Preparation method of soft package gel solid-state lithium ion battery
Through the preparation method of soft gel solid lithium-ion battery, gel electrolyte and specific process steps, the failure and safety problems caused by the growth of lithium dendrites in liquid lithium-ion batteries are solved, and high energy density and safety performance are achieved. promote.
Patent Information
- Application Number
- CN202411154762.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-08
AI Technical Summary
With the continuous increase in energy density, lithium dendrites in liquid lithium-ion batteries grow uncontrollably, resulting in battery failure and safety issues, which seriously hinders its practical application.
The preparation method of soft gel solid lithium-ion battery is adopted. By selecting components such as positive electrode sheet, negative electrode sheet, separator, gel electrolyte, and polymer monomer, lithium salt, solvent and initiator to form the gel electrolyte, and A soft gel battery is formed by baking, liquid injection, applying preloading force, standing in a room temperature, and standing in a high temperature.
It realizes the advantages of the battery's leakage prevention, high ionic conductivity, good mechanical strength, high energy density and light weight. At the same time, it improves the hardness, energy density, low temperature and safety performance of the battery, and ensures excellent cycling performance.
Smart Images

Figure CN118919838A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cylindrical lithium ion batteries, in particular to a method for preparing a soft-package gel solid-state lithium ion battery. Background Art
[0002] In recent years, with the rapid development of electric vehicles and large-scale energy storage, research on new energy storage that is resource-rich, energy-efficient and environmentally friendly has become an international research hotspot.
[0003] Among them, the development prospects of the lithium-ion battery industry chain are bright, and liquid lithium-ion batteries have shown excellent performance, such as high ionic conductivity (10-3S / cm) and good contact with electrodes.
[0004] However, safety issues in liquid lithium-ion batteries and performance degradation caused by dendrite growth seriously hinder the practical application of liquid lithium-ion batteries.
[0005] As energy density continues to increase, liquid electrolytes lead to uncontrolled growth of lithium dendrites in LIBs, battery failure, and even catastrophic safety issues. Gel polymer electrolytes have been widely studied in LIBs due to their advantages such as leakproof electrolytes, high ionic conductivity, high specific energy, good mechanical strength, high energy density, and light weight. Therefore, it is very important to prepare gel solid-state lithium-ion batteries with excellent electrical and safety performance. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a soft-package gel solid-state lithium-ion battery to solve the current safety problem of uncontrolled growth of lithium dendrites in liquid electrolyte in LIB, battery failure, and even catastrophic safety problems caused by the continuous increase in energy density.
[0007] To achieve the above object, the present invention provides the following technical solution: a method for preparing a soft-pack gel solid-state lithium-ion battery, comprising the following steps:
[0008] Step 1: Select a positive electrode sheet, a negative electrode sheet, a separator, a positive electrode ear, a negative electrode ear and a gel electrolyte;
[0009] Step 2: stack the positive electrode sheet, the separator, and the negative electrode sheet in order to obtain a bare cell;
[0010] Step 3: Select a lithium-ion battery aluminum shell, a positive electrode cover, a negative electrode cover, a positive electrode isolation ring, a Mylar film, and a side support sheet;
[0011] Step 4: First weld the bare cell to the negative electrode cover plate, wrap and fix it with Mylar film, side support sheet, and positive electrode isolation ring, and then place it in the aluminum shell of the lithium-ion battery, and then weld the positive electrode ear of the positive electrode sheet to the positive electrode cover plate, and weld the negative electrode ear of the negative electrode sheet to the negative electrode cover plate;
[0012] Step 5: seal and weld the negative electrode cover plate, the positive electrode cover plate and the aluminum shell of the lithium-ion battery to obtain a semi-finished battery cell before liquid injection;
[0013] Step 6: The semi-finished battery cell before liquid injection is baked, liquid injected, pre-tightened, allowed to stand at room temperature for soaking, allowed to stand at high temperature for curing, sealed, and divided into different capacities to obtain a soft-pack gel solid-state lithium-ion battery;
[0014] Among them, the gel electrolyte is composed of polymer monomers, lithium salts, solvents and initiators.
[0015] Wherein, the mass ratio of the polymer monomer, lithium salt, solvent and initiator is 8:5:75:4.
[0016] Wherein, the polymer monomer is one or more of methyl acrylate, ethyl acrylate, butyl acrylate and octyl acrylate.
[0017] Wherein, the lithium salt is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorobisoxalate, bis(fluorosulfonyl)imide lithium salt and lithium dioxalate borate.
[0018] Wherein, the solvent is a mixture of ethylene carbonate, dimethyl carbonate and propylene carbonate, and the mass ratio of the mixture of ethylene carbonate, dimethyl carbonate and propylene carbonate is 1:1:1.
[0019] Wherein, the initiator is a mixture of vinylene carbonate and propylene sulfite, and the mass ratio of the mixture of vinylene carbonate and propylene sulfite is 1:1.
[0020] Among them, the torque magnitude of the pre-tightening force applied to the semi-finished battery cell before liquid injection is 40-80cN.M.
[0021] Among them, the semi-finished battery cells are left to soak at room temperature for 48-72 hours before liquid injection.
[0022] The temperature of the semi-finished battery cell undergoing high-temperature static curing before liquid injection is 70-85°C, and the curing time is 2-10 hours.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention prepares a gel electrolyte through polymer monomers, lithium salts, solvents and initiators, and adds the gel electrolyte into a soft-package gel solid-state lithium ion battery, so that the soft-package gel solid-state lithium ion battery has the advantages of leak-proof electrolyte, high ion conductivity, high specific energy, good mechanical strength, high energy density and light weight; by applying a pre-tightening force to the battery, allowing it to be statically infiltrated at room temperature and statically cured at high temperature, the hardness, energy density, low temperature and safety performance of the battery are improved, and the excellent cycle performance of the battery is guaranteed. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the voltage-capacity ratio diagram for rate charging test;
[0026] Figure 2 This is the voltage-capacity ratio diagram for rate discharge test;
[0027] Figure 3 This is the voltage-capacity ratio diagram of the high temperature 55℃ discharge test;
[0028] Figure 4 This is the voltage-capacity ratio diagram of the low temperature -10℃ discharge test;
[0029] Figure 5 This is the voltage-capacity ratio diagram of the low temperature -20℃ discharge test;
[0030] Figure 6 This is a 0.5C / 1C cycle test chart at room temperature. DETAILED DESCRIPTION
[0031] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0032] A method for preparing a soft-pack gel solid-state lithium-ion battery comprises the following steps:
[0033] Step 1: Select a positive electrode sheet, a negative electrode sheet, a separator, a positive electrode ear, a negative electrode ear and a gel electrolyte, wherein the gel electrolyte is composed of a polymer monomer, a lithium salt, a solvent and an initiator, and the mass ratio of the polymer monomer, the lithium salt, the solvent and the initiator is 8:5:75:4;
[0034] Step 2: stack the positive electrode sheet, the separator, and the negative electrode sheet in order to obtain a bare cell;
[0035] Step 3: Select a lithium-ion battery aluminum shell, a positive electrode cover, a negative electrode cover, a positive electrode isolation ring, a Mylar film, and a side support sheet;
[0036] Step 4: First weld the bare cell to the negative electrode cover plate, wrap and fix it with Mylar film, side support sheet, and positive electrode isolation ring, and then place it in the aluminum shell of the lithium-ion battery, and then weld the positive electrode ear of the positive electrode sheet to the positive electrode cover plate, and weld the negative electrode ear of the negative electrode sheet to the negative electrode cover plate;
[0037] Step 5: seal and weld the negative electrode cover plate, the positive electrode cover plate and the aluminum shell of the lithium-ion battery to obtain a semi-finished battery cell before liquid injection;
[0038] Step six, the semi-finished battery cell before liquid injection is baked, liquid injected, pre-tightened (the torque applied to the semi-finished battery cell before liquid injection is 60 cN.M), allowed to soak at room temperature (the time for the semi-finished battery cell to soak at room temperature before liquid injection is 72 hours), allowed to stand at high temperature for curing (the temperature for the semi-finished battery cell to stand at high temperature for curing before liquid injection is 80°C, and the curing time is 8 hours), sealed, and divided into different volumes to obtain a soft-pack gel solid-state lithium-ion battery.
[0039] Example 2
[0040] A method for preparing a soft-pack gel solid-state lithium-ion battery comprises the following steps:
[0041] Step 1: Select a positive electrode sheet, a negative electrode sheet, a separator, a positive electrode ear, a negative electrode ear and a gel electrolyte, wherein the gel electrolyte is composed of a polymer monomer, a lithium salt, a solvent and an initiator, and the mass ratio of the polymer monomer, the lithium salt, the solvent and the initiator is 8:5:75:4;
[0042] Step 2: stack the positive electrode sheet, the separator, and the negative electrode sheet in order to obtain a bare cell;
[0043] Step 3: Select a lithium-ion battery aluminum shell, a positive electrode cover, a negative electrode cover, a positive electrode isolation ring, a Mylar film, and a side support sheet;
[0044] Step 4: First weld the bare cell to the negative electrode cover plate, wrap and fix it with Mylar film, side support sheet, and positive electrode isolation ring, and then place it in the aluminum shell of the lithium-ion battery, and then weld the positive electrode ear of the positive electrode sheet to the positive electrode cover plate, and weld the negative electrode ear of the negative electrode sheet to the negative electrode cover plate;
[0045] Step 5: seal and weld the negative electrode cover plate, the positive electrode cover plate and the aluminum shell of the lithium-ion battery to obtain a semi-finished battery cell before liquid injection;
[0046] Step six, the semi-finished battery cell before liquid injection is baked, liquid injected, pre-tightened (the torque applied to the semi-finished battery cell before liquid injection is 40 cN.M), allowed to soak at room temperature (the time for the semi-finished battery cell to soak at room temperature before liquid injection is 72 hours), allowed to stand at high temperature for curing (the temperature for the semi-finished battery cell to stand at high temperature for curing before liquid injection is 85°C, and the curing time is 4 hours), sealed, and divided into volumes to obtain a soft-pack gel solid-state lithium-ion battery.
[0047] Comparative Example 1
[0048] A method for preparing a liquid soft-pack lithium-ion battery comprises the following steps:
[0049] Step 1: Select a positive electrode sheet, a negative electrode sheet, a separator, a positive electrode ear, a negative electrode ear and a conventional electrolyte;
[0050] Step 2: stack the positive electrode sheet, the separator, and the negative electrode sheet in order to obtain a bare cell;
[0051] Step 3: Select a lithium-ion battery aluminum shell, a positive electrode cover, a negative electrode cover, a positive electrode isolation ring, a Mylar film, and a side support sheet;
[0052] Step 4: First weld the bare cell to the negative electrode cover plate, wrap and fix it with Mylar film, side support sheet, and positive electrode isolation ring, and then place it in the aluminum shell of the lithium-ion battery, and then weld the positive electrode ear of the positive electrode sheet to the positive electrode cover plate, and weld the negative electrode ear of the negative electrode sheet to the negative electrode cover plate;
[0053] Step 5: seal and weld the negative electrode cover plate, the positive electrode cover plate and the aluminum shell of the lithium-ion battery to obtain a semi-finished battery cell before liquid injection;
[0054] Step 6: The semi-finished battery cell before liquid injection is baked, liquid injected, allowed to stand at room temperature for soaking (the semi-finished battery cell before liquid injection is allowed to stand at room temperature for soaking for 72 hours), sealed, and volume divided to obtain a liquid soft-pack lithium-ion battery.
[0055] Experimental Example 1
[0056] The soft-pack gel solid-state lithium-ion batteries prepared in Example 1 and Example 2 and the soft-pack liquid lithium-ion batteries prepared in Comparative Example 1 were subjected to rate charge (0.33C, 0.5C, 1C, 2C) tests, rate discharge (0.5C, 1C, 2C) tests, high and low temperature discharge (-20°C / -10°C / 55°C) performance tests, and room temperature 25°C 0.5C / 1C cycle performance tests. The test steps are as follows:
[0057] 1. The main steps of the rate charging test are: 1) Leave for 10 minutes; 2) Charge at a constant current of 0.33C to the cut-off voltage and then charge at a constant voltage until the current drops to 0.05C; 3) Leave for 10 minutes; 4) Discharge at a constant current of 1C to the cut-off voltage; 5) Leave; 6) Charge at a constant current of 0.5C to the cut-off voltage and then charge at a constant voltage until the current drops to 0.05C; 7) Leave; 8) Discharge at a constant current of 1C to the cut-off voltage; 9) Leave for 10 minutes; 10) Charge at a constant current of 1C to the cut-off voltage and then charge at a constant voltage until the current drops to 0.05C; 11) Leave for 10 minutes; 12) Discharge at a constant current of 1C to the cut-off voltage; 13) Leave for 10 minutes; 14) Charge at a constant current of 2C to the cut-off voltage and then charge at a constant voltage until the current drops to 0.05C; 15) Leave for 10 minutes; 16) Discharge at a constant current of 1C to the cut-off voltage. The results are as follows Figure 1 As shown, Figure 1 In the figure, the outermost curve is the rate charging voltage-capacity ratio diagram of Example 1, the middle curve is the rate charging voltage-capacity ratio diagram of Example 2, and the innermost curve is the rate charging voltage-capacity ratio diagram of Comparative Example 1;
[0058] 2. The main steps of the rate discharge test are: 1) Leave for 10 minutes; 2) Charge at 0.5C constant current to the cut-off voltage and then charge at constant voltage until the current drops to 0.05C; 3) Leave for 10 minutes; 4) Discharge at 0.5C constant current to the cut-off voltage; 5) Leave for 10 minutes; 6) Charge at 0.5C constant current to the cut-off voltage and then charge at constant voltage until the current drops to 0.05C; 7) Leave; 8) Discharge at 1C constant current to the cut-off voltage; 9) Leave for 10 minutes; 10) Charge at 0.5C constant current to the cut-off voltage and then charge at constant voltage until the current drops to 0.05C; 11) Leave for 10 minutes; 12) Discharge at 2C constant current to the cut-off voltage; 13) Leave for 10 minutes; 14) Charge at 0.5C constant current to the cut-off voltage and then charge at constant voltage until the current drops to 0.05C; 15) Leave for 10 minutes; 16) Discharge at 3C constant current to the cut-off voltage; 17) Leave for 10 minutes. The results are as follows Figure 2 As shown;
[0059] 3. The main steps of high and low temperature discharge test are: 1) put aside for 10 minutes; 2) charge at 0.5C constant current to the cut-off voltage and then charge at constant voltage until the current drops to 0.05C; 3) put aside for 10 minutes; 4) discharge at 1C constant current to the cut-off voltage; 5) put aside for 10 minutes; 6) charge at 0.5C constant current to the cut-off voltage and then charge at constant voltage until the current drops to 0.05C; 7) put aside for 24 hours in -10℃, -20℃, and 55℃ environments respectively; 8) discharge at 1C constant current to the cut-off voltage; 9) put aside for 10 minutes. The results are as follows Figure 3 , Figure 4 and Figure 5 As shown;
[0060] 4. The steps of the 0.5C / 1C cycle test at room temperature are as follows: 1) Leave for 10 minutes; 2) Charge at 0.5C constant current to the cut-off voltage and then switch to constant voltage charging until the current drops to 0.05C; 3) Leave for 10 minutes; 4) Discharge at 1C constant current to the cut-off voltage; 5) Leave for 10 minutes; Repeat steps 1) to 4) until the capacity retention rate is less than 80%. Figure 6 shown.
[0061] Depend on Figure 1-6 It can be seen that a gel electrolyte is prepared by polymer monomers, lithium salts, solvents and initiators, and the gel electrolyte is added to a soft-pack gel solid-state lithium-ion battery, so that the soft-pack gel solid-state lithium-ion battery has the advantages of leak-proof electrolyte, high ion conductivity, high specific energy, good mechanical strength, high energy density and light weight; by applying a preload to the battery, allowing it to soak at room temperature and allowing it to solidify at high temperature, the hardness, energy density, low temperature and safety performance of the battery are improved, while ensuring the excellent cycle performance of the battery.
[0062] Test Example 2
[0063] The safety performance test was conducted on the soft-package gel solid lithium-ion battery prepared in Example 1 and Example 2 and the soft-package liquid lithium-ion battery prepared in Comparative Example 1. The test results are shown in the following table:
[0064] Test items Example 1 Example 2 Comparative Example 1 Over discharge No fire, no explosion, no leakage No fire, no explosion, no leakage No fire, no explosion, no leakage Overcharge No fire or explosion (10V) No fire or explosion (10V) No fire or explosion (5.475V) Short circuit test No fire, no explosion No fire or explosion No fire, no explosion Heating test No fire or explosion (200℃) No fire or explosion (200℃) No fire or explosion (130℃) Extrusion test No fire, no explosion No fire, no explosion No fire, no explosion Acupuncture test No fire or explosion No fire, no explosion No fire, no explosion Heavy object impact test No fire, no explosion No fire, no explosion No fire or explosion Drop test No fire, no explosion, no leakage No fire, no explosion, no leakage No fire, no explosion, no leakage Seawater immersion test No fire, no explosion No fire, no explosion No fire, no explosion Temperature Cycle Test No fire, no explosion, no leakage No fire, no explosion, no leakage No fire, no explosion, no leakage Low pressure test No fire, no explosion, no leakage No fire, no explosion, no leakage No fire, no explosion, no leakage
[0065] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
Claims
1. A method for preparing a soft-pack gel solid-state lithium-ion battery, characterized in that: The following steps are involved: Step 1: Select a positive electrode sheet, a negative electrode sheet, a separator, a positive electrode ear, a negative electrode ear and a gel electrolyte; Step 2: stack the positive electrode sheet, the separator, and the negative electrode sheet in order to obtain a bare cell; Step 3: Select a lithium-ion battery aluminum shell, a positive electrode cover, a negative electrode cover, a positive electrode isolation ring, a Mylar film, and a side support sheet; Step 4: First weld the bare cell to the negative electrode cover plate, wrap and fix it with Mylar film, side support sheet, and positive electrode isolation ring, and then place it in the aluminum shell of the lithium-ion battery, and then weld the positive electrode ear of the positive electrode sheet to the positive electrode cover plate, and weld the negative electrode ear of the negative electrode sheet to the negative electrode cover plate; Step 5: seal and weld the negative electrode cover plate, the positive electrode cover plate and the aluminum shell of the lithium-ion battery to obtain a semi-finished battery cell before liquid injection; Step 6: The semi-finished battery cell before liquid injection is baked, liquid injected, pre-tightened, allowed to stand at room temperature for soaking, allowed to stand at high temperature for curing, sealed, and divided into different capacities to obtain a soft-pack gel solid-state lithium-ion battery; Among them, the gel electrolyte is composed of polymer monomers, lithium salts, solvents and initiators.
2. The method for preparing a soft-package gel solid-state lithium-ion battery according to claim 1, characterized in that: The mass ratio of the polymer monomer, lithium salt, solvent and initiator is 8:5:75:
4.
3. The method for preparing a soft-package gel solid-state lithium-ion battery according to claim 1, characterized in that: The polymer monomer is one or more of methyl acrylate, ethyl acrylate, butyl acrylate and octyl acrylate.
4. The method for preparing a soft-package gel solid-state lithium-ion battery according to claim 1, characterized in that: The lithium salt is one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorobisoxalate, bisfluorosulfonyl imide lithium salt and lithium dioxalate borate.
5. The method for preparing a soft-package gel solid-state lithium-ion battery according to claim 1, characterized in that: The solvent is a mixture of ethylene carbonate, dimethyl carbonate and propylene carbonate, and the mass ratio of the mixture of ethylene carbonate, dimethyl carbonate and propylene carbonate is 1:1:
1.
6. The method for preparing a soft-package gel solid-state lithium-ion battery according to claim 1, characterized in that: The initiator is a mixture of vinylene carbonate and propylene sulfite, and the mass ratio of the mixture of vinylene carbonate and propylene sulfite is 1:
1.
7. The method for preparing a soft-package gel solid-state lithium-ion battery according to claim 1, characterized in that: The torque applied to the semi-finished battery cell before liquid injection is 40-80cN.M.
8. The method for preparing a soft-package gel solid-state lithium-ion battery according to claim 1, characterized in that: The semi-finished battery cells are left to soak at room temperature for 48-72 hours before liquid injection.
9. The method for preparing a soft-package gel solid-state lithium-ion battery according to claim 1, characterized in that: The temperature of the semi-finished battery cell for high-temperature curing before liquid injection is 70-85°C, and the curing time is 2-10 hours.
Citation Information
Cited By
Lithium battery and preparation method thereof
CN120834297A
Lithium battery and preparation method thereof
CN120834297B