Immersion method of lithium ion battery

The bubbles on the battery pole are eliminated through low-temperature storage, which solves the problem of poor infiltration of lithium-ion batteries, significantly improves the dynamic performance and capacity of the battery cell, and avoids the side effects of high-temperature storage.

CN118919864APending Publication Date: 2024-11-08ZHEJIANG LIWINON ELECTRONIC TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410992393.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Poor infiltration of lithium-ion batteries leads to degradation of cell dynamics, insufficient capacity, high impedance and dark spots, and existing methods cannot effectively solve the adsorption effect of gas in pole sheets and material particles.

Method used

Using a low-temperature storage method, the battery cell after completing the first infiltration operation is placed in an environment below room temperature, and the bubbles adsorbed on the battery electrode sheet are eliminated by using the characteristics of gas solubility with the temperature to ensure that the electrolyte is in full contact with the electrode material. This improves the wetting effect.

Benefits of technology

Through low-temperature treatment, the gas phase isolation effect is eliminated, the wetting effect of the battery cell is improved, the side effects caused by high-temperature storage are avoided, and the dynamic performance and capacity of the battery cell are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919864A_ABST
    Figure CN118919864A_ABST
Patent Text Reader

Abstract

The invention discloses an infiltration method of a lithium ion battery, and the infiltration method comprises the following steps: injecting electrolyte into a battery cell so as to execute electrolyte injection operation on the battery cell; performing first infiltration operation on the battery cell after the liquid injection operation is completed; placing the battery cell after the first infiltration operation in an environment with a first preset temperature for storage so as to execute a second infiltration operation on the battery cell; wherein the first preset temperature is larger than the freezing temperature of the electrolyte and smaller than or equal to 10 DEG C. According to the invention, the battery cell subjected to the first infiltration operation is stored in the environment lower than the room temperature in a low-temperature storage manner, and bubbles adsorbed on the battery pole piece can be eliminated by utilizing the characteristic that the solubility of gas is increased along with the reduction of the temperature, so that the electrolyte and the electrode material are in full contact, and the battery efficiency is improved. Therefore, the infiltration effect of the battery cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and in particular to an impregnation method for lithium ion batteries. Background Art

[0002] Poor wetting of lithium-ion batteries can lead to decreased dynamic performance of the battery cell, resulting in problems such as insufficient capacity, high impedance, black spots, lithium precipitation, etc. In the prior art, the method for improving the wetting of lithium-ion batteries is usually to extend the wetting time or increase the wetting temperature.

[0003] These methods can only improve the wetting effect between the solid phase and the liquid phase. In the actual process, due to the pores in the pole pieces and material particles, the gas may be adsorbed on the surface of the material particles in the form of bubbles and stored in the pores. The presence of these gases will isolate the material particles from the contact with the electrolyte, affecting the wetting effect. Summary of the invention

[0004] The main purpose of the present invention is to provide a lithium ion battery impregnation method, aiming to solve the problem that the existing battery impregnation method may generate bubbles in the pole piece and affect the impregnation effect.

[0005] To achieve the above object, the present invention provides a lithium ion battery impregnation method, the impregnation method comprising:

[0006] Injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell;

[0007] Performing a first wetting operation on the battery cell after the liquid injection operation is completed;

[0008] placing the battery cell after the first soaking operation in an environment of a first preset temperature for storage, so as to perform a second soaking operation on the battery cell;

[0009] Wherein, the first preset temperature is greater than the freezing temperature of the electrolyte and is less than or equal to 10°C.

[0010] Preferably, the first preset temperature is at least 5°C greater than the freezing temperature of the electrolyte and is less than or equal to 5°C.

[0011] Preferably, the first preset temperature is greater than -40°C and less than or equal to 0°C.

[0012] Preferably, the first preset temperature is greater than or equal to -20°C and less than 0°C.

[0013] Preferably, the step of placing the battery cell after the first soaking operation in an environment with a first preset temperature for storage includes:

[0014] Placing the battery cell after the first soaking operation in an environment of a first preset temperature and storing it for a first preset time;

[0015] The first preset duration is greater than or equal to 12 hours and less than or equal to 48 hours.

[0016] Preferably, after performing the second wetting operation on the battery cell, the wetting method further comprises:

[0017] placing the battery cell after the second soaking operation in an environment of a second preset temperature for storage, so as to perform a third soaking operation on the battery cell;

[0018] Wherein, the second preset temperature is greater than the first preset temperature.

[0019] Preferably, after performing the third soaking operation on the battery cell once, the soaking method further comprises: repeatedly performing the second soaking operation and the third soaking operation on the battery cell at least once in sequence.

[0020] Preferably, after the first soaking operation is performed on the battery cell, the second soaking operation and the third soaking operation are sequentially repeated on the battery cell for a number of times greater than or equal to 3 times and less than or equal to 10 times.

[0021] Preferably, placing the battery cell in an environment of a first preset temperature for storage comprises: placing the battery cell after the first soaking operation in an environment of the first preset temperature for storage for a second preset time;

[0022] The second preset time length X and the number of times Y of performing the second soaking operation on the battery cell in the soaking method satisfy XY≥12, where the unit of X is h and the unit of Y is times.

[0023] Preferably, the second preset duration is greater than or equal to 1 hour.

[0024] Preferably, the storing of the battery cell after the second soaking operation in an environment of a second preset temperature comprises: placing the battery cell in an environment of the second preset temperature for storage for a third preset time, wherein the third preset time is the time from when the battery cell is placed in the environment of the second preset temperature to when the surface temperature of the battery cell reaches the second preset temperature plus at least 0.5h; and / or,

[0025] The second preset temperature is greater than or equal to 20° C. and less than or equal to 45° C.

[0026] Preferably, after performing a first wetting operation on the battery cell and before performing a second wetting operation on the battery cell, the wetting method further comprises: performing a formation operation on the battery cell after completing the first wetting operation.

[0027] Preferably, performing a first wetting operation on the battery cell after the liquid injection operation is completed includes:

[0028] Placing the battery cell after the injection operation is completed in an environment of a third preset temperature for a fourth preset time period;

[0029] placing the battery cell in an environment with a fourth preset temperature for a fifth preset time;

[0030] Wherein, the third preset temperature is greater than or equal to 20° C. and less than or equal to 30° C., and the fourth preset time is greater than or equal to 12 hours and less than or equal to 48 hours;

[0031] The fourth preset temperature is 45° C.±10° C., and the fifth preset time is greater than or equal to 12 hours and less than or equal to 48 hours.

[0032] The beneficial effect of the technical solution of the present invention is that: by storing the battery cell after the first infiltration operation in an environment below room temperature in a low-temperature storage manner, the present invention can utilize the characteristic that the solubility of gas increases with decreasing temperature to eliminate bubbles adsorbed on the battery pole pieces, eliminate the gas phase isolation effect, and allow the electrolyte and the electrode material to fully contact, thereby improving the infiltration effect of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A flow chart of a lithium-ion battery impregnation method provided by one embodiment of the present invention.

[0034] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0035] The scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, top, bottom, side...) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0037] It should also be noted that when an element is referred to as being "fixed on" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element at the same time. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.

[0038] In addition, the descriptions involving "first", "second", etc. in the embodiments of the present invention are only for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features.

[0039] In view of the technical defects existing in the related art, an embodiment of the present invention provides a lithium ion battery impregnation method, referring to Figure 1 , the infiltration method comprises:

[0040] Step S100, injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell;

[0041] Step S200, performing a first wetting operation on the battery cell after the liquid injection operation is completed;

[0042] Step S300, placing the battery cell after the first soaking operation in an environment of a first preset temperature for storage, so as to perform a second soaking operation on the battery cell;

[0043] Wherein, the first preset temperature is greater than the freezing temperature of the electrolyte and is less than or equal to 10°C.

[0044] Specifically, by storing the battery cell after the first infiltration operation in an environment below room temperature in a low-temperature storage manner, the gas solubility increases with decreasing temperature, and the bubbles adsorbed on the battery pole pieces can be eliminated, so that the electrolyte can directly and fully contact the electrode material, thereby improving the infiltration effect of the battery cell. Compared with the prior art, the battery cell will have serious side reactions during high-temperature storage, causing the battery cell to expand, causing irreversible effects on the battery cell itself, while the method of the present application improves the infiltration effect of the battery cell without causing side effects on the battery cell.

[0045] In some embodiments, the first preset temperature is at least 5° C. greater than the freezing temperature of the electrolyte and is less than or equal to 5° C.

[0046] Specifically, setting the first preset temperature at least 5°C higher than the freezing temperature of the electrolyte can improve the wetting effect of the battery cell while ensuring the fluidity of the electrolyte. Therefore, the present application can also test the freezing temperature of the electrolyte before injecting the electrolyte into the battery cell to further reduce the temperature and improve the wetting effect.

[0047] In some embodiments, the first preset temperature is greater than -40°C and less than or equal to 0°C.

[0048] Specifically, since the freezing temperature of lithium-ion battery electrolyte is usually as low as -45°C, setting the first preset temperature to be greater than -40°C and less than or equal to 0°C can improve the wetting effect of the battery cell while ensuring the fluidity of the electrolyte.

[0049] In some embodiments, the first preset temperature is greater than or equal to -20°C and less than 0°C.

[0050] Specifically, since the solubility of the gas increases with decreasing temperature, and the wetting speed of the battery cell decreases with decreasing temperature, setting the first preset temperature at -20°C to 0°C can not only increase the solubility of the bubbles adsorbed on the electrode and thus improve the wetting effect of the battery cell, but also improve the wetting efficiency of the part isolated by the bubbles with the electrolyte.

[0051] In some embodiments, storing the battery cell after the first soaking operation in an environment with a first preset temperature includes:

[0052] Placing the battery cell after the first soaking operation in an environment of a first preset temperature and storing it for a first preset time;

[0053] The first preset duration is greater than or equal to 12 hours and less than or equal to 48 hours.

[0054] Specifically, after the battery cell that has completed the first infiltration operation is placed at a low temperature for storage, it takes time for the bubbles on the electrode to dissolve, and sufficient infiltration time needs to be reserved for the battery cell after the bubbles dissolve. Therefore, the first preset time is set to 12h to 48h.

[0055] In another embodiment of the present invention, after performing the second wetting operation on the battery cell, the wetting method further includes:

[0056] placing the battery cell after the second soaking operation in an environment of a second preset temperature for storage, so as to perform a third soaking operation on the battery cell;

[0057] Wherein, the second preset temperature is greater than the first preset temperature.

[0058] Specifically, another implementation method of the present application is to improve the wetting effect through temperature changes between low temperature and room temperature. This is because a large amount of gas will be generated in the battery cell during the formation process and adsorbed in the pores in the electrode piece. By storing the battery cell after the first infiltration operation in an environment below room temperature in a low-temperature storage manner, the characteristic that the solubility of gas increases with decreasing temperature can be utilized to eliminate the bubbles adsorbed on the battery electrode piece, so that the electrolyte can directly contact the electrode material, thereby improving the wetting effect of the battery cell. The battery cell after the second infiltration operation is then placed in an environment higher than the first preset temperature. The pores in the electrode piece can expand and contract with the change of temperature through thermal expansion and contraction, thereby squeezing out the bubbles. The battery cell is placed from a low-temperature environment to a normal temperature environment, so that the pores from which the bubbles have been squeezed out and the parts of the electrode piece isolated by bubbles can be quickly infiltrated with the electrolyte, thereby improving the wetting efficiency.

[0059] In some embodiments, after performing the third soaking operation on the battery cell once, the soaking method further includes: sequentially repeating the second soaking operation and the third soaking operation on the battery cell at least once.

[0060] Specifically, through the temperature cycle of "low temperature-room temperature", the pores in the pole piece can be continuously expanded and contracted to better squeeze out the bubbles in the pores.

[0061] In some embodiments, after the first soaking operation is performed on the battery cell, the second soaking operation and the third soaking operation are sequentially repeated on the battery cell for a number of times greater than or equal to 3 times and less than or equal to 10 times.

[0062] Specifically, setting the number of cycles to 3 to 10 times can optimize the wetting effect of the battery cell while also improving the wetting efficiency of the battery cell, to prevent the problem of too much cycle time wasting too much time and resulting in low wetting efficiency, where the wetting effect is not significantly improved.

[0063] In some embodiments, the placing the battery cell in an environment of a first preset temperature for storage includes: placing the battery cell after the first soaking operation in an environment of the first preset temperature for storage for a second preset time;

[0064] The second preset time length X and the number of times Y of performing the second soaking operation on the battery cell in the soaking method satisfy XY≥12, where the unit of X is h and the unit of Y is times.

[0065] Specifically, the second preset time is set to the time from when the battery cell is placed in an environment of the first preset temperature to when the temperature of the surface of the battery cell reaches the first preset temperature plus at least 0.5h. Since the battery cell is transferred from room temperature to a low temperature environment for storage, it is necessary to wait for the battery cell to slowly cool down to the ambient temperature (the first preset temperature), and when the temperature of the surface of the battery cell reaches the ambient temperature, in order to ensure that the temperature inside the battery cell can also reach the ambient temperature, and to leave enough time for the dissolution of bubbles in the battery cell and the extrusion of bubbles in the pores, it is necessary to continue to store for at least 0.5h when the surface temperature of the battery cell reaches the ambient temperature. Furthermore, by making the total time of the second preset time greater than or equal to 12h, the dual effects of low-temperature dissolving bubbles and temperature cycle squeezing bubbles can be superimposed.

[0066] In some embodiments, the second preset duration is greater than or equal to 1 hour.

[0067] Specifically, the second preset time is positively correlated with the battery cell thickness and the temperature difference between the first preset temperature and the second preset temperature (second preset temperature-first preset temperature). Therefore, a suitable second preset time can be selected according to the battery cell thickness and the temperature difference, preferably greater than or equal to 1h.

[0068] In some embodiments, the step of placing the battery cell after the second infiltration operation in an environment of a second preset temperature for storage includes: placing the battery cell in an environment of the second preset temperature for storage for a third preset time, wherein the third preset time is the time from when the battery cell is placed in the environment of the second preset temperature to when the surface temperature of the battery cell reaches the second preset temperature plus at least 0.5h; and / or,

[0069] The second preset temperature is greater than or equal to 20° C. and less than or equal to 45° C.

[0070] Specifically, the third preset time is set to the time from when the battery cell is placed in an environment of the second preset temperature to when the temperature of the surface of the battery cell reaches the second preset temperature plus at least 0.5h. Since the battery cell is transferred from a low temperature environment to a room temperature environment for storage, it is necessary to wait for the battery cell to slowly heat up to the ambient temperature (the second preset temperature), and when the temperature of the surface of the battery cell reaches the ambient temperature, in order to ensure that the temperature inside the battery cell can also reach the ambient temperature and to leave enough time for the bubbles in the pores to squeeze out, it is necessary to continue to store for at least 0.5h when the surface temperature of the battery cell reaches the ambient temperature; further, the third preset time is positively correlated with the thickness of the battery cell and the temperature difference between the first preset temperature and the second preset temperature (second preset temperature-first preset temperature). Therefore, an appropriate third preset time can be selected according to the thickness of the battery cell and the temperature difference.

[0071] In some embodiments, after performing a first soaking operation on the battery cell and before performing a second soaking operation on the battery cell, the soaking method further includes: performing a formation operation on the battery cell after completing the first soaking operation.

[0072] Specifically, since a large amount of gas is generated during the formation process of the battery cell, it may be adsorbed in the pores in the electrode piece, and the second sealing process involves exhausting air, the battery cell after the first infiltration process is subjected to a formation operation and the second infiltration operation or the second infiltration operation and the third infiltration operation are performed before the second sealing process. In this way, the bubbles in the pores can be squeezed out first, and then the air can be exhausted to achieve the best effect. It should be noted that if it is a hard shell battery cell (such as a cylindrical or square aluminum shell), since there is no second sealing process, the same effect can be achieved by using this method after formation and before sealing.

[0073] In some embodiments, performing a first wetting operation on the battery cell after the liquid injection operation is completed includes:

[0074] Placing the battery cell after the injection operation is completed in an environment of a third preset temperature for a fourth preset time period;

[0075] placing the battery cell in an environment with a fourth preset temperature for a fifth preset time;

[0076] Wherein, the third preset temperature is greater than or equal to 20° C. and less than or equal to 30° C., and the fourth preset time is greater than or equal to 12 hours and less than or equal to 48 hours;

[0077] The fourth preset temperature is 45° C.±10° C., and the fifth preset time is greater than or equal to 12 hours and less than or equal to 48 hours.

[0078] Specifically, the first infiltration operation in the present application adopts a conventional infiltration process, which will not be described in detail here.

[0079] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.

[0080] Case 1

[0081] A lithium ion battery impregnation method comprising:

[0082] Step S100, injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell;

[0083] Step S200, placing the battery cell after the liquid injection operation in an environment of 23° C. for 24 hours, and then placing the battery cell in an environment of 45° C. for 24 hours.

[0084] After completing the wetting process, the battery cells are subjected to conventional processes for formation, secondary sealing, capacity division, OCV and appearance testing to prepare finished battery cells.

[0085] Case 2

[0086] A lithium ion battery impregnation method comprising:

[0087] Step S100, injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell;

[0088] Step S200, placing the battery cell after the liquid injection operation in an environment of 23° C. for 24 hours, and then placing the battery cell in an environment of 45° C. for 24 hours;

[0089] Step S300: storing the battery cell in a -40°C environment for 24 hours.

[0090] After completing the wetting process, the battery cells are subjected to conventional processes for formation, secondary sealing, capacity division, OCV and appearance testing to prepare finished battery cells.

[0091] Case 3

[0092] A lithium ion battery impregnation method comprising:

[0093] Step S100, injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell;

[0094] Step S200, placing the battery cell after the liquid injection operation in an environment of 23° C. for 24 hours, and then placing the battery cell in an environment of 45° C. for 24 hours;

[0095] Step S300: storing the battery cell in a -20°C environment for 24 hours.

[0096] After completing the wetting process, the battery cells are subjected to conventional processes for formation, secondary sealing, capacity division, OCV and appearance testing to prepare finished battery cells.

[0097] Case 4

[0098] A lithium ion battery impregnation method comprising:

[0099] Step S100, injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell;

[0100] Step S200, placing the battery cell after the liquid injection operation in an environment of 23° C. for 24 hours, and then placing the battery cell in an environment of 45° C. for 24 hours;

[0101] Step S300: storing the battery cell in an environment of 0° C. for 24 hours.

[0102] After completing the wetting process, the battery cells are subjected to conventional processes for formation, secondary sealing, capacity division, OCV and appearance testing to prepare finished battery cells.

[0103] Case 5

[0104] A lithium ion battery impregnation method comprising:

[0105] Step S100, injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell;

[0106] Step S200, placing the battery cell after the liquid injection operation in an environment of 23° C. for 24 hours, and then placing the battery cell in an environment of 45° C. for 24 hours;

[0107] Step S300: storing the battery cell in an environment of 23° C. for 24 hours.

[0108] After completing the wetting process, the battery cells are subjected to conventional processes for formation, secondary sealing, capacity division, OCV and appearance testing to prepare finished battery cells.

[0109] Case 6

[0110] A lithium ion battery impregnation method comprising:

[0111] Step S100, injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell;

[0112] Step S200, placing the battery cell after the liquid injection operation in an environment of 23° C. for 24 hours, and then placing the battery cell in an environment of 45° C. for 24 hours;

[0113] Step S300, placing the battery cell in a high and low temperature box, lowering the temperature of the box to -20°C at a cooling rate of 2°C / min, and then leaving it for 2 hours;

[0114] Step S400, raising the temperature of the incubator to 23°C at a cooling rate of 5°C / min, and then leaving it for 2 hours.

[0115] Step S500: repeat steps S300 and S400 for 6 times in total.

[0116] After completing the wetting process, the battery cells are subjected to conventional processes for formation, secondary sealing, capacity division, OCV and appearance testing to prepare finished battery cells.

[0117] Case 7

[0118] A lithium ion battery impregnation method comprising:

[0119] Step S100, injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell;

[0120] Step S200, placing the battery cell after the liquid injection operation in an environment of 23° C. for 24 hours, and then placing the battery cell in an environment of 45° C. for 24 hours;

[0121] Step S300, forming the battery cell according to a conventional process;

[0122] Step S400, placing the battery cell in a high and low temperature box, lowering the temperature of the box to -20°C at a cooling rate of 2°C / min, and then leaving it for 2 hours;

[0123] Step S500, raising the temperature of the incubator to 23°C at a cooling rate of 5°C / min, and then leaving it for 2 hours.

[0124] Step S600: repeat steps S400 and S500 for 6 times in total.

[0125] After completing the impregnation process, the battery cells are subjected to secondary sealing, capacity division, OCV and appearance testing according to conventional processes to prepare finished battery cells.

[0126] A battery cell with a charging cut-off voltage of 4.5V, a positive electrode main material of LCO, and a negative electrode main material of graphite was selected, and the methods of Cases 1-7 were used to perform infiltration improvement operations on it.

[0127] Poor cell wetting usually manifests itself as black spots on the surface of the pole piece and high impedance, but poor wetting is difficult to detect using conventional methods due to microscopic bubbles. Since low temperatures can amplify the dynamic differences of the cell, this application uses low-temperature discharge capacity to qualitatively characterize the dynamic performance of the cell.

[0128] The specific low-temperature discharge steps are as follows:

[0129] Step S1, placing the finished battery cell in a 23°C incubator for 10 minutes;

[0130] Step S2, 0.7C constant current discharge to 3.0V;

[0131] Step S3, stand for 30 minutes;

[0132] Step S4, 0.5C constant current charging to 4.5V, then switching to constant voltage charging until the current is less than 0.02C;

[0133] Step S5, stand for 30 minutes;

[0134] Step S6, 0.2C constant current discharge to 3.0V, record the room temperature discharge capacity Q1;

[0135] Step S7, stand for 30 minutes;

[0136] Step S8, 0.5C constant current charging to 4.5V, then switching to constant voltage charging until the current is less than 0.02C;

[0137] Step S9, placing the battery cell in a -20°C incubator for 2 hours to allow the battery cell temperature to reach equilibrium with the ambient temperature;

[0138] Step S10, 0.2C constant current discharge to 3.0V, record the -20℃ discharge capacity Q2.

[0139] -20℃ discharge capacity percentage = Q2 / Q1*100%.

[0140] The finished battery cells prepared in Cases 1 to 7 were tested for -20°C low-temperature discharge capacity ratio using the above-mentioned low-temperature discharge method, and the obtained data are shown in Table 1.

[0141] Table 1 -20℃ low temperature discharge capacity ratio of finished battery cells obtained in cases 1 to 7

[0142]

[0143] Case 1 is the conventional process and serves as the reference group.

[0144] The difference between Case 2 and Case 1 is that the infiltration process after the injection process adds a low-temperature infiltration for 24 hours, and the infiltration temperature is -40°C;

[0145] The difference between Case 3 and Case 1 is that the infiltration process after the injection process adds a low-temperature infiltration for 24 hours, and the infiltration temperature is -20℃;

[0146] The difference between Case 4 and Case 1 is that the infiltration process after the injection process adds a low-temperature infiltration for 24 h, and the infiltration temperature is 0°C;

[0147] The difference between Case 5 and Case 1 is that the infiltration process after the injection process adds a low-temperature infiltration for 24 h, and the infiltration temperature is 23°C;

[0148] The difference between Case 6 and Case 1 is that the infiltration process after the injection process adds a temperature cycle, and the temperature cycle range is -20℃~23℃, the number of cycles is 6 times, and the shelf time after each battery cell temperature change is 2h;

[0149] The difference between Case 7 and Case 1 is that a temperature cycle process is added after the formation process, and the temperature cycle range is -20℃~23℃, the number of cycles is 6 times, and the shelf time after each battery cell temperature change is 2h;

[0150] The temperature cycle process parameters of Case 7 and Case 6 are exactly the same. The difference is that the temperature cycle of Case 6 is set after the battery cell filling process and before the formation process, while the temperature cycle of Case 7 is set after the battery cell formation process and before the second sealing process.

[0151] Combining the differences between cases 1 to 7 and the data in Table 1, we can see that:

[0152] (1) Low-temperature storage can improve the low-temperature discharge capability of the battery, and the optimal temperature range is -20℃~0℃; too high or too low temperature may result in insignificant wetting effect (refer to cases 1~5);

[0153] (2) Temperature cycling with a minimum temperature of <0°C can improve the low-temperature discharge capability of the battery (see cases 1, 6, and 7);

[0154] (3) The temperature cycle is set after the formation process and before the second sealing process for the best improvement effect (see cases 6 and 7). This is because during the multiple temperature cycles from "low temperature to normal temperature", the pores in the battery cell pole piece will shrink and expand with the change of temperature, thereby squeezing out the bubbles inside the battery cell and exhausting them through the subsequent second sealing process.

[0155] The above description is only a partial or preferred embodiment of the present invention. Neither the text nor the drawings can limit the scope of protection of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the overall concept of the present invention, or direct / indirect application in other related technical fields are included in the scope of protection of the present invention.

Claims

1. A lithium ion battery impregnation method, characterized in that: include: Injecting electrolyte into the battery cell to perform a liquid injection operation on the battery cell; Performing a first wetting operation on the battery cell after the liquid injection operation is completed; placing the battery cell after the first soaking operation in an environment of a first preset temperature for storage, so as to perform a second soaking operation on the battery cell; Wherein, the first preset temperature is greater than the freezing temperature of the electrolyte and is less than or equal to 10°C.

2. The lithium ion battery impregnation method according to claim 1, characterized in that: The first preset temperature is at least 5° C. greater than the freezing temperature of the electrolyte and is less than or equal to 5° C.

3. The lithium ion battery impregnation method according to claim 2, characterized in that: The first preset temperature is greater than -40°C and less than or equal to 0°C.

4. The lithium ion battery impregnation method according to claim 3, characterized in that: The first preset temperature is greater than or equal to -20°C and less than 0°C.

5. The lithium ion battery impregnation method according to any one of claims 1 to 4, characterized in that: The step of placing the battery cell after the first soaking operation in an environment with a first preset temperature for storage includes: Placing the battery cell after the first soaking operation in an environment of a first preset temperature and storing it for a first preset time; The first preset duration is greater than or equal to 12 hours and less than or equal to 48 hours.

6. The lithium ion battery impregnation method according to any one of claims 1 to 4, characterized in that: After performing a second soaking operation on the battery cell, the soaking method further includes: placing the battery cell after the second soaking operation in an environment of a second preset temperature for storage, so as to perform a third soaking operation on the battery cell; Wherein, the second preset temperature is greater than the first preset temperature.

7. The lithium ion battery impregnation method according to claim 6, characterized in that: After completing the third soaking operation once on the battery cell, the soaking method further includes: repeatedly performing the second soaking operation and the third soaking operation on the battery cell at least once in sequence.

8. The lithium ion battery impregnation method according to claim 7, characterized in that: After the first soaking operation is performed on the battery cell, the second soaking operation and the third soaking operation are sequentially repeated on the battery cell for a number of times greater than or equal to 3 times and less than or equal to 10 times.

9. The lithium ion battery impregnation method according to claim 8, characterized in that: Placing the battery cell in an environment of a first preset temperature for storage includes: placing the battery cell after the first soaking operation in an environment of the first preset temperature for storage for a second preset time; The second preset time length X and the number of times Y of performing the second soaking operation on the battery cell in the soaking method satisfy XY≥12, where the unit of X is h and the unit of Y is times.

10. The lithium ion battery impregnation method according to claim 9, characterized in that: The second preset duration is greater than or equal to 1 hour.

11. The lithium ion battery impregnation method according to claim 6, characterized in that: Placing the battery cell after the second soaking operation in an environment of a second preset temperature for storage includes: placing the battery cell in an environment of the second preset temperature for storage for a third preset time, wherein the third preset time is the time from when the battery cell is placed in the environment of the second preset temperature to when the surface temperature of the battery cell reaches the second preset temperature plus at least 0.5h; and / or, The second preset temperature is greater than or equal to 20° C. and less than or equal to 45° C.

12. The lithium ion battery impregnation method according to any one of claims 1 to 4, characterized in that: After performing a first soaking operation on the battery cell and before performing a second soaking operation on the battery cell, the soaking method further includes: performing a formation operation on the battery cell after completing the first soaking operation.

13. The lithium ion battery impregnation method according to any one of claims 1 to 4, characterized in that: The performing a first wetting operation on the battery cell after the liquid injection operation is completed includes: Placing the battery cell after the injection operation is completed in an environment of a third preset temperature for a fourth preset time period; placing the battery cell in an environment with a fourth preset temperature for a fifth preset time; Wherein, the third preset temperature is greater than or equal to 20° C. and less than or equal to 30° C., and the fourth preset time is greater than or equal to 12 hours and less than or equal to 48 hours; The fourth preset temperature is 45° C.±10° C., and the fifth preset time is greater than or equal to 12 hours and less than or equal to 48 hours.

Citation Information

Patent Citations

  • Standing method after electrolyte filling of lithium ion battery

    CN109326827A

  • High-voltage lithium ion battery, battery pole piece and infiltration method thereof

    CN113113739A

  • Liquid injection method of electrolyte containing low-temperature additive and secondary battery

    CN116454563A