Preparation method of solid-state ordered electrolyte

The inorganic solid electrolyte matrix is ​​prepared and sintered through the template method to form a directional and orderly structure, which solves the problems of low ion conductivity and thermal failure of traditional solid electrolytes, improves the thermal stability and cycling performance of all-solid state batteries, and ensures high voltage and Safety at high magnifications.

CN118919859APending Publication Date: 2024-11-08TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310512224.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The low ionic conductivity and thicker electrolyte layer of traditional solid electrolytes lead to huge interfacial impedance and overpotentials, and there are serious thermal failures, affecting the safety and electrochemical performance of all-solid-state batteries.

Method used

The inorganic solid electrolyte matrix was prepared by the template method and sintered at high temperature to form a directionally ordered porous microstructure, which increased its ionic conductivity and reduced interface impedance.

Benefits of technology

It effectively improves the thermal stability and cycling performance of all solid-state batteries, ensuring long cycles and safety at high voltage windows and high magnifications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919859A_ABST
    Figure CN118919859A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an ordered solid electrolyte. The preparation method comprises the following steps: step 1, preparing an inorganic solid electrolyte matrix by using a template method; and 2, sintering at high temperature to form a directional and ordered porous microstructure on the surface and / or in the inorganic solid electrolyte matrix. According to the method disclosed by the invention, the ionic conductivity of the solid electrolyte is improved and the interface impedance is reduced by inducing the solid electrolyte to be ordered, so that the thermal stability of the all-solid-state battery is effectively improved, and the long circularity and safety of the all-solid-state battery under a high-voltage window and high magnification are ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and more specifically, to a method for preparing a solid ordered electrolyte. Background Art

[0002] Compared with liquid electrolyte-based batteries, solid-state batteries have the advantages of being non-flammable, having good mechanical strength, and good chemical stability. Solid-state battery technology relies heavily on solid electrolytes. However, the low ionic conductivity and thick electrolyte layer of traditional solid electrolytes lead to huge interfacial impedance and overpotential. There is still a serious thermal failure phenomenon at higher voltage windows and rates, which poses a great safety hazard, especially for polymer-based solid electrolytes such as polyethylene oxide. In order to improve the ionic conductivity of solid electrolytes and further improve the electrochemical performance and safety of all-solid-state batteries, it is necessary to explore new solid electrolytes, fundamentally study their ion transport mechanism, electrochemical stability window, and mechanical properties, and find ways to improve performance. Summary of the invention

[0003] In view of the above problems, the primary purpose of the present invention is to provide a method for preparing a solid ordered electrolyte. The preparation method improves the ionic conductivity and reduces the interface impedance by inducing the order of the solid electrolyte, thereby effectively improving the thermal stability of the all-solid-state battery and ensuring the long cycle and safety of the all-solid-state battery at a high voltage window and high rate.

[0004] In order to achieve the above object, the present invention adopts the following technical solutions:

[0005] The present invention provides a method for preparing a solid ordered electrolyte, comprising the following steps:

[0006] Step 1: Prepare an inorganic solid electrolyte matrix using a template method;

[0007] Step 2: high temperature sintering to form a directional and orderly porous microstructure on the surface and / or inside of the inorganic solid electrolyte matrix.

[0008] In a preferred embodiment of the present invention, the surface and interior of the inorganic solid electrolyte matrix include a plurality of oriented and ordered porous microstructures.

[0009] In a preferred embodiment of the present invention, the thickness of the inorganic solid electrolyte matrix is ​​1 μm to 2 mm.

[0010] Furthermore, the porous microstructure includes a combination of one or more of a plurality of columnar structures, near-columnar structures, linear structures, near-linear structures, mesh structures, and multi-layer mesh structures.

[0011] In a preferred embodiment of the present invention, the porous microstructure is a linear structure or a near-linear structure.

[0012] In a preferred embodiment of the present invention, the porous microstructure is a multi-layer network structure, such as a three-dimensional network similar to an aerogel skeleton structure.

[0013] Further, the high temperature sintering specifically includes the following operations:

[0014] In air atmosphere, 0.5~10℃·min -1 The heating rate is from room temperature to 350-500℃, and then at 1-20℃·min -1 The heating rate is raised to 1250-1500°C and maintained for 12 hours. Preferably, the heating rate is 1-3°C·min -1 The heating rate is from room temperature to 350-500℃, and then at 3-5℃·min -1 The heating rate is raised to 1250-1500°C and maintained for 12 hours. The present invention adopts a two-stage gradual heating process to prevent the template from being unevenly deformed due to excessively fast heating and to prevent the rapid decomposition of salts to produce a large amount of gas that affects the template morphology.

[0015] Furthermore, the template method uses a biomass template or a non-biomass template;

[0016] The biomass template has a fiber tubular structure; the non-biomass template is selected from one or more two-dimensional materials such as graphene oxide, MXene, hexagonal boron nitride, metal organic framework compounds, covalent organic framework compounds, layered double hydroxides, etc.

[0017] In a preferred embodiment of the present invention, the biomass template is wood or sugarcane.

[0018] In a more preferred embodiment of the present invention, the biomass template has a density of 1 g cm -3 Wood of this density has a moderate amount of pores, which can ensure the addition of the precursor mixture and avoid severe shrinkage of the template during sintering.

[0019] In a preferred embodiment of the present invention, the MXene material includes but is not limited to one or more of Ti3C2, Ti2C, V2C, TiVC, Ti3CN, Ti2N, V2N, V4C3, Mo2Ti2C3, Mo2C, etc.;

[0020] The metal organic framework compound includes but is not limited to one or more of a mesh metal-organic framework material (MOF-5, etc.), a zeolite imidazolate framework material (ZIF-8, ZIF-67, etc.), a Levasil framework material (MIL-100, MIL-101, etc.), a pore-channel framework material (HKUST-1, AAO, etc.), etc.;

[0021] The covalent organic framework compound includes but is not limited to one or more of boron-containing compounds (COF-1, COF-5, COF-13, etc.), triazines (CTF-1, etc.), imines (COF-300, etc.), phenylhydrazones, ketone amines, enamines, polyimides (PI-COF-4, PI-COF-5, etc.), phthalocyanines and porphyrins (COF-366, etc.);

[0022] The layered double hydroxide includes, but is not limited to, one or more of montmorillonite, zinc-aluminum layered double hydroxide, nickel-aluminum layered double hydroxide, and the like.

[0023] Furthermore, after step 2, the method further includes the step of uniformly injecting an organic solid electrolyte into the inorganic solid electrolyte matrix.

[0024] Further, when the template is a biomass template, step 1 specifically includes the following operations:

[0025] 1) dispersing the raw materials required for the inorganic solid electrolyte in a solvent to form a precursor mixed solution;

[0026] 2) The biomass template is quickly frozen into shape using liquid nitrogen and then freeze-dried;

[0027] 3) Soaking the freeze-dried biomass template in the precursor mixture for a certain period of time, freezing it with liquid nitrogen, and freeze-drying it.

[0028] Furthermore, in the above method, in step 2), the biomass template further comprises the steps of cutting and ultrasonic cleaning with ethanol and deionized water in sequence before freezing. The cutting can be cut into different shapes as needed, preferably sheets; the purpose of the ultrasonic cleaning is to remove impurities in the pores of the biomass template.

[0029] It can be understood that in step 3), the freeze-dried biomass template is immersed in the precursor mixture, and a certain period of time is required to allow the precursor mixture to fully enter the pores of the biomass template; room temperature immersion, temperature-assisted immersion (<100°C) or negative pressure-assisted immersion at room temperature can be selected, among which negative pressure-assisted immersion at room temperature (below standard atmospheric pressure) can allow the precursor mixture to enter the pores of the biomass template faster.

[0030] Further, when the template is a non-biomass template, step 1 specifically includes the following operations:

[0031] 1) dispersing the raw materials required for the inorganic solid electrolyte in a solvent to form a precursor mixed solution;

[0032] 2) placing the suspension of the non-biomass template and the precursor mixed solution in an open container, mixing and ultrasonically dispersing;

[0033] 3) Using liquid nitrogen to uniformly cool the container from the bottom, so that the liquid in the container is directionally frozen and formed from bottom to top, and then freeze-dried.

[0034] Furthermore, in the above method, in step 2), the concentration of the non-biomass template in the suspension is 2 to 20 mg·g -1 .

[0035] In step 3), the thermal conductivity of the bottom of the container and the side wall around the bottom are different. Preferably, the difference in thermal conductivity is at least 50 W·(m·K). -1 , more preferably 100 W·(m·K) -1 For example, the bottom of the container is made of brass, and the side wall around the bottom is made of polytetrafluoroethylene.

[0036] The freezing molding takes 3 to 10 minutes. In a specific embodiment of the present invention, the freezing time can be adjusted by the volume of liquid nitrogen added and / or the distance between the liquid nitrogen interface and the bottom of the freezing container.

[0037] By utilizing the parameters defined in the present invention, such as the thermal conductivity of the container, the freezing molding time, the concentration of the non-biomass template, etc., an inorganic solid electrolyte matrix with a higher degree of order can be obtained.

[0038] Further, when the template is a non-biomass template, step 1 specifically includes the following operations:

[0039] 1) dispersing the raw materials required for the inorganic ordered solid electrolyte in a solvent to form a precursor mixed solution;

[0040] 2) Adding a lithium salt solution to the suspension of the non-biomass template and stirring evenly to obtain a mixed solution;

[0041] 3) using electric field induction to vertically align the non-biomass template in the mixed solution to form a non-biomass template nanowall;

[0042] 4) Mixing the precursor mixed solution with a mixed solution containing non-biomass template nanowalls, slowly freezing the mixture with liquid nitrogen, and freeze-drying the mixture.

[0043] Furthermore, in the above method, in step 3), the electric field induction is specifically cyclic voltammetry.

[0044] When the non-biomass template is graphene oxide, the conditions for electric field induction are: a voltage range of -0.5 to 2 V, a scan rate of 5 to 500 mV·s -1 , the number of scans is more than 10 times;

[0045] Preferably, the concentration of the non-biomass template in the suspension is 0.1 to 10 mg mL -1 ; The concentration of lithium salt solution is 0.01~1mol·L -1 .

[0046] In a specific embodiment of the present invention, the lithium salt is Li2S or LiNO3.

[0047] This method uses slow freezing, and its freezing rate is generally between 0.0001 and 0.1 cm 3 ·min -1 Within this range, the strength of the nanowall of non-biomass templates is usually low. If the freezing speed is too fast, it will cause uncontrolled growth of ice crystals and cause certain damage to the template morphology.

[0048] Further, when the non-biomass template is any one or more of graphene oxide, MXene, metal organic framework compound, hexagonal boron nitride, step one specifically includes the following operations:

[0049] 1) dispersing the raw materials required for the inorganic solid electrolyte in a solvent to form a precursor mixed solution;

[0050] 2) Generate a horizontal rotating magnetic field in a certain space, place the suspension of non-biomass template in the magnetic field, and arrange them neatly under the action of the rotating magnetic field;

[0051] 3) Under the condition of maintaining the magnetic field, the precursor mixed solution is mixed with the suspension of the non-biomass template, frozen and formed, and freeze-dried.

[0052] Among them, the above method mainly utilizes the anti-magnetism of materials such as graphene oxide, MXene, metal organic framework compounds, hexagonal boron nitride, etc. to achieve the order of induced ordered inorganic solid electrolyte matrix in a magnetic field.

[0053] Furthermore, in the above method, the horizontal rotating magnetic field is generated at a speed of 5 to 15 revolutions per second.

[0054] In a specific embodiment of the present invention, under the action of a rotating magnetic field, the non-biomass templates are arranged neatly on the xy plane.

[0055] In the suspension, the concentration of the non-biomass template is 2 to 10 mg mL -1 .

[0056] In all methods of the present invention, the template suspension is mixed with the precursor mixture to obtain a mixture. In principle, the present invention does not specifically limit the concentration of the template and the metal salt (the metal salt is the total solute in the precursor mixture), and the technician can adjust it as needed. In order to obtain a more ordered inorganic solid electrolyte matrix, the present invention preferably limits the concentration of the template in the mixed liquid to 0.5 to 4 times the total concentration of the metal salt.

[0057] In a specific embodiment of the present invention, the temperature required for freezing molding is -55°C.

[0058] It is understood that the purpose of freeze drying is to remove moisture, and the freeze drying time is generally not less than 6 hours.

[0059] It can be understood that the raw materials required for the inorganic solid electrolyte in the present invention refer to the source of the metal elements in the inorganic solid electrolyte, generally the corresponding metal salt; for example, the perovskite inorganic solid electrolyte Li 0.35 La 0.55 TiO3, the required raw materials are the corresponding lithium salts, lanthanum salts and titanium salts.

[0060] In addition, unless otherwise specified, any range described in the present invention includes the end value and any value between the end values ​​and any sub-range formed by the end value or any value between the end values. The preparation methods in the present invention are conventional methods unless otherwise specified, the raw materials used can be obtained from public commercial channels or prepared according to the prior art unless otherwise specified, the percentages are mass percentages unless otherwise specified, and the solutions are aqueous solutions unless otherwise specified.

[0061] The beneficial effects of the present invention are as follows:

[0062] The invention provides a method for preparing a solid ordered electrolyte, which improves the ionic conductivity and reduces the interface impedance of an inorganic solid electrolyte by inducing ordering of the electrolyte.

[0063] The preparation method of the present invention can regulate the order of the inorganic solid electrolyte by regulating various process parameters, thereby obtaining a highly ordered solid electrolyte, which has the following advantages: effectively shortening the distance of ion transfer, providing a fast ion transfer channel, improving the thermal stability of the all-solid-state battery, and ensuring the long cycle performance and safety of the all-solid-state battery under high voltage window and high rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0065] Figure 1 The scanning electron microscope images of the LLTO solid electrolyte matrix prepared in Example 1 at different magnification ratios are shown.

[0066] Figure 2 The graph shows the cycle performance of the battery assembled in Example 1 after 200 charge and discharge cycles.

[0067] Figure 3 The graph shows the cycle performance of the battery assembled in Example 1 after 500 charge and discharge cycles.

[0068] Figure 4 The graph shows the cycle performance of the battery assembled in Example 2 after 200 charge and discharge cycles.

[0069] Figure 5 The graph shows the cycle performance of the battery assembled in Comparative Example 2 after 200 charge and discharge cycles.

[0070] Figure 6 The graph shows the cycle performance of the battery assembled in Example 3 after 200 charge and discharge cycles.

[0071] Figure 7 The graph shows the cycle performance of the battery assembled in Comparative Example 3 after 200 charge and discharge cycles.

[0072] Figure 8 A scanning electron microscope image of the LLTO solid electrolyte matrix prepared in Example 4 is shown.

[0073] Fig. 9 The graph shows the cycle performance of the battery assembled in Example 4 after 500 charge and discharge cycles.

[0074] Fig.10 A comparison chart of the rate performance of the LLTO solid electrolyte matrix prepared in Example 4 and the commercially available LLTO solid electrolyte matrix is ​​shown.

[0075] Fig.11 The graph shows the cycle performance of the battery assembled in Comparative Example 4 after 200 charge and discharge cycles.

[0076] Fig.12 A scanning electron microscope image of the LLTO solid electrolyte matrix prepared in Example 5 is shown.

[0077] Fig.13The graph shows the cycle performance of the battery assembled in Example 5 after 500 charge and discharge cycles.

[0078] Fig.14 A scanning electron microscope image of the LLTO solid electrolyte matrix prepared in Example 6 is shown.

[0079] Fig.15 The graph shows the cycle performance of the battery assembled in Example 6 after 500 charge and discharge cycles.

[0080] Fig.16 A schematic diagram showing the operation of the magnetic field-induced graphene vertical template in Example 7 is shown.

[0081] Fig.17 The graph shows the cycle performance of the battery assembled in Example 7 after 200 charge and discharge cycles. DETAILED DESCRIPTION

[0082] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0083] In the following comparative examples, the solid phase sintering method refers to the method in Microwave synthesis of lithium lanthanumtitanate[J].Solid State Communications,2003,125(10):557-562.; the traditional hydrothermal method refers to the method in AK2Fe4O7 superionic conductor for all-solid-state potassium metalbatteries[J].Journal of Materials Chemistry,A.Materials for energy andsustainability,2018,6(18):8413-8418.

[0084] The commercially purchased LLTO solid electrolyte matrix involved below is LLTO-300nm Li 0.33 La 0.56 TiO3.

[0085] Biomass Template Method

[0086] Example 1

[0087] 1) 2 mol L containing lithium nitrate (LiNO3), lanthanum nitrate hexahydrate (La(NO3)3·6H2O) and tetrabutyl titanate (Ti(OCH2CH2CH2CH3)4) (lithium nitrate: lanthanum nitrate hexahydrate: tetrabutyl titanate molar ratio 1.5:2.2:4) -1 The nitric acid dispersion was stirred for 4 hours to obtain a LLTO precursor mixed solution.

[0088] 2) Cut wood with a density of about 1 into round pieces with a diameter of 2 cm and a thickness of 1 mm along the cross section, ultrasonicate them in 60°C ethanol for 12 hours, and then ultrasonicate them in 60°C deionized water for 12 hours. Use liquid nitrogen to quickly freeze the round wood pieces, and then freeze-dry them for 12 hours to obtain a wood template.

[0089] 3) Soak the wooden template in the LLTO precursor mixture, evacuate the mixture to -75 kPa at room temperature for 1 hour, freeze it with liquid nitrogen, and freeze-dry it for 24 hours. Place the obtained solid product in a tube furnace in an air atmosphere at 1 °C min -1 From room temperature to 350℃, then at 5℃·min -1 The temperature was raised to 1250 °C, maintained for 12 hours, then decreased to 700 °C at 2 °C per minute, and finally cooled naturally to room temperature to obtain highly ordered Li 0.35 La 0.55 TiO3 (LLTO) solid electrolyte matrix. Figure 1 This example is a SEM of the LLTO solid electrolyte matrix prepared using a wood template. From the figure, it can be seen that the LLTO solid electrolyte matrix is ​​highly ordered. PEO-LiTFSI (EO: Li = 12: 1) is added to the LLTO solid electrolyte matrix to obtain a highly ordered polymer composite electrolyte LLTO-PEO-LiTFSI.

[0090] 4) Assemble the battery: Assemble button cells using the above LLTO-PEO-LiTFSI as the electrolyte, metallic lithium as the negative electrode, and lithium iron phosphate (the mass ratio of LiFePO4, conductive carbon black, and PVDF is 8:1:1) as the positive electrode. Test the constant current charge and discharge performance and cycle performance of the battery in an environment of 60°C.

[0091] The battery has a discharge capacity of 150.1 mAh g at a voltage window of 2 to 4 V at 60°C and a discharge rate of 0.1C. -1 . Figure 2 The figure is the cycle performance diagram of the battery at 60°C, 2-4V voltage window and 0.1C charge and discharge rate. The battery still has a capacity retention rate of 91.6% after 200 cycles and a capacity retention rate of 78.6% after 500 cycles ( Figure 3 ).

[0092] Comparative Example 1

[0093] The assembly of the battery of this embodiment is the same as that of embodiment 1, except that the preparation of the LLTO solid electrolyte matrix in LLTO-PEO-LiTFSI uses the traditional solid phase sintering method without biomass template-induced ordering.

[0094] The battery has a discharge capacity of 127.2 mAh g at a rate of 0.1 C in a voltage window of 2 to 4 V at 60 °C. -1 After 200 cycles at 60°C in a voltage window of 2 to 4 V at a rate of 0.1C, the capacity retention rate of the battery was only 31.5%.

[0095] Comparing Comparative Example 1 and Example 1, it can be seen that the battery assembled with the ordered LLTO-PEO-LiTFSI electrolyte has a much higher cycle stability than the battery assembled with the disordered LLTO-PEO-LiTFSI electrolyte.

[0096] Example 2

[0097] 1) Mix tetraethyl orthosilicate (C8H2O4Si), deionized water and anhydrous ethanol, and add a small amount of dilute nitric acid to ensure the full hydrolysis of the ester to obtain solution A. Dissolve sodium nitrate (NaNO3) and zirconium oxynitrate (ZrO(NO3)2) in deionized water at 60°C to obtain solution B. Dissolve diammonium hydrogen phosphate (NH4H2PO4) in deionized water to obtain solution C (sodium nitrate: zirconium oxynitrate: tetraethyl orthosilicate: diammonium hydrogen phosphate molar ratio 3.5:2:2:1.2). Mix the above three solutions A, B and C to obtain a white precursor mixture.

[0098] 2) Cut wood with a density of about 1 into round pieces with a diameter of 2 cm and a thickness of 1 mm along the cross section, ultrasonicate them in 60°C ethanol for 12 hours, and then ultrasonicate them in 60°C deionized water for 12 hours. Use liquid nitrogen to quickly freeze the round wood pieces, and then freeze-dry them for 12 hours to obtain a wood template.

[0099] 3) Soak the wooden template in the white precursor mixture, evacuate the mixture to -75 kPa at room temperature for 1 hour, freeze it with liquid nitrogen, and then freeze-dry it for 24 hours. Place the obtained solid product in a tube furnace in an air atmosphere at 1°C / min. -1 From room temperature to 350℃, then at 5℃·min -1 Raise to 1250℃, maintain for 12 hours, then increase the temperature to 2℃·min -1 The temperature was reduced to 700 °C and then cooled naturally to room temperature to obtain highly ordered Na3Zr2Si2PO4 12(NZSP) solid electrolyte matrix. PEO-NaTFSI (EO:Na=12:1) was added to the NZSP solid electrolyte matrix to obtain a highly ordered NZSP-PEO-NaTFSI polymer composite electrolyte.

[0100] 4) Assemble the battery: Assemble button cells with the above NZSP-PEO-NaTFSI as electrolyte, metal sodium as negative electrode, and sodium vanadium phosphate (Na3V2(PO4)3, Super P, PVDF with a mass ratio of 7:2:1) as positive electrode. Then test the constant current charge and discharge performance and cycle performance of the battery at 60°C.

[0101] The battery has a discharge capacity of 102.7 mAh g at a voltage window of 1.8 to 3.8 V at 0.1 C at 60 °C. -1 . Figure 4 The figure is a cycle performance diagram of the battery at 60°C, 1.8-3.8V voltage window and 0.1C rate charge and discharge. The battery still has a capacity retention rate of 84.7% after 200 cycles.

[0102] Comparative Example 2

[0103] The assembly of the battery in this embodiment is the same as that in embodiment 2, except that the NZSP solid electrolyte matrix in NZSP-PEO-NaTFSI is prepared by using a traditional solid phase sintering method without inducing order through a biomass template.

[0104] The battery has a discharge capacity of 86.2 mAh g at a voltage window of 1.8 to 3.8 V at a discharge rate of 0.1 C at 60 °C. -1 After 200 cycles at 0.1C rate in the voltage window of 1.8-3.8V at 60°C, the capacity retention rate of the battery was only 42.8% ( Figure 5 ).

[0105] Comparing Comparative Example 2 with Example 2, it can be seen that the cycle stability of the battery assembled with the ordered NZSP-PEO-NaTFSI electrolyte is much higher than that of the battery assembled with the disordered NZSP-PEO-NaTFSI electrolyte.

[0106] Example 3

[0107] 1) Slowly add ferric nitrate to secondary deionized water and stir on a magnetic stirrer for about 10 minutes until the ferric nitrate solid is completely dissolved, weigh a certain amount of KOH (50-90 g), add it to the ferric nitrate solution, and stir for about 0.5 hour. When the temperature drops to about 30° C., the color of the solution is dark brown and there is no KOH lumps, a precursor mixed solution is obtained.

[0108] 2) Cut wood with a density of about 1 into round pieces with a diameter of 2 cm and a thickness of 1 mm along the cross section, ultrasonicate them in 60°C ethanol for 12 hours, and then ultrasonicate them in 60°C deionized water for 12 hours. Use liquid nitrogen to quickly freeze the round wood pieces, and then freeze-dry them for 12 hours to obtain a wood template.

[0109] 3) Soak the wooden template in the precursor mixture, evacuate the mixture to -75 kPa at room temperature for 1 hour, freeze it with liquid nitrogen, and freeze-dry it for 24 hours. Place the obtained solid product in a tube furnace in an air atmosphere at 1 °C min -1 From room temperature to 350℃, then at 5℃·min -1 Raise to 1250℃, maintain for 12 hours, then increase the temperature to 2℃·min -1 The temperature was lowered to 700℃ and then cooled naturally to room temperature to obtain a highly ordered K2Fe4O7 (KFO) solid electrolyte matrix. PEO-KTFSI (EO:K=12:1) was added to the KFO solid electrolyte matrix to obtain a highly ordered KFO-PEO-KTFSI polymer composite electrolyte.

[0110] 4) Assemble the battery: Assemble button cells with the above KFO-PEO-KTFSI as electrolyte, potassium metal as negative electrode, and potassium iron sulfur oxygen fluoride (KFeSO4F, conductive carbon black, PVDF with a mass ratio of 8:1:1) as positive electrode. Then test the constant current charge and discharge performance and cycle performance of the battery at 60°C.

[0111] The battery has a discharge capacity of 111.5 mAh g at a voltage window of 2.5 to 4.5 V at a discharge rate of 0.1 C at 60 °C. -1 . Figure 6 The figure is a cycle performance diagram of the battery at 60°C, 2.5-4.5V voltage window and 0.1C rate charge and discharge. The battery still has a capacity retention rate of 78.2% after 200 cycles.

[0112] Comparative Example 3

[0113] The assembly of the battery in this embodiment is the same as that in embodiment 3, except that the KFO solid electrolyte matrix in KFO-PEO-KTFSI is prepared by a conventional hydrothermal method without inducing order through a biomass template.

[0114] The battery has a discharge capacity of 95.2 mAh g at a voltage window of 2.5 to 4.5 V at a discharge rate of 0.1 C at 60 °C. -1 After 200 cycles at 60°C in the voltage window of 2.5-4.5V and 0.1C rate, the capacity retention rate of the battery was only 32.7% ( Figure 7 ).

[0115] Comparing Comparative Example 3 and Example 3, it can be seen that the cycle stability of the battery assembled with the ordered KFO-PEO-KTFSI electrolyte is much higher than that of the battery assembled with the disordered KFO-PEO-KTFSI electrolyte.

[0116] Ice template method for 2D materials

[0117] Example 4

[0118] 1) 4 mol·L containing lithium nitrate (LiNO3), lanthanum nitrate hexahydrate (La(NO3)3·6H2O) and tetrabutyl titanate (Ti(OCH2CH2CH2CH3)4) (molar ratio 1.5:2.2:4) -1 The nitric acid dispersion was stirred for 4 hours to obtain a LLTO precursor mixed solution.

[0119] 2) Add an equal volume of 10 mg g -1 The graphene oxide (GO) dispersion was further ultrasonically dispersed for 2 hours, and a directional freezing method was used (the freezing mold used a cylindrical container with a brass bottom and a polytetrafluoroethylene wall with an inner diameter of 2 cm and a height of 5 cm; freezing method: a rectangular iron block (4 cm long, 4 cm wide, and 10 cm high) was placed in an insulated container, liquid nitrogen was added to the upper surface of the iron block, and the LLTO precursor mixture containing GO was transferred to the mold and placed on the upper surface of the iron block, and frozen after 5 to 10 minutes), and then freeze-dried for 24 hours. The obtained product was placed in a tubular furnace in an air atmosphere at 1°C min -1 From room temperature to 350℃, then at 5℃·min -1 Raise to 1250℃, maintain for 12 hours, then increase the temperature to 2℃·min -1 The temperature was reduced to 700 °C and then cooled naturally to room temperature to obtain highly ordered Li 0.35 La 0.55 TiO3(LLTO) solid electrolyte matrix( Figure 8 ). PEO-LiTFSI (EO:Li=8:1) was added to LLTO to obtain a highly ordered LLTO-PEO-LiTFSI polymer composite electrolyte.

[0120] Compare the rate performance of the commercially available LLTO solid electrolyte matrix with that of the LLTO solid electrolyte matrix prepared in this example ( Fig.10 ), it can be seen that the rate performance of the highly ordered LLTO-PEO-LiTFSI is significantly improved.

[0121] 3) Assemble the battery: Assemble button cells with the above LLTO-PEO-LiTFSI as the electrolyte, metal lithium as the negative electrode, and lithium iron phosphate (the mass ratio of LiFePO4, conductive carbon black, and PVDF is 8:1:1) as the positive electrode. Then test the constant current charge and discharge performance and cycle performance of the battery at 60°C.

[0122] The battery has a discharge capacity of 158.7 mAh g at a voltage window of 2 to 4 V at 60°C and a discharge rate of 0.1C. -1 , the battery still has a capacity retention rate of 91.1% after 500 cycles ( Fig. 9 ).

[0123] Comparative Example 4

[0124] The assembly of the battery of this embodiment is the same as that of Example 4, except that the preparation of the LLTO solid electrolyte matrix in LLTO-PEO-LiTFSI uses the traditional solid phase sintering method without the ice template method to induce ordering of graphene oxide.

[0125] The battery has a discharge capacity of 127.2 mAh g at a rate of 0.1 C in a voltage window of 2 to 4 V at 60 °C. -1 After 200 cycles at 60°C with a voltage window of 2 to 4 V and a rate of 0.1C, the capacity retention rate of the battery was only 31.5% ( Fig.11 ).

[0126] Example 5

[0127] The operation of this embodiment is the same as that of embodiment 4, except that the bottom of the container is also made of polytetrafluoroethylene. The LLTO-PEO-LiTFSI polymer composite electrolyte finally obtained has a highly ordered Li 0.35 La 0.55 The microstructure of TiO3(LLTO) solid electrolyte matrix is ​​shown in Fig.12 .

[0128] The battery of this example has a specific capacity of 156.4 mAh·g at a discharge rate of 0.1C in a voltage window of 2 to 4 V at 60°C. -1 The battery has a capacity retention rate of 74.9% after 500 cycles at 0.1C rate in a voltage window of 2-4V at 60°C. Fig.13 ).

[0129] Electric Field Method for Two-Dimensional Materials

[0130] Example 6

[0131] 1) 4 mol·L containing lithium nitrate (LiNO3), lanthanum nitrate hexahydrate (La(NO3)3·6H2O) and tetrabutyl titanate (Ti(OCH2CH2CH2CH3)4) (molar ratio 1.5:2.2:4) -1 The nitric acid dispersion was stirred for 4 hours to obtain a LLTO precursor mixed solution.

[0132] 2) 1 mg·mL -1 The graphene oxide dispersion was mixed with 0.1 mol·L -1 Li2S was mixed and stirred for 12 hours. Then, the electrochemical assembly was carried out in a two-electrode system with a conductive substrate (copper or nickel sheet) as the working electrode and a platinum sheet as the reference electrode. The voltage range of the controlled cyclic voltammetry process was -0.5 to 2 V, and the scan rate was 50 mV·s -1 , scanned 20 times to generate 2.2 mg cm -2 Vertically aligned graphene oxide nanowalls.

[0133] 3) Adding the LLTO precursor mixed solution to the above graphene oxide nanowall solution to obtain mixed solution A, slowly freezing the mixed solution A with liquid nitrogen, and then freeze-drying it for 24 hours. The obtained solid product is placed in a tube furnace in an air atmosphere at 1°C min -1 The temperature was raised from room temperature to 350°C, then to 1250°C at 5°C / min, maintained for 12 hours, and then to 2°C / min. -1 The temperature was reduced to 700 °C and then cooled naturally to room temperature to obtain highly ordered Li 0.35 La 0.55 TiO3(LLTO) solid electrolyte matrix( Fig.14 ). PEO-LiTFSI (EO:Li=12:1) was added to LLTO to obtain a highly ordered LLTO-PEO-LiTFSI polymer composite electrolyte.

[0134] 4) Assemble the battery: Assemble button cells with the above LLTO-PEO-LiTFSI as the electrolyte, metal lithium as the negative electrode, and lithium iron phosphate (the mass ratio of LiFePO4, conductive carbon black, and PVDF is 8:1:1) as the positive electrode. Then test the constant current charge and discharge performance and cycle performance of the battery at 60°C.

[0135] The battery has a discharge capacity of 153.5 mAh g at a voltage window of 2 to 4 V at 60°C and a discharge rate of 0.1C. -1 . Fig.15This is the cycle performance diagram of the battery at 60°C, 2-4V voltage window and 0.1C rate charge and discharge. The battery still has a capacity retention rate of 90.5% after 500 cycles, and its cycle stability is much higher than that of the disordered LLTO-PEO-LiTFSI electrolyte.

[0136] Magnetic Field Method for Two-Dimensional Materials

[0137] Example 7

[0138] 1) 4 mol·L containing lithium nitrate (LiNO3), lanthanum nitrate hexahydrate (La(NO3)3·6H2O) and tetrabutyl titanate (Ti(OCH2CH2CH2CH3)4) (molar ratio 1.5:2.2:4) -1 The nitric acid dispersion was stirred for 4 hours to obtain a LLTO precursor mixed solution.

[0139] 2) If Fig.16 , containing 7 mg·mL -1 A 50mL centrifuge tube of graphene suspension is placed between two 5cm thick NdFeB magnet cubes, mounted on a motor, which generates a horizontal rotating magnetic field at a speed of 5-15 revolutions per second. The magnetic field strength is adjustable over a large distance. Due to the strong anti-magnetism of graphene sheets, they are neatly arranged on the xy plane swept by the rotating magnetic field to obtain a template solution.

[0140] 3) Add the LLTO precursor mixture to the above template solution, place a large plastic beaker filled with liquid nitrogen outside the centrifuge tube, keep the magnetic field in place to freeze the mixture, and then freeze-dry for 24 hours. Place the obtained solid product in a tube furnace in an air atmosphere at 1°C min -1 From room temperature to 350℃, then at 5℃·min -1 Raise to 1250℃, maintain for 12 hours, then increase the temperature to 2℃·min -1 The temperature was reduced to 700 °C and then cooled naturally to room temperature to obtain highly ordered Li 0.35 La 0.55 TiO3 (LLTO) solid electrolyte matrix. PEO-LiTFSI (EO:Li=12:1) was added to LLTO to obtain a highly ordered LLTO-PEO-LiTFSI polymer composite electrolyte.

[0141] 4) Assemble the battery: Assemble button cells with the above LLTO-PEO-LiTFSI as the electrolyte, metal lithium as the negative electrode, and lithium iron phosphate (the mass ratio of LiFePO4, conductive carbon black, and PVDF is 8:1:1) as the positive electrode. Then test the constant current charge and discharge performance and cycle performance of the battery at 60°C.

[0142] The battery has a discharge capacity of 148.1 mAh g at a voltage window of 2 to 4 V at 60°C and a discharge rate of 0.1C. -1 . Fig.17 The figure shows the cycle performance of the battery at 60°C, 2-4V voltage window and 0.1C rate charge and discharge. The battery still has a capacity retention rate of 91.6% after 200 cycles, and its cycle stability is much higher than that of the disordered LLTO-PEO-LiTFSI electrolyte.

[0143] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made on the basis of the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A method for preparing a solid ordered electrolyte, characterized in that: The following steps are involved: Step 1: Prepare an inorganic solid electrolyte matrix using a template method; Step 2: high temperature sintering to form a directional and orderly porous microstructure on the surface and / or inside of the inorganic solid electrolyte matrix.

2. The preparation method according to claim 1, characterized in that The porous microstructure includes a combination of one or more of a plurality of columnar structures, near-columnar structures, linear structures, near-linear structures, mesh structures, and multi-layer mesh structures.

3. The preparation method according to claim 1, characterized in that: The high temperature sintering specifically includes the following operations: In air atmosphere, 0.5~10℃·min -1 The heating rate is from room temperature to 350-500℃, and then at 1-20℃·min -1 The heating rate is increased to 1250-1500°C and maintained for 12 hours.

4. The preparation method according to claim 1, characterized in that: The template method uses a biomass template or a non-biomass template; The biomass template has a fiber tubular structure. Preferably, the biomass template is wood or sugarcane, and more preferably has a density of 1 g·cm -3 of wood; The non-biomass template is selected from one or more two-dimensional materials such as graphene oxide, MXene, hexagonal boron nitride, metal organic framework compounds, covalent organic framework compounds, layered double hydroxides, etc.

5. The preparation method according to claim 1, characterized in that: After step 2, the method further includes the step of uniformly injecting an organic solid electrolyte into the inorganic solid electrolyte matrix.

6. The preparation method according to claim 4, characterized in that: When the template is a biomass template, step 1 specifically includes the following operations: 1) dispersing the raw materials required for the inorganic solid electrolyte in a solvent to form a precursor mixed solution; 2) The biomass template is quickly frozen into shape using liquid nitrogen and then freeze-dried; 3) The freeze-dried biomass template is immersed in the precursor mixture for a certain period of time, and then frozen into shape using liquid nitrogen and freeze-dried; Preferably, in step 2), the biomass template further comprises the steps of cutting and ultrasonically cleaning with ethanol and deionized water in sequence before freezing.

7. The preparation method according to claim 4, characterized in that: When the template is a non-biomass template, step 1 specifically includes the following operations: 1) dispersing the raw materials required for the inorganic solid electrolyte in a solvent to form a precursor mixed solution; 2) placing the suspension of the non-biomass template and the precursor mixed solution in an open container, mixing and ultrasonically dispersing; 3) using liquid nitrogen to uniformly cool the container from the bottom to freeze the liquid in the container from bottom to top, followed by freeze drying; Preferably, in step 2), the concentration of the non-biomass template in the suspension is 2 to 20 mg·g -1 ; Preferably, in step 3), the thermal conductivity of the bottom of the container and the side wall around the bottom are different, and preferably, the difference in thermal conductivity is at least 50 W·(m·K). -1 , more preferably 100 W·(m·K) -1 ; Preferably, the freezing molding takes 3 to 10 minutes.

8. The preparation method according to claim 4, characterized in that: When the template is a non-biomass template, step 1 specifically includes the following operations: 1) dispersing the raw materials required for the inorganic ordered solid electrolyte in a solvent to form a precursor mixed solution; 2) Adding a lithium salt solution to the suspension of the non-biomass template and stirring the mixture to obtain a mixed solution; 3) using electric field induction to vertically align the non-biomass template in the mixed solution to form a non-biomass template nanowall; 4) Mixing the precursor mixed solution with a mixed solution containing non-biomass template nanowalls, slowly freezing the mixture with liquid nitrogen, and freeze-drying the mixture.

9. The preparation method according to claim 8, characterized in that: In step 3), the electric field induction is specifically cyclic voltammetry; When the non-biomass template is graphene oxide, the conditions for electric field induction are: a voltage range of -0.5 to 2 V, a scan rate of 5 to 500 mv·s -1 , the number of scans is more than 10 times; Preferably, the concentration of the non-biomass template in the suspension is 0.1 to 10 mg mL -1 ; The concentration of lithium salt solution is 0.01~1mol·L -1 .

10. The preparation method according to claim 4, characterized in that: When the non-biomass template is any one or more of graphene oxide, MXene, metal organic framework compound, hexagonal boron nitride, step 1 specifically includes the following operations: 1) The raw materials required for the inorganic solid electrolyte are dispersed in a solvent to form a precursor mixed solution; 2) Generate a horizontal rotating magnetic field in a certain space, place the suspension of non-biomass template in the magnetic field, and arrange them neatly under the action of the rotating magnetic field; 3) Under the condition of maintaining the magnetic field, the precursor mixed solution is mixed with the suspension of the non-biomass template, frozen into shape by liquid nitrogen, and freeze-dried; Preferably, the horizontal rotating magnetic field is generated at a speed of 5 to 15 revolutions per second; preferably, the concentration of the non-biomass template in the suspension is 2 to 10 mg·mL -1 .