Method for implementing liquid-phase coating of sodium-containing high-entropy oxide ultrathin layer on sodium ion battery layered oxide positive electrode material

Through liquid phase washing and coating technology, the layered oxide positive electrode material of sodium ion battery is coated with metal salts such as Co, Cu, La, etc., and combined with thickener and organic solvent, the uneven material and high cost in the prior art are solved. The problem of improving the cycle rate performance and stability of the battery is suitable for large-scale production.

CN118919686APending Publication Date: 2024-11-08HUNAN NORMAL UNIVERSITY

Patent Information

Application Number
CN202410985835.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing sodium ion battery layered oxide positive electrode materials have shortcomings in circulation performance and battery rate performance, and the solid phase hybrid coating method leads to uneven materials and high costs, affecting commercial production.

Method used

The liquid phase washing and coating method is adopted, and metal salts containing Co, Cu, La, Al are uniformly coated, combined with thickener and organic solvents, reduce sodium precipitation, and improve material stability through heat treatment to form a protective shell. Reduce side effects.

Benefits of technology

It improves the cycling rate performance and electrochemical performance of sodium ion batteries, reduces production costs, and achieves uniform coating and stability improvement of materials, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919686A_ABST
    Figure CN118919686A_ABST
Patent Text Reader

Abstract

The invention provides a process method for coating a high-entropy oxide ultrathin layer on a layered oxide positive electrode material of a sodium-ion battery while reducing residual alkali on the surface of the layered oxide positive electrode material through low-temperature liquid-phase washing. The coating material can be any sodium ion battery layered oxide positive electrode material, coating elements at least comprise four metal elements, namely cobalt (Co), copper (Cu), lanthanum (La) and aluminum (Al), and one or more of niobium (Nb), zinc (Zn), cerium (Ce), yttrium (Y) and magnesium (Mg) metal elements can be additionally selected. In the low-temperature liquid phase washing process, a thickening agent and an organic solvent are added, and residual alkali and metal salt on the surface of the material are utilized to preliminarily form a hydroxide layer on the surface of the material. The technical characteristics of low temperature, the thickening agent and the organic solvent can effectively inhibit dissolution and sodium separation of the positive electrode material during water washing. And then low-temperature heat treatment is carried out in the dehumidified oxygen-containing mixed gas, so that a uniform and ultrathin oxide protection layer is formed on the surface of the sodium ion layered oxide positive electrode material. The high-entropy oxide ultrathin coating layer can effectively prevent the substrate positive electrode material from being in direct contact with air or electrolyte, the structural stability of the positive electrode material is improved, meanwhile, the coating layer has good sodium ion conductivity, and finally good rate activity and cycling stability of the high-entropy coated positive electrode material are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a method for implementing liquid-phase coating of an ultra-thin layer of high-entropy oxide on a layered oxide positive electrode material of a sodium ion battery. Background Art

[0002] Sodium-ion batteries are expected to replace lithium-ion batteries in the field of large-scale energy storage due to their abundant sodium resources and low cost. Due to the high specific capacity of the negative electrode material, the positive electrode material determines the energy density of the battery. The structural stability of the positive electrode material during the sodium insertion and extraction process also has an important impact on the cycle and rate performance of the battery. At present, there are many types of layered oxide positive electrode materials, such as P2 phase, P3 phase, O2 phase, O3 phase, mixed phase structure, etc. However, these materials generally have poor cycle performance and low discharge capacity under high current.

[0003] To solve the above problems, the most commonly used method is solid phase mixing coating. However, solid phase mixing will lead to uneven mixing of materials, and long-term exposure of materials to air will also damage and cause irreversible precipitation of sodium. The nano oxides used in solid phase coating are expensive and used in large quantities, which significantly increases the material production cost and is not conducive to commercial production. Liquid phase coating can achieve uniform coating and the metal salt is cheap. The sodium source of sodium ion positive electrode materials in pure water precipitates seriously. The appropriate addition of thickeners and organic solvents can reduce the precipitation of sodium in the material. Carrying out water washing and coating at the same time can also reduce costs on a large scale. In liquid phase washing, aluminum (Al) elements can play a buffering role, copper (Cu) elements play a role in accelerating element fusion in secondary sintering, and cobalt (Co) and lanthanum (La) form a protective shell on the surface to reduce the side reactions between the material and the electrolyte.

[0004] This invention is proposed in order to improve the electrochemical performance of sodium ion layered oxide positive electrode materials and reduce production costs. Summary of the invention

[0005] The purpose of the present invention is to provide a liquid phase washing and coating method for layered oxide positive electrode materials of sodium ion batteries, which can reduce residual alkali and achieve uniform coating of high entropy oxides. In addition, the addition of thickeners and organic solvents can also reduce the precipitation of sodium sources in the material during water washing. The modified material can reduce the secondary particle breakage caused by charging and discharging in the electrolyte and the dissolution of the material in the transition metal layer, which is beneficial to improving the cycle rate performance of sodium ion batteries, and has low cost and is expected to achieve large-scale production.

[0006] The technical solution adopted by the present invention to solve its technical problem is: the coated material is a sodium ion layered oxide positive electrode material, the coating material contains Co, Cu, La, Al, and can also contain one or more salts of Nb, Zn, Ce, Y, and Mg metal elements; the ratio of the total mass of the coated metal salt to the mass of the positive electrode is 1:1000 to 1:500.

[0007] The liquid phase washing coating method of the sodium ion layered oxide positive electrode material comprises the following steps:

[0008] (1) dissolving a certain amount of metal salts in a liquid mixed solvent to obtain a metal salt solution;

[0009] (2) adding a thickener to the salt solution obtained in step (1), stirring thoroughly, and dissolving;

[0010] (3) Add a certain amount of material to step (2), stir at low temperature for a certain period of time, and obtain a black suspension. After suction filtration, washing, and vacuum drying, the coated material is obtained;

[0011] (4) heat treating a certain amount of the coating material in a dehumidified oxygen-containing mixed gas at a certain temperature for a certain time to obtain a modified material;

[0012] Furthermore, in step (1), the metal salt may be one or a mixture of sulfate, nitrate, chloride, acetate;

[0013] Furthermore, in step (1), the mixed solvent is one or a mixture of pure water, ethanol, methanol, and ethylene glycol;

[0014] Furthermore, in step (1), the mass fraction of pure water in the mixed solvent is above 60%;

[0015] Furthermore, in step (1), the mass ratio of the mixed solvent to the positive electrode material is 4:5 to 6:5;

[0016] Furthermore, in step (2), the amount of the thickener is 0.5% to 2% of the mass of the positive electrode;

[0017] Furthermore, in step (2), the amount of the thickener may be one or a mixture of glucose, hydroxyethyl cellulose, and hydroxymethyl cellulose;

[0018] Furthermore, in step (3), the stirring time is 1 to 10 minutes;

[0019] Furthermore, in step (3), the low temperature is 0 to 10°C, the vacuum drying temperature is 60 to 80°C, and the drying time is 4 to 8h;

[0020] Furthermore, in step (4), the filtration method includes various solid-liquid separation methods such as vacuum filtration, high-speed centrifugation, plate and frame filter press, etc.;

[0021] Furthermore, in step (4), the heat treatment reaction time is 0.5 to 3 hours;

[0022] Furthermore, in step (4), the dehumidified oxygen-containing mixed gas is one or a mixture of dehumidified air, an oxygen-nitrogen mixed gas containing 20% ​​to 30% oxygen, and an oxygen-argon mixed gas containing 20% ​​to 30% oxygen;

[0023] Furthermore, in step (4), the heat treatment temperature is 300-700°C.

[0024] The beneficial effects of the present invention are as follows: by reducing residual alkali during liquid phase washing and coating the sodium ion layered oxide positive electrode material, the coating performance of the material is increased. The scheme is simple to operate, easy to repeat, and conducive to large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The raw material O3-NaNi in Example 1 of the present invention 0.33 Fe 0.33 Mn 0.33 XRD patterns of O2 and modified materials;

[0026] Figure 2 Left: O3-NaNi before coating in implementation case 1 0.33 Fe 0.33 Mn 0.33 O2 layered cathode material, the right is the modified cathode material in implementation case 1;

[0027] Figure 3 The SEM results of the modified material in Example 1 of the present invention and the mapping test of the elements;

[0028] Figure 4 This is a HRTEM image of the primary particle surface and a local enlarged image of the coating layer of the modified material in Example 1 of the present invention;

[0029] Figure 5 The XPS graph of the corresponding elements of the modified product in Example 1 of the present invention;

[0030] Figure 6 The raw material O3-NaNi in Example 1 of the present invention 0.33 Fe 0.33 Mn 0.33 Half-cell cycle performance diagram of O2 and modified materials;

[0031] Figure 7 The raw material O3-NaNi in Example 1 of the present invention0.33 Fe 0.33 Mn 0.33 Half-cell rate performance diagram of O2 and modified materials;

[0032] Figure 8 The raw material O3-NaNi in Example 1 of the present invention 0.33 Fe 0.33 Mn 0.33 The first cycle charge and discharge curves of half-cell of O2 and modified materials; DETAILED DESCRIPTION

[0033] The present invention is further described in the following examples, but the embodiments of the present invention are not limited thereto.

[0034] Example 1

[0035] (1) According to the mass ratio of positive electrode to coating metal salt of 1000:1, 0.1 g of each of cobalt sulfate, copper sulfate, lanthanum sulfate, aluminum sulfate, magnesium sulfate, zinc sulfate, cerium carbonate, and manganese sulfate were weighed, and O3-NaNi 0.33 Fe 0.33 Mn 0.33 100g of O2 positive electrode material, 70g of water and 30g of ethanol were measured and mixed, 1g of glucose was first added to the mixed solvent, and then the metal salt was dissolved in the mixed solvent. After stirring to fully dissolve, the positive electrode material was poured into the metal salt solution, stirred and reacted at 5°C in an ice water bath for 1min, and then high-speed centrifuged, washed, and vacuum dried at 80°C for 6h to obtain the coated material;

[0036] (2) Weigh 50g of the coated material and place it in a magnetic boat. Keep it at a constant temperature of 400℃ for 3h under dehydrated air to obtain the modified material. Weigh 0.9g of the modified material, 0.05g of acetylene black (conductive agent), and 0.05g of PVDF (HSV900, binder), grind them thoroughly, add 2.5g of NMP to disperse and mix, and slurry them evenly. Then, pull the slurry onto aluminum foil to make a sheet with a coating thickness of 200μm. After being dried at 110℃ with a blast, cut it into discs with a diameter of 12mm, and assemble the battery in a glove box. Use a metal sodium sheet as the counter electrode, a mixture of sodium hexafluorophosphate and ethylene carbonate as the electrolyte, and Whatman GF / D as the diaphragm to assemble it into a CR2032 button battery test (1C=120mAh·g -1 ). The 0.1C discharge capacity of the raw material is 138.51 mAh g -1 , 1C capacity is 130.21mAh·g -1 The cycle retention rate after 100 cycles is 65.10%; the 0.1C discharge capacity of the modified material is 144.15 mAh g -1 , 1C capacity is 135.48mAh·g -1, the 100-cycle cycle retention rate is 76.87%.

[0037] Example 2

[0038] (1) According to the mass ratio of positive electrode to coated metal salt of 500:1, 0.2 g each of cobalt sulfate, copper sulfate, lanthanum sulfate, aluminum sulfate, zinc sulfate, iridium oxalate, and magnesium sulfate were weighed. 0.67 Li 0.03 Fe 0.33 Mn 0.55 Ti 0.09 100g of O2 positive electrode material, 70g of water and 20g of ethylene glycol were measured and mixed, 2g of sodium citrate was first added to the mixed solvent, and then the metal salt was dissolved in the mixed solvent. After stirring to fully dissolve, the positive electrode material was poured into the metal salt solution, stirred in an ice water bath at 5°C for 4min, and filtered under reduced pressure, washed, and dried at 80°C in vacuum for 4h to obtain the coated material;

[0039] (2) Weigh 50g of the coated material and place it in a magnetic boat. Keep it at a constant temperature of 500℃ for 2h under dehydrated air to obtain the modified material. Weigh 0.9g of the modified material, 0.05g of acetylene black (conductive agent), and 0.05g of PVDF (HSV900, binder), grind them thoroughly, add 2.5g of NMP to disperse and mix, and after slurrying, stretch the slurry on aluminum foil to make a sheet with a coating thickness of 200μm. After being dried at 110℃ with a blast, cut it into discs with a diameter of 12mm, and assemble the battery in a glove box. Use a metal sodium sheet as the counter electrode, a mixture of sodium hexafluorophosphate and ethylene carbonate as the electrolyte, and Whatman GF / D as the diaphragm to assemble it into a CR2032 button battery (1C=120mAh·g -1 ). The 0.1C discharge capacity of the raw material is 126.37 mAh g -1 , 1C capacity is 116.78mAh·g -1 The 100-cycle retention rate is 83.45%; the 0.1C discharge capacity of the modified material is 126.56 mAh g -1 , 1C capacity is 118.30mAh g -1 , the 100-cycle cycle retention rate is 88.39%.

[0040] Example 3

[0041] (1) According to the mass ratio of positive electrode to coated metal salt of 500:1, 0.2 g of cobalt sulfate, copper sulfate, lanthanum sulfate, aluminum sulfate, zinc sulfate, iridium sulfate, and niobium oxalate were weighed, and P2-O3 mixed phase structure Na 0.78 Ni 0.22 Fe 0.2 Mn 0.4 Mg 0.12Ti 0.06 100g of O2 positive electrode material, 70g of water and 25g of methanol were measured and mixed, 1g of hydroxymethyl cellulose was first added to the mixed solvent, and then the metal salt was dissolved in the mixed solvent. After stirring to fully dissolve, the positive electrode material was poured into the sulfate solution, stirred and reacted at 10°C in an ice water bath for 3min, and then high-speed centrifugation, washing, and vacuum drying at 70°C for 4h were performed to obtain the coated material;

[0042] (2) Weigh 50g of the coated material and place it in a magnetic boat. Keep it at a constant temperature of 450℃ for 3h in an oxygen-nitrogen mixed gas containing 20-30% oxygen to obtain the modified material. Weigh 0.9g of the modified material, 0.05g of acetylene black (conductive agent), and 0.05g of PVDF (HSV900, binder). After grinding them thoroughly, add 2.5g of NMP to disperse and mix them. After slurrying, stretch the slurry onto aluminum foil to make a sheet with a coating thickness of 200μm. After being dried at 110℃ with a blast, cut it into discs with a diameter of 12mm, and assemble the battery in a glove box. Use a metal sodium sheet as the counter electrode, a mixture of sodium hexafluorophosphate and ethylene carbonate as the electrolyte, and Whatman GF / D as the diaphragm to assemble it into a CR2032 button battery (1C=120mAh·g -1 ). The 0.1C discharge capacity of the raw material is 130.21 mAh g -1 , 1C capacity is 118.52mAh·g -1 The 100-cycle cycle retention rate is 70.59%; the 0.1C discharge capacity of the modified material is 132.76 mAh g -1 , 1C capacity is 122.93mAh·g -1 , the 100-cycle cycle retention rate is 79.43%.

[0043] Example 4

[0044] (1) According to the mass ratio of positive electrode to coated metal salt of 500:1, 0.2 g of cobalt sulfate, copper sulfate, lanthanum sulfate, aluminum sulfate, and zinc sulfate were weighed, and P3-NaNi 0.33 Fe 0.33 Mn 0.33 100g of O2 positive electrode material, 70g of water, 30g of ethanol and 10g of ethylene glycol were measured and mixed, 1g of glucose and 1g of sodium citrate were first added to the mixed solvent, and then the metal salt was dissolved in the mixed solvent. After stirring to fully dissolve, the positive electrode material was poured into the sulfate solution, and stirred in an ice water bath at 0℃ for 5min, and then filtered by plate and frame, washed, and dried in vacuum at 60℃ for 6h to obtain the coated material;

[0045] (2) Weigh 50g of the coated material and place it in a magnetic boat. Keep it at a constant temperature of 600℃ for 1h in an oxygen-argon gas mixture containing 20-30% oxygen to obtain the modified material. Weigh 0.9g of the modified material, 0.05g of acetylene black (conductive agent), and 0.05g of PVDF (HSV900, binder), grind them thoroughly, add 2.5g of NMP to disperse and mix, and after slurrying, stretch the slurry on aluminum foil to make a sheet with a coating thickness of 200μm. After being dried at 110℃ with a blast, cut it into discs with a diameter of 12mm, and assemble the battery in a glove box. Use a metal sodium sheet as the counter electrode, a mixture of sodium hexafluorophosphate and ethylene carbonate as the electrolyte, and Whatman GF / D as the diaphragm to assemble it into a CR2032 button battery (1C=120mAh·g -1 ). The 0.1C discharge capacity of the raw material is 132.22mAh·g -1 , 1C capacity is 123.41mAh·g -1 The 100-cycle retention rate is 67.24%; the 0.1C discharge capacity of the modified material is 135.84 mAh g -1 , 1C capacity is 126.88mAh·g -1 , the 100-cycle cycle retention rate is 78.27%.

Claims

1. A method for coating a sodium ion battery layered oxide cathode material with an ultra-thin layer of high entropy oxide in a liquid phase, It is characterized in that The layered oxide sodium ion battery positive electrode material is subjected to a low-temperature liquid phase washing process, wherein the residual alkali reacts with the metal cation to coat a layer of metal hydroxide, is filtered, vacuum dried, and heat-treated at no higher than 700° C. under a dehumidified oxygen-containing mixed gas to transform the layered oxide into a thin layer of high entropy oxide to form a high entropy oxide protective layer; the liquid phase solvent is pure water with a thickener added or a liquid phase solution of an organic solvent miscible with pure water; The coating material is a salt containing different metal elements such as cobalt (Co), copper (Cu), lanthanum (La), and aluminum (Al), and one or more salts containing metal elements such as niobium (Nb), zinc (Zn), cerium (Ce), yttrium (Y), and magnesium (Mg) are selected; The sodium ion battery layered oxide positive electrode material may refer to P2 phase, P3 phase, O2 phase, O3 phase, or mixed phase positive electrode material.

2. The surface modification method according to claim 1, It is characterized in that The liquid phase solvent is pure water, ultrapure water, or a mixed solvent with one or more of ethanol, methanol, and ethylene glycol, the volume fraction of pure water is 60% to 100%; the mass ratio of the liquid phase solvent to the positive electrode material is 4:5 to 6:

5.

3. The surface modification method according to claim 1, It is characterized in that In an ice water bath at 0-10°C, the washing time is 1-10 minutes.

4. The coating material of the sodium ion battery positive electrode material according to claim 1, It is characterized in that The coating layer has a thickness of 5 to 50 nm, which is a nano-scale coating.

5. The thickener according to claim 1 can be a mixture of one or more of glucose, citric acid, sodium citrate, hydroxyethyl cellulose, and hydroxymethyl cellulose; the amount of the thickener is 0.5-2% of the mass of the positive electrode material.

6. According to claim 1, the salt corresponding to the metal element can be one or a mixture of oxalate, sulfate, carbonate, etc.; the ratio of the mass of the coated metal salt to the mass of the material is 1:1000 to 2:

500.

7. According to claim 1, the filtration method includes various solid-liquid separation methods such as vacuum filtration, high-speed centrifugation, plate and frame filter press, etc.

8. The sintering temperature of the heat-treated coated material according to claim 1 is 300-700°C and the sintering time is 0.5-3h.

Citation Information

Patent Citations

  • Sodium-containing oxide positive electrode material, preparation method and application thereof, positive plate and application thereof

    CN114843498A

  • Sodium ion positive electrode material and preparation method thereof

    CN115425200A

  • Perovskite type high-entropy oxide and preparation method and application thereof

    CN115837275A

  • Preparation method and application of sodium ion battery positive electrode material coated with high-entropy oxide material

    CN116332145A

  • Coated modified sodium ion positive electrode material, preparation method and sodium ion battery

    CN116799173A

Cited By

  • Process method of liquid-phase coated sodium aluminum phosphate ultrathin layer for layered oxide positive electrode material of sodium-ion battery