Flame-retardant gelatinous symmetrical electrolyte membrane and preparation method thereof
By growing MOF materials containing carboxylic acid and tetraazole on a glass fiber substrate, combined with flame retardant and polymer monomer, a flame retardant gel-like electrolyte membrane was prepared through in-situ polymerization steps, which solved the high temperature of lithium batteries The problems of flammable and uneven transmission of lithium ions have improved the safety and stability of the battery.
Patent Information
- Application Number
- CN202411022354.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The solid electrolyte membrane of existing lithium batteries is flammable and easy to crack under high temperature environments, and lacks flame retardant effects, poses safety hazards, and the transmission of lithium ions is uneven, affecting the stability and safety performance of the battery.
The MOF material containing carboxylic acid and tetraazole was grown on a glass fiber substrate by spray coating, combined with the flame retardant triethyl phosphate and polymer monomer, and the flame retardant gel was prepared by in-situ ultraviolet light and thermal polymerization steps. Symmetrical electrolyte membrane improves the compatibility of electrolytes and separators and the transmission uniformity of lithium ions.
It achieves the improvement of the safety performance of the battery at high temperatures, extends the battery life, reduces energy consumption and environmental pollution, improves the stability and safety of the battery, ensures good contact between the electrolyte and the electrode, and enhances the safety of the lithium battery. performance.
Smart Images

Figure CN118919836A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a method for preparing a flame-retardant gel-like symmetrical electrolyte membrane, and also relates to a flame-retardant gel-like symmetrical electrolyte membrane. Background Art
[0002] Nowadays, lithium-ion batteries exist in all aspects of our daily life, study, and work. For example, mobile phones, computers, electric vehicles, etc. are indispensable. This means that the cycle stability and safety performance of lithium batteries must be higher, and the service life must be longer. This series of characteristics are closely related to the electrolyte, and the organic components in the traditional lithium battery liquid electrolyte have safety hazards such as flammability and leakage. In recent years, researchers have been committed to the research of solid electrolytes, using non-flammable solid electrolytes to replace traditional liquid electrolytes to improve this problem. For example, Professor Guo Hong's team at Yunnan University has designed a gel polymer electrolyte to replace the electrolyte, which can form a LiF-Li3N double protective layer SEI on the lithium metal negative electrode side, thereby inhibiting the growth of lithium dendrites and promoting the rapid migration of lithium ions. It has an increasingly broad application prospect in the development and design of high specific capacity and high energy density lithium batteries.
[0003] As a major branch of solid electrolytes, polymer electrolytes have attracted widespread attention due to their high safety, excellent flexible design capabilities, flexible adjustability, and good contact with electrodes. The synthesis process of polymer electrolytes is relatively simple. Usually, polymer monomers, initiators, cross-linking agents, etc. are added to the electrolyte, and the electrolyte is solidified through thermal polymerization or photopolymerization. It has low requirements for external conditions such as temperature and pressure, and is suitable for large-scale batch production in factories.
[0004] The document with application number "202310450066.X" discloses "a method for preparing a polymer electrolyte membrane and a solid-state battery", but the problem is that the prepared polymer electrolyte lacks flame retardant effect, and there are safety hazards of flammability and easy decomposition when working under high-temperature overheating conditions. It also does not involve the compatibility between the diaphragm and the electrolyte and the transmission of lithium ions during the operation of the lithium battery.
[0005] Therefore, the preparation of a solid electrolyte membrane with high safety performance, strong mechanical properties and excellent compatibility with the separator is the research focus of researchers in the battery field. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a flame-retardant gel-like symmetrical electrolyte membrane, which solves the problem that the existing electrolyte membrane is flammable and easy to decompose when working in a high temperature or overheated environment, improves the compatibility between the diaphragm and the electrolyte, and improves the uneven transmission of lithium ions on the lithium metal electrode side of the battery.
[0007] Another object of the present invention is to provide a flame-retardant gel-like symmetrical electrolyte membrane.
[0008] The technical solution adopted by the present invention is a method for preparing a flame-retardant gel-like symmetrical electrolyte membrane, and the specific operating steps are as follows:
[0009] S1: Dissolve zinc nitrate hexahydrate (Zn(NO3)2.6H2O) in deionized water (H2O) and prepare a colorless transparent solution A by a magnetic stirrer; weigh 5-aminotetrazolyl (CH3N5) and pyromellitic acid (C 10 H6O8) were dissolved in deionized water (H2O) and made into a colorless and transparent solution B by a magnetic stirrer;
[0010] S2: Place the glass fiber (GF) on a heating plate, use a spray gun to evenly spray solution A on it, let it stand and then wash it with ethanol, then use a spray gun to evenly spray solution B on it, let it stand and then wash it with ethanol to obtain composite glass fiber C.
[0011] S3: Under room temperature, soak C in deionized water (H2O) for 1-3 hours, take it out, and then soak it in ethanol for 12-24 hours and take it out; place the treated C in an oven at 120°C to dry, and obtain a modified diaphragm (AHF-5@GF) D loaded with carboxylic acid and tetrazole MOF materials;
[0012] S4: Prepare a precursor solution: add polyethylene glycol diacrylate (PEGDA) monomer, flame retardant triethyl phosphate (TEP), and electrolyte fluoroethylene carbonate (FEC) in a volume ratio of 12:8:1 into a small glass bottle, add LiTFSI (1 mol / L), initiator azobisisobutyronitrile (AIBN) (2 mg / mL), add a magnetic bar and stir on a stirrer for 5-10 minutes to form a precursor solution E;
[0013] S5: The precursor solution E is dropped onto the prepared modified membrane (AHF-5@GF), and the membrane is first irradiated with UV light for in-situ UV photopolymerization, and then placed in an oven for in-situ thermal polymerization, and finally a flame-retardant gel-like symmetrical electrolyte membrane is obtained.
[0014] The present invention is also characterized in that:
[0015] Furthermore, in the above step 1, the stirring time is 1-2 hours, and the pH value of solution B is adjusted to 6-7 with a diluted tetramethylammonium hydroxide solution.
[0016] Furthermore, in the above step 2, the temperature of the heating plate is 170-190° C., and the distance between the spray gun and the glass fiber is 10-15 cm.
[0017] Furthermore, in the above step 2, the volume ratio of solution A and solution B in each rotation spraying is 1:2, and the stabilization time after spraying solution A and solution B is 10-20 seconds.
[0018] Furthermore, in the above step 4, the polyethylene glycol diacrylate (PEGDA) monomer and the initiator azobisisobutyronitrile (AIBN) used to prepare the precursor solution should be stored away from light.
[0019] Furthermore, in the above step 4, the precursor solution E is prepared in a glove box protected by argon gas, and the water oxygen value in the glove box is not higher than 0.01 ppm.
[0020] Furthermore, in the above step 5, the UV light polymerization time is 10-15 min, and the oven temperature of the in-situ thermal polymerization is 60-80°C.
[0021] Furthermore, in the above step 5, for button batteries, the size of the composite battery modified separator D (AHF-5@GF) is 18 mm, and the volume range of the added precursor solution is 0.038-0.04 ml / cm 2 .
[0022] The second technical solution adopted by the present invention is: a flame-retardant gel-like symmetrical electrolyte membrane is prepared by using a preparation method of a flame-retardant gel-like symmetrical electrolyte membrane.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention firstly uses a spraying method to in-situ grow a MOF material containing carboxylic acid and tetrazole on a glass fiber (GF) substrate to prepare a composite battery modified diaphragm (AHF-5@GF). Then, the precursor solution with added flame retardant is subjected to a dual polymerization step of in-situ ultraviolet polymerization and in-situ thermal polymerization. The process is simple and has a fast reaction speed, which reduces solvent volatilization and environmental pollution. It can be completed in a short time, reduces energy consumption, has high stability and reliability, and thus prepares a gel-like symmetrical electrolyte membrane with flame retardant effect, and improves the safety performance of lithium batteries.
[0025] 2. The flame retardant triethyl phosphate (TEP) added to the precursor solution prepared by the present invention can generate free radicals PO. with flame retardant properties at high temperatures, which can capture combustible free radicals H. and OH. to undergo chemical reactions, reduce the heat release value of the battery, thereby delaying and preventing the combustion of the electrolyte and extending the battery life.
[0026] 3. The polymer monomer (PEGDA) and the initiator (AIBN) are added to the precursor solution prepared by the present invention. During the thermal polymerization process, the carbonyl group on the PEGDA molecule can react with the nitrile group on the AIBN molecule and the amino group on the AHF-5MOF to form a regular and orderly cross-linked network, which can effectively adsorb liquid components. The formed gel-state electrolyte can improve the compatibility between the electrolyte and the separator, ensure good contact between the electrolyte and the electrode, and thus enhance the stability of the battery.
[0027] 4. The solvent used in the MOF-loaded modified diaphragm prepared by the present invention is deionized water (H2O), which is green and environmentally friendly compared to other chemical solvents, has abundant resources, and is low in price, and can be used for large-scale industrial production.
[0028] 5. The lithium battery assembled with the flame-retardant gel-like symmetrical electrolyte membrane prepared by the present invention has a charge and discharge capacity of 117 mAhg after 100 cycles at a rated capacity of 1C. -1 , the Coulombic efficiency is 99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a preparation flow chart of the present invention;
[0030] Figure 2 It is the XRD comparison diagram of AHF-5MOF simulation, hydrothermal synthesis of crystalline powder AHF-5MOF, and modified diaphragm (AHF-5@GF) in Example 1 of the present invention;
[0031] Figure 3 is a cycle diagram of the assembled lithium ion battery of Example 1 of the present invention at a current density of 1C;
[0032] Figure 4 It is a rate diagram of the assembled lithium-ion battery of Example 1 of the present invention at different current densities. DETAILED DESCRIPTION
[0033] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0034] Example 1
[0035] The preparation method of the flame-retardant gel-like symmetrical electrolyte membrane of the present invention is as follows Figure 1 , the specific steps are as follows:
[0036] Step 1: Dissolve zinc nitrate hexahydrate (Zn(NO3)2.6H2O) in deionized water (H2O) and stir for 1-2 hours to disperse it into a colorless transparent solution A with a concentration of 0.05 mol / L. Then weigh 5-aminotetrazolyl (CH3N5) and pyromellitic acid (C 10H6O8) were dissolved in deionized water (H2O), the pH value was adjusted to 6-7 with a diluted tetramethylammonium hydroxide solution, and stirred for 1-2 hours to disperse it into a colorless transparent solution B with a concentration of 0.075 mol / L.
[0037] Step 2: Cut the glass fiber into a circle with a diameter of 18 mm according to the size of the button battery shell. Place the glass fiber on a 170°C heating plate, with the distance between the spray gun and the glass fiber being 10-15 cm. Use the spray gun to evenly spray 1 mL of solution A, let it stand for 10 seconds and then wash it with ethanol. Then use the spray gun to evenly spray 2 mL of solution B, let it stand for 10 seconds and then wash it with ethanol. Spray 10 times to obtain composite glass fiber C.
[0038] Step 3, at room temperature, soak C in deionized water (H2O) for 1 hour, take it out, soak it in ethanol for 12 hours, take it out, and then place it in a 120°C oven for drying to obtain a modified diaphragm D (AHF-5@GF) loaded with carboxylic acid and tetrazole MOF materials.
[0039] Step 4, prepare a precursor solution, in a glove box filled with argon, take polyethylene glycol diacrylate (PEGDA) monomer, flame retardant triethyl phosphate (TEP), electrolyte fluorocarbonate (FEC) in a volume ratio of 12:8:1 into a small glass bottle, then add LiTFSI (1 mol / L), initiator azobisisobutyronitrile (AIBN) (2 mg / mL), then add a magnetic bar and stir on a stirrer for 5-10 minutes to form a precursor solution E, the water oxygen value in the glove box is less than 0.01 ppm;
[0040] Step 5, drop 100 μl of precursor solution E into the modified membrane D (AHF-5@GF), allow the precursor solution to completely infiltrate the modified membrane D, first use ultraviolet light for in-situ photopolymerization for 10-15 minutes, and then transfer to a 60°C oven for in-situ thermal polymerization for 1 hour, and finally obtain a gel-like symmetrical electrolyte membrane F with flame retardant effect.
[0041] Example 2
[0042] The method for preparing the flame-retardant gel-like symmetrical electrolyte membrane of the present invention comprises the following specific steps:
[0043] Step 1: Dissolve zinc nitrate hexahydrate (Zn(NO3)2.6H2O) in deionized water (H2O) and stir for 1-2 hours to disperse it into a colorless transparent solution A with a concentration of 0.05 mol / L. Then weigh 5-aminotetrazolyl (CH3N5) and pyromellitic acid (C 10H6O8) were dissolved in deionized water (H2O), the pH value was adjusted to 6-7 with a diluted tetramethylammonium hydroxide solution, and stirred for 1-2 hours to disperse it into a colorless transparent solution B with a concentration of 0.075 mol / L.
[0044] Step 2: Cut the glass fiber into a circle with a diameter of 18 mm according to the button battery shell. Place the glass fiber on a 180°C heating plate, with the distance between the spray gun and the glass fiber being 10-15 cm. Use the spray gun to evenly spray 2 mL of solution A, let it stand for 20 seconds and then wash it with ethanol. Then use the spray gun to evenly spray 4 mL of solution B, let it stand for 20 seconds and then wash it with ethanol. Spray 10 times to obtain composite glass fiber C.
[0045] Step 3, at room temperature, soak C in deionized water (H2O) for 1 hour, take it out, soak it in ethanol for 12 hours, take it out, and then place it in a 120°C oven for drying to obtain a modified diaphragm D loaded with carboxylic acid and tetrazole MOF materials.
[0046] Step 4, prepare a precursor solution, in a glove box filled with argon, take polyethylene glycol diacrylate (PEGDA) monomer, flame retardant triethyl phosphate (TEP), electrolyte fluorocarbonate (FEC) in a volume ratio of 12:8:1 into a small glass bottle, then add LiTFSI (1 mol / L), initiator azobisisobutyronitrile (AIBN) (2 mg / mL), then add a magnetic bar and stir on a stirrer for 5-10 minutes to form a precursor solution E, the water oxygen value in the glove box is less than 0.01 ppm;
[0047] Step 5, drop 100 μl of precursor solution E into the modified membrane D, allow the precursor solution to completely infiltrate the modified membrane D, first use ultraviolet light for in-situ photopolymerization for 10-15 minutes, and then transfer to a 60°C oven for in-situ thermal polymerization for 1 hour, and finally obtain a gel-like symmetrical electrolyte membrane F with flame retardant effect.
[0048] Example 3
[0049] The method for preparing the flame-retardant gel-like symmetrical electrolyte membrane of the present invention comprises the following specific steps:
[0050] Step 1: Dissolve zinc nitrate hexahydrate (Zn(NO3)2.6H2O) in deionized water (H2O) and stir for 1-2 hours to disperse it into a colorless transparent solution A with a concentration of 0.05 mol / L. Then weigh 5-aminotetrazolyl (CH3N5) and pyromellitic acid (C 10H6O8) were dissolved in deionized water (H2O), the pH value was adjusted to 6-7 with a diluted tetramethylammonium hydroxide solution, and stirred for 1-2 hours to disperse it into a colorless transparent solution B with a concentration of 0.075 mol / L.
[0051] Step 2: Cut the glass fiber into a circle with a diameter of 18 mm according to the size of the button battery shell. Place the glass fiber on a 170°C heating plate, with the distance between the spray gun and the glass fiber being 10-15 cm. Use the spray gun to evenly spray 1 mL of solution A, let it stand for 10 seconds and then wash it with ethanol. Then use the spray gun to evenly spray 2 mL of solution B, let it stand for 10 seconds and then wash it with ethanol. Spray 10 times to obtain composite glass fiber C.
[0052] Step 3, at room temperature, soak C in deionized water (H2O) for 1 hour, take it out, soak it in ethanol for 12 hours, take it out, and then place it in a 120°C oven for drying to obtain a modified diaphragm D loaded with carboxylic acid and tetrazole MOF materials.
[0053] Step 4, prepare a precursor solution, in a glove box filled with argon, take polyethylene glycol diacrylate (PEGDA) monomer, flame retardant triethyl phosphate (TEP), electrolyte fluorocarbonate (FEC) in a volume ratio of 40:10:1 into a small glass bottle, then add LiTFSI (1 mol / L), initiator azobisisobutyronitrile (AIBN) (2 mg / mL), then add a magnetic bar and stir on a stirrer for 5-10 minutes to form a precursor solution E, the water oxygen value in the glove box is less than 0.01 ppm;
[0054] Step 5, drop 100 μl of precursor solution E into the modified membrane D, allow the precursor solution to completely infiltrate the modified membrane D, first use ultraviolet light for in-situ photopolymerization for 10-15 minutes, and then transfer to a 60°C oven for in-situ thermal polymerization for 1 hour, and finally obtain a gel-like symmetrical electrolyte membrane F with flame retardant effect.
[0055] Example 4
[0056] The method for preparing the flame-retardant gel-like symmetrical electrolyte membrane of the present invention comprises the following specific steps:
[0057] Step 1: Dissolve zinc nitrate hexahydrate (Zn(NO3)2.6H2O) in deionized water (H2O) and stir for 1-2 hours to disperse it into a colorless transparent solution A with a concentration of 0.05 mol / L. Then weigh 5-aminotetrazolyl (CH3N5) and pyromellitic acid (C 10H6O8) were dissolved in deionized water (H2O), the pH value was adjusted to 6-7 with a diluted tetramethylammonium hydroxide solution, and stirred for 1-2 hours to disperse it into a colorless transparent solution B with a concentration of 0.075 mol / L.
[0058] Step 2: Cut the glass fiber into a circle with a diameter of 18 mm according to the size of the button battery shell. Place the glass fiber on a 170°C heating plate, with the distance between the spray gun and the glass fiber being 10-15 cm. Use the spray gun to evenly spray 1 mL of solution A, let it stand for 10 seconds and then wash it with ethanol. Then use the spray gun to evenly spray 2 mL of solution B, let it stand for 10 seconds and then wash it with ethanol. Spray 10 times to obtain composite glass fiber C.
[0059] Step 3, at room temperature, soak C in deionized water (H2O) for 1 hour, take it out, soak it in ethanol for 12 hours, take it out, and then place it in a 120°C oven for drying to obtain a modified diaphragm D loaded with carboxylic acid and tetrazole MOF materials.
[0060] Step 4, prepare a precursor solution, in a glove box filled with argon, take polyethylene glycol diacrylate (PEGDA) monomer, flame retardant triethyl phosphate (TEP), electrolyte fluorocarbonate (FEC) in a volume ratio of 20:4:1 into a small glass bottle, then add LiTFSI (1 mol / L), initiator azobisisobutyronitrile (AIBN) (2 mg / mL), then add a magnetic bar and stir on a stirrer for 5-10 minutes to form a precursor solution E, the water oxygen value in the glove box is less than 0.01 ppm;
[0061] Step 5, drop 100 μl of precursor solution E into the modified membrane D, allow the precursor solution to completely infiltrate the modified membrane D, first use ultraviolet light for in-situ photopolymerization for 10-15 minutes, and then transfer to a 60°C oven for in-situ thermal polymerization for 1 hour, and finally obtain a gel-like symmetrical electrolyte membrane F with flame retardant effect.
[0062] Example 5
[0063] The method for preparing the flame-retardant gel-like symmetrical electrolyte membrane of the present invention comprises the following specific steps:
[0064] Step 1: Dissolve zinc nitrate hexahydrate (Zn(NO3)2.6H2O) in deionized water (H2O) and stir for 1-2 hours to disperse it into a colorless transparent solution A with a concentration of 0.05 mol / L. Then weigh 5-aminotetrazolyl (CH3N5) and pyromellitic acid (C 10H6O8) were dissolved in deionized water (H2O), the pH value was adjusted to 6-7 with a diluted tetramethylammonium hydroxide solution, and stirred for 1-2 hours to disperse it into a colorless transparent solution B with a concentration of 0.075 mol / L.
[0065] Step 2: Cut the glass fiber into a circle with a diameter of 18 mm according to the size of the button battery shell. Place the glass fiber on a 170°C heating plate, with the distance between the spray gun and the glass fiber being 10-15 cm. Use the spray gun to evenly spray 1 mL of solution A, let it stand for 10 seconds and then wash it with ethanol. Then use the spray gun to evenly spray 2 mL of solution B, let it stand for 10 seconds and then wash it with ethanol. Spray 10 times to obtain composite glass fiber C.
[0066] Step 3, at room temperature, soak C in deionized water (H2O) for 1 hour, take it out, soak it in ethanol for 12 hours, take it out, and then place it in a 120°C oven for drying to obtain a modified diaphragm D loaded with carboxylic acid and tetrazole MOF materials.
[0067] Step 4, prepare a precursor solution, in a glove box filled with argon, take polyethylene glycol diacrylate (PEGDA) monomer, flame retardant triethyl phosphate (TEP), electrolyte fluoroethylene carbonate (FEC) in a volume ratio of 5:5:1 into a small glass bottle, then add LiTFSI (1 mol / L), initiator azobisisobutyronitrile (AIBN) (2 mg / mL), then add a magnetic bar and stir on a stirrer for 5-10 minutes to form a precursor solution E, the water oxygen value in the glove box is less than 0.01 ppm;
[0068] Step 5, drop 100 μl of precursor solution E into the modified membrane D, allow the precursor solution to completely infiltrate the modified membrane D, first use ultraviolet light for in-situ photopolymerization for 10-15 minutes, and then transfer to a 60°C oven for in-situ thermal polymerization for 1 hour, and finally obtain a gel-like symmetrical electrolyte membrane F with flame retardant effect.
[0069] The above embodiment 1 is the best embodiment, and the following is the experimental data of the product prepared in embodiment 1:
[0070] like Figure 2 As shown, Figure 2 The simulation curve in the figure is the standard curve of AHF-5MOF; the AHF-5 powder curve is the curve obtained by XRD testing the AHF-5MOF powder synthesized by the hydrothermal method; the AHF-5@GF curve is the curve obtained by XRD testing the modified diaphragm D (AHF-5@GF) prepared by the present invention. It can be seen from the comparison of the above three XRD curves that AHF-5 is successfully grown in situ on the glass fiber, that is, the modified diaphragm AHF-5@GF loaded with carboxylic acid and tetrazole MOF materials is successfully prepared.
[0071] The precursor solution is in liquid state before the double polymerization step. When the glass bottle containing the precursor solution is inverted, the solution can be clearly observed to flow along the bottle wall. However, after the double polymerization, the precursor solution is observed to turn into a transparent gel state. When the glass bottle is inverted again, the solution condenses at the bottom of the glass bottle and does not flow along the bottle wall. A small piece is picked up with tweezers and pressed several times, and it can be felt that it has good elasticity. That is, the precursor solution is successfully polymerized and transformed from liquid to gel state, which significantly reduces the fluidity of the electrolyte and prevents leakage of the electrolyte.
[0072] The electrolyte membrane prepared by the method of the present invention was subjected to a flame retardancy test. The AHF-5@GF modified diaphragm D burned after 10 seconds, leaving only a small amount of residue, while the flame retardant electrolyte membrane still maintained its original shape after 10 seconds, indicating that the electrolyte membrane prepared by the present invention has a certain flame retardant effect.
[0073] like Figure 3 As shown in the figure, the cycle diagram of the assembled lithium-ion battery of Example 1 of the present invention at a current density of 1C is shown, and the charge-discharge specific capacity and coulomb efficiency of the battery after 100 cycles at a current density of 1C are shown. It can be seen that the charge-discharge capacity at a high current density of 1C is 117 mAh g -1 , and its Coulombic efficiency is 99%.
[0074] like Figure 4 As shown in Figure 1, the rate diagram of the lithium ion battery assembled in Example 1 of the present invention at different current densities. The charge and discharge specific capacities of the lithium battery assembled with the flame-retardant gel-like symmetrical electrolyte membrane at current densities of 0.1C, 0.2C, and 0.5C are 150, 140, and 144 mAh g, respectively. -1 , the efficiency is also close to 100%.
[0075] Compared with traditional liquid electrolytes, the dual polymerization steps of in-situ photopolymerization and in-situ thermal polymerization are adopted to make the electrolyte and the separator fully contact, thereby improving the compatibility between the electrolyte and the separator; the gel electrolyte reduces the risk of electrolyte leakage; the flame retardant triethyl phosphate (TEP) is introduced into the electrolyte to give the electrolyte a flame retardant effect, thereby improving the safety performance of the lithium battery; the unique regular channels on AHF-5@GF enable the uniform transmission of lithium ions.
[0076] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a flame-retardant gel-like symmetrical electrolyte membrane, characterized in that: Firstly, the AHF-5MOF material was in situ grown on a glass fiber substrate by high-temperature spraying to obtain a composite battery modified membrane AHF-5@GF. Then, the modified membrane AHF-5@GF was placed in a polymer precursor solution introduced with a flame retardant. Through the dual polymerization steps of in-situ UV photopolymerization and in-situ thermal polymerization, a gel-like symmetrical electrolyte membrane with flame retardant effect was finally formed.
2. The method for preparing a flame-retardant gel-like symmetrical electrolyte membrane according to claim 1, characterized in that: The specific steps are as follows: Step 1: dissolving zinc nitrate hexahydrate in deionized water, and preparing a colorless transparent solution A by a magnetic stirrer; then weighing 5-aminotetrazolyl and pyromellitic acid in a molar ratio of 2:1, dissolving them in deionized water, and preparing a colorless transparent solution B by a magnetic stirrer; Step 2: placing the glass fiber on a heating plate, using a spray gun to evenly spray solution A on the glass fiber, washing with ethanol after standing still, and then evenly spraying solution B on it, and washing with ethanol after standing still, to obtain composite glass fiber C; Step 3: Under room temperature, the composite glass fiber C is immersed in deionized water for 1 h to 3 h, taken out, and then immersed in ethanol for 12 h to 24 h, and taken out; the treated composite glass fiber C is placed in an oven for drying to obtain a modified diaphragm D loaded with carboxylic acid and tetrazole MOF materials; Step 4: Prepare a precursor solution: weigh polyethylene glycol diacrylate monomer, flame retardant triethyl phosphate, and electrolyte ethylene fluorocarbonate in a small glass bottle, add 1 mol / L lithium bistrifluoromethanesulfonyl imide LiTFSI and 2 mg / mL initiator azobisisobutyronitrile, add a stirring magnet and stir on a stirrer for 5-10 minutes to form a precursor solution E; Step 5: The precursor solution E is dripped onto the prepared modified membrane D, the membrane is irradiated with UV light for in-situ UV photopolymerization, and then transferred to an oven for in-situ thermal polymerization, and finally a flame-retardant gel-like symmetrical electrolyte membrane is obtained.
3. The method for preparing a flame-retardant gel-like symmetrical electrolyte membrane according to claim 2, characterized in that: In step 1, the stirring time is 1-2 hours, and the pH value of the prepared solution B is adjusted to 6-7 with a diluted tetramethylammonium hydroxide solution.
4. The method for preparing a flame-retardant gel-like symmetrical electrolyte membrane according to claim 3, wherein in step 2, the temperature of the heating plate is 170-190°C, and the distance between the spray gun and the glass fiber is 10-15 cm.
5. The method for preparing a flame-retardant gel-like symmetrical electrolyte membrane according to claim 2, characterized in that: In the step 2, the volume ratio of solution A and solution B in each rotation spraying is 1:2, and the stabilization time after spraying solution A and solution B is 10-20 seconds.
6. The method for preparing a flame-retardant gel-like symmetrical electrolyte membrane according to claim 2, characterized in that: In step 4, the polyethylene glycol diacrylate monomer and the initiator azobisisobutyronitrile used to prepare the precursor solution need to be stored away from light.
7. The method for preparing a flame-retardant gel-like symmetrical electrolyte membrane according to claim 2, characterized in that: In step 4, the precursor solution E is prepared in a glove box protected by argon gas, and the water oxygen value in the glove box is not higher than 0.01 ppm.
8. The method for preparing a flame-retardant gel-like symmetrical electrolyte membrane according to claim 2, characterized in that: In step 5, the UV polymerization step is carried out in a glove box, the photopolymerization time is 15-20 minutes, and in the in-situ thermal polymerization step, the temperature of the oven is set in the range of 60-80°C.
9. The method for preparing a flame-retardant gel-like symmetrical electrolyte membrane according to claim 2, characterized in that: In step 5, for button batteries, the size of the composite battery modified diaphragm D is 18 mm, and the volume range of the added precursor solution is 0.038-0.04 ml / cm 2 .
10. A flame-retardant gel-like symmetrical electrolyte membrane, characterized in that: The flame-retardant gel-like symmetrical electrolyte membrane is prepared by the method for preparing the flame-retardant gel-like symmetrical electrolyte membrane according to any one of claims 1 to 9.
Citation Information
Patent Citations
MOFs material with high gas adsorbability as well as preparation method and application of MOFs material
CN112341633A
High-strength flame-retardant composite gel polymer electrolyte as well as preparation method and application thereof
CN117543090A
Composite glass fiber diaphragm and preparation method thereof
CN117613506A
Cited By
Low-temperature solid electrolyte based on MOF self-assembly and low-temperature micromolecule synergy and preparation method thereof
CN122118064A