Product for magnesium alloying of molten steel as well as manufacturing method and application of product

By coating nano-aluminum powder and nano-silicon powder on the surface of magnesium oxide particles, forming composite core-shell structure powder, the problem of difficulty in adding magnesium to liquid steel is solved, the yield of magnesium and the toughness of steel are improved, and magnesium oxidation is achieved uniform distribution and efficient reaction of the substance.

CN119020551APending Publication Date: 2024-11-26ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411120999.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Under the conditions of large-line energy welding, it is difficult to effectively add magnesium to liquid steel, resulting in low yield and unstable magnesium. In the prior art, the magnesium splashing phenomenon is serious, affecting the toughness of the steel.

Method used

By coating nano-aluminum powder and/or nano-silicon powder on the surface of magnesium oxide particles, a composite core-shell structure powder is formed to improve the reactivity and wettability of magnesium oxide, so that it can be directly added to the steel and through mechanical means The ball milling process is coated under a low temperature inert atmosphere to prevent contact of magnesium oxides from air, forming a smaller particle size and evenly distributed magnesium oxide inclusions.

Benefits of technology

It improves the yield of magnesium and the uniformity and reactivity of magnesium oxides in the molten steel, extends the residence time of magnesium oxides in the molten steel, enhances the toughness and corrosion resistance of the steel, and reduces splashing. Improves the yield of magnesium and the toughness of the steel plate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020551A_ABST
    Figure CN119020551A_ABST
Patent Text Reader

Abstract

The invention discloses a product for magnesium alloying of molten steel and a manufacturing method and application of the product, and belongs to the technical field of steel smelting. The product for molten steel magnesium alloying comprises a shell and a powder core wrapped in the shell, the powder core adopts powder of a composite core-shell structure, magnesium oxide particles serve as an inner core of the powder core, and the surfaces of the magnesium oxide particles are wrapped with a modifier; the modifier comprises nano aluminum powder and / or nano silicon powder. The surface of the micron magnesium oxide particle is directly coated with a layer of modifier to form the composite core-shell structure powder, so that the problems that in the prior art, magnesium oxide cannot be directly added into molten steel through an external adding method, or magnesium is directly added into the molten steel, the reaction is violent, and a serious splashing phenomenon is generated can be effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of steel smelting, and more specifically to a product for magnesium alloying of molten steel, a preparation method thereof and an application thereof. Background Art

[0002] With the rapid development of shipbuilding and marine engineering, the requirements for steel quality are constantly increasing. In the modern shipbuilding industry, high-energy-line welding technology is usually used, which causes serious coarsening of the grains in the heat-affected zone of welding, forming a brittle structure, which seriously affects the performance of steel. Therefore, the steel industry has introduced the concept of "oxide metallurgy", among which the third-generation oxide metallurgy technology uses stable, fine and dispersed oxides and sulfides containing Mg or Ca at a high temperature of 1673K to pin austenite grains and optimize the structure. It is an important way to solve the deterioration of toughness under high-energy-line welding conditions.

[0003] Since the boiling point of metal Mg is 1107℃, its vapor pressure is as high as 2.0×10 6 Pa, the metallic Mg added by the external addition method will vaporize rapidly, causing serious splashing, and it is difficult to diffuse into the molten steel to form fine dispersed magnesium oxides, resulting in a low magnesium yield.

[0004] For example, the Chinese patent application No. 201610871499.2 discloses a magnesium treatment process for ship plate steel, which adds Mg-Al-Fe alloy cored wire after alloy fine-tuning in the LF process or after vacuum treatment in the RH process; secondly, according to the acid-soluble aluminum content of the steel, the aluminum feeding amount and the magnesium treatment wire feeding amount are coordinated under the premise of ensuring the magnesium treatment effect of the Mg-Al-Fe alloy cored wire; then, in the LF or RH process, the cored wire feeding method is used to add Mg-Al-Fe alloy cored wire to the ship plate steel liquid, and finally the finished molten steel is obtained. This process improves the mechanical properties and stability of ship plate steel to a certain extent, but adding magnesium to the molten steel by the wire feeding method is still prone to cause a large amount of magnesium to overflow in the form of steam, causing the molten steel to roll violently, and the magnesium recovery rate is low and unstable.

[0005] The Chinese patent application number 202110556844.4 discloses a product and method for magnesium or magnesium-calcium treatment of molten steel. The product of the application is composed of a sealed shell and an alloying material encapsulated in the shell, and the alloying material includes magnesium oxide, a composite reducing agent and a stabilizing diluent. The application is to insert the product deep into the molten steel and use the energy of the molten steel to stimulate the reduction reaction of magnesium oxide. This method can effectively inhibit the rapid evaporation of magnesium during the magnesium modification and denaturation of inclusions in the steel, reducing the gasification and oxidation loss of magnesium. However, due to the presence of the reducing agent, it is difficult to obtain magnesium oxide later, which will affect the toughness of steel used in high-energy line welding technology, and is therefore not suitable for oxide metallurgy under high-energy line welding conditions.

[0006] For another example, the Chinese patent application No. 201710378210.8 discloses a method for producing microalloyed steel for high-energy wire welding. The production method of the application includes converter steelmaking, LF ladle furnace or VD furnace refining and rolling process. Before leaving the station after the LF ladle furnace or VD furnace refining, the oxygen is fixed to control the [O] in the molten steel at 20-45PPm, and then the AlMg alloy cored wire is fed. The AlMg alloy cored wire has a metal magnesium wire as the inner core, and the outer layer of the magnesium wire is coated with aluminum strip and low-carbon steel strip in sequence. The production process of the application can effectively improve and enhance the low-temperature impact performance of the steel plate and the welding fusion line to a certain extent, and reduce the amount of precious alloys such as Ni, Nb, and V in the microalloyed steel, but the splashing phenomenon of magnesium in the cored wire feeding process is still relatively serious. Summary of the invention

[0007] The purpose of the present invention is to provide a product for magnesium alloying of molten steel, a preparation method and application thereof, by directly coating a layer of modifier on the surface of micron magnesium oxide particles to form a composite core-shell structure powder, thereby effectively solving the problem in the prior art that magnesium oxide cannot be directly added to molten steel by an external addition method, or that direct addition of magnesium to molten steel results in a violent reaction and severe splashing.

[0008] In order to achieve the above object, the technical solution provided by the present invention is:

[0009] The first aspect of the present invention provides a product for magnesium alloying of molten steel, comprising an outer shell and a powder core wrapped inside the outer shell, wherein the powder core is a powder of a composite core-shell structure, with magnesium oxide particles as the inner core, and the surface of the magnesium oxide particles is wrapped with a modifier; the modifier comprises nano aluminum powder and / or nano silicon powder.

[0010] In order to solve the problem that ship plate steel is prone to toughness degradation under high-energy-line welding conditions, the prior art usually uses oxide metallurgy technology to improve the toughness of steel. However, due to the poor wettability of magnesium oxide, it is generally impossible to add it directly to the molten steel. Therefore, the prior art usually adds single magnesium or magnesium-containing alloys directly to the molten steel in the form of cored wire. However, metallic magnesium is relatively active and is prone to severe splashing during the feeding process of molten steel, thereby affecting the magnesium recovery rate.

[0011] Based on the above situation, the present invention uses magnesium oxide particles as the core and uses nano aluminum powder and / or nano silicon powder to modify the magnesium oxide particles, thereby effectively improving the reactivity and wettability of magnesium oxide with molten steel, allowing magnesium oxide to be directly added to the molten steel, and solving the problem of serious splashing when adding molten steel in the form of elemental magnesium or alloy magnesium, thereby improving the yield of magnesium. Among them, when the modifier contains nano aluminum powder and nano silicon powder at the same time, the particle size of the composite magnesium oxide inclusions in the obtained steel sample is smaller and the distribution uniformity is better. This is due to the reactivity of magnesium and aluminum elements, and the combination of nano silicon powder reducing the wetting angle between magnesium oxide and molten steel, improving the wettability of magnesium oxide powder and molten steel, so that magnesium oxide can stay in the molten steel for a longer time, thereby facilitating obtaining a higher magnesium yield.

[0012] As a further preferred embodiment of any technical solution of the first aspect of the present invention, the magnesium oxide particles include magnesium oxide and / or magnesium titanate. When the magnesium oxide particles preferably include magnesium titanate, the effect is better. When magnesium titanate powder is added to molten steel, it will decompose to generate magnesium oxide and titanium dioxide. The presence of titanium dioxide is conducive to further improving the wettability of magnesium oxide with molten steel, so that magnesium oxide can stay in the molten steel for a longer time, thereby further improving the recovery rate of magnesium in the molten steel.

[0013] As a further preferred embodiment of any technical solution of the first aspect of the present invention, the volume ratio of the magnesium oxide particles to the nano-aluminum powder is 1:1.5 to 1:4, and the volume ratio of the magnesium oxide particles to the nano-silicon powder is 1:1.5 to 1:4; thereby further ensuring the reactivity and wettability of magnesium oxide with molten steel, thereby ensuring the recovery rate of magnesium in the molten steel and the toughness of the steel plate.

[0014] As a further preferred embodiment of any technical solution of the first aspect of the present invention, the particle size of the magnesium oxide particles is 50nm-3μm; the particle size of the nano silicon powder is 20-100nm; and the particle size of the nano aluminum powder is 2-10μm. Among them, the smaller particle size of the magnesium oxide is helpful to induce the nucleation of acicular ferrite, thereby achieving the effect of grain refinement.

[0015] It should be noted that the role of the shell in the present application is mainly to wrap the powder core of the composite core-shell structure so as to add it to the molten steel. As one implementation method, the shell adopts a hollow structure, which is wrapped around the outside of the powder core to form an overall block structure. For example, a hollow steel shell can be used for sealing and wrapping, or the powder core can be sintered into a block in advance and then wrapped with a tungsten mesh.

[0016] As another preferred implementation, the outer shell is made of steel strip, which is wrapped around the outside of the powder core to form a cored wire product; the steel strip is preferably a cold-rolled steel strip. More preferably, the thickness of the outer shell steel strip is 0.8 mm to 1.2 mm, and the diameter of the cored wire product obtained after coating is Φ3.0 mm to Φ5.0 mm, so that it is not only convenient to put magnesium oxide into the molten steel, but also conducive to successfully introducing magnesium oxide into the molten steel, and further ensuring the recovery rate of magnesium.

[0017] The second aspect of the present invention provides a method for manufacturing any product for magnesium alloying of molten steel as described in the first aspect, comprising: coating a powder core of a composite core-shell structure with an outer shell.

[0018] As a further solution of any technical solution of the second aspect of the present invention, it also includes: coating the surface of the magnesium oxide particles with the modifier powder to form a powder core with a composite core-shell structure.

[0019] As a further preferred embodiment of any technical solution of the second aspect of the present invention, the process of coating the modifier powder on the surface of the magnesium oxide particles comprises: mechanically milling the powder containing the magnesium oxide particles and the modifier under a low temperature inert atmosphere, wherein the low temperature is -3°C to 3°C. By mechanically milling under a low temperature inert atmosphere, the modifier is coated on the surface of the magnesium oxide particles to form a composite core-shell structure powder, thereby effectively preventing the magnesium oxide particles from contacting with air for reaction.

[0020] As a further preferred embodiment of any technical solution of the second aspect of the present invention, the method further comprises: before coating the modifier powder on the surface of the magnesium oxide particles, pre-ball milling the magnesium oxide particles.

[0021] As a further preferred embodiment of any technical solution of the second aspect of the present invention, during the mechanical ball milling of the powder containing magnesium oxide particles and the modifier and the pre-ball milling of the magnesium oxide particles, the low temperature state inside the equipment is maintained by introducing low-temperature nitrogen, and the nitrogen introduction rate is 2 to 10 L / min.

[0022] More preferably, the rotation speed of the ball milling and pre-ball milling is 300-500 rpm, and the ball milling time is 3-6 h.

[0023] A third aspect of the present invention provides a use of any product for magnesium alloying of molten steel as described in the first aspect in magnesium treatment of molten steel for ship plate steel.

[0024] The product of the present invention can directly introduce magnesium oxide into molten steel from the outside, and improve the bulk density and uniformity of magnesium oxide, improve its induced nucleation effect, and thus improve the performance of steel. Among them, the induced nucleation effect can improve the crystal structure in the molten steel, reduce the formation of defects and irregular oxides, and improve the strength, toughness and corrosion resistance of the steel.

[0025] In addition, the present invention adds magnesium oxide and / or magnesium titanate externally and analyzes the characteristics of magnesium oxide body density, IGF nucleation ability and toughness. The toughness of the steel sample can be used as the final evaluation index, and a model for the influence of the uniformity of magnesium oxide inclusions and the induced nucleation ability on the toughness of the final sample based on the external addition of magnesium oxide is established, thereby facilitating the effective control of the toughness of the ship plate steel product finally produced.

[0026] In summary, the technical solution provided by the present invention can achieve the following beneficial effects compared with the prior art:

[0027] (1) The present invention forms a composite powder with a core-shell structure by modifying the surface of magnesium oxide particles, thereby effectively improving the reactivity of magnesium oxide particles with molten steel, reducing the wetting angle between non-wetting magnesium oxide and molten steel, and improving the wettability between magnesium oxide and molten steel, thereby prolonging its residence time in molten steel, and further dissolving, diffusing, and suspending the oxide in molten steel, thereby achieving effective addition. This method solves the problem that non-wetting magnesium oxide is difficult to directly add to molten steel, and improves the uniform dispersibility of non-wetting magnesium oxide; wherein, the modifier on the surface of magnesium oxide particles preferably comprises nano-aluminum powder and nano-silicon powder, thereby facilitating further improving the recovery rate of magnesium in molten steel.

[0028] (2) The magnesium oxide particles of the present invention preferably further contain magnesium titanate, which is beneficial to further improve the wettability of magnesium oxide with molten steel, prolong its residence time in the molten steel, and thus further improve the recovery rate of magnesium in the molten steel. At the same time, by optimizing and controlling the particle size of the magnesium oxide particles, it is helpful to induce the nucleation of acicular ferrite, which can further achieve the effect of grain refinement.

[0029] (3) The present invention utilizes a mechanical ball milling process to coat the modifier on the surface of magnesium oxide to form a powder with a composite core-shell structure, which can not only effectively ensure the uniformity of the modifier coating, but also facilitate the control of the coating thickness; in addition, by ball milling and coating in a low-temperature liquid nitrogen atmosphere, it can also effectively avoid the magnesium oxide particles from contacting with air for reaction, which is beneficial to further ensure the magnesium yield.

[0030] (4) The present invention pre-ball-mills the magnesium oxide particles before coating and modifying them, which not only makes the magnesium oxide powder more evenly distributed and improves its activity and processability, but also reduces the range of particle size distribution, increases the surface area and surface activation energy of the magnesium oxide, and thus enhances its coating effect with nano-aluminum powder and nano-silicon powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The metallographic structure of the as-cast sample in Example 4 of the present invention;

[0032] Figure 2 The oxide distribution of Example 2 (corresponding to a) and Example 4 (corresponding to b) of the present invention;

[0033] Figure 3 A comparison of the oxide particle sizes of Example 2 (corresponding to a) and Example 4 (corresponding to b) of the present invention;

[0034] Figure 4 The present invention provides a relationship model between the toughness of the steel sample and the uniformity of magnesium oxide and the IGF nucleation index. DETAILED DESCRIPTION

[0035] In order to further understand the content of the present invention, the present invention is now described in detail in conjunction with specific embodiments.

[0036] Example 1

[0037] Put magnesium oxide powder (purity>99.9%) into a ball mill, add grinding balls at a ball-to-material ratio of 6:1, place the ball mill in a planetary ball mill, introduce nitrogen at a rate of 3L / min, and keep the temperature in the ball mill at around 0°C to eliminate the heat generated by friction during ball milling. Pre-ball milling of magnesium oxide powder is performed at a speed of 400rpm and a ball milling time of 4h to reduce the distribution range of magnesium oxide particle size, increase the surface area and surface activation energy of magnesium oxide, and enhance its coating effect with nano-aluminum powder.

[0038] Subsequently, under a low-temperature inert atmosphere, nano-aluminum powder (nano-aluminum powder having a particle size of 2 to 3 μm) was added into a ball mill at a volume ratio of 2:1 to magnesium oxide, and grinding balls were added at a ball-to-material ratio of 6:1. The ball milling was performed again at a rotation speed of 400 rpm for 4 hours, thereby forming a layer of nano-aluminum powder on the surface of the magnesium oxide powder, which helps to improve its wettability with molten steel.

[0039] The composite core-shell structure powder after ball milling is used as the core, and a 1.0 mm cold-rolled steel strip is used as the outer shell to roll it into a core wire with a diameter of Φ4.0 mm. The core wire can be quickly immersed in the molten steel to accelerate the diffusion rate of magnesium oxide.

[0040] DH36 ship plate steel was melted in a vacuum induction furnace. After the molten steel was clarified, magnesium oxide powder treated by cored wire was added and kept warm for 20 minutes. The final solidified steel sample was water quenched at 1200℃, and rectangular steel blocks with a length, width and height of 55*10*10mm were cut out for impact test.

[0041] Example 2

[0042] Magnesium titanate powder (purity>99%, particle size<3μm) was placed in a ball mill, and grinding balls were added at a ball-to-material ratio of 6:1. The ball mill was placed in a planetary ball mill, and nitrogen was introduced at a rate of 3L / min. The temperature in the ball mill was maintained at about 0°C. The magnesium titanate powder was pre-milled at a rotation speed of 400rpm and a ball milling time of 4h.

[0043] Subsequently, under a low-temperature inert atmosphere, nano-aluminum powder (nano-aluminum powder having a particle size of 2 to 3 μm) was added into a ball mill at a volume ratio of 2:1 to magnesium titanate, and grinding balls were added at a ball-to-material ratio of 6:1. The ball milling was performed again at a rotation speed of 400 rpm for 4 hours, thereby forming a layer of nano-aluminum powder on the surface of the magnesium titanate powder to obtain a powder with a composite core-shell structure.

[0044] The composite core-shell structure powder after ball milling is used as the core, and a 1.0 mm cold-rolled steel strip is used as the outer shell to roll it into a core wire with a diameter of Φ4.0 mm. The core wire can be quickly immersed in the molten steel to accelerate the diffusion rate of magnesium titanate.

[0045] According to the thermodynamic reaction equation:

[0046] MgO+TiO 2 =MgO·TiO 2 (s)

[0047] [Ti] + 2[O] = TiO 2 (s)

[0048] Combining the above two formulas, we can get

[0049] MgO·TiO2(s)=MgO(s)+[Ti]+2[O]

[0050] According to the thermodynamic reaction equation 2[Ti]+3[O]=Ti 2 O 3 (s) We can get:

[0051] [Ti]+3 / 2[O]=1 / 2Ti 2 O3 (s)

[0052] Combining formula (1-1) and (1-2), we can get:

[0053] MgO·TiO 2 (s)=MgO(s)+1 / 2Ti 2 O 3 (s)+1 / 2[O]

[0054] According to formula (1-3), when T = 1873K, That is, the reaction proceeds to the right, MgO·TiO 2 Decomposes to form MgO and Ti 2 O 3 .

[0055] Based on thermodynamic data, it can be further verified that when magnesium titanate powder is added to molten steel, it will decompose to form magnesium oxide, thereby increasing the recovery rate of magnesium in the steel sample.

[0056] In a vacuum induction furnace, DH36 ship plate steel was melted. After the molten steel was clarified, magnesium titanate powder treated by cored wire was added and kept warm for 20 minutes. The final solidified steel sample was water quenched at 1200℃, and rectangular steel blocks with a length, width and height of 55*10*10mm were cut out for impact test.

[0057] Small discs were cut from the four process samples and inlaid and polished. Finally, the oxide number density and magnesium content were counted under a SEM scanning electron microscope. Figure 2 shown.

[0058] Example 3

[0059] Put magnesium oxide powder (purity>99.9%) into a ball mill, add grinding balls at a ball-to-material ratio of 6:1, place the ball mill in a planetary ball mill, introduce nitrogen at a rate of 3L / min, maintain the temperature in the ball mill at around 0°C, pre-mill the magnesium oxide powder at a rotation speed of 400rpm, and mill for 4h.

[0060] Subsequently, under a low-temperature inert atmosphere, nano-aluminum powder and nano-silicon powder (particle size of 20-50 nm) were added to a ball mill in a volume ratio of 3:4:1 to magnesium oxide, and grinding balls were added in a ball-to-material ratio of 6:1. The ball milling was performed again at a speed of 400 rpm and a ball milling time of 4 hours, thereby forming a layer of composite powder of nano-aluminum powder and nano-silicon powder on the surface of the magnesium oxide powder.

[0061] The composite core-shell structure powder after ball milling is used as the core, and a 1.0 mm cold-rolled steel strip is used as the outer shell to roll it into a core wire with a diameter of Φ4.0. The core wire can be quickly immersed in the molten steel to accelerate the diffusion rate of magnesium oxide.

[0062] DH36 ship plate steel was melted in a vacuum induction furnace. After the molten steel was clarified, magnesium oxide powder treated by cored wire was added and kept warm for 20 minutes. The final solidified steel sample was water quenched at 1200℃, and rectangular steel blocks with a length, width and height of 55*10*10mm were cut out for impact test.

[0063] Example 4

[0064] Magnesium titanate powder (purity>99%, particle size<3μm) was placed in a ball mill, and grinding balls were added at a ball-to-material ratio of 6:1. The ball mill was placed in a planetary ball mill, and nitrogen was introduced at a rate of 3L / min. The temperature in the ball mill was maintained at about 0°C. The magnesium titanate powder was pre-milled at a rotation speed of 400rpm and a ball milling time of 4h.

[0065] Subsequently, under a low-temperature inert atmosphere, nano-aluminum powder and nano-silicon powder (particle size of 20-50 nm) were added to a ball mill at a volume ratio of 1.5:1.5:1 to magnesium titanate, and grinding balls were added at a ball-to-material ratio of 6:1. The ball milling was performed again at a rotation speed of 400 rpm and a ball milling time of 4 hours, thereby forming a layer of composite powder of nano-aluminum powder and nano-silicon powder on the surface of the magnesium titanate powder.

[0066] The composite core-shell structure powder after ball milling is used as the core, and a 1.0 mm cold-rolled steel strip is used as the outer shell to roll it into a core wire with a diameter of Φ4.0 mm. The core wire can be quickly immersed in the molten steel to accelerate the diffusion rate of magnesium titanate.

[0067] In a vacuum induction furnace, DH36 ship plate steel was melted, and after the molten steel was clarified, magnesium titanate powder treated by cored wire was added and kept warm for 20 minutes. The final solidified steel sample was water quenched at 1200°C, and rectangular steel blocks with a length, width and height of 55*10*10mm were cut out for impact test; steel blocks with a diameter of 15-20mm and a height of 10-20mm were cut out, the surface was polished, and then etched with 5% nitric acid solution to observe its metallographic structure.

[0068] Small discs were cut from the four process samples and inlaid and polished. Finally, the oxide number density and magnesium content were counted under a SEM scanning electron microscope. Figure 2 As shown. By observing the metallographic structure, Figure 1 It can be seen that the oxides in the steel sample promote the formation of a large amount of intragranular acicular ferrite.

[0069] Example 5

[0070] Put magnesium oxide powder (purity>99.9%) into a ball mill, add grinding balls at a ball-to-material ratio of 6:1, place the ball mill in a planetary ball mill, introduce nitrogen at a rate of 3L / min, maintain the temperature in the ball mill at around 0°C, pre-mill the magnesium oxide powder at a rotation speed of 400rpm, and mill for 4h.

[0071] Subsequently, under a low-temperature inert atmosphere, nano-silicon powder (particle size of 70-100 nm) was added into a ball mill at a volume ratio of 2:1 to magnesium oxide, and grinding balls were added at a ball-to-material ratio of 6:1. The ball milling was performed again at a rotation speed of 400 rpm for 4 hours, thereby forming a layer of nano-silicon powder on the surface of the magnesium oxide powder.

[0072] The composite core-shell structure powder after ball milling is used as the core, and a 1.0 mm cold-rolled steel strip is used as the outer shell to roll it into a core wire with a diameter of Φ4.0 mm.

[0073] DH36 ship plate steel was melted in a vacuum induction furnace. After the molten steel was clarified, magnesium oxide powder treated by cored wire was added and kept warm for 20 minutes. The final solidified steel sample was water quenched at 1200℃, and rectangular steel blocks with a length, width and height of 55*10*10mm were cut out for impact test.

[0074] Example 6

[0075] Magnesium titanate powder (purity>99%, particle size<3μm) was placed in a ball mill, and grinding balls were added at a ball-to-material ratio of 6:1. The ball mill was placed in a planetary ball mill, and nitrogen was introduced at a rate of 3L / min. The temperature in the ball mill was maintained at about 0°C. The magnesium titanate powder was pre-milled at a rotation speed of 400rpm and a ball milling time of 4h.

[0076] Subsequently, under a low-temperature inert atmosphere, nano-silicon powder (particle size of 70-100 nm) was added into a ball mill at a volume ratio of 2:1 to magnesium titanate, and grinding balls were added at a ball-to-material ratio of 6:1. The ball milling was performed again at a speed of 400 rpm for 4 hours, thereby forming a layer of nano-silicon powder on the surface of the magnesium titanate powder.

[0077] The composite core-shell structure powder after ball milling was used as the core, and a 1.0 mm cold-rolled steel strip was used as the outer shell to roll it into a core wire with a diameter of Φ4.0 mm.

[0078] In a vacuum induction furnace, DH36 ship plate steel was melted. After the molten steel was clarified, magnesium titanate powder treated by cored wire was added and kept warm for 20 minutes. The final solidified steel sample was water quenched at 1200℃, and rectangular steel blocks with a length, width and height of 55*10*10mm were cut out for impact test.

[0079] Example 7

[0080] Magnesium titanate powder (purity>99%, particle size<3μm) was placed in a ball mill, and grinding balls were added at a ball-to-material ratio of 6:1. The ball mill was placed in a planetary ball mill, and nitrogen was introduced at a rate of 3L / min. The temperature in the ball mill was maintained at about 0°C. The magnesium titanate powder was pre-milled at a rotation speed of 400rpm and a ball milling time of 4h.

[0081] Subsequently, under a low-temperature inert atmosphere, nano-aluminum powder and nano-silicon powder were added into a ball mill at a volume ratio of 1.5:1.5:1 to magnesium titanate, and grinding balls were added at a ball-to-material ratio of 6:1. The ball milling was performed again at a rotation speed of 400 rpm for 4 hours, thereby forming a layer of composite powder of nano-aluminum powder and nano-silicon powder on the surface of the magnesium titanate powder.

[0082] The ball-milled composite core-shell structure powder was sintered to form a block structure, and then wrapped with a tungsten mesh. DH36 ship plate steel was melted in a vacuum induction furnace. After the molten steel was clarified, the composite core-shell structure powder wrapped with a tungsten mesh was put into the molten steel from the top and kept warm for 20 minutes. The final solidified steel sample was water quenched at 1200℃, and a rectangular steel block with a length, width and height of 55*10*10mm was cut out for impact test.

[0083] Comparative Example 1

[0084] A magnesium alloy (purity>99.9%) is placed in a graphite mold, nitrogen is introduced at a rate of 3L / min, the temperature in the ball mill is maintained at around 0°C, and a 1.0mm cold-rolled steel strip is used as the outer shell to roll the powder formed by ball milling into a cored wire with a diameter of Φ4.0mm. The cored wire can be quickly immersed in the molten steel to accelerate the diffusion rate of the magnesium alloy.

[0085] In a vacuum induction furnace, DH36 ship plate steel was melted. After the molten steel was clarified, magnesium alloy treated by cored wire was added and kept warm for 20 minutes. The final solidified steel sample was water quenched at 1200℃, and rectangular steel blocks with a length, width and height of 55*10*10mm were cut out for impact test.

[0086] Comparative Example 2

[0087] Magnesium oxide powder (purity> 99.9%) was placed in a graphite mold, nitrogen was introduced at a rate of 3 L / min, the temperature in the ball mill was maintained at about 0°C, and a 1.0 mm cold-rolled steel strip was used as the outer shell to roll the powder formed by ball milling into a cored wire with a diameter of Φ4.0 mm.

[0088] DH36 ship plate steel was melted in a vacuum induction furnace. After the molten steel was clarified, magnesium oxide powder treated by cored wire was added and kept warm for 20 minutes. The final solidified steel sample was water quenched at 1200℃, and rectangular steel blocks with a length, width and height of 55*10*10mm were cut out for impact test.

[0089] The steels prepared in Examples 1 to 7 and Comparative Examples 1 to 2 were subjected to IGF nucleation, impact energy and oxide characteristic detection experiments, and the results are shown in the following table:

[0090] Table 1 IGF nucleation, impact energy and oxide characteristic test results of the steel produced in Examples 1 to 7 and Comparative Examples 1 to 2

[0091]

[0092]

[0093] As can be seen from Table 1, in Comparative Example 1, magnesium alloy is directly added, and the bulk density of oxide in the steel sample is relatively small. Since the saturated vapor pressure of magnesium alloy is relatively high when it is added to molten steel, it is easy to cause splashing and cannot become an effective component in the steel. Therefore, it is found under SEM electron microscope that the oxide is basically an original component in the steel, and the average size and size range are too large to induce nucleation. In Comparative Example 2, magnesium oxide is directly coated on cold-rolled steel strip as the core wire. Since the wettability of magnesium oxide with molten steel is relatively poor, it is also difficult to become an effective component in the steel. The bulk density of oxide in the steel sample is also small, and nucleation cannot be induced. Therefore, magnesium alloy and magnesium oxide are not suitable for direct application in the external addition method.

[0094] In both Example 1 and Example 2, nano-aluminum powder is added as a modifier to improve the wettability of magnesium oxide powder with molten steel. In both Example 5 and Example 6, nano-silicon powder is added to reduce the wetting angle between magnesium oxide and molten steel, thereby improving the wettability of magnesium oxide powder with molten steel. As shown in Table 1, the bulk density of the steel sample oxide obtained in Example 1, Example 2, Example 5, and Example 6 increases to a certain extent, and the IGF nucleation index also increases. It is found under SEM electron microscope that magnesium oxide is successfully introduced. However, due to the relatively large particle size of the oxide, the toughness of the steel sample is relatively low. Figure 3 shown.

[0095] Compared with Examples 1, 2, 5, and 6, Examples 3 and 4 both add nano aluminum powder and nano silicon powder at the same time. As shown in Table 1, the bulk density is significantly improved, and the IGF nucleation index is also significantly improved. Observation under a SEM electron microscope found that the introduced composite magnesium oxide inclusions have a smaller particle size and better distribution uniformity. This is due to the reactivity of magnesium and aluminum elements, and the combination of nano silicon powder reducing the wetting angle between magnesium oxide and molten steel, and improving the wettability of magnesium oxide powder and molten steel, so that magnesium oxide can stay in the molten steel for a longer time, thereby obtaining a better magnesium yield.

[0096] Compared with Example 3, the magnesium oxide used in Example 4 is magnesium titanate. As shown in Table 1, the bulk density and IGF nucleation index of the oxide in Example 4 are both improved relative to Example 3, and the toughness of the final steel sample is also better. It can be seen from the thermodynamic data that at a temperature of 1873K, when magnesium titanate powder is added to molten steel, it will decompose to generate magnesium oxide and titanium dioxide. Titanium dioxide can improve the wettability of magnesium oxide with molten steel, allowing magnesium oxide to stay in the molten steel, thereby achieving a better yield than Example 3 using magnesium oxide. By comparing Example 4 with Example 7, it can be seen that the use of cored wire to feed the material is better than directly feeding it into the molten steel, and the yield of magnesium is better.

[0097] Comparing Examples 1-7 and Comparative Examples 1 and 2, the results show that the product of the present application can successfully introduce magnesium oxide into the steel sample, and no violent splashing occurs during the experiment. Compared with the direct addition of magnesium oxide powder and magnesium alloy in Comparative Examples 1 and 2, the danger of operation is reduced and the magnesium recovery rate in the steel sample is improved. According to the results of the impact test on the steel sample in Table 1, the toughness of the steel sample obtained by using the product of the present invention to treat the molten steel with magnesium alloy is significantly improved. Among them, the toughness improvement of Example 3 and Example 4 is the most obvious, and the impact test performance is the best.

[0098] Example 8

[0099] Magnesium titanate powder (purity> 99%, particle size< 3μm) was placed in a ball mill, and grinding balls were added at a ball-to-material ratio of 5:1. The ball mill was placed in a planetary ball mill, and nitrogen was introduced at a rate of 2L / min. The temperature in the ball mill was maintained at about -3°C. The magnesium titanate powder was pre-milled at a rotation speed of 300rpm and a ball milling time of 6h.

[0100] Subsequently, under a low-temperature inert atmosphere, nano-aluminum powder (nano-aluminum powder having a particle size of 7 to 10 μm) and nano-silicon powder (having a particle size of 40 to 70 nm) were added to a ball mill at a volume ratio of 3:2:1 to magnesium titanate, and grinding balls were added at a ball-to-material ratio of 5:1. The ball milling was performed again at a rotation speed of 300 rpm for 6 hours, thereby forming a layer of composite powder of nano-aluminum powder and nano-silicon powder on the surface of the magnesium titanate powder.

[0101] The ball-milled composite core-shell structure powder was used as the core, and a 1.2 mm cold-rolled steel strip was used as the outer shell to roll it into a cored wire with a diameter of Φ5.0 mm. The cored wire obtained in this embodiment was used for magnesium alloying of molten steel, and the effect was similar to that of Example 4.

[0102] Example 9

[0103] Magnesium titanate powder (purity> 99%, particle size< 3μm) was placed in a ball mill, and grinding balls were added at a ball-to-material ratio of 7:1. The ball mill was placed in a planetary ball mill, and nitrogen was introduced at a rate of 10L / min. The temperature in the ball mill was maintained at about 3°C. The magnesium titanate powder was pre-milled at a rotation speed of 500rpm and a ball milling time of 3h.

[0104] Subsequently, under a low-temperature inert atmosphere, nano-aluminum powder (nano-aluminum powder having a particle size of 7 to 10 μm) or nano-silicon powder is added to a ball mill at a volume ratio of 4:1 to magnesium titanate, and grinding balls are added at a ball-to-material ratio of 7:1. The ball milling is performed again at a rotation speed of 500 rpm for 3.5 hours, thereby forming a layer of nano-aluminum powder or nano-silicon powder on the surface of the magnesium titanate powder.

[0105] The ball-milled composite core-shell structure powder was used as the core, and a 0.8 mm cold-rolled steel strip was used as the outer shell to roll it into a cored wire with a diameter of Φ3.0 mm. The cored wire obtained in this embodiment was used for magnesium alloying of molten steel, and the effect was similar to that of Example 2.

[0106] Example 10

[0107] Put magnesium oxide powder into a ball mill, add grinding balls at a ball-to-material ratio of 5:1, place the ball mill in a planetary ball mill, introduce nitrogen at a rate of 7 L / min, maintain the temperature in the ball mill at around 1°C, pre-mill the magnesium titanate powder at a rotation speed of 450 rpm, and mill for 3.5 h.

[0108] Subsequently, under a low-temperature inert atmosphere, nano-aluminum powder and nano-silicon powder were added into a ball mill in a volume ratio of 2:2:1 to magnesium oxide, and grinding balls were added in a ball-to-material ratio of 5:1. The ball milling was performed again at a rotation speed of 450 rpm for 3 hours, thereby forming a layer of composite powder of nano-aluminum powder and nano-silicon powder on the surface of the magnesium oxide powder.

[0109] The ball-milled composite core-shell structure powder was used as the core, and a 1.2 mm cold-rolled steel strip was used as the outer shell to roll it into a cored wire with a diameter of Φ4.5 mm. The cored wire obtained in this embodiment was used for magnesium alloying of molten steel, and the effect was similar to that of Example 3.

[0110] In summary, magnesium oxide was successfully introduced into the molten steel by externally adding core-shell structure powder. Different from the internal generation method of magnesium oxide by adding magnesium alloy, this external addition method can achieve the purpose of increasing the magnesium recovery rate in the molten steel by controlling the type of added particles.

[0111] The core-shell structure powder composed of magnesium oxide and nano-aluminum powder and / or nano-silicon powder is added externally, which can effectively introduce magnesium oxide into the molten steel. This method effectively improves the reactivity and wettability of magnesium oxide in the molten steel by adding nano-aluminum powder and / or nano-silicon powder. The uniformity of oxide inclusions and the IGF nucleation index directly affect the toughness of the steel sample. According to the impact test and theoretical analysis, the relationship between the uniformity of magnesium oxide and the IGF nucleation index on the toughness of the steel sample satisfies the following model (such as Figure 4 shown):

[0112]

[0113] Among them, Ak is the impact energy to measure the toughness of the steel sample, the unit is J, D m To determine the uniformity of magnesium oxide in the treated steel,

[0114] P m is the IGF nucleation index based on magnesium oxide, and B, C, D, E, and F are fitting constants.

[0115] The relationship between the toughness of the steel sample and the uniformity of magnesium oxide and the IGF nucleation index satisfies the formula:

[0116] Ak=(117~393)+(42~61) / {[1+exp(((2.156~4.582)-D m ) / (0.781~1.697)))×

[0117] (1+exp(((0.0176~0.712)-P m ) / (0.177~0.577)]}

[0118] Among them, Ak is the impact energy to measure the toughness of the steel sample, the unit is J, D m is the uniformity of magnesium oxide in the treated steel, P m is the IGF nucleation index based on magnesium oxide.

Claims

1. A product for magnesium alloying of molten steel, characterized in that: It comprises an outer shell and a powder core wrapped in the outer shell. The powder core adopts a powder with a composite core-shell structure, with magnesium oxide particles as the inner core, and the surface of the magnesium oxide particles is coated with a modifier; the modifier comprises nano aluminum powder and / or nano silicon powder.

2. The product for magnesium alloying of molten steel according to claim 1, characterized in that: The magnesium oxide particles include magnesium oxide and / or magnesium titanate.

3. The product for magnesium alloying of molten steel according to claim 1 or 2, characterized in that: The volume ratio of the magnesium oxide particles to the nano-aluminum powder is 1:1.5 to 1:4, and the volume ratio of the magnesium oxide particles to the nano-silicon powder is 1:1.5 to 1:4; And / or the particle size of the magnesium oxide particles is 50nm-3μm; the particle size of the nano silicon powder is 20-100nm; the particle size of the nano aluminum powder is 2-10μm.

4. The product for magnesium alloying of molten steel according to claim 1 or 2, characterized in that: The outer shell is made of steel strip, which is wrapped around the outside of the powder core to form a cored wire product; or the outer shell is made of a hollow sealing structure, which is wrapped around the outside of the powder core to form an overall block structure.

5. The product for magnesium alloying of molten steel according to claim 4, characterized in that: The diameter of the cored wire is Φ3.0 mm to Φ5.0 mm, and the thickness of the outer shell steel strip is 0.8 mm to 1.2 mm.

6. A method for producing a product for magnesium alloying of molten steel as claimed in any one of claims 1 to 5, characterized in that: include: The powder core of the composite core-shell structure is sealed and coated by an outer shell.

7. The method for producing a product for magnesium alloying of molten steel according to claim 6, characterized in that: Also includes: The modifier powder is coated on the surface of the magnesium oxide particles to form a powder core with a composite core-shell structure.

8. The method for producing a product for magnesium alloying of molten steel according to claim 7, characterized in that: The method of coating the modifier powder on the surface of the magnesium oxide particles comprises: Mechanically ball milling the powder containing magnesium oxide particles and the modifier under a low temperature inert atmosphere, wherein the low temperature is -3°C to 3°C; and / or Before mechanically ball-milling the powder containing magnesium oxide particles and the modifier, the magnesium oxide particles are pre-ball-milled.

9. The method for producing a product for magnesium alloying of molten steel according to claim 8, characterized in that: During the mechanical ball milling of the powder containing magnesium oxide particles and the modifier and the pre-ball milling of the magnesium oxide particles, low-temperature nitrogen is introduced to maintain the low temperature state inside the equipment, and the nitrogen introduction rate is 2 to 10 L / min; the rotation speed of the ball milling and pre-ball milling is 300 to 500 rpm, and the ball milling time is 3 to 6 hours.

10. Use of the product for magnesium alloying of molten steel as claimed in any one of claims 1 to 5 in magnesium treatment of molten steel for ship plate steel.