Silicon-oxygen negative electrode material and preparation method thereof
By introducing a network coupling structure of nanoscale alloy phase and silicon phase into silicon oxide and coating the surface with amorphous carbon, the problems of low initial coulombic efficiency and poor battery cycle performance of silicon-oxygen anode materials are solved, realizing a lithium-ion battery anode material with high energy density and safety.
Patent Information
- Application Number
- CN202410605626.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-15
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional graphite-based anode materials cannot meet the high energy density and high safety requirements of next-generation lithium-ion batteries. Silicon-oxygen anode materials have low initial coulombic efficiency and poor battery cycle performance, which limits their large-scale application.
Nanoscale alloy phase particles and nanoscale silicon phase are introduced into the silicon oxide phase to form a network coupling structure, and an amorphous carbon phase is coated on the surface. Silicon-oxygen anode materials are prepared by segmented heating and carbon deposition process.
It improves the structural stability and lithium-ion transport rate of silicon-oxygen anode materials, alleviates the volume expansion effect, and enhances capacity retention and first coulombic efficiency, making it suitable for large-scale production.
Smart Images

Figure CN118919668A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery materials, and in particular to a silicon-oxygen negative electrode material and a preparation method thereof. Background Art
[0002] In recent years, lithium-ion batteries have been widely used in various fields of the national economy. New fields such as new energy vehicles, electronic information, and 3C communications have put forward higher energy density and higher safety requirements for lithium-ion batteries. With the breakthroughs in the research and development of positive electrode materials such as high specific capacity and high voltage, traditional graphite negative electrode materials can no longer meet the performance requirements of the next generation of lithium-ion batteries. Negative electrode materials with higher capacity and better performance are urgently needed to be developed.
[0003] Silicon-based anode materials have higher theoretical specific capacity than graphite-based anode materials. As a silicon-based anode material, silicon oxide (SiO x ) has a small volume expansion rate and a high theoretical specific capacity, and is low in cost and has abundant raw material reserves, so it is considered to be a negative electrode material with great application prospects. However, compared with traditional graphite negative electrodes, silicon-oxygen negative electrode materials have a lower first coulombic efficiency and poor battery cycle performance, which limits the large-scale application of silicon-oxygen negative electrode materials. Summary of the invention
[0004] In view of this, in order to solve at least one of the above technical problems, the present application provides a silicon-oxygen negative electrode material.
[0005] In addition, the present application also provides a method for preparing a silicon-oxygen negative electrode material.
[0006] An embodiment of the present application provides a silicon-oxygen negative electrode material, which includes a silicon-oxygen negative electrode material matrix and an amorphous carbon phase coated on the surface of the silicon-oxygen negative electrode material matrix, wherein the silicon-oxygen negative electrode material matrix includes: a silicon oxide phase, a plurality of nanoscale alloy phase particles and a nanoscale silicon phase, wherein the silicon oxide phase serves as a matrix phase, a plurality of the nanoscale silicon alloy phase particles are dispersed in the silicon oxide phase, the nanoscale silicon phase is distributed in the silicon oxide phase in a network shape and wraps each of the nanoscale alloy phase particles, and the amorphous carbon phase has a plurality of pore structures.
[0007] In some possible embodiments, the nano-sized alloy phase particles are A a X b The alloy, wherein A is at least one of an alkali metal element, an alkaline earth metal element and a semi-metal element, X is at least one transition metal element, 1.0≤a≤3.0, 2.0≤b≤6.0, 0.17≤a / b≤1.50.
[0008] In some possible embodiments, the content of the nano-scale alloy phase particles in the silicon-oxygen negative electrode material is 1 wt % to 10 wt %.
[0009] In some possible embodiments, the grain size of the nanoscale alloy phase particles is 5 to 50 nm, the distance between any two adjacent nanoscale alloy phase particles is 3 to 20 nm, and the grain size of the nanoscale silicon phase is 0.5 to 2 nm.
[0010] In some possible embodiments, the silicon oxide phase includes at least one of silicon monoxide and silicon dioxide.
[0011] The present application also provides a method for preparing a silicon-oxygen negative electrode material, the preparation method comprising the following steps:
[0012] mixing silicon, silicon oxide, a first metal material and a second metal material to obtain a mixture;
[0013] adding a binder to the mixture, mixing and performing agglomeration treatment to obtain a mixture mass;
[0014] Heating the mixture mass to sublime the substance in the mixture mass, and cooling and depositing the substance in the mixture mass in a collecting device to obtain a silicon-oxygen precursor; and
[0015] The silicon-oxygen precursor is placed in a heating device, and a carbon source gas is introduced to heat the silicon-oxygen precursor, so as to deposit an amorphous carbon phase on the surface of the silicon-oxygen precursor to obtain the silicon-oxygen negative electrode material.
[0016] In some possible embodiments, in the step of heating the mixture, the heating process includes a first stage of heating, a second stage of heating and a third stage of heating performed in sequence; the first stage of heating is to increase the temperature to 400-500°C at a heating rate of 5-10°C / min and keep it warm for 20-30 minutes; the second stage of heating is to increase the temperature to 900-1200°C at a heating rate of 8-10°C / min and keep it warm for 20-30 minutes; the third stage of heating is to increase the temperature to 1450-1550°C at a heating rate of 5-8°C / min and keep it warm for 4-6 hours.
[0017] In some possible embodiments, the first metal material includes at least one of alkali metal elements and their corresponding compounds, alkaline earth metal elements and their corresponding compounds, and semi-metal elements and their corresponding compounds, and the second metal material includes at least one of transition metal elements and their corresponding compounds.
[0018] In some possible embodiments, the total mass of the first metal material and the second metal material is 3% to 10% of the total mass of the silicon oxide and the silicon; the mass ratio of the metal elements in the first metal material and the second metal material is 0.17 to 1.50; and the mass ratio of the silicon oxide to the silicon is 1.9 to 2.4.
[0019] In some possible embodiments, the binder includes at least one of water glass, carboxymethyl cellulose, polyvinyl alcohol, polyacrylate, polystyrene and epoxy resin; the mass percentage of the binder to the mixture is 0.2% to 1%.
[0020] Compared with the prior art, the silicon-oxygen negative electrode material provided in the embodiment of the present application, in the silicon-oxygen negative electrode material matrix, the nano-scale alloy phase particles are uniformly dispersed in the silicon oxide phase as the matrix, and at the same time, the nano-scale silicon phase is distributed in the silicon oxide phase in a network and wraps each nano-scale alloy phase particle, that is, the nano-scale coupling structure of the silicon phase-alloy phase is dispersed in the silicon oxide phase, which improves the structural stability of the silicon-oxygen negative electrode material, effectively alleviates the volume expansion effect of the silicon-oxygen negative electrode material during the battery cycle, and improves the capacity retention rate of the silicon-oxygen negative electrode material. Moreover, the introduction of nano-scale silicon phase and nano-scale alloy phase particles can also effectively improve the first coulomb efficiency of the silicon-oxygen negative electrode material; the amorphous carbon phase on the surface of the silicon-oxygen negative electrode material matrix and the nano-scale coupling structure of the silicon phase-alloy phase constitute an effective lithium ion transmission channel, which accelerates the transmission rate of lithium ions in the silicon-oxygen negative electrode material. In addition, the preparation method of the silicon-oxygen negative electrode material provided in the embodiment of the present application is simple in process, low in cost, easy to realize mechanization and automation, which is conducive to the large-scale production of silicon-oxygen negative electrode materials and has excellent commercial prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of the structure of the silicon-oxygen negative electrode material provided in an embodiment of the present application.
[0022] Figure 2 This is a process flow chart of the method for preparing the silicon-oxygen negative electrode material provided in an embodiment of the present application.
[0023] Figure 3 This is the XRD diffraction spectrum of the silicon-oxygen negative electrode material prepared in Examples 1 and 2 of the present application.
[0024] Figure 4 This is a TEM image of the silicon-oxygen negative electrode material prepared in Example 1 of the present application. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0026] See also Figure 1 As shown, an embodiment of the present application provides a silicon-oxygen negative electrode material 100, which includes a silicon-oxygen negative electrode material matrix 10 and an amorphous carbon phase 20 coated on the surface of the silicon-oxygen negative electrode material matrix 10; the silicon-oxygen negative electrode material matrix 10 includes: a silicon oxide phase 11, a plurality of nanoscale alloy phase particles 12 and a nanoscale silicon phase 13, wherein the silicon oxide phase 11 serves as a matrix, a plurality of the nanoscale silicon alloy phase particles 12 are dispersed in the silicon oxide phase 11, the nanoscale silicon phase 13 is distributed in the silicon oxide phase 11 in a network shape and wraps each of the nanoscale alloy phase particles 12, that is, the nanoscale silicon phase 13 includes a coating portion 15 coated on the surface of the nanoscale alloy phase particle 12 and a coupling portion 16 connecting any two adjacent coating portions 15, so that the nanoscale silicon phase 13 and the nanoscale alloy phase particles 12 form a nanoscale coupling structure 14.
[0027] In some embodiments, the silicon oxide phase may include at least one of silicon monoxide and silicon dioxide. The silicon oxide phase 11 serves as the matrix of the silicon-oxygen negative electrode material matrix 10. The silicon oxide phase 11 can restrict the expansion volume when silicon expands during the reaction by utilizing the good elasticity of silicon oxide.
[0028] In some embodiments, the thickness of the amorphous carbon phase 20 may be 1 to 10 nm, further 1.5 to 10 nm, further 1.5 to 6 nm, illustratively 1.5 nm, 2 nm, 3.5 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm or 10 nm, etc. The amorphous carbon phase 20 and the nanoscale coupling structure 14 may form a lithium ion transmission channel, accelerate the transmission rate of lithium ions in the silicon-oxygen negative electrode material 100, and thus improve the conductivity of the silicon-oxygen negative electrode material 100.
[0029] In some embodiments, the structural formula of the nano-sized alloy phase particles 12 may be A a X b, A can be at least one of an alkali metal element, an alkaline earth metal element and a semi-metal element, X can be at least one transition metal element, 1.0≤a≤3.0, 2.0≤b≤6.0, 0.17≤a / b≤1.50. In the nano-sized alloy phase particles 12, both A and X have good electrical conductivity, A and X co-sublimate to form a mixed atmosphere, and A is formed under the mixed atmosphere. a X b The alloy phase forms a nano-scale coupling structure 14 with the nano-silicon phase 13 induced in situ and is evenly dispersed in the amorphous silicon oxide phase 11. The evenly dispersed nano-scale coupling structure 14 can greatly improve the structural stability of the silicon-oxygen negative electrode material 100. a X b The alloy phase has good ionic and electronic conductivity and can be used as a Li + The nano-scale alloy phase particles 12 provide a channel for ion transfer and promote the transfer of electrons. In addition, due to their uniform and small size, the silicon-oxygen negative electrode material 100 is not prone to stress concentration during the electrochemical cycle, further improving the structural stability of the silicon-oxygen negative electrode material 100. Specifically, the nano-scale alloy phase particles 12 can be a binary alloy phase, and further, A can be Si.
[0030] In some embodiments, the content of the nano-scale alloy phase particles 12 in the silicon-oxygen negative electrode material can be 1wt% to 10wt%, further can be 1wt% to 5wt%, further can be 1wt% to 3wt%, and can be 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%, etc. If the content of the nano-scale alloy phase particles 12 is too low (lower than 1%) or too high (higher than 10%), it will cause the capacity of the material to decay and reduce the conductivity, and it is not conducive to relieving the expansion and contraction of the silicon-oxygen negative electrode material, and it is impossible to maintain the stability of the battery structure during the cyclic charge and discharge process, reducing the stability and cycle life of the battery. Therefore, in this embodiment, the content of the nano-scale alloy phase particles in the silicon-oxygen negative electrode material is controlled within the above range, which can effectively alleviate the volume expansion effect of the silicon-oxygen negative electrode material during the battery cycle, and improve the capacity retention rate and the first coulomb efficiency of the silicon-oxygen negative electrode material.
[0031] In some embodiments, the grain size of the nano-scale alloy phase particles 12 may be 5 to 50 nm, further 5 to 30 nm, further 5 to 20 nm, and illustratively may be 5 nm, 7 nm, 9 nm, 10 nm, 12 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm or 50 nm, etc. The grain size of the nano-scale alloy phase particles 12 is small, and there are many grain boundaries, and the grain boundaries are the parts with stronger structure of the crystal material. The volume expansion of the silicon-oxygen negative electrode material 100 is easy to occur during the electrochemical cycle, and these uniformly dispersed alloy phase particles can pin the nano-scale silicon phase 13 to inhibit the expansion effect, thereby improving the structural stability and cycle performance of the silicon-oxygen negative electrode material 100. The distance between any two adjacent nano-scale alloy phase particles 12 may be 3 to 20 nm, further 3 to 15 nm, further 3 to 10 nm, and illustratively may be 3 nm, 4 nm, 5 nm, 7 nm, 10 nm, 12 nm, 15 nm, 16 nm, 18 nm or 20 nm, etc. The above-mentioned limitation on the distance between two adjacent nano-scale alloy phase particles 12 is conducive to reducing the path of ion transmission in the silicon-oxygen negative electrode material and improving the charge and discharge rate and cycle stability of the silicon-oxygen negative electrode material.
[0032] In some embodiments, the particle size of the nano-scale silicon phase 13 can be 0.5 to 2 nm, further can be 0.5 to 1 nm, and can be 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, 1.0 nm, 1.2 nm, 1.4 nm, 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm, 1.9 nm or 2.0 nm, etc. The particle size of the nano-scale silicon phase 13 is limited to the range of 0.5 to 2 nm, and a nano-scale silicon phase 13 with a small particle size is obtained to achieve a better wrapping effect on the nano-scale alloy phase particles 12. The nano-scale silicon phase 13 and the nano-scale alloy phase particles 12 form a nano-scale coupling structure 14, which produces a synergistic effect, improves the cycle stability of the silicon-oxygen negative electrode material, and can also simultaneously achieve high specific capacity and high conductivity, thereby improving the overall performance of the silicon-oxygen negative electrode material. Limiting the nano-sized alloy phase particles 12, nano-sized silicon phases 13 and nano-sized coupling structures 14 can improve the electrochemical activity of silicon-oxygen negative electrode materials, slow down the volume expansion of silicon-oxygen negative electrode materials, increase the ion and electron transfer rates and improve the stability of silicon-oxygen negative electrode materials.
[0033] In some embodiments, the amorphous carbon phase 20 has a plurality of pore structures, which are beneficial for alleviating the volume expansion effect of the silicon-oxygen negative electrode material 100 during battery cycling.
[0034] In the embodiment of the present application, a nano-scale silicon phase 13 and a nano-scale alloy phase particle 12 are formed in the parent silicon oxide phase 11. The metal elements in the nano-scale alloy phase particle 12 can react with lithium, promote the insertion and extraction of lithium, improve the conductivity of the silicon-oxygen negative electrode material 100, and thus improve the first coulomb efficiency of the silicon-oxygen negative electrode material 100; the nano-scale silicon phase 13 is distributed in the silicon oxide phase 11 in a network and wraps each nano-scale alloy phase particle 12, that is, a nano-scale coupling structure 14 of the silicon phase-alloy phase is dispersed in the silicon oxide phase 11. In the physical phase matrix 11, the structural stability of the silicon-oxygen negative electrode material 100 is improved, the volume expansion effect of the silicon-oxygen negative electrode material 100 during the battery cycle is effectively alleviated, and the capacity retention rate of the silicon-oxygen negative electrode material 100 is improved; in addition, the amorphous carbon phase 20 on the surface of the silicon-oxygen negative electrode material matrix 10 and the nanoscale coupling structure 14 of the silicon phase-alloy phase constitute a lithium ion transmission channel, which accelerates the transmission rate of lithium ions in the silicon-oxygen negative electrode material 100, and can also further alleviate the volume expansion effect of the silicon-oxygen negative electrode material 100.
[0035] See also Figure 2 As shown, the method for preparing the silicon-oxygen negative electrode material provided in the embodiment of the present application specifically comprises the following steps:
[0036] Step S1, mixing silicon, silicon oxide, a first metal material and a second metal material to obtain a mixture.
[0037] Specifically, silicon and silicon oxide are premixed in a certain proportion, and then a certain amount of the first metal material and the second metal material are added and uniformly mixed in a high-speed mixer to obtain a mixture. It is understandable that the mixing process is not limited to being carried out in a high-speed mixer, and any method that can achieve mixing of silicon, the first metal material and the second metal material is possible.
[0038] In some embodiments, the first metal material may include at least one of alkali metal elements and their corresponding compounds, alkaline earth metal elements and their corresponding compounds, and semi-metal elements and their corresponding compounds, and the second metal material may include at least one of transition metal elements and their corresponding compounds.
[0039] In some embodiments, the alkali metal element may include at least one of Li, Na, K, Rb, and Cs.
[0040] In some embodiments, the alkaline earth metal element may include at least one of Be, Ba, Ca, Sr, and the like.
[0041] In some embodiments, the semi-metal element may include at least one of Si, B, As, Sb, etc. Further, the semi-metal element may be Si.
[0042] In some embodiments, the transition metal element may include at least one of Mn, Al, Mg, Co, Ti, Cu, Zn, Y, La, Ni, etc. Further, the transition metal element may be at least one of Mn, Al, Mg, etc.
[0043] In some embodiments, the mass ratio of the silicon oxide to the silicon may be 1.9 to 2.4, and further may be 1.9 to 2.2. For example, the mass ratio of silicon oxide to silicon may be 1.9, 2.0, 2.1, 2.2, 2.3 or 2.4, etc. By limiting the ratio of the two to the above range, silicon can be fully and evenly dispersed in the elastic silicon oxide, which can effectively inhibit the generation of cracks and alleviate the risk of expansion of the negative electrode material.
[0044] In some embodiments, the total mass of the first metal material and the second metal material can be 3% to 10% of the total mass of the silicon oxide and the silicon, and can further be 5% to 10%. For example, it can be 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%. If the ratio of the two is too low (less than 3%), the metal doping content in the material will be too little, and it will not be able to effectively improve the capacity retention rate and the first coulomb efficiency of the silicon-oxygen negative electrode material; if the ratio of the two is too high (greater than 10%), it may cause the metal material to agglomerate, unable to be wrapped by silicon and evenly dispersed inside the silicon oxide, which is not conducive to improving the structural stability, capacity retention rate and first coulomb efficiency of the material. Therefore, in this embodiment, the total mass ratio of the first metal material and the second metal material is controlled within the above range, so that the formed nano-scale alloy phase particles can form nano-scale coupling with nano-scale silicon and be evenly distributed in the silicon oxide, effectively alleviating the volume expansion effect of the silicon-oxygen negative electrode material during the battery cycle, and improving the capacity retention rate and the first coulomb efficiency of the silicon-oxygen negative electrode material. In some embodiments, silicon, silicon oxide, the first metal material and the second metal material are fully mixed using a high-speed mixer, and the high-speed mixing time may be 90 to 120 minutes.
[0045] In some embodiments, the mass ratio of the metal elements in the first metal material and the second metal material can be 0.17 to 1.50, further can be 0.17 to 1.40, further can be 0.20 to 1.30, and can be 0.17, 0.2, 0.3, 0.4, 0.6, 0.8, 1.0, 1.1, 1.3, 1.4 or 1.5, etc. Under the limited ratio conditions, a stable alloy phase is easily formed in a vacuum high temperature atmosphere, and it is not easy to decompose or precipitate to form a metal element during the cooling deposition process, so as to ensure the formation of an alloy phase structure and obtain a coupled structure of an alloy phase and a nano-silicon phase. A lower or higher ratio is easy to cause the precipitation of a metal element during the gas phase reaction, and is also easy to promote the growth of the nanostructure.
[0046] Step S2, adding a binder into the mixture and mixing the mixture to form a mass to obtain a mixture mass.
[0047] Specifically, a certain amount of a specific binder and salt-free water are added to the mixture raw materials, and the mixture is mixed and agglomerated by a agglomerating machine, and then dried in a vacuum constant temperature oven to obtain a dry mixture agglomerate.
[0048] In some embodiments, the binder may include at least one of water glass, carboxymethyl cellulose, polyvinyl alcohol, polyacrylate, polystyrene and epoxy resin, etc. The binder can firmly bind the materials of the silicon-oxygen negative electrode material together, thereby ensuring that the material will not fall off or peel off during the charging and discharging process, thereby maintaining the structural stability of the material; at the same time, the binder itself usually has a certain conductivity, which can help the transmission of lithium electrons and improve the overall conductivity of the material.
[0049] In some embodiments, the mass percentage of the binder and the mixture can be 0.2% to 1%. The present application limits the proportion of the binder according to the specific design of the silicon-oxygen negative electrode material. If the proportion of the binder is too high (higher than 1%), the resistance may be increased, resulting in a decrease in the performance of the silicon-oxygen negative electrode material; if the proportion is too low (lower than 0.2%), the silicon-oxygen negative electrode material may have insufficient adhesion, and may easily fall off or peel off, affecting the structural stability and cycle life of the silicon-oxygen negative electrode material.
[0050] In some embodiments, in step S2, a dispersant may be added and mixed together. The dispersant may be water. The mass percentage of the water and the mixture may be 20% to 30%. This may allow the mixture to be better mixed and a more uniform mixture mass may be obtained.
[0051] In some embodiments, the mixed agglomerate is mixed and agglomerated using a agglomerate machine, and the particle size of the obtained mixed agglomerate can be controlled to be 0.1 to 1 mm. By controlling the particle size of the mixed agglomerate within the above range, it is possible to ensure that the components in the mixed agglomerate after the mixed agglomerate are evenly distributed, improve the sintering effect, and the raw materials for mixed agglomeration are more likely to form a dense structure during the sintering process, and the sintering effect is more uniform and stable.
[0052] In some embodiments, the drying temperature may be 200-280°C.
[0053] Step S3, heating the mixture mass to sublime the substances in the mixture mass, and cooling and depositing the substances in the mixture mass in a collecting device to obtain a silicon-oxygen precursor.
[0054] Specifically, the mixture mass obtained in step S2 is heated in a three-stage heating manner under vacuum conditions to sublime the substances in the mixture mass, cooled and deposited in a collecting device, and a silicon-oxygen precursor is collected, and the collected silicon-oxygen precursor is crushed and ground.
[0055] In some embodiments, the heating process can be a three-stage heating, including a first stage heating, a second stage heating and a third stage heating performed in sequence; the first stage heating can be to raise the temperature to 400-500°C at a heating rate of 5-10°C / min and keep it warm for 20-30 minutes; the second stage heating can be to raise the temperature to 900-1200°C at a heating rate of 8-10°C / min and keep it warm for 20-30 minutes; the third stage heating can be to raise the temperature to 1450-1550°C at a heating rate of 5-8°C / min and keep it warm for 4-6 hours.
[0056] In this application, after the raw materials are pre-treated by adding a binder to form a mass and drying, they will form dense and uniform agglomerate particles, which provides a good prerequisite for the subsequent vacuum heating deposition to prepare silicon oxide precursors. By adopting three-stage heating, the mixture mass is pre-heated at a low heating temperature. The first stage is low-temperature heating and heat preservation. One is to volatilize the moisture inside the material that is not easy to dry, the second is to ensure that the temperature of each part of the material is uniform, and the third is to further solidify the binder so that the mixture mass forms a higher strength dense mass; then the second stage of heating is carried out under higher temperature conditions, so that the high-strength and dense mixture mass partially melts to form a multi-component solid solution, avoiding the low melting and boiling point phase from reacting and sublimating first and providing good prerequisites for subsequent gas phase sublimation; finally, the temperature is raised again for the third stage of high-temperature heating, and the solid solution phase formed by the raw material begins to sublimate continuously under high temperature conditions to form a mixed atmosphere, and silicon oxide is formed in the mixed atmosphere. During the cooling and deposition process, silicon oxide forms an amorphous matrix, and A and X first form uniform alloy phase crystal cells in the matrix and grow to form a nano alloy phase A. a X b , nano alloy phase A a X b Induce silicon to nucleate at the edge of its grains and grow to form nano-silicon, while the nano-silicon further grows and connects with each other to form a network structure, and finally the nano-silicon and nano-alloy phase A a X b A coupling structure is formed.
[0057] In some embodiments, the heated gas pressure condition is less than or equal to 10Pa.
[0058] In some embodiments, the particle size D50 of the silicon oxide precursor can be controlled to be 1 to 10 μm, and further can be 1 to 6 μm, and can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, etc. Limiting the particle size of the silicon oxide precursor is beneficial to subsequent heating. A smaller particle size can increase the specific surface area of the silicon oxide precursor, which is beneficial to subsequent carbon deposition and increases the coating effect; improve the performance of silicon oxide negative electrode materials, and use a particle size of 1 to 10 μm to optimize the structure and micromorphology of the material, which helps to improve the capacity, cycle stability and charge and discharge performance of the material. The silicon oxide precursor with a nanoscale coupling structure of silicon phase-alloy phase is obtained through the heating process of step S3. The nanoscale silicon phase and nanoscale alloy phase particles dispersed in the matrix, and the nanoscale coupling structure formed by the two can improve the structural stability of the silicon-oxygen negative electrode material, greatly alleviate the volume expansion effect of the silicon-oxygen negative electrode material during the battery cycle, and improve the capacity retention rate and first coulombic efficiency of the silicon-oxygen negative electrode material.
[0059] Step S4, placing the silicon-oxygen precursor in a heating device, and introducing a carbon source gas for heating, so as to deposit an amorphous carbon phase on the surface of the silicon-oxygen precursor to obtain the silicon-oxygen negative electrode material.
[0060] Specifically, a carbon source gas is introduced into the heating device to heat the silicon-oxygen precursor, and then the temperature is lowered to room temperature with the furnace under protective gas conditions, and amorphous carbon is deposited on the surface of the silicon-oxygen precursor to obtain the silicon-oxygen negative electrode material. The amorphous carbon phase may not have a clear crystal structure, the main element is C element, and has a certain pore structure, and a reserved expansion space can alleviate the volume expansion effect of the silicon-oxygen negative electrode material.
[0061] In some embodiments, the heating device may be a rotary kiln.
[0062] In some embodiments, the carbon source gas may include at least one of methane, acetylene, propylene, ethylene, methanol, methyl chloride, propane, ethane, isobutane, cyclopropane, n-butane, isobutylene, and the like.
[0063] In some embodiments, in the step of heating the silicon oxide precursor, the heating process may be to increase the temperature to 700-900° C. at a heating rate of 5-10° C. / min and keep the temperature for 90-120 min.
[0064] In some embodiments, the protective gas may include at least one of nitrogen, argon, and neon.
[0065] Through the heating deposition process of step S4, a layer of amorphous carbon is formed on the surface of the silicon-oxygen precursor, and the nano-scale coupling structure of the outer amorphous carbon phase and the silicon phase-alloy phase constitutes a lithium ion transmission channel, which improves the transmission rate of lithium ions in the silicon-oxygen negative electrode material. In addition, the amorphous carbon phase can not only enhance the conductivity of the silicon-oxygen negative electrode material, but also alleviate the volume expansion effect of the silicon-oxygen negative electrode material.
[0066] Compared with the prior art, the silicon-oxygen negative electrode material and the method for preparing the silicon-oxygen negative electrode material provided in the embodiments of the present application have the following beneficial effects:
[0067] 1. By adding metal materials to silicon oxide and using segmented heating, a silicon-oxygen precursor with a nanoscale coupling structure of silicon phase-alloy phase is obtained. The nanoscale coupling structure of the nanoscale silicon phase and the alloy phase dispersed in the silicon oxide phase can improve the structural stability of the silicon-oxygen negative electrode material, effectively alleviate the volume expansion effect of the silicon-oxygen negative electrode material during the battery cycle, and improve the capacity retention rate and first coulomb efficiency of the silicon-oxygen negative electrode material.
[0068] 2. A layer of amorphous carbon is formed on the surface of the silicon-oxygen precursor by using a carbon deposition process. The nanoscale coupling structure of the outer amorphous carbon phase and the silicon phase-alloy phase constitutes a lithium ion transmission channel, thereby improving the transmission rate of lithium ions in the negative electrode material.
[0069] 3. This preparation method has simple process, low cost, easy mechanization and automation, which is conducive to the large-scale production of silicon-oxygen negative electrode materials and has excellent commercial prospects.
[0070] The above silicon-oxygen negative electrode material and its preparation method are further described below through specific examples.
[0071] Example 1
[0072] Step 1. Weigh 60 g of silicon powder (Si) and 120 g of silicon dioxide powder (SiO2), mix them in a high-speed mixer at 1000 r / min for 60 min, then weigh 9 g of manganese powder and add it to the Si / SiO2 mixture and continue mixing for 30 min to obtain a uniformly mixed Si / SiO2 / Mn mixture.
[0073] Step 2, weigh 1g of water glass and stir it thoroughly with 40ml of salt water to prepare a mixed binder, add the prepared mixed binder and 150g of Si / SiO2 / Mn mixture into a mixing agglomerator, mix and agglomerate, and dry in a high-temperature oven at 200°C to obtain a granular Si / SiO2 / Mn mixture agglomerate with a particle size of 0.1-1mm.
[0074] Step 3: The dried mixture was heated to 400°C at a heating rate of 6°C / min under the condition of ≤10Pa in a vacuum induction furnace and kept warm for 30min, then heated to 1200°C at a heating rate of 10°C / min and kept warm for 30min, then heated to 1500°C at a heating rate of 6°C / min and kept warm for 4h, and finally cooled to room temperature with the furnace, and crushed and ground to obtain a silicon oxide precursor SiO with a particle size D50 of 5μm. x -Mn.
[0075] Step 4: Using methane as a carbon source, a silicon oxide precursor SiO x -Mn was subjected to a 120-min heating carbon deposition treatment, and after cooling to room temperature in an argon atmosphere, a new silicon-oxygen negative electrode material with nanoscale coupled dispersed distribution of silicon and manganese-silicon alloy phases was obtained.
[0076] Example 2
[0077] Step 1. Weigh 60 g of silicon powder (Si) and 120 g of silicon dioxide powder (SiO2), mix them in a high-speed mixer at 1000 r / min for 60 min, then weigh 18 g of manganese oxide and add it to the Si / SiO2 mixture and continue mixing for 30 min to obtain a uniformly mixed Si / SiO2 / MnO mixture.
[0078] Step 2: Weigh 1 g of carboxymethyl cellulose and stir it with 35 ml of salt-free water to prepare a mixed binder. Add the prepared mixed binder and 150 g of Si / SiO2 / MnO mixture into a mixing agglomerator for mixed agglomeration and dry it in a high-temperature oven at 200°C to obtain a granular Si / SiO2 / MnO mixture agglomerate with a particle size of 0.1 to 1 mm.
[0079] Step 3: The dried mixture was heated to 400°C at a rate of 5°C / min under a condition of ≤10Pa in a vacuum induction furnace and kept warm for 30min, then heated to 1200°C at a rate of 8°C / min and kept warm for 30min, then heated to 1500°C at a rate of 5°C / min and kept warm for 4h, and finally cooled to room temperature in the furnace, and crushed and ground to obtain a silicon oxide precursor SiO with a particle size D50 of 5μm. x -Mn.
[0080] Step 4: Using methane as a carbon source, a silicon oxide precursor SiO x -Mn was subjected to a 100 min heating carbon deposition treatment, and after being furnace cooled to room temperature in an argon atmosphere, a new silicon-oxygen negative electrode material with nanoscale coupled dispersed distribution of silicon and manganese-silicon alloy phases was obtained.
[0081] Example 3
[0082] Step 1. Weigh 60 g of silicon powder (Si) and 120 g of silicon dioxide powder (SiO2), mix them in a high-speed mixer at 1000 r / min for 60 min, then weigh 15 g of aluminum powder, add it to the Si / SiO2 mixture and continue mixing for 30 min to obtain a uniformly mixed Si / SiO2 / Al mixture.
[0083] Step 2: Weigh 1.2 g of water glass and stir it with 35 ml of salt water to prepare a mixed binder. Add the prepared mixed binder and 150 g of Si / SiO2 / Al mixture into a mixing agglomerator for mixed agglomeration and dry it in a high-temperature oven at 200°C to obtain a granular Si / SiO2 / Al mixture agglomerate with a particle size of 0.1 to 1 mm.
[0084] Step 3: The dried mixture was heated to 400°C at a heating rate of 8°C / min under the condition of ≤10Pa in a vacuum induction furnace and kept warm for 20min, then heated to 1200°C at a heating rate of 10°C / min and kept warm for 20min, then heated to 1500°C at a heating rate of 5°C / min and kept warm for 4h, and finally cooled to room temperature in the furnace, and crushed and ground to obtain a silicon oxide precursor SiO with a particle size D50 of 5μm. x -Al.
[0085] Step 4: Using acetylene as a carbon source, a silicon oxide precursor SiO x -Al was subjected to a 100-min heating carbon deposition treatment, and after cooling to room temperature in an argon atmosphere, a new silicon-oxygen negative electrode material with nanoscale coupled dispersed distribution of silicon and aluminum-silicon alloy phases was obtained.
[0086] Example 4
[0087] Step 1. Weigh 60 g of silicon powder (Si) and 120 g of silicon dioxide powder (SiO2), mix them in a high-speed mixer at 1000 r / min for 60 min, then weigh 12 g of magnesium powder, add it to the Si / SiO2 mixture and continue mixing for 30 min to obtain a uniformly mixed Si / SiO2 / Mg mixture.
[0088] Step 2, weigh 0.8g of water glass and stir it thoroughly with 30ml of salt water to prepare a mixed binder, add the prepared mixed binder and 150g of Si / SiO2 / Mg mixture into a mixing agglomerator, perform mixed agglomeration treatment and dry it in a high-temperature oven at 150°C to obtain a granular Si / SiO2 / Al mixture agglomerate with a particle size of 0.1-1mm.
[0089] Step 3: The dried mixture was heated to 400°C at a rate of 5°C / min under a condition of ≤10Pa in a vacuum induction furnace and kept warm for 25min, then heated to 1200°C at a rate of 8°C / min and kept warm for 25min, then heated to 1500°C at a rate of 5°C / min and kept warm for 4h, and finally cooled to room temperature in the furnace, and crushed and ground to obtain a silicon oxide precursor SiO with a particle size D50 of 5μm. x -Mg.
[0090] Step 4: Using acetylene as a carbon source, a silicon oxide precursor SiO x -Mg was sintered and carbon-deposited for 120 min, and then cooled to room temperature in an argon atmosphere to obtain a new silicon-oxygen negative electrode material with nanoscale coupled dispersed distribution of silicon and magnesium-silicon alloy phases.
[0091] Comparative Example 1
[0092] Step 1: Weigh 60 g of silicon powder (Si) and 120 g of silicon dioxide powder (SiO2), and mix them in a high-speed mixer at 1000 r / min for 60 min to obtain a uniformly mixed Si / SiO2 mixture.
[0093] Step 2: Drying in a high temperature oven at 200°C.
[0094] Step 3: The dried mixture was heated to 400°C at a heating rate of 5°C / min under the condition of ≤10Pa in a vacuum induction furnace and kept warm for 30min, then heated to 1200°C at a heating rate of 10°C / min and kept warm for 30min, then heated to 1500°C at a heating rate of 5°C / min and kept warm for 4h, and finally cooled to room temperature with the furnace, and crushed and ground to obtain a silicon oxide precursor SiO with a particle size D50 of 5μm. x .
[0095] Step 4: Using acetylene as a carbon source, a silicon oxide precursor SiO x The sintering carbon deposition treatment was carried out for 120 minutes, and the silicon-oxygen negative electrode material was obtained after cooling to room temperature in a nitrogen atmosphere.
[0096] Comparative Example 2
[0097] Zhengzhou Juhuang New Materials Technology Co., Ltd. commercially sells F50-3 silicon-oxygen negative electrode material.
[0098] The following tests were performed on the silicon-oxygen negative electrode materials obtained in Example 1, Example 2, Example 3, Example 4, Comparative Example 1 and Comparative Example 2.
[0099] 1. The silicon-oxygen negative electrode materials obtained in Example 1 and Example 2 were analyzed by X-ray diffraction (XRD). The results are as follows: Figure 3 As shown, it can be found that Si and Mn appear in the amorphous diffraction patterns of the silicon-oxygen negative electrode materials of Example 1 and Example 2. 27 Si 47 The crystal diffraction peak and XRD results show that the silicon-oxygen negative electrode material containing crystalline silicon and manganese-silicon alloy phase can be prepared by the process provided in the embodiments of the present application.
[0100] 2. The silicon-oxygen negative electrode material obtained in Example 1 was analyzed by transmission electron microscopy (TEM). The results are as follows: Figure 4 The results show that there are nano-scale spherical crystal particles in the silicon-oxygen negative electrode material of Example 1, and there are irregular small nano-crystals on the edge of the nano-scale spherical crystal particles. Combined with the XRD results, it can be judged that the nano-scale spherical crystal particles are Mn 27 Si 47 Crystals, irregular nanocrystals are nanoscale crystalline silicon, indicating that the silicon-oxygen negative electrode material prepared by the process method provided in the embodiment of the present application has a coupling structure of nanoscale silicon alloy phase and nanoscale silicon phase.
[0101] 3. Electrochemical performance tests were performed on Example 1, Example 2, Example 3, Example 4, Comparative Example 1 and Comparative Example 2. The results of the electrochemical performance tests are shown in Table 1.
[0102] Table 1
[0103]
[0104] Electrochemical tests were carried out on Example 1, Example 2, Example 3, Example 4, Comparative Example 1 and Comparative Example 2 in the voltage range of 0.005V to 1.5V and at a rate of 0.1C, and the test results are shown in Table 1. The results show that after modification, although the Si content of Examples 1-4 is reduced, a relatively high capacity is still maintained, which is basically the same as the capacity of Comparative Example 1-2. The first efficiency of Examples 1-4 is significantly improved compared to that of Comparative Example 1-2, and the first coulombic efficiency in Example 1 reaches 82%. The 50 battery cycle capacity retention rate of Examples 1-4 is also greatly improved compared to Comparative Example 1-2, which is 31% higher than that of Comparative Example 1-2. At the same time, the resistivity of Examples 1-4 is significantly reduced compared to Comparative Example 1-2, which is 76% lower than that of Comparative Example 1-2.
[0105] It can be seen from this that the first coulomb efficiency of the silicon-oxygen negative electrode material is improved by forming nano-scale silicon phase and nano-scale alloy phase particles in Examples 1-4 of the present application; by adding metal materials to the silicon-oxygen negative electrode material and using a three-stage heating process to deposit nano-scale silicon phase and nano-scale alloy phase, the obtained nano-scale silicon phase is distributed in the silicon oxide phase in a network and wraps each nano-scale alloy phase particle, that is, a nano-scale coupling structure of silicon phase-alloy phase is formed and dispersed in the silicon oxide phase matrix, which improves the stability of the structure of the silicon-oxygen negative electrode material, effectively alleviates the volume expansion effect of the silicon-oxygen negative electrode material during the battery cycle, and improves the capacity retention rate of the silicon-oxygen negative electrode material. Therefore, the silicon-oxygen negative electrode material of Examples 1-4 not only improves the first coulomb efficiency, but also improves the capacity retention rate of the silicon-oxygen negative electrode material. In addition, a layer of amorphous carbon is formed on the surface of the silicon-oxygen precursor, and the nano-scale coupling structure of the outer amorphous carbon phase and the silicon phase-alloy phase constitutes a lithium ion transfer channel, which improves the transfer rate of lithium ions in the negative electrode material and reduces the resistivity of the silicon-oxygen material.
[0106] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.
Claims
1. A silicon-oxygen negative electrode material, characterized in that: It includes a silicon-oxygen negative electrode material matrix and an amorphous carbon phase coated on the surface of the silicon-oxygen negative electrode material matrix, wherein the silicon-oxygen negative electrode material matrix includes: a silicon oxide phase, a plurality of nanoscale alloy phase particles and a nanoscale silicon phase, wherein the silicon oxide phase serves as a matrix phase, a plurality of the nanoscale alloy phase particles are dispersed in the silicon oxide phase, the nanoscale silicon phase is distributed in the silicon oxide phase in a network shape and wraps each of the nanoscale alloy phase particles, and the amorphous carbon phase has a plurality of pore structures.
2. The silicon-oxygen negative electrode material according to claim 1, characterized in that: The nano-scale alloy phase particles are A a X b The alloy, wherein A is at least one of an alkali metal element, an alkaline earth metal element and a semi-metal element, X is at least one transition metal element, 1.0≤a≤3.0, 2.0≤b≤6.0, 0.17≤a / b≤1.
50.
3. The silicon-oxygen negative electrode material according to claim 1, characterized in that: The content of the nano-scale alloy phase particles in the silicon-oxygen negative electrode material is 1 wt% to 10 wt%.
4. The silicon-oxygen negative electrode material according to claim 1, characterized in that: The grain size of the nano-scale alloy phase particles is 5 to 50 nm, and the distance between any two adjacent nano-scale alloy phase particles is 3 to 20 nm; The grain size of the nano-scale silicon phase is 0.5-2 nm.
5. The silicon-oxygen negative electrode material according to claim 1, characterized in that: The silicon oxide phase includes at least one of silicon monoxide and silicon dioxide.
6. A method for preparing a silicon-oxygen negative electrode material, characterized in that: include: mixing silicon, silicon oxide, a first metal material and a second metal material to obtain a mixture; Adding a binder to the mixture, mixing and performing agglomeration treatment to obtain a mixture mass; Heating the mixture mass to sublime the substance in the mixture mass, and cooling and depositing the substance in the mixture mass in a collecting device to obtain a silicon-oxygen precursor; as well as The silicon-oxygen precursor is placed in a heating device, and a carbon source gas is introduced to heat the precursor, so that an amorphous carbon phase is deposited on the surface of the silicon-oxygen precursor to obtain the silicon-oxygen negative electrode material.
7. The preparation method according to claim 6, characterized in that: In the step of heating the mixture mass, the heating process includes a first stage of heating, a second stage of heating and a third stage of heating performed sequentially; The first stage of heating is to raise the temperature to 400-500°C at a heating rate of 5-10°C / min and keep the temperature for 20-30min; The second stage of heating is to raise the temperature to 900-1200°C at a heating rate of 8-10°C / min and keep the temperature for 20-30min; The third stage of heating is to raise the temperature to 1450-1550° C. at a heating rate of 5-8° C. / min and keep the temperature for 4-6 hours.
8. The preparation method according to claim 6, characterized in that: The first metal material includes at least one of alkali metal elements and their corresponding compounds, alkaline earth metal elements and their corresponding compounds, and semi-metal elements and their corresponding compounds, and the second metal material includes at least one of transition metal elements and their corresponding compounds.
9. The preparation method according to claim 6, characterized in that: The total mass of the first metal material and the second metal material is 3% to 10% of the total mass of the silicon oxide and the silicon; The mass ratio of the metal elements in the first metal material and the second metal material is 0.17 to 1.50; The mass ratio of the silicon oxide to the silicon is 1.9 to 2.
4.
10. The preparation method according to claim 6, characterized in that: The binder comprises at least one of water glass, carboxymethyl cellulose, polyvinyl alcohol, polyacrylate, polystyrene and epoxy resin; The mass percentage of the binder to the mixture is 0.2% to 1%.