer to measure the viscosity of the slurry at the same solid content.

[0049] The sedimentation stability of the slurry after standing for 48 hours is to let the slurry stand in a 500ml beaker for 48 hours, and test the change in solid content of the upper and lower layers. If the solid content of the upper layer decreases by more than 2% and the solid content of the lower layer increases by more than 2%, it means that the slurry has settled.

[0050] The flexibility of the pole piece is to take the pole piece after rolling and fold it in half to observe the light transmission and brittle fracture. The pole piece is folded 180° each time, and if it is not light-transmissive, it is folded in the opposite direction 180° until light is transmitted after folding (both slight and severe are considered light transmission in Table 3), and the current fold number is recorded. The more folds, the softer the pole piece and the better the flexibility. For example, in Table 3, one slight fold means that slight light transmission occurs after only one fold, and there is no need to fold it twice; one severe fold means that severe light transmission occurs after only one fold, and there is no need to fold it twice; two slight folds mean that slight light transmission occurs after the second fold, and there is no need to fold it three times, which also means that it is not light-transmissive when folded once; two severe folds mean that severe light transmission occurs after the second fold, and there is no need to fold it twice, which also means that it is not light-transmissive when folded once.

[0051] The peel strength test is conducted using a tensile machine, and the larger the value, the better. The comprehensive evaluation of electrode processing is a comprehensive evaluation of the electrode's slurry processing, coating, and roller pressing performance.

[0052] The resistivity test of the electrode sheet is tested using a resistivity testing instrument. After rolling, the positive electrode sheet is cut into three positive electrode segments of 6 to 8 cm in length and 5 to 7 cm in width from different positions using ceramic scissors. The resistivity tester is set to a pressure of 25 MP and a holding time of 25 s. The diaphragm resistivity of 6 points is tested for each positive electrode segment. There are a total of 18 points in the three positive electrode segments. The average value is taken to obtain the diaphragm resistivity.

[0053] The comprehensive evaluation of electrode processing is to score the viscosity of the slurry, the stability of the sedimentation of the slurry after standing for 48 hours, the flexibility of the electrode, the peel strength, and the resistivity of the electrode, and then add up the scores, with a full score of 5 points. Among them, in the viscosity of the slurry, 1 point is for moderate viscosity, and 0 point is for low or high viscosity; in the sedimentation stability of the slurry after standing for 48 hours, 1 point is for no sedimentation, 0.5 point is for slight sedimentation, and 0 point is for severe sedimentation; in the flexibility of the electrode, 1 point is for opacity at one fold (i.e. more than two folds, including slight and severe two folds), 0.5 point is for slight one fold, and 0 point is for severe one fold; in the peel strength, 1 point is for a tensile force value greater than 15, 0.5 point is for less than 15, and 0 point is for less than 12; in the resistivity of the electrode, 1 point is for a resistivity value less than 40, 0.5 point is for 40-50, and 0 point is for a resistivity value greater than 50.

[0054] On the basis of Example 2, the present invention further changes the proportions of the three monomers in the second binder, as shown in Table 2 below: Comparative Examples 13-18 and Examples 18-26.

[0055] Table 2

[0056]

[0057] The test results of Comparative Examples 13-18 and Examples 18-26 in Table 2 are shown in Table 4. The test methods of the performance parameters in Table 4 are the same as those described above and will not be repeated here.

[0058] For Table 1, in Table 3 below, the proportion of the main material (lithium cobalt oxide) in Comparative Example 1 is relatively low, and does not meet the high energy density (ED) requirements. The amount of carbon black added in Example 5 is relatively small, and the proportion of the main material is large, which belongs to a relatively extreme solution. The overall slurry stability is poor and the resistivity of the pole piece membrane is large. If the main material (lithium cobalt oxide) is used as a single variable (Comparative Examples 1-2, Examples 1-3), the main material proportion is low, which will result in insufficient energy density. If the main material proportion is high, the slurry processing is difficult to ensure. If the conductive agent (conductive carbon black, carbon nanotubes) is used as a single variable (Comparative Examples 3-4, Examples 4-6), the slurry is easy to settle when the conductive agent is less and the amount of carbon black is more, and the membrane resistance is high, and the dispersion effect is poor. When the first binder is used as a single variable (Comparative Examples 5-6, Examples 4, 8), if the proportion is high, the pole piece has good flexibility and can achieve the target compaction, but the slurry is easy to settle and the peel strength is low. When the second binder is used as a single variable (Comparative Examples 7-8, Examples 9-11), if the proportion is high, the electrode sheet is brittle, the target compaction cannot be achieved, and the slurry viscosity is high, but the peel strength is large. For example, in Comparative Examples 9-10 and Examples 12-14, when the molecular weight of the first binder is low, the slurry viscosity is low, the slurry is easy to settle, and the molecular weight is too high, the flexibility is poor; for example, in Comparative Examples 11-12 and Examples 15-17, when the molecular weight of the second binder is high, the slurry is difficult to disperse, the slurry viscosity is high, and the coating is affected. The positive electrode sheet is brittle, but the peel strength is high.

[0059] Table 3

[0060]

[0061]

[0062] For Table 2, in Table 4, such as Comparative Examples 13-14 and Examples 18-20, if the proportion of the first monomer is high, the slurry is prone to low viscosity, easy to settle, and poor stability; if the proportion of the first monomer is low, the proportion of the second and third monomers is high. If the proportion of the second monomer is high, the dispersion of the electrode is poor, the main material is easy to aggregate and settle, affecting the coating, and the electrode is brittle. If the proportion of the third monomer is high, the electrode has good flexibility, but the electrode is easy to expand and fall off during the cycle, affecting the cycle performance. As in Comparative Examples 15-16 and Examples 21-23, the proportion of the second monomer is too high, the slurry viscosity is high, dispersion is difficult, and it is unstable. The pole piece is brittle after rolling, which will result in low pole piece compaction and failure to achieve the target energy density. If the proportion is too low, the pole piece cohesion is poor, the swelling is large, and the cycle deteriorates. As in Comparative Examples 17-18 and Examples 24-26, the proportion of the third monomer is high, the pole piece flexibility is good, the slurry dispersion is good, but the cohesion between the powders is low, and the electrical properties deteriorate; the proportion is low, the slurry stability is poor, and the pole piece flexibility is poor. Under normal circumstances, high peel strength and cohesion, good suspension stability and pole piece flexibility are guaranteed for the pole piece, and the amount of the second monomer is made as small as possible as small as the amount of the third monomer.

[0063] Table 4

[0064]

[0065] It should be understood that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. For those skilled in the art, the technical solutions described in the above embodiments can be modified, or some of the technical features therein can be replaced by equivalents; and all these modifications and replacements should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A positive electrode sheet, characterized in that: comprising a current collector and an electrode layer coated on the current collector; In terms of mass percentage, the electrode layer comprises: Lithium cobalt oxide 97.7%~98.5% Conductive agent 0.4%~1.2% First binder 0.4%~1.0% Second binder 0.2%~0.6% Wherein, the first binder is an emulsion homopolymer binder, and the second binder is a suspension copolymer binder.

2. The positive electrode sheet according to claim 1, characterized in that: The molecular weight of the first binder is 80-95w, and the molecular weight of the second binder is 130w-150w.

3. The positive electrode sheet according to claim 1 or 2, characterized in that: The second binder is formed by suspension copolymerization of a first monomer, a second monomer and a third monomer; the first monomer is vinylidene fluoride, the second monomer is acrylonitrile, and the third monomer is one or two of vinyl acetate, methyl acrylate, ethyl acrylate, methyl methacrylate, isooctyl acrylate and butyl acrylate.

4. The positive electrode sheet according to claim 3, characterized in that: In the second binder, by mass percentage, the first monomer accounts for 91% to 96%, the second monomer accounts for 0.5% to 3.5%, and the third monomer accounts for 1% to 5.5%.

5. The positive electrode sheet according to claim 3, characterized in that: The first binder is formed by homopolymerization of vinylidene fluoride monomer emulsion.

6. The positive electrode sheet according to claim 1, characterized in that: The conductive agent is one or two of conductive carbon black, conductive graphite, carbon nanotubes, and graphene.

7. The positive electrode sheet according to claim 1, characterized in that: The conductive agent is conductive carbon black and carbon nanotubes, the lithium cobalt oxide accounts for 97.7% to 98%, the conductive carbon black accounts for 0.3% to 0.6%, the carbon nanotubes account for 0.3% to 0.5%, the first binder accounts for 0.4% to 0.7%, and the second binder accounts for 0.4% to 0.6%.

8. The positive electrode sheet according to claim 1, characterized in that: The conductive agent is conductive carbon black and carbon nanotubes, the lithium cobalt oxide accounts for 98% to 98.4%, the conductive carbon black accounts for 0.5% to 0.6%, the carbon nanotubes account for 0.2% to 0.5%, the first binder accounts for 0.4% to 0.5%, and the second binder accounts for 0.5% to 0.6%.

9. The positive electrode sheet according to claim 1, characterized in that: The conductive agent is conductive carbon black and carbon nanotubes, the lithium cobalt oxide accounts for 97.7% to 98%, the conductive carbon black accounts for 0.3% to 0.6%, the carbon nanotubes account for 0.3% to 0.5%, the first binder accounts for 0.6% to 1%, and the second binder accounts for 0.2% to 0.3%.

10. A lithium ion battery, characterized in that: Comprising the positive electrode sheet as described in any one of claims 1 to 9.