Preparation method of battery and battery

By cutting off the air bag in the low-electric state during the decomposition and capacity separation of lithium-ion batteries, the problem of reflux of harmful gases of lithium supplement agents consumes active lithium ions is solved, and the reversible discharge capacity of the battery and the efficiency of the first circle of the Kulun are improved. , extends the battery life.

CN118919869APending Publication Date: 2024-11-08CHONGQING TALENT NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193132.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the charging process, lithium-ion batteries form solid electrolyte phase interface masks, which consume active lithium ions, resulting in irreversible capacity loss and reduced efficiency of the first circle of Coulon. After adding lithium supplement agent, harmful gases reflux consume active lithium ions, further reducing the reversible capacity.

Method used

When the battery is dissolved and divided into capacity, discharge the air bag to a low-electric state of 0% SOC to 30% SOC to cut off the air bag to ensure that the harmful gases generated by the lithium supplement do not consume active lithium ions, and are subject to constant current and constant voltage charging and negative pressure treatment Improve the reversible discharge capacity of the battery and the first-circle Coulomb efficiency.

Benefits of technology

It significantly improves the reversible discharge capacity of the battery and the first-round Coulomb efficiency, extends the service life of the battery, and reduces the battery aging speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919869A_ABST
    Figure CN118919869A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a battery and the battery. The preparation method of the battery comprises the steps that a positive pole piece, a negative pole piece and an isolating membrane are assembled and put into a shell, electrolyte is injected, a battery cell main body is obtained, and at least one of the positive pole piece and the negative pole piece comprises a lithium supplementing agent; and performing formation and capacity grading on the battery cell main body, and cutting off the air bag when the battery cell main body is discharged to a 0% SOC-30% SOC state to obtain the battery. According to the preparation method of the battery provided by the invention, the reversible discharge capacity of the obtained battery is obviously improved, and the first-circle coulombic efficiency is obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a method for preparing a battery and a battery. Background Art

[0002] As people's awareness of energy conservation gradually increases, green and low-carbon demand has expanded the space for the growth of new energy vehicle consumption, making the consumption of the new energy vehicle industry in a steady growth state. The energy storage market on the demand side of lithium-ion batteries is expanding rapidly.

[0003] Lithium-ion batteries are a type of energy storage device with excellent properties such as high energy density, excellent cycle stability, environmental friendliness, and rapid charge and discharge. During the first charging process of lithium-ion batteries, a solid electrolyte interface (SEI) is formed, which consumes part of the active lithium ions from the positive electrode, resulting in irreversible capacity loss of the battery. Adding lithium supplements is an important way to solve the problem of battery capacity loss, and can significantly improve the battery energy density and coulomb efficiency. However, after adding lithium supplements, the lithium supplements will produce harmful gases (such as O2, etc.), which will flow back into the battery to consume active lithium ions, reducing the reversible gram capacity of the battery and the first-cycle coulomb efficiency. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a method for preparing a battery and a battery, wherein the battery prepared by the method has a significantly improved reversible discharge capacity and a significantly improved first-cycle coulombic efficiency.

[0005] In a first aspect of the present invention, the present invention provides a method for preparing a battery, comprising:

[0006] Assembling a positive electrode sheet, a negative electrode sheet and a separator and placing them in a shell, injecting an electrolyte to obtain a battery cell body, wherein at least one of the positive electrode sheet and the negative electrode sheet includes a lithium supplement;

[0007] The battery cell body is formed and divided into different capacities, and when the battery cell is discharged to a state of 0% SOC to 30% SOC, the air bag is cut off to obtain a battery.

[0008] According to the preparation method of the battery of the above embodiment of the present invention, during battery formation and capacity division, when discharging to a low power state of 0% SOC ~ 30% SOC, the air bags are cut off. When discharging to a low power state of 0% SOC ~ 30% SOC, most of the lithium in the battery exists in the form of positive electrode active material at the positive electrode, which is relatively stable, and the concentration of unstable active lithium ions at the negative electrode is low. Therefore, by cutting off the air bags, even if the harmful gases generated by the lithium supplement flow back, the active lithium ions will not be consumed. Cutting off the air bags at this low power state can increase the reversible discharge capacity of the battery, thereby improving the initial efficiency of the battery.

[0009] In addition, the method for preparing the battery according to the above embodiment of the present invention may also have the following additional technical features:

[0010] In some embodiments of the present invention, the step of dividing the capacity includes: charging the formed battery cell body at constant current and constant voltage to 100% SOC.

[0011] In some embodiments of the present invention, the constant voltage is above 4.2V, preferably 4.2V to 4.5V.

[0012] In some embodiments of the present invention, the formed battery cell body is charged to 100% SOC at a constant current and constant voltage of 0.1C-0.5C.

[0013] In some embodiments of the present invention, the steps of forming and dividing the battery body, and cutting off the air bag when discharging to a state of 0% SOC to 30% SOC to obtain a battery include: forming and dividing the battery body, and discharging to a state of 0% SOC to 30% SOC, setting clamps on both sides of the battery body to compress the battery body, cutting off the air bag, and obtaining a battery.

[0014] In some embodiments of the present invention, the pressure of the clamping plate is 0.3 MPa to 0.5 MPa.

[0015] In some embodiments of the present invention, the battery cell body is formed and divided under negative pressure.

[0016] In some embodiments of the present invention, after the battery cell body is sealed, the battery cell body is formed and divided under negative pressure.

[0017] In some embodiments of the present invention, the negative pressure ranges from -90 kPa to -80 kPa.

[0018] In some embodiments of the present invention, the positive electrode plate includes the lithium supplement agent.

[0019] In some embodiments of the present invention, the air bag is connected to the negative electrode plate.

[0020] In some embodiments of the present invention, the formation includes: charging the battery body at a constant current of 0.05C to 0.1C to 50% SOC to 70% SOC at a pressure of 0.3MPa to 0.5MPa and a temperature below 50°C.

[0021] In some embodiments of the present invention, the steps of assembling the positive electrode sheet, the negative electrode sheet and the isolation membrane and placing them in a shell, injecting an electrolyte to obtain a battery cell body include: mixing, homogenizing, coating and rolling the positive electrode active material, the lithium supplement, the first conductive agent and the first binder to obtain the positive electrode sheet; mixing, homogenizing, coating and rolling the negative electrode active material, the second conductive agent and the second binder to obtain the negative electrode sheet; placing the positive electrode sheet and the negative electrode sheet stack into a shell, encapsulating and injecting an electrolyte to obtain the battery cell body.

[0022] In the second aspect of the present invention, the present invention provides a battery, which includes a battery prepared by the method described in the second aspect, and compared with the prior art, the battery has a reversible heat release capacity and a first-cycle coulombic efficiency.

[0023] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0025] Figure 1 A schematic flow chart of a method for preparing a battery according to an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0026] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0027] In a first aspect of the present invention, the present invention provides a method for preparing a battery, comprising:

[0028] S1: Assemble the positive electrode sheet, the negative electrode sheet and the separator and place them in a shell, inject electrolyte to obtain a battery cell body, wherein at least one of the positive electrode sheet and the negative electrode sheet includes a lithium supplement;

[0029] According to some embodiments of the present invention, step S1 comprises:

[0030] S11: mixing, homogenizing, coating, and rolling the positive electrode active material, the lithium supplement agent, the first conductive agent, and the first binder to obtain a positive electrode sheet;

[0031] According to some embodiments of the present invention, the positive electrode active material includes at least one of lithium iron phosphate, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium-rich manganese-based positive electrode material and lithium iron manganese phosphate.

[0032] According to some embodiments of the present invention, the first conductive agent includes at least one of conductive carbon black, carbon nanotubes (CNTs) and graphene.

[0033] According to some embodiments of the present invention, the first binder includes at least one of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-chlorotrifluoroethylene copolymer, polyethylene oxide and polyvinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene copolymer.

[0034] According to some embodiments of the present invention, the positive electrode sheet also includes a positive electrode current collector. The slurry obtained after homogenization is coated on the positive electrode current collector, and then the positive electrode sheet can be formed through steps such as drying and rolling.

[0035] S12: mixing, homogenizing, coating, and rolling the negative electrode active material, the second conductive agent, and the second binder to obtain a negative electrode sheet;

[0036] According to some embodiments of the present invention, the negative electrode active material includes at least one of graphite, silicon oxygen, silicon carbon, lithium titanate or metallic lithium.

[0037] According to some embodiments of the present invention, the second conductive agent includes at least one of conductive carbon black, carbon nanotubes and graphene.

[0038] According to some embodiments of the present invention, the second binder includes at least one of styrene-butadiene rubber (SBR), polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinylidene fluoride-chlorotrifluoroethylene copolymer, polyethylene oxide and polyvinylidene fluoride-trifluoroethylene-chlorotrifluoroethylene copolymer.

[0039] According to some embodiments of the present invention, the negative electrode sheet also includes a negative electrode current collector. The slurry obtained after homogenization is coated on the negative electrode current collector, and then the negative electrode sheet can be formed through steps such as drying and rolling.

[0040] S13: placing the positive electrode sheet and the negative electrode sheet stack into a shell, encapsulating them, and injecting electrolyte to obtain a battery cell body.

[0041] According to some embodiments of the present invention, the electrolyte includes a lithium salt, and the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethylsulfonyl)imide, lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium bis(oxalatoborate), lithium difluorooxalatoborate and lithium trifluoromethanesulfonate.

[0042] According to some embodiments of the present invention, the electrolyte further includes a solvent, and the solvent includes carbonates (such as ethylene carbonate EC, dimethyl carbonate DMC, diethyl carbonate DEC, etc.) and organic ethers (such as 1,2-dimethoxypropane DMP, ethylene glycol dimethyl ether DME, etc.).

[0043] According to some embodiments of the present invention, the electrolyte may further include additives for improving certain performances of the battery, such as reversible capacity, cycle performance, rate performance and safety performance. The additives may be common additives in the art.

[0044] According to some embodiments of the present invention, after the positive electrode sheet and the negative electrode sheet are stacked, they are placed in an aluminum-plastic film with holes punched out to form a dry battery cell. The baked dry battery cell is then filled with liquid and left to stand to obtain a battery cell body.

[0045] S2: forming and dividing the battery cell body, and when the battery cell is discharged to a state of 0% SOC to 30% SOC, cutting off the air bag to obtain a battery.

[0046] As an example, after the battery cell body is divided into different capacities, the discharge states that can be achieved are 0% SOC, 10% SOC, 20% SOC, 30% SOC, and so on.

[0047] Specifically, during battery formation and capacity division, when discharging to a low power state of 0% SOC ~ 30% SOC, the air bags are cut off. When discharging to a low power state of 0% SOC ~ 30% SOC, most of the lithium in the battery exists in the form of positive electrode active material at the positive electrode, which is relatively stable, and the concentration of unstable active lithium ions at the negative electrode is low. Therefore, if the air bags are cut off, even if the harmful gases generated by the lithium supplement flow back, the active lithium ions will not be consumed. Cutting off the air bags at this low power state can increase the reversible discharge capacity of the battery, thereby improving the initial efficiency of the battery.

[0048] It can be understood that SOC (State of Charge), that is, the state of charge of the battery, is an indicator that describes the current remaining power of the battery. When discharged to 0% SOC ~ 30% SOC, that is, the remaining power of the battery discharge is 0 ~ 30%. Because during the discharge process, lithium ions are released from the negative electrode active material and migrate to the positive electrode through the electrolyte. In the state of discharging to 0% SOC ~ 30% SOC, a part of the lithium ions of the battery are released from the negative electrode and embedded in the positive electrode active material, so that the remaining power of the battery is 0 ~ 30%, but a considerable part of the lithium ions still remain in the negative electrode. That is, at this time, most of the lithium in the battery exists in the form of positive electrode active material at the positive electrode, which is relatively stable, and the concentration of unstable active lithium ions at the negative electrode is low.

[0049] It is understandable that in order to ensure the normal production of batteries, a part of the aluminum-plastic film will be reserved as an air bag when the battery is packaged (sealed) to store the gas generated by the formation. This part of the aluminum-plastic film is called an air bag. During the battery exhaust process, the equipment will puncture the air bag to extract the formation gas, then reseal the battery, and finally cut off the air bag.

[0050] According to some embodiments of the present invention, the step of dividing the capacity includes: charging the formed battery body with constant current and constant voltage to 100% SOC. It can be understood that constant current and constant voltage charging refers to charging under the conditions of constant current and voltage. Constant current and constant voltage charging is an efficient battery charging strategy that prevents overcharging by first charging quickly with a constant current and then switching to a constant voltage when the voltage is close to the rated value. This method can reduce heat generation, extend battery life, improve safety, and optimize battery performance. It is suitable for a variety of battery types, reduces charging time, while reducing the battery aging rate and increasing the controllability and compatibility of the charging process.

[0051] According to some embodiments of the present invention, the constant voltage is above 4.2V, for example, it can be 4.21V, 4.3V, 4.4V, 4.5V, 4.6V, 4.7V, 4.8V, 4.9V, 5.0V, etc. The constant voltage is controlled within the above range to ensure that the lithium replenisher is fully decomposed while the positive electrode active material fully reacts, and the lithium replenishment effect is fully exerted, which can increase the reversible discharge capacity of the battery and thus improve the first efficiency of the battery. According to other embodiments of the present invention, the constant voltage is 4.2V to 4.5V.

[0052] According to some embodiments of the present invention, the formed battery body is charged to 100% SOC at a constant current and constant voltage of 0.1C-0.5C. For example, it can be 0.1C, 0.2C, 0.3C, 0.4C, 0.5C, etc. Taking 0.33C constant current and constant voltage charging as an example, 0.33C constant current and constant voltage charging means that the battery is charged at 33% of the rated capacity current during the constant current stage. Using a lower charging rate such as 0.33C helps to reduce the heat generation of the battery during the charging process, prolong the service life of the battery, and reduce the battery performance degradation that may be caused by fast charging.

[0053] According to some embodiments of the present invention, step S2 comprises:

[0054] The battery body is formed and divided into different capacities, and discharged to a state of 0% SOC to 30% SOC. Clamps are arranged on both sides of the battery body to compress the battery body, and the air bags are cut off to obtain a battery.

[0055] Specifically, the pressure of the clamping plate causes the harmful gases generated by formation and separation to gather at the gas pocket position, effectively reducing the gas reflux and consumption of active lithium. This method can increase the full electric reversible gram capacity of the battery with added positive electrode lithium supplement and improve the initial efficiency.

[0056] According to some embodiments of the present invention, the pressure of the splint is 0.3MPa to 0.5MPa. For example, it can be 0.3MPa, 0.35MPa, 0.4MPa, 0.45MPa, 0.5MPa, etc. The pressure of the splint is controlled within the above range. The pressure makes the harmful gases generated by formation and separation gather at the air bag position, effectively reducing the gas reflux consumption of active lithium. This method can increase the full electric reversible capacity of the battery with the addition of positive electrode lithium supplement and improve the initial efficiency.

[0057] According to some embodiments of the present invention, the battery cell body is formed and divided under negative pressure. In this way, the pressure and negative pressure of the clamping plate can further cause the harmful gases generated by the formation and division to gather at the gas bag position, further reducing the consumption of active lithium by gas reflux, further increasing the full electric reversible gram capacity of the battery with the positive electrode lithium supplement, and improving the initial efficiency.

[0058] According to some embodiments of the present invention, after the battery body is sealed, the battery body is formed and divided under negative pressure. Specifically, during the formation and division under negative pressure, the harmful gas generated is directly discharged from the unsealed position of the battery, which can also prevent the harmful gas from flowing back and consuming active lithium, thereby increasing the reversible discharge capacity of the battery and further improving the initial efficiency of the battery.

[0059] According to some embodiments of the present invention, the negative pressure ranges from -90kPa to -80kPa. For example, it can be -90kPa, -88kPa, -86kPa, -84kPa, -82kPa, -80kPa, etc. Controlling the negative pressure range within the above range is sufficient to allow formation and separation under negative pressure, and the generated harmful gases are directly discharged from the unsealed position of the battery, and the harmful gases can be prevented from flowing back to consume active lithium, which can increase the reversible discharge capacity of the battery, thereby improving the initial efficiency of the battery.

[0060] According to some embodiments of the present invention, the positive electrode plate includes the lithium supplement agent, which has good stability and low cost, is an important way to solve the problem of battery capacity loss, and can significantly improve the battery energy density and coulomb efficiency.

[0061] It can be understood that the present invention does not limit the types of lithium supplements, which may include lithium-rich ternary compounds, lithium-rich binary compounds, and phase-transformation-based composite materials, etc. Specifically, the lithium supplement includes but is not limited to lithium nickelate, lithium iron phosphate, Li2O, Li2O2, LiF, Li2S, Li3N, etc.

[0062] According to some embodiments of the present invention, the air bag is connected to the negative electrode plate. Therefore, since the active lithium ions on the negative electrode plate are less stable than those on the positive electrode plate and are more likely to react with harmful gases, the air bag is connected to the negative electrode plate. The gas on the negative electrode plate can be transferred to the air bag in time, which can prevent the harmful gas from flowing back and consuming the active lithium, and can increase the reversible discharge capacity of the battery, thereby improving the initial efficiency of the battery.

[0063] According to some embodiments of the present invention, the forming comprises:

[0064] The battery body is charged at a constant current of 0.05C to 0.1C to 50% SOC to 70% SOC under a pressure of 0.3MPa to 0.5MPa and a temperature below 50°C.

[0065] As an example, the pressure can be 0.3MPa, 0.35MPa, 0.4MPa, 0.45MPa, 0.5MPa, etc.; the temperature can be 5℃, 10℃, 20℃, 30℃, 40℃, 49℃, etc.; the current of constant current charging can be 0.05C, 0.07C, 0.09C, 0.1C, etc.; it can be charged to 50% SOC, 60% SOC, 70% SOC, etc.

[0066] The above-mentioned formation method helps to protect battery materials, improve safety, extend battery life, optimize battery performance, reduce heat loss and side reactions during charging, and at the same time helps to reduce the gas path area, improve formation uniformity, form a stable SEI layer, reduce the risk of lithium dendrites, and has good environmental friendliness.

[0067] Figure 1 A detailed and specific embodiment of the battery preparation method of the present invention is given, specifically:

[0068] Step 1: dry-mix (NCM + lithium supplement), conductive agent, and binder in a ratio of 98:1:1, and then roll-coat to obtain the positive electrode. The negative electrode is prepared in the same way.

[0069] Step 2: The positive and negative electrodes and the isolation film are stacked to obtain bare cells. The bare cells and the punched aluminum-plastic film are packaged to become dry cells. The baked dry cells are filled with liquid and left to stand.

[0070] The third step: After formation and capacity division, the air bag cutting method is used in the low-power state of the battery cell to increase the full-electric reversible capacity and improve the initial efficiency.

[0071] In summary, according to the method for preparing a battery of the present invention, during battery formation and capacity division, when discharging to a low power state of 0% SOC to 30% SOC, the air bags are cut off. When discharging to a low power state of 0% SOC to 30% SOC, most of the lithium in the battery exists in the form of positive electrode active material at the positive electrode, which is relatively stable, and the concentration of unstable active lithium ions at the negative electrode is low. Therefore, by cutting off the air bags, even if the harmful gases generated by the lithium supplement flow back, the active lithium ions will not be consumed. Cutting off the air bags at this low power state can increase the reversible discharge capacity of the battery, thereby improving the initial efficiency of the battery.

[0072] In the second aspect of the present invention, the present invention proposes a battery, which is prepared by the method described in the first aspect. According to an embodiment of the present invention, compared with the prior art, in the battery, when the battery is formed and divided, when the battery is discharged to a low power state of 0% SOC to 30% SOC, the air bag is cut off, and when the battery is discharged to a low power state of 0% SOC to 30% SOC, most of the lithium in the battery exists in the form of positive electrode active material at the positive electrode, which is relatively stable, and the concentration of unstable active lithium ions at the negative electrode is low. Therefore, if the air bag is cut off, even if the harmful gas generated by the lithium supplement flows back, the active lithium ions will not be consumed. Cutting off the air bag at this low power state can increase the reversible discharge capacity of the battery, thereby improving the initial efficiency of the battery. It should be noted that the features and advantages described above for the preparation method of the battery are also applicable to the battery, and will not be repeated here.

[0073] The scheme of the present disclosure will be explained below in conjunction with the examples. Those skilled in the art will appreciate that the following examples are only used to illustrate the present disclosure and should not be considered to limit the scope of the present disclosure. Where specific techniques or conditions are not indicated in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. Where the manufacturers of reagents or instruments are not indicated, they are all conventional products that can be obtained commercially.

[0074] Example 1

[0075] Step 1: Dry-mix the positive electrode active material (NCM811 + lithium supplement lithium nickel oxide, the mass ratio of the two is 25:1), the conductive agent CNT, and the binder PVDF in a ratio of 98:1:1 - blend the slurry, and obtain the positive electrode sheet by coating and roller pressing.

[0076] The negative electrode active material (graphite + silicon oxide material, the mass ratio of graphite to silicon oxide material is 3:1), the conductive agent CNT, and the binder SBR are dry-mixed in a ratio of 98:1:1 - blended into a slurry, and the negative electrode sheet is obtained by coating and roller pressing.

[0077] Step 2: The positive electrode sheet, the negative electrode sheet and the isolation film are stacked to obtain a bare cell. The bare cell and the punched aluminum-plastic film are packaged to form a dry cell. The baked dry cell is filled with liquid and left to stand.

[0078] Step 3: After the battery is filled with liquid, it undergoes the formation process: charging at a constant current of 0.33C to 60% SOC at a pressure of 0.3MPa and a temperature of <50°C;

[0079] The fourth step is capacity division: clamping plates are set on both sides of the battery body to press the battery body tightly. Under the clamping plate pressure of 0.3-0.5MPa, first charge at a constant current of 0.33C to 4.3V, then charge at a constant current of 0.05C to 100% SOC, and then discharge at 0.33C to 30% SOC; cut off the air bag in this state.

[0080] Among them, the third step and the fourth step are carried out under negative pressure, and the pressure of the negative pressure is -90kPa.

[0081] Example 2

[0082] It is basically the same as Example 1, except that in the fourth step, the battery is discharged at 0.33C to 0% SOC; the air bag is cut off at this electrical state.

[0083] Example 3

[0084] It is basically the same as Example 1, except that in the fourth step, the battery is discharged at 0.33C to 15% SOC; the air bag is cut off at this electrical state.

[0085] Example 4

[0086] It is basically the same as Example 1, except that in the fourth step, 0.33C constant current charging is performed to 4.2V.

[0087] Example 5

[0088] It is basically the same as Example 1, except that in the fourth step, 0.33C constant current charging is performed to 4.5V.

[0089] Example 6

[0090] It is basically the same as Example 1, except that in the fourth step, no clamping plates are provided on both sides of the battery cell body.

[0091] Example 7

[0092] It is basically the same as Example 1, except that the negative pressure in the third and fourth steps is -80 kPa.

[0093] Example 8

[0094] It is basically the same as Example 1, except that the negative pressure in the third and fourth steps is -60 kPa.

[0095] Example 9

[0096] It is basically the same as Example 1, except that the pressure of the negative pressure in the third step and the fourth step is 0 kPa.

[0097] Comparative Example 1

[0098] It is basically the same as Example 1, except that, after charging to 100% SOC in the fourth step, the air bag is sheared off without discharging.

[0099] Comparative Example 2

[0100] It is basically the same as Example 1, except that in the fourth step, the battery is discharged at 0.33C to 60% SOC; the air bag is cut off at this electrical state.

[0101] Comparative Example 3

[0102] It is basically the same as Example 1, except that in the fourth step, no clamping plates are provided on both sides of the battery cell body and after charging to 100% SOC, the air pockets are not cut off without discharging.

[0103] Testing and analysis

[0104] The batteries of the above-mentioned embodiment and comparative example were tested for charging capacity, discharging capacity and first efficiency (first cycle coulomb efficiency), respectively. The specific operations are as follows:

[0105] 1.Charging capacity test:

[0106] The capacitive charging process first uses constant current charging during the charging process. When the battery voltage reaches the rated value, it switches to constant voltage charging. The capacitive charging equipment automatically calculates the battery charging capacity according to the changes in voltage and current, and the charging capacity can be directly read.

[0107] 2. Discharge capacity test:

[0108] During the discharge process, the battery is discharged at a constant current until it reaches the rated voltage. The capacity division equipment calculates the battery capacity based on the changes in voltage and current and directly reads the discharge capacity.

[0109] 3. First effect test:

[0110] First effect = discharge capacity / charge capacity × 100%.

[0111] The test results are shown in Table 1.

[0112] Table 1

[0113]

[0114]

[0115] Combined with Table 1, it can be obtained that in Example 2, the assimilation-capacity separation process, the air bag is cut off by removing the splint in the low-power state, and the full-electric reversible discharge capacity is 203.14 mAh / g. The first efficiency is about 15% higher than that of the battery discharged to 100% SOC (Comparative Example 1); the first efficiency is increased by about 9% when the battery is discharged to 60% SOC (Comparative Example 2); the first efficiency is increased by about 23% when the battery is discharged to 100% SOC without the splint (Comparative Example 3). It can be seen that in the embodiment of the present application, when the battery is discharged to a low power state of 0% SOC to 30% SOC, the air bag is cut off, and the full-electric reversible discharge capacity of the battery is significantly improved, and the first efficiency is significantly improved.

[0116] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", "some implementation schemes" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.

[0117] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a battery, It is characterized in that include: Assembling a positive electrode sheet, a negative electrode sheet and a separator and placing them in a shell, injecting an electrolyte to obtain a battery cell body, wherein at least one of the positive electrode sheet and the negative electrode sheet includes a lithium supplement; The battery cell body is formed and divided into different capacities, and when the battery cell is discharged to a state of 0% SOC to 30% SOC, the air bag is cut off to obtain a battery.

2. The method according to claim 1, It is characterized in that The steps of capacity division include: The formed battery cell is charged to 100% SOC using constant current and constant voltage.

3. The method according to claim 2, It is characterized in that The constant voltage is 4.2V or more, preferably 4.2V to 4.5V; Preferably, the formed battery cell body is charged to 100% SOC at a constant current and constant voltage of 0.1C-0.5C.

4. The method according to any one of claims 1 to 3, It is characterized in that The steps of forming and dividing the battery body, and cutting off the air bag when the battery is discharged to a state of 0% SOC to 30% SOC, to obtain a battery include: The battery body is formed and divided into different capacities, and discharged to a state of 0% SOC to 30% SOC. Clamps are arranged on both sides of the battery body to compress the battery body, and the air bags are cut off to obtain a battery.

5. The method according to claim 4, It is characterized in that The pressure of the clamping plate is 0.3MPa to 0.5MPa; Preferably, the battery cell body is formed and divided under negative pressure.

6. The method according to any one of claims 1 to 3, It is characterized in that After the battery cell body is sealed, the battery cell body is formed and divided under negative pressure.

7. The method according to claim 6, It is characterized in that The negative pressure ranges from -90 kPa to -85 kPa.

8. The method according to any one of claims 1 to 3, It is characterized in that The positive electrode plate includes the lithium supplement agent; Preferably, the air bag is connected to the negative electrode plate.

9. The method according to any one of claims 1 to 3, It is characterized in that The formation comprises: The battery body is charged at a constant current of 0.05C to 0.1C to 50% SOC to 70% SOC under a pressure of 0.3MPa to 0.5MPa and a temperature below 50°C.

10. The method according to any one of claims 1 to 3, It is characterized in that The steps of assembling the positive electrode sheet, the negative electrode sheet and the separator and placing them in a shell, injecting electrolyte, and obtaining a battery body include: The positive electrode active material, the lithium supplement agent, the first conductive agent, and the first binder are mixed, homogenized, coated, and rolled to obtain a positive electrode sheet; The negative electrode active material, the second conductive agent and the second binder are mixed, homogenized, coated and rolled to obtain a negative electrode sheet; the positive electrode sheet and the negative electrode sheet stack are placed in a shell, packaged and injected with electrolyte to obtain a battery cell body.

11. A battery, It is characterized in that The battery is prepared by the method according to any one of claims 1 to 10.