Positive electrode material, preparation method thereof and electrochemical device

By covering the surface of the core of the positive electrode material with a rest angle of less than 50°, a high-flowability cladding layer is formed, which solves the problems of poor fluidity and slow sieving speed of the ternary positive electrode material, and improves production efficiency and product quality. Reduced costs.

CN118919694APending Publication Date: 2024-11-08NANTONG RESHINE NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411172536.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The ternary cathode material has poor fluidity and slow screening speed during the production process, resulting in reduced production efficiency, unstable product quality and increased production costs.

Method used

The core surface of the positive electrode material is coated with a fluid substance with a rest angle less than 50°, forming a high-flow coating layer. The mass percentage of the fluid substance to the core is 0.05% to 0.2%, and the sieving speed is increased by sintering treatment To 150kg/h~250kg/h.

Benefits of technology

It improves the fluidity and electrochemical properties of the cathode material, improves screening efficiency and product quality, reduces production costs, and improves comprehensive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919694A_ABST
    Figure CN118919694A_ABST
Patent Text Reader

Abstract

The invention discloses a positive electrode material, a preparation method thereof and an electrochemical device, the positive electrode material comprises an inner core and a coating layer coated on the surface of the inner core, the coating layer contains a flowing substance, the repose angle theta of the flowing substance is less than or equal to 50 degrees, the mass percent of the flowing substance in the coating layer to the inner core is 0.05%-0.2%, and the positive electrode material is sieved under the condition of 400 meshes. And the sieving speed of the positive electrode material is 150 kg / h to 250 kg / h. The surface of the inner core is properly coated with the substance with good fluidity, so that the fluidity of the positive electrode material is improved, the problems of poor fluidity and low sieving efficiency of the positive electrode material in the sieving process are solved, and the comprehensive performance of the positive electrode material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of new energy materials, and in particular to a positive electrode material and a preparation method thereof, and an electrochemical device. Background Art

[0002] Ternary cathode materials, such as lithium nickel cobalt manganese oxide, are widely used in electric vehicles, portable electronic devices, and energy storage systems due to their excellent electrochemical properties and high energy density. However, ternary cathode materials have problems with poor fluidity and slow screening speed during the production process. These problems will lead to reduced production efficiency of ternary cathode materials, unstable product quality, and increased production costs. Summary of the invention

[0003] In view of this, in order to solve at least one of the above technical problems, an embodiment of the present application provides a positive electrode material.

[0004] In addition, the embodiments of the present application also provide a method for preparing the aforementioned positive electrode material, and an electrochemical device using the positive electrode material.

[0005] An embodiment of the present application provides a positive electrode material, which includes a core and a coating layer coated on the surface of the core, the coating layer contains a fluidity substance, the angle of repose θ of the fluidity substance is ≤50°, the mass percentage of the fluidity substance in the coating layer to the core is 0.05% to 0.2%, and the positive electrode material is sieved under 400 mesh conditions, and the sieving speed is 150kg / h to 250kg / h.

[0006] In some possible embodiments, the fluid material includes at least one of graphite, talc, molybdenum disulfide and boron nitride.

[0007] In some possible embodiments, the bulk density of the positive electrode material is 0.8 g / cm 3 ~1.0g / cm 3 .

[0008] In some possible embodiments, the coating layer has a thickness of 1 nm to 3 nm.

[0009] In some possible embodiments, the particle size D50 of the positive electrode material is 2 μm to 10 μm.

[0010] The present application also provides a method for preparing a positive electrode material, comprising:

[0011] Mixing a fluid substance with a cathode material substrate to obtain a mixed material, wherein the angle of repose θ of the fluid substance is ≤50°, and the mass percentage of the fluid substance to the cathode material substrate is 0.05% to 0.2%; and

[0012] The mixed material is sintered to obtain the positive electrode material, wherein the mixed material is sieved under 400 mesh conditions, and the sieving speed of the positive electrode material is 150kg / h to 250kg / h.

[0013] In some possible embodiments, the fluid material includes at least one of graphite, talc, molybdenum disulfide and boron nitride.

[0014] In some possible embodiments, in the step of mixing the fluid substance with the positive electrode material substrate, the mixing is dry mixing.

[0015] In some possible embodiments, in the step of mixing the fluid substance with the positive electrode material substrate, the mixing rotation speed is 1000 rpm to 2000 rpm.

[0016] In some possible embodiments, in the step of sintering the mixed material, the sintering temperature is 300° C. to 500° C., and the sintering time is 5 h to 15 h.

[0017] In addition, an embodiment of the present application further provides an electrochemical device, which includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet includes a positive electrode material, and the positive electrode material is the aforementioned positive electrode material.

[0018] Compared with the prior art, the present application achieves a positive electrode material having a stable, uniform, high-fluidity coating layer with a suitable coating amount by coating the inner core surface of the positive electrode material with a fluid substance having a repose angle of less than 50°, thereby reducing the adsorption force between the positive electrode material particles, thereby improving the fluidity of the positive electrode material while taking into account the electrochemical properties of the positive electrode material, solving the problem of low screening efficiency of the positive electrode material during the screening process, and improving the comprehensive performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A process flow chart of the method for preparing the positive electrode material provided in an embodiment of the present application.

[0020] Figure 2 This is a schematic diagram of the structure of the electrochemical device provided in an embodiment of the present application.

[0021] Figure 3A This is a scanning electron microscope image of the positive electrode material of Example 1 of the present application.

[0022] Figure 3B This is a scanning electron microscope image of the positive electrode material of comparative example 1 of the present application.

[0023] Figure 4This is a comparison chart of the charge capacity of batteries prepared with the positive electrode materials in Examples 1-4 of the present application and Comparative Examples 1-3.

[0024] Figure 5 This is a comparison chart of the power cycle performance of batteries prepared with the positive electrode materials in Examples 1-4 of the present application and Comparative Examples 1-3.

[0025] Figure 6 This is a comparison chart of the loose density of the positive electrode materials in Examples 1-4 of the present application and Comparative Examples 1-3.

[0026] Figure 7 This is a comparison chart of the screening speeds of the positive electrode materials in Examples 1-4 and Comparative Examples 1-3 of the present application. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0028] Positive electrode materials (especially ternary positive electrode materials) may have poor fluidity during the production process, which leads to slow screening speed of positive electrode materials, reduced production efficiency, increased production costs, and unstable product quality. The inventors of this application have found that the fluidity of positive electrode materials may be related to the particle size and shape, surface characteristics, water content, etc. of the positive electrode materials, and the screening speed of positive electrode materials may also be related to factors such as the screening equipment and the type of additives used.

[0029] To this end, an embodiment of the present application provides a positive electrode material with good fluidity, the positive electrode material comprising a core and a coating layer coated on the surface of the core, the coating layer containing a fluidity substance, the repose angle θ of the fluidity substance ≤ 50°, the mass percentage of the fluidity substance in the coating layer to the core is 0.05% to 0.2%, and the positive electrode material is sieved under 400 mesh conditions, and the sieving speed is 150kg / h to 250kg / h.

[0030] The repose angle test refers to GB / T 11986-1989. The fluid material is evenly poured into a funnel with a smooth inner wall, and the funnel is gently smoothed to allow the fluid material to pass through it. After the fluid material is naturally stabilized, the repose angle θ=arctan(h / r) of the accumulation formed by the fluid material is measured, where h is the cone height of the accumulation and r is the radius of the accumulation.

[0031] When the repose angle θ of the fluid material is ≤50°, it indicates that the fluid material has good and suitable circulation. By forming a coating layer with high fluidity on the surface of the inner core of the positive electrode material, the adsorption force between the positive electrode material particles is effectively reduced, and the surface properties of the positive electrode material are improved, thereby improving the fluidity of the positive electrode material, improving the screening efficiency of the positive electrode material during the screening process, and also improving the quality of the positive electrode material. The repose angle θ of the fluid material can further be 30° to 50°. Within this range, the fluid material can have a good coating effect and make the structure of the positive electrode material more stable, while taking into account both economy and practicality.

[0032] In the positive electrode material, the mass percentage of the fluid substance in the coating layer to the core is 0.05% to 0.2%. The fluid substance in the above range can effectively improve the surface fluidity of the positive electrode material, and at the same time, it can also minimize the thickness of the coating layer so that the thickness of the coating layer is not too thick, so as to take into account the energy density, electrochemical properties and production costs of the positive electrode material, and improve the comprehensive performance of the positive electrode material. If the mass percentage of the coating layer and the core in the positive electrode material is too low (less than 0.02%), it will lead to poor coating effect, poor fluidity of the positive electrode material, and it is difficult to effectively improve the screening speed of the positive electrode material; if the mass percentage of the coating layer and the core in the positive electrode material is too high (higher than 0.2%), it will lead to a decrease in the capacity and cycle performance of the positive electrode material, and the comprehensive performance will be affected. The mass percentage of the coating layer and the core in the positive electrode material can further be 0.1% to 0.2%, and can be 0.05%, 0.08%, 0.1%, 0.12%, 0.15%, 0.18% or 0.2%, etc.

[0033] When an appropriate amount of the above-mentioned fluid material is used as a coating layer, the screening speed of the positive electrode material can reach 150kg / h to 250kg / h. The screening speed of the positive electrode material within the above range indicates that the positive electrode material has good fluidity and a faster screening speed, which is beneficial to improve the production efficiency of the positive electrode material while reducing production costs. The screening speed of the positive electrode material can further be 175kg / h to 215kg / h, and can be exemplarily 150kg / h, 170kg / h, 180kg / h, 195kg / h, 203kg / h, 206kg / h, 210kg / h, 212kg / h, 215kg / h, 230kg / h, 240kg / h or 250kg / h, etc.

[0034] In some embodiments, the fluid material may include at least one of graphite, talc, molybdenum disulfide, boron nitride, etc. The fluid materials mentioned above all have good lubricity, chemical stability and electrical conductivity, which are beneficial to improving the fluidity of the positive electrode material and the electrochemical performance of the positive electrode material.

[0035] Exemplarily, the fluid material can be graphite. Since graphite has good fluidity, it can effectively reduce the adsorption force between the positive electrode material particles. By coating a certain amount of graphite on the surface of the inner core to form a uniform coating layer, the surface properties of the positive electrode material can be improved to solve the problems of poor fluidity and low screening efficiency of the positive electrode material during the screening process. Moreover, graphite also has good conductivity and can improve the overall conductivity of the positive electrode material. In addition, the graphite coating can also provide protection for the positive electrode material and reduce the oxidation and degradation of the positive electrode material.

[0036] In some embodiments, the bulk density of the positive electrode material can be 0.8 g / cm 3 ~1.0g / cm 3 . The higher the bulk density of the positive electrode material, the better the fluidity of the positive electrode material. This is because the excellent fluidity of the positive electrode material makes the positive electrode material more compact when stacked and can be more evenly filled in the container, reducing the gaps between the positive electrode material particles, thereby increasing the bulk density of the positive electrode material. The bulk density of the positive electrode material is within the above range, which means that the battery prepared from the positive electrode material contains more active materials per unit volume, thereby ensuring the energy density and power density of the battery. The bulk density of the positive electrode material can further be 0.9g / cm 3 ~1.0g / cm 3 , which can be 0.8 g / cm 3 , 0.85g / cm 3 , 0.9g / cm 3 , 0.95g / cm 3 or 1.0g / cm 3 wait.

[0037] In some embodiments, the coating layer may have a thickness of 1 nm to 3 nm. A coating layer of suitable thickness may improve the fluidity of the positive electrode material while also improving the conductivity of the positive electrode material, thereby maintaining the buckling performance of the manufactured battery. Moreover, a coating layer of suitable thickness may also provide an additional protective layer for the positive electrode material, reducing the surface side reactions of the positive electrode material during use, thereby improving the long-term stability and durability of the positive electrode material. The coating layer may further have a thickness of 1.5 nm to 2 nm, and may be 1 nm, 1.5 nm, 2 nm, 2.5 nm, or 3 nm, etc., for example.

[0038] In some embodiments, the particle size D50 of the positive electrode material may be 2 μm to 10 μm. The uniformity of the particle size and shape of the positive electrode material also has a certain influence on the fluidity of the positive electrode material. Therefore, controlling the particle size of the positive electrode material is conducive to further improving the fluidity of the positive electrode material, thereby improving production efficiency and product quality. The particle size D50 of the positive electrode material may further be 5 μm to 8 μm, and may be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, for example.

[0039] Compared with the prior art, the positive electrode material provided in the embodiment of the present application has the following beneficial effects:

[0040] 1. The coating layer of the positive electrode material provided in the embodiment of the present application contains a high-fluidity substance, which can effectively reduce the adsorption between the positive electrode material particles, give the positive electrode material good fluidity, and improve the loose density, screening speed and production efficiency of the positive electrode material, which is of great significance in industrial production.

[0041] 2. The content of high fluidity substances in the positive electrode material is moderate, which can effectively improve the surface fluidity of the positive electrode material on the one hand, and reduce the production cost of the positive electrode material on the other hand.

[0042] See also Figure 1 As shown, the preparation method of the positive electrode material provided in the embodiment of the present application specifically includes the following steps:

[0043] Step S1, mixing the fluid substance with the positive electrode material substrate to obtain a mixed material, wherein the repose angle θ of the fluid substance is ≤50°, and the mass percentage of the fluid substance to the positive electrode material substrate is 0.05% to 0.2%.

[0044] Taking nickel-cobalt-manganese ternary positive electrode material as an example, a certain amount of fluid substance and lithium-nickel-cobalt-manganese oxide substrate are fully mixed to obtain a coated ternary positive electrode material mixture, wherein the repose angle θ of the fluid substance is ≤50°, and the repose angle θ of the fluid substance can further be 30°~50°.

[0045] The mass percentage of the fluid substance to the positive electrode material substrate is 0.05% to 0.2%. The fluid substance within this content range can form an effective and uniform coating layer on the substrate surface, improve the fluidity and conductivity of the positive electrode material, and control the production cost at the same time.

[0046] In some embodiments, the fluid material may include at least one of graphite, talc, molybdenum disulfide, and boron nitride. The above fluid materials all have good lubricity, chemical stability, and electrical conductivity, which are beneficial to improving the fluidity and electrochemical properties of the positive electrode material. Exemplarily, the fluid material may be graphite. Compared with graphite derivatives such as graphene and graphite oxide, graphite is relatively easier to obtain and process, and has a greater cost advantage.

[0047] In some embodiments, the mixing method may be dry mixing. Dry mixing does not require the use of liquid or solvent. Liquid media may cause adhesion and agglomeration between raw material particles, while dry mixing can effectively avoid the above problems, thereby maintaining the fluidity and uniformity of raw material particles; and dry mixing has little effect on the particle morphology, so the original morphology and properties of the mixed raw materials can be maintained. It is understood that the mixing method includes but is not limited to dry mixing, and any method that can fully mix the raw materials without adverse effects is acceptable.

[0048] In some embodiments, dry mixing can be performed in a high-speed mixer, and the mixing speed can be 1000 rpm to 2000 rpm. A suitable speed is conducive to further mixing the raw materials to ensure the uniformity of subsequent sintering. The mixing speed can further be 1500 rpm to 2000 rpm, and can be illustratively 1000 rpm, 1200 rpm, 1400 rpm, 1500 rpm, 1800 rpm or 2000 rpm, etc.

[0049] Step S2, sintering the mixed material in step S1 to obtain a positive electrode material, wherein the mixed material is sieved under 400 mesh conditions, and the sieving speed of the obtained positive electrode material is 150kg / h to 250kg / h.

[0050] In some embodiments, the sintering temperature may be 300°C to 500°C. Low-temperature sintering in the range of 300°C to 500°C is beneficial to maintaining the stability of the fluid material, and can effectively attach the fluid material to the surface of the positive electrode material substrate to form a stable coating layer. At the same time, low-temperature sintering can avoid recrystallization of the positive electrode material substrate, resulting in reduced performance; lower sintering temperatures can also help control the thickness of the coating layer to ensure that the coating layer is uniform and not too thick. The sintering temperature may further be 350°C to 450°C, and may be 300°C, 350°C, 400°C, 450°C or 500°C, etc., for example.

[0051] In some embodiments, the sintering time may be 5 hours to 15 hours. Adequate sintering time can enhance the adhesion between the coating layer and the cathode material substrate, ensuring that the coating layer will not fall off during subsequent processing or use. The sintering time may further be 10 hours to 15 hours, and may be 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, or 15 hours, etc.

[0052] In some embodiments, the sintering atmosphere can be air or oxygen, which is beneficial to control the oxidation of the fluid substance and the positive electrode material substrate, optimize the adhesion of the coating layer, avoid degradation of the positive electrode material, and balance production costs and process requirements.

[0053] Compared with the prior art, the method for preparing the positive electrode material provided in the embodiment of the present application has the following beneficial effects:

[0054] 1. By adding fluid materials for coating, the fluidity of the positive electrode material is effectively improved, the screening speed of the positive electrode material is increased, and the quality of the positive electrode material is improved.

[0055] 2. By controlling the coating amount of the fluid substance, a uniform and stable coating layer is further formed to ensure the comprehensive performance of the positive electrode material and control the production cost.

[0056] 3. By adopting a dry mixing method, the adverse effects of solvents on the fluidity and uniformity of the positive electrode material can be avoided, which is conducive to further improving the fluidity and quality stability of the positive electrode material.

[0057] 4. Low-temperature sintering is beneficial to maintaining the stability of the fluid substance, effectively attaching the fluid substance to the surface of the positive electrode material substrate to form a stable and uniform coating layer, and avoiding the recrystallization of the positive electrode material substrate to affect the performance.

[0058] 5. This preparation method is simple, efficient, and low-cost, which is conducive to the large-scale production of positive electrode materials and has excellent commercial prospects.

[0059] See also Figure 2 As shown, an embodiment of the present application also provides an electrochemical device (such as a battery), wherein the electrochemical device 100 includes a positive electrode plate 10, a negative electrode plate 20, an isolation membrane 30 and an electrolyte 40, wherein the positive electrode plate 10 includes a positive electrode material, and the positive electrode material is the positive electrode material as described above.

[0060] The electrochemical device 100 prepared using the aforementioned positive electrode material has a faster processing speed and a shorter production cycle due to the improved screening speed of the positive electrode material, thereby effectively improving production efficiency; and a higher screening speed can more evenly distribute the positive electrode material, ensuring the uniformity and consistency of the positive electrode material, thereby improving the performance stability of the electrochemical device.

[0061] The above-mentioned positive electrode material and its preparation method and electrochemical device are further described below through specific examples.

[0062] Example 1

[0063] Step 1: Weigh 200kg LiNi x Co y Mn 1-x-y The O2 ternary positive electrode material substrate is the positive electrode material substrate, wherein x=0.6, y=0.2, that is, the positive electrode material is Ni:Co:Mn with a molar percentage of 6:2:2, and is put into a high-speed mixer with a feeding weight of 200 kg; graphite is weighed according to 0.10% of the mass of the positive electrode material substrate, and is put into a high-speed mixer and mixed at a rotation speed of 1500 rpm to obtain a mixed material.

[0064] Step 2: Sinter the mixed material in an air atmosphere at a sintering temperature of 400° C. for 10 h to obtain a positive electrode material.

[0065] Example 2

[0066] The specific process of the preparation process refers to Example 1, and the difference from Example 1 is that the amount of graphite in step 1 is 0.05% of the mass of the positive electrode material substrate, and the preparation method of the remaining positive electrode materials is basically the same as that in Example 1, which will not be described in detail here.

[0067] Example 3

[0068] The specific process of the preparation process refers to Example 1, and the difference from Example 1 is that the amount of graphite in step 1 is 0.15% of the mass of the positive electrode material substrate, and the preparation method of the remaining positive electrode materials is basically the same as that in Example 1, which will not be described in detail here.

[0069] Example 4

[0070] The specific process of the preparation process refers to Example 1, and the difference from Example 1 is that the amount of graphite in step 1 is 0.20% of the mass of the positive electrode material substrate, and the preparation method of the remaining positive electrode materials is basically the same as that in Example 1, which will not be described in detail here.

[0071] Comparative Example 1

[0072] The specific process of the preparation process refers to Example 1. The difference from Example 1 is that no graphite is added in step 1, and the preparation method of the remaining positive electrode materials is basically the same as that of Example 1, which will not be described in detail here.

[0073] Comparative Example 2

[0074] The specific process of the preparation process refers to Example 1, and the difference from Example 1 is that the amount of graphite in step 1 is 0.02% of the mass of the positive electrode material substrate, and the preparation method of the remaining positive electrode materials is basically the same as that of Example 1, which will not be described in detail here.

[0075] Comparative Example 3

[0076] The specific process of the preparation process refers to Example 1, and the difference from Example 1 is that the amount of graphite in step 1 is 0.25% of the mass of the positive electrode material substrate, and the preparation method of the remaining positive electrode materials is basically the same as that in Example 1, which will not be described in detail here.

[0077] The following tests were performed on the positive electrode materials obtained in Examples 1-4 and Comparative Examples 1-3.

[0078] 1. The positive electrode materials prepared in Example 1 and Comparative Example 1 were observed and tested by scanning electron microscope. The results of Example 1 are as follows: Figure 3A As shown, the results of comparative example 1 are as follows Figure 3B shown.

[0079] Depend on Figure 3A and Figure 3B It can be seen that the positive electrode material of Example 1 can form a uniform and smooth coating layer after sintering. However, in Comparative Example 1, no graphite is added, and the primary particles of the positive electrode material after sintering are irregular in shape and have a spotty surface, which easily increases the adsorption force between the positive electrode material particles, thereby reducing the fluidity of the positive electrode material and affecting the screening speed.

[0080] 2. The electrical performance of the battery prepared with the positive electrode materials obtained in Examples 1-4 and Comparative Examples 1-3 was tested. The results of the first discharge capacity test are as follows: Figure 4 As shown, the capacity retention test results after 100 cycles are as follows Figure 5 shown.

[0081] The electrical performance test conditions are as follows: the prepared positive electrode material, conductive carbon and binder polyvinylidene fluoride are mixed evenly in a mass ratio of 8:1:1 to make a button battery. The constant current charge and discharge test is carried out using the LAND battery test system. During the test, the operating voltage range is 2.8V to 4.25V, the charge and discharge rates are 0.1C / 0.1C, and the CV cutoff current is 0.01C. The first discharge capacity of the battery prepared with the positive electrode materials obtained in Examples 1-4 and Comparative Example 1 at 0.1C, and the capacity retention rate of the battery after 100 cycles at 45°C with a charge and discharge current of 1C are measured.

[0082] The results of the electrical performance test show that under the voltage range of 2.8 to 4.25V and the discharge condition of 0.1C rate, the first discharge capacity of the battery prepared by the positive electrode material in Example 1 reaches 180.5mAh / g; under the high temperature environment of 45°C, the voltage range of 2.8 to 4.25V, the discharge rate of 1C, and the interval cycle test cycle of 100 cycles, the capacity retention rate reaches 96.6%, which can meet the performance requirements of the battery, and the capacity and cycle performance of the battery prepared by the positive electrode material of Examples 1-4 are basically the same as those of the battery prepared by the positive electrode material of Comparative Example 1, indicating that the graphite coating has basically no negative impact on the performance of the battery. The battery withholding capacity prepared by the positive electrode material of Comparative Example 3 is lower than that of Examples 1-4, indicating that excessive addition of graphite will have a certain impact on the battery capacity.

[0083] 3. The batteries prepared from the positive electrode materials obtained in Examples 1-4 and Comparative Examples 1-3 were subjected to bulk density test and sieving speed test. The bulk density test results are as follows: Figure 6 The screening speed test results are shown in Figure 7 shown.

[0084] The bulk density test conditions are as follows: measured using the Scott bulk density meter, a powder bulk density test developed in accordance with GB / T1479.2-2011 (Determination of bulk density of metal powders - Part 2: Scott volumetric method). The volume of the cylindrical cup is V (cm 3 ), the weight of the cylindrical cup is recorded as G1. Use a spoon to gently place the positive electrode material on the screen of the upper combined funnel, and use a small brush to gently brush the material to pass through the screen, through the cloth box, the square funnel, and into the cylindrical cup until it is full and powder overflows. Take out the cylindrical cup, and use a stainless steel ruler to scrape the part of the material that overflows the cylindrical cup. Take out the cup and wipe off the powder attached to the outer surface, and weigh the weight of the cylindrical cup and powder G2, accurate to 0.01g. The following equation can then be used to calculate the loose density, loose density = (weight of cylindrical cup and powder - cup weight) / cup volume = (G2-G1) / V.

[0085] The sieving speed test conditions are as follows: place a positive electrode material sample with a mass of m (kg) on ​​a 400-mesh sieve, sieve it manually or with a vibrating sieve, and record the time t (h) taken for the entire sample to be sieved, that is, the sieving speed s = m / t (kg / h).

[0086] The results show that compared with comparative examples 1-2, the bulk density and sieving speed of the positive electrode materials in examples 1-4 are significantly improved. Among them, the bulk density of the positive electrode material in example 1 is 0.966 g / cm 3 , while the comparative example 1 is only 0.854g / cm 3The screening speed of the positive electrode material in Example 1 reached 200 kg / h, which is about twice the screening speed of the positive electrode material in Comparative Example 1. Due to the excessive coating of graphite (coating amount is 0.25%), although the bulk density and screening speed of the positive electrode material of Comparative Example 3 are high, compared with Examples 1-4, the first discharge gram capacity and cycle performance of the battery prepared using the positive electrode material of Comparative Example 3 are reduced, especially the first discharge gram capacity is significantly reduced, and the overall performance of the positive electrode material is not good.

[0087] It can be seen that compared with comparative examples 1-3, embodiments 1-4 can effectively improve the fluidity of the positive electrode material while maintaining the good electrochemical properties of the positive electrode material because they are coated with an appropriate amount of fluidity material, thereby increasing the loose density and screening speed of the positive electrode material and improving the comprehensive performance of the positive electrode material.

[0088] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, but the present invention is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. A positive electrode material, characterized in that: The invention comprises an inner core and a coating layer coated on the inner core, wherein the coating layer contains a fluid substance, the repose angle θ of the fluid substance is ≤50°, the mass percentage of the fluid substance in the coating layer to the inner core is 0.05% to 0.2%, and the positive electrode material is sieved under 400 mesh conditions, and the sieving speed of the positive electrode material is 150kg / h to 250kg / h.

2. The positive electrode material according to claim 1, characterized in that The fluid material includes at least one of graphite, talc, molybdenum disulfide and boron nitride.

3. The positive electrode material according to claim 1, characterized in that The bulk density of the positive electrode material is 0.8 g / cm 3 ~1.0g / cm 3 g.

4. The positive electrode material according to claim 1, characterized in that The coating layer has a thickness of 1 nm to 3 nm.

5. The positive electrode material according to claim 1, characterized in that The particle size D50 of the positive electrode material is 2 μm to 10 μm.

6. A method for preparing a positive electrode material, characterized in that: include: Mixing a fluid substance with a cathode material substrate to obtain a mixed material, wherein the angle of repose θ of the fluid substance is ≤50°, and the mass percentage of the fluid substance to the cathode material substrate is 0.05% to 0.2%; and The mixed material is sintered to obtain the positive electrode material, wherein the mixed material is sieved under 400 mesh conditions, and the sieving speed of the positive electrode material is 150kg / h to 250kg / h.

7. The method for preparing the positive electrode material according to claim 6, characterized in that: The fluid material includes at least one of graphite, talc, molybdenum disulfide and boron nitride.

8. The method for preparing the positive electrode material according to claim 6, characterized in that: In the step of mixing the fluid substance with the positive electrode material substrate, the mixing is dry mixing; In the step of mixing the fluid substance with the positive electrode material substrate, the mixing rotation speed is 1000 rpm to 2000 rpm.

9. The method for preparing the positive electrode material according to claim 6, characterized in that: In the step of sintering the mixed material, the sintering temperature is 300° C. to 500° C., and the sintering time is 5 h to 15 h.

10. An electrochemical device, characterized in that: The electrochemical device comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises a positive electrode material, and the positive electrode material is the positive electrode material as described in any one of claims 1 to 5 or the positive electrode material prepared by the preparation method of the positive electrode material as described in any one of claims 6 to 9.