Outer packaging material for all-solid-state battery, method for producing same, and all-solid-state battery

By introducing a combination of a substrate layer, a barrier layer, and a heat-fusion resin layer into the outer packaging material of all-solid-state batteries, the amount of hydrogen sulfide permeation through the heat-fusion resin layer is controlled, thus solving the problem of hydrogen sulfide leakage in the event of damage to all-solid-state batteries and improving battery safety.

CN118919963APending Publication Date: 2024-11-08DAI NIPPON PRINTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410986796.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-01-23
Filing Date
2020-01-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The outer packaging material of existing all-solid-state batteries is prone to hydrogen sulfide gas leakage when damaged, and trace amounts of water vapor may enter the interior, leading to the generation and leakage of hydrogen sulfide. Existing technologies are unable to effectively suppress this problem.

Method used

The outer packaging material consists of a substrate layer, a barrier layer, and a heat-melting resin layer. The hydrogen sulfide permeation of the heat-melting resin layer is controlled to be below 1.0×10-9cc·mm/cm2·sec·cmHg. By optimizing the material composition and structural design, hydrogen sulfide leakage is reduced.

Benefits of technology

It effectively suppresses the leakage of hydrogen sulfide generated inside the all-solid-state battery to the outside, improving the safety and reliability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919963A_ABST
    Figure CN118919963A_ABST
Patent Text Reader

Abstract

The invention provides an outer packaging material for an all-solid-state battery, a manufacturing method thereof and the all-solid-state battery, wherein the outer packaging material can effectively prevent hydrogen sulfide generated in the all-solid-state battery containing a sulfide solid electrolyte material from leaking to the outside. This outer packaging material for an all-solid-state battery is used in an all-solid-state battery containing a sulfide solid electrolyte material, and comprises a laminate having at least a base layer, a barrier layer, and a heat-fusible resin layer in this order from the outside. The outer packaging material for all-solid-state batteries is characterized in that the heat-fusible resin layer contains at least one of a polyester and a fluororesin, and the hydrogen sulfide transmission amount of the resin constituting the heat-fusible resin layer is 1.0 * 10 <-9 > cc * mm / cm2 * sec * cmHg or less.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This case is filed on January 23, 2020 、Application No. 202080010363.7 、The name of the invention is All solid state battery Battery outer packaging material, manufacturing method thereof and all-solid battery A divisional application for a patent application. Technical Field

[0002] The present invention relates to an outer packaging material for an all-solid battery, a method for producing the same, and an all-solid battery. Background Art

[0003] All-solid batteries in which the electrolyte is a solid electrolyte are known. All-solid batteries do not use organic solvents in the battery and therefore have the advantages of high safety and a wide operating temperature range.

[0004] It is known that sulfide-based inorganic solid electrolytes have high ion conductivity. However, as described in Patent Document 1, for example, sulfide-based inorganic solid electrolytes contain sulfur compounds that may generate toxic hydrogen sulfide when reacting with water. Therefore, in the event of damage to the all-solid-state battery, there is a risk of reacting with moisture in the air to generate hydrogen sulfide gas.

[0005] On the other hand, in recent years, with the high performance of electric vehicles, hybrid electric vehicles, personal computers, cameras, mobile phones, etc., batteries are required to have various shapes, and to be thinner and lighter. However, in the past, metal outer packaging materials often used in batteries have the disadvantages of being difficult to follow the diversification of shapes and having a limit to lightweighting. Therefore, as an outer packaging material that is easy to process into a variety of shapes and can achieve thinning and lightweighting, a film-like outer packaging material obtained by laminating a substrate / barrier layer / thermofusible resin layer in sequence has been proposed.

[0006] In such a film-like outer packaging material, a space for accommodating battery elements is usually formed by molding into a bag shape or using a mold, and battery elements such as electrodes and solid electrolytes are arranged in the space, and heat-fusible resin layers are heat-fused to each other to obtain a battery in which the battery elements are accommodated on the inner side of the outer packaging material.

[0007] By applying such a film-like outer casing material to an outer casing material of an all-solid-state battery, it is expected that electric vehicles, hybrid electric vehicles, and the like can be reduced in weight.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application Publication No. 2008-103288 Summary of the invention

[0011] Technical problem to be solved by the invention

[0012] Patent Document 1 proposes the following technology: in an all-solid-state battery using a sulfide-based inorganic solid electrolyte, in order to cope with the generation of hydrogen sulfide gas when the all-solid-state battery is damaged, the outer casing of the all-solid-state battery is further covered with an adsorbent and / or a material containing an alkaline substance.

[0013] However, in the case of using a film-shaped outer packaging material obtained by sequentially stacking a substrate / barrier layer / thermo-fusible resin layer, not only is it possible for hydrogen sulfide to be generated inside the all-solid-state battery when the all-solid-state battery is damaged, but also a trace amount of water vapor may intrude into the interior of the all-solid-state battery from the heat-welded portions of the heat-welded resin layers, etc., to generate hydrogen sulfide inside the all-solid-state battery. Furthermore, the inventors of the present invention conducted a study and found that hydrogen sulfide generated inside the all-solid-state battery may leak to the outside through the heat-welded resin layer.

[0014] Under such circumstances, a main object of the present invention is to provide an all-solid-state battery outer casing material that can effectively suppress the leakage of hydrogen sulfide generated inside an all-solid-state battery containing a sulfide solid electrolyte material to the outside.

[0015] Means for solving technical problems

[0016] The inventors of the present invention have conducted intensive research to solve the above technical problems. As a result, they have found that, in an all-solid-state battery outer packaging material composed of a laminated body having at least a base layer, a barrier layer, and a heat-fusible resin layer in this order from the outside, by setting the hydrogen sulfide permeation rate of the resin constituting the heat-fusible resin layer to a predetermined value or less, hydrogen sulfide generated inside an all-solid-state battery containing a sulfide solid electrolyte material can be effectively suppressed from leaking to the outside.

[0017] The present invention has been completed by further repeated studies based on these findings. That is, the present invention provides the following aspects.

[0018] An all-solid battery outer packaging material for an all-solid battery containing a sulfide solid electrolyte material, the all-solid battery outer packaging material is composed of a laminate having at least a substrate layer, a barrier layer and a heat-fusible resin layer in order from the outside, the all-solid battery outer packaging material is characterized in that: the hydrogen sulfide permeation amount of the resin constituting the heat-fusible resin layer is 1.0×10 -9 cc mm / cm 2 ·sec·cmHg or less.

[0019] Effects of the Invention

[0020] The present invention can provide an outer packaging material for an all-solid-state battery that can effectively inhibit the leakage of hydrogen sulfide generated inside an all-solid-state battery containing a sulfide solid electrolyte material to the outside. In addition, the present invention can also provide a method for manufacturing an outer packaging material for an all-solid-state battery and an all-solid-state battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic diagram showing an example of a cross-sectional structure of an all-solid-state battery to which the all-solid-state battery casing material of the present invention is applied.

[0022] Figure 2 This is a schematic diagram showing an example of a cross-sectional structure of an all-solid-state battery to which the all-solid-state battery casing material of the present invention is applied.

[0023] Figure 3 This is a schematic plan view of an example of an all-solid-state battery to which the all-solid-state battery casing material of the present invention is applied.

[0024] Figure 4 This is a schematic cross-sectional view showing an example of the laminated structure of the all-solid-state battery casing material of the present invention.

[0025] Figure 5 This is a schematic cross-sectional view showing an example of the laminated structure of the all-solid-state battery casing material of the present invention.

[0026] Figure 6 This is a schematic cross-sectional view showing an example of the laminated structure of the all-solid-state battery casing material of the present invention.

[0027] Figure 7 This is a schematic cross-sectional view showing an example of the laminated structure of the all-solid-state battery casing material of the present invention.

[0028] Figure 8 This is a schematic cross-sectional view showing an example of the laminated structure of the all-solid-state battery casing material of the present invention.

[0029] Fig. 9 This is a schematic diagram for explaining a method for measuring the hydrogen sulfide permeation amount of the resin constituting the thermally adhesive resin layer in the example. DETAILED DESCRIPTION

[0030] The all-solid battery outer packaging material of the present invention is used for an all-solid battery containing a sulfide solid electrolyte material, wherein the all-solid battery outer packaging material is composed of a laminate having at least a substrate layer, a barrier layer and a heat-fusible resin layer in order from the outside, and the all-solid battery outer packaging material is characterized in that the hydrogen sulfide permeation amount of the resin constituting the heat-fusible resin layer is 1.0×10 -9cc mm / cm 2 ·sec·cmHg or less. The all-solid-state battery outer casing material of the present invention has such a structure, and when used as an outer casing material for an all-solid-state battery containing a sulfide solid electrolyte material, it can effectively suppress the leakage of hydrogen sulfide generated inside the all-solid-state battery to the outside.

[0031] The all-solid battery outer packaging material of the present invention is described in detail below. In this specification, the numerical range represented by "to" means "above" or "below". For example, the expression of 2 to 15 mm means 2 mm or more and 15 mm or less.

[0032] 1. Laminated structure of outer packaging materials for all-solid-state batteries

[0033] The all-solid battery outer packaging material 10 of the present invention is, for example, Figures 4 to 9 As shown, it is composed of a laminated body having at least a substrate layer 1, a barrier layer 3 and a heat-fusible resin layer 4 in order from the outside. In the outer packaging material 10 for all-solid batteries, the heat-fusible resin layer 4 becomes the innermost layer. When the all-solid battery is assembled using the outer packaging material 10 for all-solid batteries and the battery element, the battery element is accommodated in a space formed by heat-fusing the peripheral portion while the heat-fusible resin layer 4 of the outer packaging material 10 for all-solid batteries is opposite to each other. In the all-solid battery to which the outer packaging material 10 for all-solid batteries of the present invention is applied, the heat-fused peripheral portion of the space (recess) in which the battery element is accommodated is preferably flat except for the portion where the metal terminal is present. In addition, in the all-solid battery to which the outer packaging material 10 for all-solid batteries of the present invention is applied, it is not necessary to configure a substance for absorbing hydrogen sulfide (a hydrogen sulfide absorbing substance different from the resin constituting the heat-fusible resin layer) at the peripheral portion of the space (recess) in which the battery element is accommodated.

[0034] like Figures 5 to 8 As shown in the schematic diagram of , in the all-solid battery outer packaging material 10, it is preferred that a barrier layer protective film 3a is provided on the surface of the barrier layer 3 on the side of the heat-fusible resin layer 4. In addition, it is preferred that a barrier layer protective film 3b is provided on the surface of the barrier layer 3 on the side of the base material layer 1. Figures 6 to 8 A schematic diagram showing a case where the outer packaging material 10 for an all-solid-state battery has barrier layer protective films 3a and 3b on both sides of the barrier layer 3. In addition, as described later, in the outer packaging material 10, the barrier layer protective film 3a may be provided only on the surface of the barrier layer 3 on the side of the heat-fusible resin layer 4, or the barrier layer protective films 3a and 3b may be provided on both sides of the barrier layer 3.

[0035] The outer packaging material 10 for the all-solid battery can be, for example, Figure 7 , 8As shown in FIG. 1 , an adhesive layer 2 is provided between the substrate layer 1 and the barrier layer 3 (in the case of a barrier layer protective film 3 b, between the substrate layer 1 and the barrier layer protective film 3 b) as required for the purpose of improving the adhesion between these layers. Figure 7 and Figure 8 As shown in the figure, between the barrier layer 3 and the heat-fusible resin layer 4 (in the case of a barrier layer protective film 3a, between the barrier layer protective film 3a and the heat-fusible resin layer 4), an adhesive layer 5 is provided as needed for the purpose of improving the adhesion between these layers. Figure 8 As shown, on the outer side of the base material layer 1 (the side opposite to the thermally fusible resin layer 4 side), a surface coating layer 6 and the like are provided as necessary.

[0036] The details of each layer constituting the outer packaging material 10 will be described in detail in the section “3. Each layer for forming the outer packaging material”.

[0037] The thickness of the laminated body constituting the all-solid battery outer packaging material 10 is not particularly limited, but from the viewpoint of reducing costs and improving energy density, it is preferably about 10000 μm or less, about 8000 μm or less, or about 5000 μm or less. From the viewpoint of maintaining the function of the all-solid battery outer packaging material 10 for protecting the battery element, it is preferably about 100 μm or more, about 150 μm or more, or about 200 μm or more. m or more, and the preferred range includes, for example, about 100 to 10000 μm, about 100 to 8000 μm, about 100 to 5000 μm, about 150 to 10000 μm, about 150 to 8000 μm, about 150 to 5000 μm, about 200 to 10000 μm, about 200 to 8000 μm, and about 200 to 5000 μm, with about 100 to 500 μm being particularly preferred.

[0038] The details of each layer constituting the all-solid-state battery outer casing material 10 will be described in detail in the section “3. Each layer for forming the all-solid-state battery outer casing material”.

[0039] 2. All-solid-state batteries

[0040] There are no particular restrictions on the all-solid-state battery to which the all-solid-state battery outer packaging material 10 of the present invention is applied (hereinafter, sometimes referred to as "outer packaging material 10"), except that the solid electrolyte layer 40 contains a sulfide solid electrolyte material and a specific outer packaging material 10 is used. That is, there are no particular restrictions on the components (electrodes, terminals, etc.) other than the solid electrolyte layer 40 and the outer packaging material 10, as long as they are components that can be used in the all-solid-state battery, and components used in known all-solid-state batteries can be used. Below, taking the all-solid-state battery 70 of the present invention as an example, the method of applying the all-solid-state battery outer packaging material 10 of the present invention to the all-solid-state battery is specifically described.

[0041] like Figures 1 to 3 As shown in the schematic diagram of , the all-solid battery 70 of the present invention contains a battery element including at least a single cell 50 in a package formed by the outer packaging material 10 for the all-solid battery of the present invention, and the single cell 50 includes a positive electrode active material layer 31, a negative electrode active material layer 21, and a solid electrolyte layer 40 stacked between the positive electrode active material layer 31 and the negative electrode active material layer 21. More specifically, the positive electrode active material layer 31 is stacked on the positive electrode collector 32 to form the positive electrode layer 30, and the negative electrode active material layer 21 is stacked on the negative electrode collector 22 to form the negative electrode layer 20. The positive electrode collector 32 and the negative electrode collector 22 are respectively connected to the terminal 60 exposed to the outside, thereby being electrically connected to the external environment. The solid electrolyte layer 40 is stacked between the positive electrode layer 30 and the negative electrode layer 20, and the positive electrode layer 30, the negative electrode layer 20 and the solid electrolyte layer 40 constitute the single cell 50. The battery element of the all-solid-state battery 70 may include only one unit cell 50 or may include a plurality of unit cells 50 . Figure 1 FIG. 7 shows an all-solid-state battery 70 including two single cells 50 as battery elements. Figure 2 2 shows an all-solid-state battery 70 in which three unit cells 50 are stacked to form a battery element.

[0042] In the all-solid battery 70, in a state where the terminals 60 connected to the positive electrode layer 30 and the negative electrode layer 20 are extended to the outside, the battery element is covered in a manner that a flange portion (an area where the heat-fusible resin layers 4 are in contact with each other) can be formed on the periphery of the battery element, and the heat-fusible resin layers 4 of the flange portion are heat-sealed to each other to seal it, thereby forming an all-solid battery using an outer packaging material for an all-solid battery. In the case where the battery element is accommodated in a package formed by the outer packaging material 10 for an all-solid battery of the present invention, the package is formed in a manner that the heat-fusible resin portion of the outer packaging material 10 for an all-solid battery of the present invention becomes the inside (the surface in contact with the battery element). As described above, in the all-solid battery 70 of the present invention, the heat-fused peripheral portion of the space (recess) where the battery element is accommodated is preferably flat except for the portion where the metal terminal exists. In addition, in the all-solid battery 70 of the present invention, it is not necessary to configure a substance for absorbing hydrogen sulfide (a hydrogen sulfide absorbing substance different from the resin constituting the heat-fusible resin layer) on the periphery of the space (recess) where the battery element is accommodated.

[0043] As described above, there are no particular restrictions on the all-solid battery to which the outer packaging material 10 of the present invention is applied, as long as the solid electrolyte contains a sulfide solid electrolyte material and a specific outer packaging material 10 is used, and the same applies to the all-solid battery 70 of the present invention. Next, the materials and the like constituting the battery element of the all-solid battery to which the outer packaging material 10 of the present invention is applied are exemplified.

[0044] As described above, in the battery element of the all-solid-state battery 70, the single cell 50 is composed of at least the positive electrode layer 30, the negative electrode layer 20 and the solid electrolyte layer 40. The positive electrode layer 30 has a structure in which the positive electrode active material layer 31 is stacked on the positive electrode collector 32. The negative electrode layer 20 has a structure in which the negative electrode active material layer 21 is stacked on the negative electrode collector 22. Moreover, the positive electrode collector 32 and the negative electrode collector 22 are respectively connected to the terminal 60 exposed to the outside, thereby being electrically connected to the external environment.

[0045] [Positive Electrode Active Material Layer 31]

[0046] The positive electrode active material layer 31 is a layer containing at least a positive electrode active material. The positive electrode active material layer 31 may contain a solid electrolyte material, a conductive material, a binder, etc., as necessary, in addition to the positive electrode active material.

[0047] There are no particular restrictions on the positive electrode active material, and examples thereof include oxide active materials, sulfide active materials, and the like. In the case where the all-solid battery is an all-solid lithium battery, examples of the oxide active material used as the positive electrode active material include LiCoO2, LiMnO2, LiNiO2, LiVO2, LiNi 1 / 3 Co 1 / 3Mn 1 / 3 O2 and other rock salt layered active materials, LiMn2O4, Li(Ni 0.5 Mn 1.5 )O4 and other spinel active materials, LiFePO4, LiMnPO4 and other olivine active materials, Li2FeSiO4, Li2MnSiO4 and other Si-containing active materials, etc. In addition, as sulfide active materials used as positive electrode active materials of all-solid-state lithium batteries, for example, copper chevron, iron sulfide, cobalt sulfide, nickel sulfide, etc. can be cited.

[0048] The shape of the positive electrode active material is not particularly limited, and an example thereof is a particle shape. The average particle size (D 50 ) is preferably about 0.1 to 50 μm. The content of the positive electrode active material in the positive electrode active material layer 31 is preferably about 10 to 99 mass %, and more preferably about 20 to 90 mass %.

[0049] The positive electrode active material layer 31 preferably further contains a solid electrolyte material. This can improve the ion conductivity in the positive electrode active material layer 31. The solid electrolyte material contained in the positive electrode active material layer 31 is the same as the solid electrolyte material exemplified in the solid electrolyte layer 40 described later. The content of the solid electrolyte material in the positive electrode active material layer is preferably about 1 to 90 mass %, and more preferably about 10 to 80 mass %.

[0050] The positive electrode active material layer 31 may further contain a conductive material. By adding a conductive material, the electronic conductivity of the positive electrode active material layer can be improved. As the conductive material, for example, acetylene black, Ketjen black, carbon fiber, etc. can be cited. In addition, the positive electrode active material layer may further contain a binding material. As the binding material, for example, fluorine-containing binding materials such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF) can be cited.

[0051] The thickness of the positive electrode active material layer 31 can be appropriately set according to the size of the all-solid-state battery, and is preferably about 0.1 to 1000 μm.

[0052] [Positive electrode current collector 32]

[0053] Examples of the material constituting the positive electrode current collector 32 include stainless steel (SUS), aluminum, nickel, iron, titanium, and carbon.

[0054] The thickness of the positive electrode current collector 32 can be appropriately set according to the size of the all-solid-state battery, and is preferably about 10 to 1000 μm.

[0055] [Negative Electrode Active Material Layer 21]

[0056] The negative electrode active material layer 21 is a layer containing at least a negative electrode active material. The negative electrode active material layer 21 may contain a solid electrolyte material, a conductive material, a binder, etc., in addition to the negative electrode active material, as necessary.

[0057] There are no particular restrictions on the negative electrode active material, and examples thereof include carbon active materials, metal active materials, oxide active materials, and the like. Examples of carbon active materials include graphites such as mesocarbon microbeads (MCMB) and highly oriented graphite (HOPG), and amorphous carbons such as hard carbon and soft carbon. Examples of metal active materials include In, Al, Si, and Sn. Examples of oxide active materials include Nb2O5, Li4Ti5O 12 , SiO, etc.

[0058] The shape of the negative electrode active material is not particularly limited, and examples thereof include particle shape and film shape. The average particle size (D 50 ) is preferably about 0.1 to 50 μm. The content of the negative electrode active material in the negative electrode active material layer 21 is, for example, about 10 to 99 mass %, more preferably about 20 to 90 mass %.

[0059] The negative electrode active material layer 21 preferably further contains a solid electrolyte material. This can improve the ion conductivity in the negative electrode active material layer 21. In addition, the solid electrolyte material contained in the negative electrode active material layer 21 is the same as the solid electrolyte material exemplified in the solid electrolyte layer 40 described later. The content of the solid electrolyte material in the negative electrode active material layer 21 is preferably about 1 to 90 mass %, and more preferably about 10 to 80 mass %.

[0060] The negative electrode active material layer 21 may further contain a conductive material. In addition, the negative electrode active material layer 21 may further contain a binder. The conductive material and the binder are the same as those exemplified in the positive electrode active material layer 31 described above.

[0061] The thickness of the negative electrode active material layer 21 can be appropriately set depending on the size of the all-solid-state battery, and is preferably about 0.1 to 1000 μm.

[0062] [Negative Electrode Collector 22]

[0063] Examples of the material constituting the negative electrode current collector 22 include stainless steel (SUS), copper, nickel, and carbon.

[0064] The thickness of the negative electrode current collector 22 can be appropriately set according to the size of the all-solid battery, and is preferably about 10 to 1000 μm.

[0065] [Solid electrolyte layer 40]

[0066] The solid electrolyte layer 40 is a layer containing a sulfide solid electrolyte material.

[0067] Sulfide solid electrolyte materials are more ion-conductive than oxide solid electrolyte materials, and are therefore preferred. When applied to a solid-state battery containing a sulfide solid electrolyte material, the all-solid-state battery outer packaging material 10 of the present invention can effectively suppress the leakage of hydrogen sulfide generated inside the solid-state battery to the outside.

[0068] In addition, specific examples of sulfide solid electrolyte materials include Li2S-P2S5, Li2S-P2S5-LiI, Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (where m and n are positive numbers; Z is any one of Ge, Zn, and Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li x MO y (where x and y are positive numbers; M is any one of P, Si, Ge, B, Al, Ga, and In), etc. The above description of "Li2S-P2S5" refers to a sulfide solid electrolyte material formed using a raw material composition containing Li2S and P2S5, and the same applies to other descriptions. In addition, the sulfide solid electrolyte material may be sulfide glass or crystallized sulfide glass.

[0069] The content of the solid electrolyte material in the solid electrolyte layer 40 is not particularly limited, but is preferably 60% by mass or more, more preferably 70% by mass or more, and further preferably 80% by mass or more. The solid electrolyte layer may contain a binder or may consist only of a solid electrolyte material.

[0070] The thickness of the solid electrolyte layer 40 can be appropriately set according to the size of the all-solid battery, and is preferably about 0.1 to 1000 μm, and more preferably about 0.1 to 300 μm.

[0071] The all-solid battery 70 of the present invention can be used in an environment that is restricted from the outside under high pressure. As the pressure for restricting the all-solid battery 70 from the outside, from the viewpoint of appropriately suppressing the peeling between the solid electrolyte and the negative electrode active material layer (and then between the solid electrolyte and the positive electrode active material layer), preferably about 0.1MPa or more, more preferably 5MPa or more, and further preferably about 1MPa or more can be cited. In addition, preferably about 100MPa or less can be cited, and more preferably about 30MPa or less can be cited. As a preferred range, about 0.1 to 100MPa, about 0.1 to 70MPa, about 5 to 100MPa, about 5 to 70MPa, about 10 to 100MPa, and about 1 to 30MPa can be cited. As a method for restricting the all-solid battery 70 from the outside under high pressure, a method of clamping the all-solid battery with a metal plate or the like and fixing it under high pressure pressing (for example, fastening it with a vise or the like) can be cited.

[0072] As a method of restricting the all-solid battery 70 from the outside under high pressure, there can be cited a method of clamping the all-solid battery with metal plates and fixing it under high pressure pressing (for example, tightening it with a vise or the like) or a method of gas pressurization.

[0073] In addition, from the same point of view, the temperature when restricting the all-solid-state battery 70 from the outside is preferably above 20°C, more preferably above 40°C. In addition, it is preferably below 200°C, more preferably below 150°C. As the preferred range, it is about 20 to 150°C.

[0074] The shape of the all-solid-state battery 70 of the present invention is not particularly limited, and is preferably Figure 3 As shown in the schematic diagram of , it is rectangular when viewed from above. Moreover, the ratio of the length of the first side of the all-solid-state battery 70, which is rectangular when viewed from above, to the length of the second side in the direction perpendicular to the first side (the length of the first side: the length of the second side) is preferably about 1:1 to 1:5. When the second side is too long relative to the length of the first side, when the outer packaging material 10 is molded to form the molding portion M described later, the second side is difficult to be fixed to the mold, and the R value (radius of curvature) of the ridge portion (the first curved portion described later) of the molding portion M along the second side tends to become too large.

[0075] like Figure 1 to Figure 3 As shown in the schematic diagram of , in the all-solid-state battery 70 of the present invention, the battery element is preferably housed in a molding portion M which is rectangular in shape when viewed from above, and the molding portion M is formed in such a way that the outer packaging material 10 extends from the side of the thermally fusible resin layer 4 to the side of the barrier layer 3. Figure 1 FIG. 7 shows a figure in which a molded portion M is formed on one side of a solid-state battery 70. Figure 2 The figure shows that the molded portion M is formed on both sides of the all-solid-state battery 70.

[0076] In the present invention, it is preferred that: when the all-solid-state battery 70 is viewed from the barrier layer 3 side, the two sides ( Figures 1 to 3 The straight line (refer to Figure 3 In the cross section in the thickness direction of the outer packaging material 10 on the dashed line Y in the y direction and the dashed line Z in the z direction), the outer packaging material 10 has the first curved portion R1 (see Figure 2 R1z in) and the second bend R2 (refer to Figure 2 R2z in the figure), the R value (curvature radius) of the first curved portion R1 is greater than 1 mm. When the R value (curvature radius) is greater than 1 mm, the force of stretching the outer packaging material 10 does not become too large at the corners (corners) of the rectangular molded portion M, and it is possible to suppress the generation of pinholes and the like in the barrier layer 3 before reaching the specified molding depth. When the outer packaging material 10 is molded using a mold, the molded portion M having the first curved portion R1 and the second curved portion R2 is formed in such a manner that the outer packaging material 10 extends from the heat-fusible resin layer 4 side to the barrier layer 3 side. In the molded portion M, the first curved portion R1 is located at a position protruding to the outside of the all-solid-state battery.

[0077] exist Figure 3 In the schematic diagram, the cross-sectional view on the dotted line Z is Figure 2 Corresponding to the schematic diagram of FIG. 1 , the molded portion M has a first curved portion R1z and a second curved portion R2z in sequence from the center portion to the end portion of the outer packaging material 10. Figure 3 In the schematic diagram, in the cross section on the dotted line Y, the molding portion M has a first bend R1y and a second bend R2y in sequence from the center to the end of the outer packaging material 10. The first bend R1z refers to the first bend in the z direction. Similarly, the second bend R2z refers to the second bend in the z direction, the first bend R1y refers to the first bend in the y direction, and the second bend R2y refers to the second bend in the y direction. Regarding the first bend R1y, similarly to the R value of the first bend R1, when the R value (radius of curvature) is greater than 1 mm, the force of stretching the outer packaging material 10 will not become too large at the corners (corners) of the rectangular molding portion M, and it is possible to suppress the generation of pinholes in the barrier layer 3 before reaching the specified molding depth. Therefore, the R value (radius of curvature) is preferably greater than 1 mm.

[0078] In the present invention, the R values ​​(radii of curvature) of the first curved portion R1 and the second curved portion R2 are respectively the barrier layer 3 side of the outer packaging material 10 (i.e., the outer surface side of the outer packaging material 10, for example Figure 2The R value (radius of curvature) of the surface (the area surrounded by the dotted line in the figure).

[0079] In the all-solid battery 70, when the dead space inside the battery is minimized and the volume energy density is increased, if Figure 3 As explained in , the first side parallel to the y direction of the all-solid-state battery that is rectangular in shape when viewed from above is the short side, and the second side parallel to the z direction is the long side. Preferably, the R value (radius of curvature) of the first bend R1z of the all-solid-state battery that is rectangular in shape when viewed from above along the short side parallel to the y direction where the terminal is set is greater than the R value (radius of curvature) of the first bend R1y along the long side parallel to the z direction.

[0080] 3. Used to form each layer of outer packaging material for all-solid-state batteries

[0081] The outer packaging material 10 of the present invention is composed of a laminated body having at least a base layer 1, a barrier layer 3 and a heat-fusible resin layer 4 in this order from the outside, and the hydrogen sulfide permeation amount of the resin constituting the heat-fusible resin layer 4 is 1.0×10 -9 cc mm / cm 2 ·sec·cmHg or less Next, each layer constituting the outer packaging material 10 of the present invention will be described in detail.

[0082] [Base material layer 1]

[0083] In the present invention, the base material layer 1 is a layer provided as needed on the outside of the barrier layer 3 (on the outside of the barrier layer protective film 3b when the barrier layer protective film 3b is provided) for the purpose of fulfilling the function as a base material of the outer packaging material 10. The base material layer 1 is located on the outer layer side of the outer packaging material 10.

[0084] There is no particular limitation on the material for forming the base layer 1 as long as it has a function as a base material, that is, at least insulating properties. The base layer 1 can be formed using, for example, a resin, and the resin may contain additives described below.

[0085] When the substrate layer 1 is formed of a resin, the substrate layer 1 may be, for example, a resin film formed of a resin, or may be formed by coating a resin. The resin film may be an unstretched film or a stretched film. As a stretched film, a uniaxially stretched film and a biaxially stretched film may be cited, preferably a biaxially stretched film. As a stretching method for forming a biaxially stretched film, for example, a sequential biaxial stretching method, an inflation method, a simultaneous biaxial stretching method, etc. may be cited. As a method for coating a resin, a roll coating method, a gravure coating method, an extrusion coating method, etc. may be cited.

[0086] Examples of the resin used to form the substrate layer 1 include polyester, polyamide, polyolefin, epoxy resin, acrylic resin, fluororesin, polyurethane, silicone resin, phenolic resin and the like, or modified products of these resins. In addition, the resin forming the substrate layer 1 may be a copolymer of these resins, or a modified product of a copolymer. Furthermore, it may be a mixture of these resins.

[0087] As the resin forming the base material layer 1, polyester and polyamide are preferred among them.

[0088] Specific examples of polyester include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, and copolyesters. In addition, examples of copolyesters include copolyesters having ethylene terephthalate as a main component of a repeating unit. Specifically, there can be mentioned copolymer polyesters in which ethylene terephthalate is polymerized with ethylene isophthalate as the main body of the repeating unit (hereinafter, abbreviated as poly(terephthalic acid / isophthalic acid)ethylene glycol), poly(terephthalic acid / adipate)ethylene glycol, poly(terephthalic acid / sodium sulfoisophthalate)ethylene glycol, poly(terephthalic acid / sodium isophthalate)ethylene glycol, poly(terephthalic acid / phenyl-dicarboxylic acid)ethylene glycol, poly(terephthalic acid / decanedicarboxylic acid)ethylene glycol, etc. These polyesters may be used alone or in combination of two or more.

[0089] In addition, specific examples of polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (I represents isophthalic acid, and T represents terephthalic acid) containing structural units derived from terephthalic acid and / or isophthalic acid; and polyamides. Aromatic polyamides such as MXD6 (poly(m-xylylene adipamide)); alicyclic polyamides such as polyamide PACM6 (poly(bis(4-aminocyclohexyl)methane adipamide); polyamides obtained by copolymerizing lactam components and isocyanate components such as 4,4'-diphenylmethane-diisocyanate; polyesteramide copolymers as copolymers of copolymerized polyamides and polyesters or polyalkylene ether glycols; polyamides such as copolymers of these. These polyamides may be used alone or in combination of two or more.

[0090] The substrate layer 1 preferably comprises at least one of a polyester film, a polyamide film and a polyolefin film, preferably comprises at least one of a stretched polyester film, a stretched polyamide film and a stretched polyolefin film, more preferably comprises at least one of a stretched polyethylene terephthalate film, a stretched polybutylene terephthalate film, a stretched nylon film and a stretched polypropylene film, and further preferably comprises at least one of a biaxially stretched polyethylene terephthalate film, a biaxially stretched polybutylene terephthalate film, a biaxially stretched nylon film and a biaxially stretched polypropylene film.

[0091] The substrate layer 1 may be a single layer or may be composed of two or more layers. When the substrate layer 1 is composed of two or more layers, the substrate layer 1 may be a laminated body obtained by laminating resin films using an adhesive or the like, or a laminated body obtained by co-extruding resins to form two or more layers of resin films. In addition, a laminated body of two or more layers of resin films obtained by co-extruding resins may be directly used as the substrate layer 1 in an unstretched state, or the laminated body may be uniaxially stretched or biaxially stretched to form the substrate layer 1. When the substrate layer 1 is a single layer, it is preferred that the substrate layer 1 is composed of a single layer of a polyester resin.

[0092] In the substrate layer 1, as specific examples of a laminate of two or more layers of resin films, there can be mentioned a laminate of a polyester film and a nylon film, a laminate of two or more layers of nylon films, a laminate of two or more layers of polyester films, etc., preferably a laminate of a stretched nylon film and a stretched polyester film, a laminate of two or more layers of stretched nylon films, and a laminate of two or more layers of stretched polyester films. For example, in the case where the substrate layer 1 is a laminate of two layers of resin films, preferably a laminate of a polyester resin film and a polyester resin film, a laminate of a polyamide resin film and a polyamide resin film, or a laminate of a polyester resin film and a polyamide resin film, more preferably a laminate of a polyethylene terephthalate film and a polyethylene terephthalate film, a laminate of a nylon film and a nylon film, or a laminate of a polyethylene terephthalate film and a nylon film.

[0093] In the case where the substrate layer 1 is a laminate of two or more layers of resin films, the two or more layers of resin films can be laminated via an adhesive. As for the preferred adhesive, the same adhesive as the adhesive exemplified in the adhesive layer 2 described later can be cited. In addition, as a method for laminating two or more layers of resin films, there is no particular restriction, and a known method can be adopted, such as dry lamination, sandwich lamination, extrusion lamination, hot lamination, etc., and a preferred dry lamination method can be cited. In the case of laminating them by dry lamination, it is preferred to use a polyurethane adhesive as the adhesive. At this time, as the thickness of the adhesive, for example, about 2 to 5 μm can be cited. In addition, it is also possible to form an anchor coating on the resin film and laminate it. The anchor coating can cite the same layer as the adhesive exemplified in the adhesive layer 2 described later. At this time, as the thickness of the anchor coating, for example, about 0.01 to 1.0 μm can be cited.

[0094] In addition, additives such as lubricants, flame retardants, antiblocking agents, antioxidants, light stabilizers, tackifiers, and antistatic agents may be present on at least one of the surface and the inside of the base layer 1. The additives may be used alone or in combination of two or more.

[0095] In the present invention, from the viewpoint of improving the formability of the outer packaging material 10, it is preferred that a lubricant is present on the surface of the substrate layer 1. As a lubricant, there is no particular limitation, and preferred amide lubricants can be cited. As a specific example of an amide lubricant, for example, saturated fatty acid amide, unsaturated fatty acid amide, substituted amide, hydroxymethyl amide, saturated fatty acid bisamide, unsaturated fatty acid bisamide, fatty acid ester amide, aromatic bisamide, etc. can be cited. As a specific example of saturated fatty acid amide, lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, hydroxystearic acid amide, etc. can be cited. As a specific example of unsaturated fatty acid amide, oleic acid amide, erucic acid amide, etc. can be cited. As a specific example of substituted amide, N-oleyl palmitic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, N-stearyl erucic acid amide, etc. can be cited. In addition, as a specific example of hydroxymethyl amide, hydroxymethyl stearic acid amide, etc. can be cited. Specific examples of saturated fatty acid bisamides include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, N,N'-distearyl adipamide, N,N'-distearyl sebacic acid amide, etc. Specific examples of unsaturated fatty acid bisamides include ethylene bisoleic acid amide, ethylene biserucic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipamide, N,N'-dioleyl sebacic acid amide, etc. Specific examples of fatty acid ester amides include stearic acid stearamide ethyl ester, etc. Specific examples of the aromatic bisamide include meta-xylylene bisstearic acid amide, meta-xylylene bishydroxystearic acid amide, N,N′-distearylisophthalic acid amide, etc. The lubricant may be used alone or in combination of two or more.

[0096] When a lubricant is present on the surface of the base material layer 1, the amount of the lubricant is not particularly limited, but is preferably about 3 mg / m 2 More preferably 4 to 15 mg / m 2 About 5-14 mg / m 2 about.

[0097] The lubricant present on the surface of the base layer 1 may be obtained by causing the lubricant contained in the resin constituting the base layer 1 to ooze out, or may be obtained by coating the lubricant on the surface of the base layer 1 .

[0098] The thickness of the substrate layer 1 is not particularly limited as long as it can function as a substrate, and can be, for example, about 3 to 50 μm, preferably about 10 to 35 μm. In the case where the substrate layer 1 is a laminate of two or more layers of resin films, the thickness of the resin films constituting each layer can be preferably about 2 to 25 μm.

[0099] [Adhesive layer 2]

[0100] In the outer packaging material 10, the adhesive layer 2 is provided as a layer between the substrate layer 1 and the barrier layer 3 (or the substrate layer 1 and the barrier layer protective film 3b if there is a barrier layer protective film 3b) for the purpose of improving the adhesion between them.

[0101] The adhesive layer 2 is formed of an adhesive capable of bonding the substrate layer 1 to the barrier layer 3 (or the barrier layer protective film 3b). The adhesive used in the formation of the adhesive layer 2 is not limited, and may be any of a chemical reaction type, a solvent volatilization type, a heat-melting type, a hot pressing type, and the like. In addition, it may be a two-component curing adhesive (two-component adhesive), a one-component curing adhesive (one-component adhesive), or a resin that does not accompany a curing reaction. In addition, the adhesive layer 2 may be a single layer or a multilayer.

[0102] As the adhesive component contained in the adhesive, specifically, polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, and copolyesters can be cited; polyethers; polyurethanes; epoxy resins; phenolic resins; polyamides such as nylon 6, nylon 66, nylon 12, and copolyamides; polyolefin resins such as polyolefins, cyclic polyolefins, acid-modified polyolefins, and acid-modified cyclic polyolefins; polyvinyl acetate; cellulose; (meth) acrylic resins; polyimides; polycarbonates; amino resins such as urea resins and melamine resins; rubbers such as chloroprene rubber, nitrile rubber, and styrene-butadiene rubber; silicone resins, etc. These adhesive components can be used alone or in combination of two or more. Among these adhesive components, polyurethane adhesives can be cited as preferred. In addition, the resins that become these adhesive components can be used in combination with appropriate curing agents to improve the bonding strength. The curing agent can be appropriately selected from polyisocyanates, polyfunctional epoxy resins, oxazoline group-containing polymers, polyamine resins, acid anhydrides, and the like, depending on the functional groups of the adhesive component.

[0103] As the polyurethane adhesive, for example, there can be mentioned a polyurethane adhesive comprising a main agent containing a polyol compound and a curing agent containing an isocyanate compound. There can be mentioned a two-component curing type polyurethane adhesive preferably using a polyol such as polyester polyol, polyether polyol and acrylic polyol as a main agent and using an aromatic or aliphatic polyisocyanate as a curing agent. In addition, as the polyol compound, it is preferred to use a polyester polyol having a hydroxyl group in the side chain in addition to the hydroxyl group at the end of the repeating unit.

[0104] In addition, the adhesive layer 2 is allowed to add other components as long as it does not damage the adhesion, and can contain a colorant, a thermoplastic elastomer, a tackifier, a filler, etc. By making the adhesive layer 2 contain a colorant, the outer packaging material 10 can be colored. As the colorant, known colorants such as pigments and dyes can be used. In addition, the colorant can be used only 1 kind, or two or more kinds can be mixed and used.

[0105] The type of pigment is not particularly limited as long as it is within the range that does not impair the adhesiveness of the adhesive layer 2. Examples of organic pigments include pigments such as azo, phthalocyanine, quinacridone, anthraquinone, dioxazine, indigothioindigo, perinone-perylene, isoindoline, and benzimidazolone. Examples of inorganic pigments include pigments such as carbon black, titanium oxide, cadmium, lead, chromium oxide, and iron. In addition, examples include fine powder of mica, fish scale foil, and the like.

[0106] Among the colorants, carbon black is preferred in order to make the outer packaging material 10 appear black, for example.

[0107] The average particle size of the pigment is not particularly limited, and may be, for example, about 0.05 to 5 μm, preferably about 0.08 to 2 μm. The average particle size of the pigment is a median particle size measured by a laser diffraction / scattering particle size distribution measuring device.

[0108] The content of the pigment in the adhesive layer 2 is not particularly limited as long as the packaging material 10 can be colored, and is, for example, about 5 to 60% by mass, preferably 10 to 40% by mass.

[0109] The thickness of the adhesive layer 2 is not particularly limited as long as the substrate layer 1 and the barrier layer 3 can be bonded together. For example, the thickness may be about 1 μm or more, about 2 μm or more, about 10 μm or less, about 5 μm or less, and the preferred range may be about 1 to 10 μm, about 1 to 5 μm, about 2 to 10 μm, and about 2 to 5 μm.

[0110] [Coloring Layer]

[0111] The colored layer is a layer (not shown) provided between the substrate layer 1 and the barrier layer 3 (or barrier layer protective film 3b) as required. In the case of having an adhesive layer 2, a colored layer may be provided between the substrate layer 1 and the adhesive layer 2, or between the adhesive layer 2 and the barrier layer 3 (or barrier layer protective film 3b). In addition, a colored layer may be provided outside the substrate layer 1. By providing a colored layer, the outer packaging material 10 can be colored.

[0112] The coloring layer can be formed, for example, by applying ink containing a colorant to the surface of the base layer 1 or the surface of the barrier layer 3 (in the case of a barrier layer protective film 3b, the surface of the barrier layer protective film 3b). As the colorant, a known colorant such as a pigment or a dye can be used. In addition, a single colorant may be used, or two or more colorants may be mixed and used.

[0113] Specific examples of the colorant contained in the colored layer include the same colorants as those exemplified in the section of the "adhesive layer 2".

[0114] [Barrier layer 3]

[0115] In the outer packaging material 10 , the barrier layer 3 is a layer capable of at least suppressing the intrusion of moisture.

[0116] As the barrier layer 3, for example, metal foil, vapor-deposited film, resin layer, etc. having barrier properties can be cited. As the vapor-deposited film, metal vapor-deposited film, inorganic oxide vapor-deposited film, carbon-containing inorganic oxide vapor-deposited film, etc. can be cited. As the resin layer, polyvinylidene chloride, polymers with chlorotrifluoroethylene (CTFE) as the main component, polymers with tetrafluoroethylene (TFE) as the main component, polymers with fluoroalkyl groups, and polymers with fluoroalkyl units as the main component, such as fluorine-containing resins, ethylene-vinyl alcohol copolymers, etc. can be cited. In addition, as the barrier layer 3, resin films provided with at least one layer of these vapor-deposited films and resin layers can also be cited. The barrier layer 3 can be provided with multiple layers. The barrier layer 3 preferably includes a layer composed of a metal material. As the metal material constituting the barrier layer 3, specifically, aluminum alloy, stainless steel, titanium steel, steel plate, etc. can be cited. When a metal foil is used, it is preferably included at least one of an aluminum alloy foil and a stainless steel foil.

[0117] From the viewpoint of improving the formability of the outer packaging material 10, the aluminum alloy foil is preferably a soft aluminum alloy foil composed of an annealed aluminum alloy, etc., and from the viewpoint of further improving the formability, it is preferably an aluminum alloy foil containing iron. In the aluminum alloy foil containing iron (100% by mass), the content of iron is preferably 0.1 to 9.0% by mass, and more preferably 0.5 to 2.0% by mass. By making the content of iron more than 0.1% by mass, an outer packaging material with better formability can be obtained. By making the content of iron less than 9.0% by mass, an outer packaging material with better flexibility can be obtained. As a soft aluminum alloy foil, for example, an aluminum alloy foil having a composition specified in JIS H4160:1994A8021H-O, JIS H4160:1994A8079H-O, JIS H4000:2014A8021P-O or JIS H4000:2014A8079P-O can be cited. Furthermore, silicon, magnesium, copper, manganese, etc. may be added as needed. Softening may be performed by annealing treatment or the like.

[0118] In addition, examples of stainless steel foil include austenitic, ferrite, austenite-ferrite, martensitic, and precipitation hardened stainless steel foils. In order to provide an outer packaging material 10 having excellent formability, the stainless steel foil is preferably made of austenitic stainless steel.

[0119] Specific examples of the austenitic stainless steel constituting the stainless steel foil include SUS304, SUS301, and SUS316L. Among them, SUS304 is particularly preferred.

[0120] The thickness of the barrier layer 3 may be, in the case of a metal foil, any thickness as long as it can function as a barrier layer capable of at least inhibiting the intrusion of moisture, and may be, for example, about 9 to 200 μm. The thickness of the barrier layer 3 may be, for example, preferably about 85 μm or less, more preferably about 50 μm or less, further preferably about 40 μm or less, and particularly preferably about 35 μm or less, and may be, for example, preferably about 10 μm or more, further preferably about 20 μm or more, and more preferably about 25 μm or more. Preferred ranges of the thickness include about 10 to 85 μm, about 10 to 50 μm, about 10 to 40 μm, about 10 to 35 μm, about 20 to 85 μm, about 20 to 50 μm, about 20 to 40 μm, about 20 to 35 μm, about 25 to 85 μm, about 25 to 50 μm, about 25 to 40 μm, and about 25 to 35 μm. When the barrier layer 3 is composed of an aluminum alloy foil, the above range is particularly preferred, and about 25 to 85 μm and about 25 to 50 μm are particularly preferred. In addition, in particular, when the barrier layer 3 is composed of a stainless steel foil, the thickness of the stainless steel foil is preferably about 60 μm or less, more preferably about 50 μm or less, further preferably about 40 μm or less, further preferably about 30 μm or less, and particularly preferably about 25 μm or less. In addition, it is preferably about 10 μm or more, and more preferably about 15 μm or more. As the preferred range of thickness, about 10 to 60 μm, about 10 to 50 μm, about 10 to 40 μm, about 10 to 30 μm, about 10 to 25 μm, about 15 to 60 μm, about 15 to 50 μm, about 15 to 40 μm, about 15 to 30 μm, about 15 to 25 μm, about 15 to 60 μm, about 15 to 50 μm, about 15 to 40 μm, about 15 to 30 μm, and about 15 to 25 μm.

[0121] [Barrier layer protective films 3a, 3b]

[0122] In the outer packaging material 10, a barrier layer protective film 3a is preferably provided on the surface of the barrier layer 3 on the side of the heat-fusible resin layer 4. In addition, a barrier layer protective film 3b is also preferably provided on the surface of the barrier layer 3 on the side of the base material layer 1. In the outer packaging material 10, for example, the barrier layer protective film 3a may be provided only on the surface of the barrier layer 3 on the side of the heat-fusible resin layer 4, or the barrier layer protective films 3a and 3b may be provided on both surfaces of the barrier layer 3.

[0123] When the barrier layer protective film 3a of the outer packaging material 10 was analyzed using time-of-flight secondary ion mass spectrometry, the PO3 - The peak intensity P PO3 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO3 / CrPO4 It is preferably in the range of 6 to 120.

[0124] In an all-solid-state battery, in order to suppress the peeling between the solid electrolyte and the negative electrode active material layer and the positive electrode active material layer, it is expected that the all-solid-state battery is continuously restricted by high pressure pressing from the outside of the outer packaging material even when in use. However, when the solid electrolyte and the negative electrode active material layer and the positive electrode active material layer are continuously restricted from the outside of the outer packaging material of the all-solid-state battery in a high-pressure state, the heat-fusible resin layer of the outer packaging material is strongly pressed on the battery element, and the thickness of the heat-fusible resin layer (inner layer) of the outer packaging material becomes thinner, and the barrier layer laminated in the outer packaging material may contact the solid electrolyte. In particular, in a state where the barrier layer of the outer packaging material is in contact with the solid electrolyte containing a sulfide solid electrolyte material, when electricity is passed between them, an alloy is generated on the surface of the barrier layer, and there is a problem of barrier layer degradation. In the all-solid-state battery 70 of the present invention, when a barrier layer protective film 3a having a peak intensity ratio within the above-mentioned specific range is provided on the surface of the barrier layer 3 of the outer packaging material 10, the all-solid-state battery 70 is restricted under a high-voltage state. Thus, even when the solid electrolyte comprising a sulfide solid electrolyte material penetrates the thermally fusible resin layer 4, the adhesive layer 5, etc., and when electricity is passed between the barrier layer 3 and the solid electrolyte layer 40, it is difficult to generate an alloy on the surface of the barrier layer 3, thereby effectively suppressing the degradation of the barrier layer 3.

[0125] In the present invention, the PO3 - The peak intensity P PO3 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO3 / CrPO4 The preferred range is 6 to 120. From the viewpoint of more effectively suppressing the degradation of the barrier layer 3, the ratio P PO3 / CrPO4 The lower limit is preferably about 10 or more, and the upper limit is preferably about 115 or less, more preferably about 110 or less, and further preferably about 50 or less. PO3 / CrPO4 The preferred range of may be about 6 to 115, about 6 to 110, about 6 to 50, about 10 to 120, about 10 to 115, about 10 to 110, about 10 to 50, among which about 10 to 50 is more preferred, and about 25 to 30 is further particularly preferred.

[0126] In addition, in the present invention, when the barrier layer protective film 3a is analyzed using time-of-flight secondary ion mass spectrometry, the PO2 - The peak intensity P PO2 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO2 / CrPO4 It is preferably in the range of 7-70.

[0127] From PO2- The peak intensity P PO2 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO2 / CrPO4 It is preferably in the range of 7 to 70, and from the viewpoint of more effectively suppressing the degradation of the barrier layer 3, as the ratio P PO2 / CrPO4 The lower limit is preferably about 10 or more, the upper limit is preferably about 65 or less, and more preferably about 50 or less. PO2 / CrPO4 The preferred range of may be about 7 to 70, about 7 to 65, about 7 to 50, about 10 to 70, about 10 to 65, about 10 to 50, among which about 10 to 50 is more preferred, and about 15 to 20 is further particularly preferred.

[0128] In the present invention, when barrier layer protective films 3a and 3b are provided on both sides of the barrier layer 3, it is preferred that the peak intensity ratio P of any one of the barrier layer protective films 3a and 3b is PO3 / CrPO4 are all within the above range, and preferably P PO2 / CrPO4 are also within the above range.

[0129] The method of analyzing the barrier layer protection films 3 a and 3 b using time-of-flight secondary ion mass spectrometry can be specifically performed using a time-of-flight secondary ion mass spectrometer under the following measurement conditions.

[0130] (Measurement conditions)

[0131] Primary ion: Doubly charged ion of bismuth cluster (Bi3 ++ )

[0132] 1st ion acceleration voltage: 30kV

[0133] Mass range (m / z): 0~1500

[0134] Measuring range: 100μm×100μm

[0135] Scan number: 16 scan / cycle

[0136] Number of pixels (1 side): 256 pixels

[0137] Etching ions: Ar gas cluster ion beam (Ar-GCIB)

[0138] Etching ion acceleration voltage: 5.0kV

[0139] In addition, the presence of chromium in the barrier layer protective film can be confirmed using X-ray photoelectron spectroscopy. Specifically, first, in the outer packaging material, the layers (adhesive layer, hot-melt resin layer, adhesive layer, etc.) laminated on the barrier layer are physically peeled off. Next, the barrier layer is placed in an electric furnace and the organic components present on the surface of the barrier layer are removed at about 300°C for about 30 minutes. Then, the presence of chromium is confirmed using X-ray photoelectron spectroscopy of the surface of the barrier layer.

[0140] The barrier layer protection films 3 a and 3 b can be formed by subjecting the surface of the barrier layer 3 to a chemical conversion treatment using a treatment solution containing a chromium compound such as chromium oxide.

[0141] As a chemical conversion treatment using a treatment solution containing a chromium compound, for example, the following method can be cited: a material in which a chromium compound such as chromium oxide is dispersed in phosphoric acid and / or its salt is applied to the surface of the barrier layer 3, and then sintered to form a barrier layer protective film on the surface of the barrier layer 3.

[0142] The peak intensity ratio P of barrier layer protective films 3a and 3b PO3 / CrPO4 , and the peak intensity ratio P PO2 / CrPO4 The barrier layer protective films 3 a and 3 b can be adjusted by, for example, the composition of the treatment solution for forming the barrier layer protective films 3 a and 3 b , the temperature and time of the sintering treatment after the treatment, and other production conditions.

[0143] The ratio of the chromium compound to phosphoric acid and / or its salt in the treatment solution containing the chromium compound is not particularly limited. PO3 / CrPO4 , and the peak intensity ratio P PO2 / CrPO4 From the viewpoint of setting the above ranges, the ratio of phosphoric acid and / or its salt to 100 parts by mass of the chromium compound is preferably about 30 to 120 parts by mass, more preferably about 40 to 110 parts by mass. As phosphoric acid and its salt, for example, condensed phosphoric acid and its salt may be used.

[0144] In addition, the treatment liquid containing the chromium compound may also contain an anionic polymer and a crosslinking agent for crosslinking the anionic polymer. As the anionic polymer, poly(meth)acrylic acid or its salt, a copolymer with (meth)acrylic acid or its salt as the main component, etc. may be mentioned. In addition, as the crosslinking agent, a compound having any functional group of an isocyanate group, a glycidyl group, a carboxyl group and an oxazoline group, a silane coupling agent, etc. may be mentioned. The anionic polymer and the crosslinking agent may be one kind, or two or more kinds, respectively.

[0145] In addition, from the viewpoint of effectively suppressing the degradation of the barrier layer 3, the treatment liquid containing the chromium compound preferably contains an aminophenol polymer. In the treatment liquid containing the chromium compound, the content of the aminophenol polymer is preferably about 100 to 400 parts by mass, and more preferably about 200 to 300 parts by mass, relative to 100 parts by mass of the chromium compound. In addition, the weight average molecular weight of the aminophenol polymer is preferably about 5000 to 20000. The weight average molecular weight of the aminophenol polymer is a value measured by gel permeation chromatography (GPC) under the condition of using polystyrene as a standard sample.

[0146] The solvent of the treatment liquid containing a chromium compound is not particularly limited as long as it is a solvent that can disperse the components contained in the treatment liquid and evaporate by subsequent heating, and water is preferred. The solid content concentration of the treatment liquid containing a chromium compound can be, for example, about 1 to 15% by mass. In addition, the surface temperature of the barrier layer when the treatment liquid is applied to the surface of the barrier layer and heated to form a barrier layer protective film can be preferably about 190 to 220°C, and the heating time can be about 3 to 6 seconds. By adopting such a temperature and heating time, the solvent can be evaporated appropriately and the barrier layer protective film can be formed appropriately.

[0147] The solid content concentration of the chromium compound contained in the treatment solution for forming the barrier layer protective films 3a and 3b is not particularly limited, and can be obtained by adjusting the peak intensity ratio P PO3 / CrPO4 , and the peak intensity ratio P PO2 / CrPO4 From the viewpoint of effectively suppressing the degradation of the barrier layer 3 by setting the respective contents within the above-specified ranges, preferably about 7.0 to 12.0 mass %, more preferably about 8.0 to 11.0 mass %, and further preferably about 9.0 to 10.0 mass %.

[0148] The thickness of the barrier layer protective films 3a and 3b is not particularly limited, but is preferably about 1 nm to 10 μm, more preferably about 1 to 100 nm, and further preferably about 1 to 50 nm from the viewpoint of effectively suppressing the degradation of the barrier layer 3. The thickness of the barrier layer protective film can be measured by observation using a transmission electron microscope, or by a combination of observation using a transmission electron microscope and energy dispersive X-ray spectroscopy or electron beam energy loss spectroscopy.

[0149] From the same point of view, as the barrier layer 3, every 1m 2 The amount of the barrier layer protective films 3a and 3b on the surface is preferably about 1 to 500 mg, more preferably about 1 to 100 mg, and further preferably about 1 to 50 mg.

[0150] Examples of a method for applying the treatment liquid containing a chromium compound onto the surface of the barrier layer include a bar coating method, a roll coating method, a gravure coating method, and a dipping method.

[0151] From the above peak intensity ratio P PO3 / CrPO4 , and the peak intensity ratio P PO2 / CrPO4 From the viewpoint of effectively suppressing the degradation of the barrier layer 3 by setting the respective ranges as described above, the heating temperature when the treatment liquid is subjected to sintering treatment to form a barrier layer protective film is preferably about 170 to 250° C., and more preferably about 180 to 230° C. From the same viewpoint, the sintering treatment time is preferably about 2 to 10 seconds, and more preferably about 3 to 6 seconds.

[0152] From the viewpoint of more effectively performing the chemical conversion treatment on the surface of the barrier layer 3, before setting the barrier layer protective films 3a, 3b on the surface of the barrier layer 3, it is preferred to perform a degreasing treatment by a known treatment method such as an alkali immersion method, an electrolytic cleaning method, an acid cleaning method, an electrolytic acid cleaning method, or an acid activation method.

[0153] [Thermal Fusible Resin Layer 4]

[0154] In the all-solid battery outer packaging material 10 of the present invention, the heat-fusible resin layer 4 corresponds to the innermost layer and is a layer (sealing layer) that performs the function of sealing the battery element by heat-fusion bonding the heat-fusible resin layers 4 when assembling the all-solid battery.

[0155] In the all-solid-state battery outer packaging material 10 of the present invention, the hydrogen sulfide permeation rate of the resin constituting the heat-fusible resin layer 4 is 1.0×10 -9 cc mm / cm 2 ·sec·cmHg or less The hydrogen sulfide permeation rate of the resin constituting the thermally adhesive resin layer 4 can be specifically measured by the method described in Examples.

[0156] The hydrogen sulfide permeation rate of the resin constituting the heat-adhesive resin layer 4 is preferably about 8.0×10 -10 cc mm / cm 2 ·sec·cmHg or less, more preferably about 5.0×10 -10 cc mm / cm 2 ·sec·cm Hg or less. In addition, the lower limit of the hydrogen sulfide permeation amount can be, for example, about 1.0×10 -10 cc mm / cm 2 ·sec·cmHg, etc.

[0157] In addition, as the heat-fusible resin layer 4, each 1m 2 The water vapor transmission rate is preferably about 15.0 g / m2 / 24h or less, more preferably about 10.0g / m 2 / 24h or less, more preferably about 8.0g / m 2 / 24h or less, more preferably 1.0g / m 2 / 24h or less. In addition, the lower limit of the total water vapor transmission rate can be, for example, about 5.0 g / m 2 / 24h, about 1.0g / m 2 / 24h, about 0.1g / m 2 / 24h, etc. The water vapor transmission rate is measured as follows.

[0158] <Every 1m 2 Measurement of water vapor transmission rate>

[0159] The thickness of the heat-adhesive resin layer 4 per m was measured by the following method. 2 Water vapor transmission rate (single-sided area) (g / m 2 / 24h). The water vapor transmission rate was measured using an isobaric method based on the method specified in ISO15106-5 2008, at a temperature of 40°C, a relative humidity of 90%, a measurement period of 24 hours, and a measurement area of ​​8cmφ. 2 The water vapor transmission rate is converted into m using the ISO water vapor transmission rate measurement method. 2 The obtained value.

[0160] The hydrogen sulfide permeation rate is 1.0×10 -9 cc mm / cm 2 ·sec·cmHg or less resins include, for example, polyester, fluororesin, cellophane, etc., preferably polyester and fluororesin. As polyester, specifically, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, copolyester, etc., preferably polyethylene terephthalate. In addition, as fluororesin, preferably polytetrafluoroethylene (PTFE), tetrafluoroethylene-ethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), etc. can be mentioned. As the resin constituting the heat-fusible resin layer 4, polytetrafluoroethylene, which has very small hydrogen sulfide permeability and water vapor permeability, is particularly preferred.

[0161] The heat-fusible resin layer 4 may be formed of one resin alone or a blended polymer of two or more resins. The heat-fusible resin layer 4 may be formed of only one layer or two or more layers of the same or different resins.

[0162] In addition, the heat-fusible resin layer 4 may contain a lubricant or the like as needed. When the heat-fusible resin layer 4 contains a lubricant, the moldability of the all-solid battery outer packaging material 10 can be improved. There is no particular limitation on the lubricant, and a known lubricant can be used. One lubricant may be used alone, or two or more lubricants may be used in combination.

[0163] The lubricant is not particularly limited, but an amide lubricant is preferred. Specific examples of the lubricant include the lubricants exemplified in the substrate layer 1. The lubricant may be used alone or in combination of two or more.

[0164] When a lubricant is present on the surface of the heat-fusible resin layer 4, the amount of lubricant present is not particularly limited, but from the viewpoint of improving the moldability of the electronic packaging material, 10 to 50 mg / m is preferred. 2 About 15 to 40 mg / m 2 about.

[0165] The lubricant present on the surface of the thermally adhesive resin layer 4 may be obtained by causing the lubricant contained in the resin constituting the thermally adhesive resin layer 4 to ooze out, or by coating the lubricant on the surface of the thermally adhesive resin layer 4 .

[0166] In addition, the thickness of the heat-fusible resin layer 4 is not particularly limited as long as the function of sealing the battery element by heat-fusible resin layers can be exerted. From the viewpoint of effectively suppressing the leakage of hydrogen sulfide to the outside, it is preferably 10 μm or more, more preferably 20 μm or more, and further preferably 30 μm or more. In addition, the thickness of the heat-fusible resin layer 4 is, for example, about 100 μm or less, preferably about 85 μm or less, and more preferably about 60 μm or less. As a preferred range, it can be 10 to 100 μm, 10 to 85 μm, 10 to 60 μm, 20 to 100 μm, 20 to 85 μm, 20 to 60 μm, 30 to 100 μm, 30 to 85 μm, and 30 to 60 μm.

[0167] [Adhesive layer 5]

[0168] In the all-solid-state battery outer packaging material 10 of the present invention, the adhesive layer 5 is a layer provided between the barrier layer 3 (or the barrier layer protective film 3 a ) and the heat-fusible resin layer 4 as necessary in order to firmly adhere them.

[0169] The adhesive layer 5 is formed of a resin capable of bonding the barrier layer 3 (or the barrier layer protective film 3a) and the heat-fusible resin layer 4. As the resin used for forming the adhesive layer 5, for example, the same adhesive as exemplified in the adhesive layer 2 can be used.

[0170] As the resin used in forming the adhesive layer 5, a resin containing a polyolefin skeleton, such as a polyolefin and an acid-modified polyolefin, is preferred. The fact that the resin constituting the adhesive layer 5 contains a polyolefin skeleton can be analyzed, for example, by infrared spectroscopy, gas chromatography-mass spectrometry, etc. In addition, when the resin constituting the adhesive layer 5 is analyzed by infrared spectroscopy, it is preferred to detect a peak derived from maleic anhydride. For example, when maleic anhydride-modified polyolefin is measured by infrared spectroscopy, a peak at a wave number of 1760 cm -1 Nearby and wave number 1780cm -1 In the case where the adhesive layer 5 is a layer composed of maleic anhydride-modified polyolefin, when measured by infrared spectroscopy, a peak derived from maleic anhydride is detected near the surface of the adhesive layer 5. However, when the acid modification degree is low, the peak becomes smaller and there is a situation where it cannot be detected. In this case, analysis can be performed by nuclear magnetic resonance spectroscopy.

[0171] As polyolefins, specifically, polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene can be cited; ethylene-α-olefin copolymers; polypropylenes such as homopolymer polypropylene, block copolymers of polypropylene (for example, block copolymers of propylene and ethylene), and random copolymers of polypropylene (for example, random copolymers of propylene and ethylene); propylene-α-olefin copolymers; terpolymers of ethylene-butene-propylene, etc. Among them, polypropylene is preferred. The polyolefin resin in the case of a copolymer may be a block copolymer or a random copolymer. These polyolefin resins may be used alone or in combination of two or more.

[0172] In addition, the polyolefin may also be a cyclic polyolefin. Cyclic polyolefin is a copolymer of an olefin and a cyclic monomer. As the olefin constituting the above-mentioned cyclic polyolefin, for example, ethylene, propylene, 4-methyl-1-pentene, styrene, butadiene, isoprene, etc. can be cited. In addition, as the cyclic monomer constituting the cyclic polyolefin, for example, cyclic olefins such as norbornene can be cited; cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornene can be cited. Among them, preferred cyclic olefins can be cited, and more preferably norbornene.

[0173] Acid-modified polyolefin refers to a polymer modified by block polymerization or graft polymerization of polyolefin with an acid component. As the acid-modified polyolefin, the above-mentioned polyolefin, a copolymer obtained by copolymerizing the above-mentioned polyolefin with a polar molecule such as acrylic acid or methacrylic acid, or a polymer such as a cross-linked polyolefin can also be used. In addition, as the acid component used in the acid modification, for example, carboxylic acids or anhydrides thereof such as maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, and itaconic anhydride can be cited.

[0174] The acid-modified polyolefin may be an acid-modified cyclic polyolefin. The acid-modified cyclic polyolefin refers to a polymer obtained by copolymerizing a part of the monomers constituting the cyclic polyolefin with an acid component, or by block polymerization or graft polymerization of the acid component on the cyclic polyolefin. The acid-modified cyclic polyolefin is the same as described above. In addition, the acid component used in the acid modification is the same as the acid component used in the modification of the above-mentioned polyolefin.

[0175] Preferred examples of the acid-modified polyolefin include polyolefins modified with carboxylic acid or its anhydride, polypropylene modified with carboxylic acid or its anhydride, maleic anhydride-modified polyolefin, and maleic anhydride-modified polypropylene.

[0176] The adhesive layer 5 preferably contains an acid-modified polyolefin from the viewpoint of firmly bonding the barrier layer 3 (or barrier layer protective film 3a) to the heat-fusible resin layer 4. As the acid-modified polyolefin, polyolefin modified with carboxylic acid or its anhydride, polypropylene modified with carboxylic acid or its anhydride, maleic anhydride-modified polyolefin, and maleic anhydride-modified polypropylene are particularly preferred.

[0177] In addition, from the viewpoint of making the thickness of the all-solid battery outer packaging material 10 thin and excellent in shape stability after molding, it is more preferable that the adhesive layer 5 is a cured product of a resin composition containing an acid-modified polyolefin and a curing agent. As the acid-modified polyolefin, the above-mentioned acid-modified polyolefins can be preferably exemplified.

[0178] In addition, the adhesive layer 5 is preferably a cured product of a resin composition comprising an acid-modified polyolefin and at least one selected from a compound having an isocyanate group, a compound having an oxazoline group and a compound having an epoxy group, and is particularly preferably a cured product of a resin composition comprising an acid-modified polyolefin and at least one selected from a compound having an isocyanate group and a compound having an epoxy group. In addition, the adhesive layer 5 preferably comprises at least one selected from polyurethane, polyester and epoxy resin, and more preferably comprises polyurethane and epoxy resin. As polyester, for example, amide ester resin is preferably used. Amidoester resin is usually generated by the reaction of carboxyl and oxazoline groups. The adhesive layer 5 is more preferably a cured product of a resin composition comprising at least one of these resins and the above-mentioned acid-modified polyolefin. In the case of unreacted products of curing agents such as compounds having an isocyanate group, compounds having an oxazoline group, and epoxy resins remaining in the adhesive layer 5, the presence of unreacted products can be confirmed, for example, by a method selected from infrared spectroscopy, Raman spectroscopy, time-of-flight secondary ion mass spectrometry (TOF-SIMS), etc.

[0179] In addition, from the viewpoint of further improving the adhesion between the barrier layer 3 and the adhesive layer 5, the adhesive layer 5 is preferably a cured product of a resin composition containing a curing agent, and the curing agent has at least one selected from an oxygen atom, a heterocyclic ring, a C=N bond, and a COC bond. As a curing agent having a heterocyclic ring, for example, a curing agent having an oxazoline group, a curing agent having an epoxy group, etc. can be cited. In addition, as a curing agent having a C=N bond, a curing agent having an oxazoline group, a curing agent having an isocyanate group, etc. can be cited. In addition, as a curing agent having a COC bond, a curing agent having an oxazoline group, a curing agent having an epoxy group, polyurethane, etc. can be cited. The fact that the adhesive layer 5 is a cured product of a resin composition containing these curing agents can be confirmed, for example, by methods such as gas chromatography-mass spectrometry (GCMS), infrared spectroscopy (IR), time-of-flight secondary ion mass spectrometry (TOF-SIMS), and X-ray photoelectron spectroscopy (XPS).

[0180] There are no particular restrictions on the compound having an isocyanate group. From the viewpoint of effectively improving the adhesion between the barrier layer 3 (or the barrier layer protective film 3a) and the adhesive layer 5, preferred polyfunctional isocyanate compounds can be cited. Polyfunctional isocyanate compounds are not particularly limited as long as they are compounds having two or more isocyanate groups. Specific examples of polyfunctional isocyanate curing agents include pentane diisocyanate (PDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), substances obtained by polymerizing or ureating them, mixtures thereof, or copolymers with other polymers. In addition, adducts, biuret bodies, isocyanurate bodies, etc. can be cited.

[0181] The content of the compound having an isocyanate group in the adhesive layer 5 is preferably in the range of 0.1 to 50% by mass, and more preferably in the range of 0.5 to 40% by mass in the resin composition constituting the adhesive layer 5. This can effectively improve the adhesion between the barrier layer 3 (or the barrier layer protective film 3a) and the adhesive layer 5.

[0182] As long as the compound with oxazoline group is the compound with oxazoline skeleton, it is not particularly limited.As the specific example of the compound with oxazoline group, the compound with polystyrene main chain, the compound with acrylic acid main chain etc. can be enumerated.In addition, as commercially available product, the EPOCROS series etc. that for example Japan Catalyst Co., Ltd. produces can be enumerated.

[0183] The ratio of the compound having an oxazoline group in the adhesive layer 5 is preferably in the range of 0.1 to 50% by mass, and more preferably in the range of 0.5 to 40% by mass in the resin composition constituting the adhesive layer 5. This can effectively improve the adhesion between the barrier layer 3 (or the barrier layer protective film 3a) and the adhesive layer 5.

[0184] As a compound having an epoxy group, for example, an epoxy resin can be cited. As the epoxy resin, there is no particular limitation as long as it is a resin that can form a cross-linked structure using the epoxy group present in the molecule, and a known epoxy resin can be used. As the weight average molecular weight of the epoxy resin, preferably about 50 to 2000, more preferably about 100 to 1000, and further preferably about 200 to 800 can be cited. In addition, in the first invention, the weight average molecular weight of the epoxy resin is a value measured by gel permeation chromatography (GPC) under the condition of using polystyrene as a standard sample.

[0185] Specific examples of the epoxy resin include glycidyl ether derivatives of trimethylolpropane, bisphenol A diglycidyl ether, modified bisphenol A diglycidyl ether, novolac glycidyl ether, glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, etc. The epoxy resin may be used alone or in combination of two or more.

[0186] The proportion of the epoxy resin in the adhesive layer 5 is preferably in the range of 0.1 to 50 mass %, more preferably in the range of 0.5 to 40 mass %, in the resin composition constituting the adhesive layer 5. This can effectively improve the adhesion between the barrier layer 3 (or the barrier layer protective film 3a) and the adhesive layer 5.

[0187] The polyurethane is not particularly limited, and known polyurethanes can be used. The adhesive layer 5 may be, for example, a cured product of a two-component curable polyurethane.

[0188] The ratio of the polyurethane in the adhesive layer 5 is preferably in the range of 0.1 to 50% by mass, and more preferably in the range of 0.5 to 40% by mass, in the resin composition constituting the adhesive layer 5 .

[0189] When the adhesive layer 5 is a cured product of a resin composition comprising the above-mentioned acid-modified polyolefin and at least one selected from a compound having an isocyanate group, a compound having an oxazoline group and an epoxy resin, the acid-modified polyolefin functions as a main agent, and the compound having an isocyanate group, the compound having an oxazoline group and the compound having an epoxy group respectively function as a curing agent.

[0190] The thickness of the adhesive layer 5 is preferably about 50 μm or less, about 40 μm or less, about 30 μm or less, about 20 μm or less, or about 5 μm or less, and preferably about 0.1 μm or more, or about 0.5 μm or more. The range of the thickness is preferably about 0.1 to 50 μm, about 0.1 to 40 μm, about 0.1 to 30 μm, about 0.1 to 20 μm, about 0.1 to 5 μm, about 0.5 to 50 μm, about 0.5 to 40 μm, about 0.5 to 30 μm, about 0.5 to 20 μm, or about 0.5 to 5 μm. More specifically, in the case of a cured product of the adhesive, acid-modified polyolefin, and curing agent exemplified in the adhesive layer 2, the thickness is preferably about 1 to 10 μm, and more preferably about 1 to 5 μm. When polyolefin or acid-modified polyolefin is used, the thickness is preferably about 2 to 50 μm, and more preferably about 10 to 40 μm. When the adhesive layer 5 is a cured product of a resin composition containing an adhesive or an acid-modified polyolefin and a curing agent as exemplified in the adhesive layer 2, the adhesive layer 5 can be formed, for example, by applying the resin composition and curing it by heating or the like. When polyolefin or acid-modified polyolefin is used, it can be formed, for example, by extrusion molding.

[0191] [Surface covering]

[0192] The outer packaging material 10 of the present invention can be provided with a surface covering layer 6 on the substrate layer 1 (on the side of the substrate layer 1 opposite to the barrier layer 3) as required for the purpose of improving at least one of designability, damage resistance, and formability. The surface covering layer 6 is a layer located on the outermost side of the outer packaging material 10 when the outer packaging material 10 is used to assemble an all-solid battery.

[0193] The surface coating layer 6 can be formed of a resin such as polyvinylidene chloride, polyester, polyurethane, acrylic resin, epoxy resin, etc.

[0194] When the resin forming the surface coating layer 6 is a curable resin, the resin may be either a one-component curable resin or a two-component curable resin, preferably a two-component curable resin. Examples of the two-component curable resin include two-component curable polyurethane, two-component curable polyester, and two-component curable epoxy resin. Among them, two-component curable polyurethane is preferred.

[0195] As two-component curable polyurethane, for example, polyurethane comprising a main agent containing a polyol compound and a curing agent containing an isocyanate compound can be cited. Two-component curable polyurethane preferably using polyols such as polyester polyols, polyether polyols and acrylic polyols as a main agent and aromatic or aliphatic polyisocyanates as a curing agent can be cited. In addition, as a polyol compound, it is preferred to use a polyester polyol having a hydroxyl group in the side chain in addition to the hydroxyl group at the end of the repeating unit.

[0196] The surface coating layer 6 may contain the above-mentioned lubricant, anti-blocking agent, matting agent, flame retardant, antioxidant, tackifier, antistatic agent and other additives on at least one of the surface and the inside of the surface coating layer 6 as required, depending on the functionality of the surface coating layer 6 or its surface. As additives, for example, microparticles with an average particle size of about 0.5 nm to 5 μm can be cited. The average particle size of the additive is the median particle size measured by a laser diffraction / scattering particle size distribution measuring device.

[0197] The additive may be any of an inorganic substance and an organic substance. In addition, there is no particular limitation on the shape of the additive, and examples thereof include spherical, fibrous, plate-like, amorphous, and flaky shapes.

[0198] As the specific example of additive, talc, silicon dioxide, graphite, kaolin, montmorillonite, mica, hydrotalcite, silica gel, zeolite, aluminum hydroxide, magnesium hydroxide, zinc oxide, magnesium oxide, aluminum oxide, neodymium oxide, antimony oxide, titanium oxide, cerium oxide, calcium sulfate, barium sulfate, calcium carbonate, calcium silicate, lithium carbonate, calcium benzoate, calcium oxalate, magnesium stearate, aluminum oxide, carbon black, carbon nanotube, high melting point nylon, acrylic resin, cross-linked acrylic acid, cross-linked styrene, cross-linked polyethylene, benzoguanamine, gold, aluminum, copper, nickel, etc. can be enumerated. One kind of additive can be used alone, and two or more kinds can be used in combination. Among these additives, from the viewpoints of dispersion stability, cost, etc., preferred silicon dioxide, barium sulfate, titanium oxide can be enumerated. In addition, various surface treatments such as insulation treatment and high dispersibility treatment can also be implemented on the surface of the additive.

[0199] The method of forming the surface coating layer 6 is not particularly limited, and an example thereof includes a method of applying a resin for forming the surface coating layer 6. When an additive is added to the surface coating layer 6, the resin mixed with the additive may be applied.

[0200] The thickness of the surface coating layer 6 is not particularly limited as long as the above-mentioned function as the surface coating layer 6 can be exhibited, and is, for example, about 0.5 to 10 μm, preferably about 1 to 5 μm.

[0201] Regarding the method for manufacturing the outer packaging material 10 for all-solid-state batteries, there are no particular restrictions as long as a laminated body formed by stacking the layers possessed by the outer packaging material 10 for all-solid-state batteries of the present invention can be obtained, and a method including the steps of stacking at least a base material layer 1, a barrier layer 3 and a thermally fusible resin layer 4 in sequence from the outside can be cited.

[0202] An example of a method for manufacturing the outer packaging material 10 for an all-solid-state battery of the present invention is as follows. First, a substrate layer 1, an adhesive layer 2, and a barrier layer 3 are formed (a laminated body (hereinafter, sometimes also referred to as "laminated body A") in sequence with a barrier layer protective film 3a and / or laminated thereon as needed). The formation of the laminated body A can be specifically carried out by the following dry lamination method: the adhesive used in the formation of the adhesive layer 2 is applied to the substrate layer 1 or to the barrier layer 3 whose surface has been chemically converted as needed by a coating method such as a gravure coating method and a roll coating method, and after drying it, the barrier layer 3 or the substrate layer 1 is laminated to cure the adhesive layer 2.

[0203] Next, the heat-fusible resin layer 4 is laminated on the barrier layer 3 of the laminate A. When the heat-fusible resin layer 4 is laminated directly on the barrier layer 3, the resin component constituting the heat-fusible resin layer 4 may be coated on the barrier layer 3 of the laminate A by a gravure coating method, a roll coating method, or the like. In addition, when an adhesive layer 5 is provided between the barrier layer 3 and the heat-fusible resin layer 4, examples thereof include: (1) a method of laminating the adhesive layer 5 and the heat-fusible resin layer 4 on the barrier layer 3 of the laminate A by coextrusion (coextrusion lamination method); (2) a method of separately forming a laminate having the adhesive layer 5 and the heat-fusible resin layer 4 laminated thereon, and laminating it on the barrier layer 3 of the laminate A by a heat lamination method; (3) a method of laminating the adhesive layer 5 and the heat-fusible resin layer 4 on the barrier layer 3 of the laminate A by extrusion. (4) a method in which a molten adhesive layer 5 is poured between the barrier layer film 3 of the laminate A and the hot-melt adhesive layer 4 which is pre-formed in sheet form, and the laminate A and the hot-melt adhesive layer 4 are bonded together via the adhesive layer 5 (sandwich lamination method), etc.

[0204] When a surface covering layer is provided, the surface covering layer is laminated on the surface of the substrate layer 1 on the side opposite to the barrier layer 3. The surface covering layer can be formed, for example, by coating the above-mentioned resin for forming the surface covering layer on the surface of the substrate layer 1. The order of the step of laminating the barrier layer 3 on the surface of the substrate layer 1 and the step of laminating the surface covering layer on the surface of the substrate layer 1 is not particularly limited. For example, after the surface covering layer is formed on the surface of the substrate layer 1, the barrier layer 3 may be formed on the surface of the substrate layer 1 on the side opposite to the surface covering layer.

[0205] As described above, a laminated body is formed which has, in order, a surface covering layer provided as required / base material layer 1 / adhesive layer 2 provided as required / barrier layer 3 whose surface is chemically converted as required / adhesive layer 5 provided as required / thermo-fusible resin layer 4. In order to strengthen the adhesion between the adhesive layer 2 provided as required and the adhesive layer 5, a heating treatment such as a hot roll contact type, a hot air type, a near infrared type, or a far infrared type may be further performed. As the conditions for such a heating treatment, for example, a heating treatment at about 150 to 250° C. for about 1 to 5 minutes may be mentioned.

[0206] In the all-solid battery outer packaging material 10, for each layer constituting the laminate, in order to improve or stabilize the film forming properties, lamination processing, and the adaptability to the secondary processing (bag forming, embossing molding) of the final product as required, surface activation treatments such as corona treatment, sandblasting, oxidation treatment, and ozone treatment can be performed. For example, by subjecting at least one surface of the substrate layer 1 to corona treatment, the film forming properties, lamination processing, and the adaptability to the secondary processing of the final product can be improved or stabilized. In addition, for example, by subjecting the surface of the substrate layer 1 on the side opposite to the barrier layer 3 to corona treatment, the printing adaptability of the ink on the surface of the substrate layer 1 can be improved.

[0207] Example

[0208] The present invention will be described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.

[0209] <Hydrogen sulfide permeation rate of resin constituting thermally adhesive resin layer>

[0210] like Fig. 9 As shown in the schematic diagram, under the test temperature (approximately 23±5°C), each resin film (thickness recorded in Table 1) used as a heat-fusible resin layer for the outer packaging material of the all-solid-state battery was used as a sample, and the hydrogen sulfide permeation amount of the resin constituting the heat-fusible resin layer was obtained according to the following steps. The results are shown in Table 1.

[0211] (1) The sample A is placed between the separable flask upper portion 100 and the separable flask lower portion 200 .

[0212] (2) Nitrogen gas was introduced at 50 ml / min from the vent 101 of the upper portion 100 of the separable flask, and hydrogen sulfide gas (H2S concentration: 20±5 volume ppm / N2) was introduced at 50 ml / min from the vent 201 of the lower portion 200 of the separable flask.

[0213] (3) Under the following sampling conditions, a resin bag was connected to the vent port 101 of the upper portion 100 of the separable flask, and 0.5 L of sample gas was collected over 10 minutes.

[0214] Sampling conditions: After 48 hours, a total of 1 sampling

[0215] (4) The concentration of the sample gas trapped in the resin bag was measured using a gas chromatograph-flame photometric detector (GC-FPD).

[0216] (5) Based on the sample gas concentration (volume ppb) obtained by measurement, the permeation amount per hour (nL / hr) was calculated using the following calculation formula 1, and the permeability (cc / m 2 ·day). The unit is converted to cc·mm / cm 2 ·sec·cmHg.

[0217] Calculation formula 1: Permeation (nL / hr) = concentration (volume ppb ≈ nL / L) × gas volume collected per hour (L / hr)

[0218] Since the test flow rate is 50mL / min, the amount of gas collected per hour is 3L.

[0219] Calculation formula 2: Transmittance (cc / m 2 ·day)=permeation (nL / hr)×24(hr) / 10 6 / Effective test area (m 2 )

[0220] The effective test area is 0.00465m2 using the opening area of ​​the removable flask 2 .

[0221] <Every 1m 2 Water vapor transmission rate>

[0222] The hydrogen sulfide permeation rate per m of each resin film used in the measurement was measured by the following method. 2 Water vapor transmission rate (single-sided area) (g / m 2 / 24h). The measurement was conducted using a water vapor transmission rate measuring device based on the isobaric method (PERMATRAN manufactured by MOCON) under the conditions of a temperature of 40°C, a relative humidity of 90%, a measurement period of 24 hours, and a measurement area of ​​8cmφ in accordance with the method specified in ISO15106-5 2008. 2 The water vapor transmission rate is converted into m using the ISO water vapor transmission rate measurement method. 2 The results are shown in Table 1.

[0223] <Evaluation of hydrogen sulfide leakage when used as outer packaging material>

[0224] For two sheets of outer packaging materials (3.00 mm long and 1.50 mm wide in a plan view) composed of a laminated body in which a base layer (30 μm) / adhesive layer (3 μm) / barrier layer (40 μm) / thermo-melting resin layer (thickness of the resin film described in Table 1) is laminated in this order, it is assumed that the peripheral edge (4 sides) is heat-fused with a width of 3 mm (the thickness of each heat-melting resin layer is reduced to 95% in the heat-melting portion) of the all-solid-state battery, and the hydrogen sulfide leakage (hydrogen sulfide permeation cc) from the heat-melting resin layer for 10 years is calculated using the value of hydrogen sulfide permeation obtained from the above <Hydrogen sulfide permeation of the resin constituting the heat-melting resin layer>. In this calculation, the hydrogen sulfide permeation of the barrier layer is assumed to be 0 cc, and the calculation is performed on the assumption that hydrogen sulfide permeates from the heat-melting portion of the heat-melting resin layer. The results are shown in Table 1.

[0225] [Table 1]

[0226]

[0227] [Example 1]

[0228] As a substrate layer, a laminated film is prepared in which a polyethylene terephthalate film (12 μm) / adhesive layer (2-component curable polyurethane adhesive (polyol compound and aromatic isocyanate compound), thickness 3 μm) / biaxially stretched nylon film (thickness 15 μm) is laminated in sequence. In addition, a barrier layer composed of an aluminum alloy foil (JIS H4160:1994A8021H-O, thickness 40 μm) is prepared. A chemical conversion treatment is performed on both sides of the barrier layer by the method described later to form a barrier layer protective film (thickness 10 nm). Then, the barrier layer and the substrate layer are laminated by a dry lamination method. Specifically, a 2-component curable polyurethane adhesive (polyol compound and aromatic isocyanate compound) is applied to one surface of the barrier layer protective film formed on the surface of the barrier layer to form an adhesive layer (thickness 3 μm after curing). Next, after laminating the adhesive layer and the biaxially stretched nylon film, an aging treatment was performed to prepare a laminate of substrate layer / adhesive layer / barrier layer protective film / barrier layer / barrier layer protective film. Next, a two-component curable polyurethane adhesive (polyol compound and aromatic isocyanate compound, thickness after curing 3 μm) as an adhesive layer and a polytetrafluoroethylene film (thickness 50 μm) in Table 1 as a heat-fusible resin layer were laminated on the barrier layer protective film of the obtained laminate, and an adhesive layer / heat-fusible resin layer was laminated. Next, the obtained laminate is aged and heated to obtain an outer packaging material composed of a laminate having a substrate layer (polyethylene terephthalate film (12 μm) / adhesive layer (3 μm) / biaxially stretched nylon film (15 μm)) / adhesive layer (3 μm) / barrier layer protective film (10 nm) / barrier layer (40 μm) / barrier layer protective film (10 nm) / adhesive layer (3 μm) / thermo-fusible resin layer (50 μm) laminated in sequence.

[0229] The barrier layer protective films on both sides of the barrier layer were formed as follows: a treatment liquid containing 43 parts by mass of an aminophenol polymer, 16 parts by mass of chromium fluoride, and 13 parts by mass of phosphoric acid relative to 100 parts by mass of water was prepared, the treatment liquid was applied to both sides of the barrier layer (film thickness after drying was 10 nm), and the surface temperature of the barrier layer was heated and dried for about 3 to 6 seconds at a temperature of about 190 to 230° C.

[0230] [Example 2]

[0231] As the heat-fusible resin layer, the polyethylene terephthalate film (thickness 50 μm) in Table 1 was used. Otherwise, the same operation as in Example 1 was carried out to obtain an outer packaging material consisting of a laminated body in which base layers (polyethylene terephthalate film (12 μm) / adhesive layer (3 μm) / biaxially stretched nylon film (15 μm)) / adhesive layer (3 μm) / barrier layer protective film (10 nm) / barrier layer (40 μm) / barrier layer protective film (10 nm) / adhesive layer (3 μm) / heat-fusible resin layer (40 μm) were laminated in this order.

[0232] [Example 3]

[0233] The same operation as in Example 1 was carried out except that no barrier layer protective film was formed on the surface of the barrier layer, thereby obtaining an outer packaging material comprising a laminated body in which base layer (polyethylene terephthalate film (12 μm) / adhesive layer (3 μm) / biaxially stretched nylon film (15 μm)) / adhesive layer (3 μm) / barrier layer (40 μm) / adhesive layer (3 μm) / thermofusible resin layer (50 μm) were laminated in this order.

[0234] [Example 4]

[0235] The same operation as in Example 2 was carried out except that no barrier layer protective film was formed on the surface of the barrier layer, thereby obtaining an outer packaging material comprising a laminated body in which base layer (polyethylene terephthalate film (12 μm) / adhesive layer (3 μm) / biaxially stretched nylon film (15 μm)) / adhesive layer (3 μm) / barrier layer (40 μm) / adhesive layer (3 μm) / thermo-fusible resin layer (50 μm) were laminated in this order.

[0236] <Time-of-flight secondary ion mass spectrometry>

[0237] The barrier layer protective film was analyzed in the following manner. First, the barrier layer and the adhesive layer were peeled off. At this time, they were not physically peeled off using water or an organic solvent, an acid or alkali aqueous solution, or the like. After the barrier layer and the adhesive layer were peeled off, since the adhesive layer remained on the surface of the barrier layer, the remaining adhesive layer was removed by etching using Ar-GCIB. The surface of the barrier layer obtained in this way was analyzed by time-of-flight secondary ion mass spectrometry. - PO2 - and PO3 - The peak intensity P CrPO4 , P PO2 , P PO3 , peak intensity P PO2 Relative to the peak intensity P CrPO4 Ratio P PO2 / CrPO4 , peak intensity P PO3Relative to the peak intensity P CrPO4 Ratio P PO3 / CrPO4 They are shown in Table 1. In Examples 3 and 4, no barrier layer protective film is formed on the surface of the barrier layer. Therefore, in Table 1, regarding CrPO4 - The peak intensity P CrPO4 Items with “-” are indicated.

[0238] The details of the measurement device and measurement conditions of the time-of-flight secondary ion mass spectrometry are as follows. Measurement device: Time-of-flight secondary ion mass spectrometry device TOF.SIMS5 manufactured by ION-TOF

[0239] (Measurement conditions)

[0240] Primary ion: Doubly charged ion of bismuth cluster (Bi3 ++ )

[0241] 1st ion acceleration voltage: 30kV

[0242] Mass range (m / z): 0~1500

[0243] Measuring range: 100μm×100μm

[0244] Scan number: 16 scan / cycle

[0245] Number of pixels (1 side): 256 pixels

[0246] Etching ions: Ar gas cluster ion beam (Ar-GCIB)

[0247] Etching ion acceleration voltage: 5.0kV

[0248] <Evaluation of barrier layer degradation caused by confinement under high pressure pressing>

[0249] A hole of φ1 mm is opened on the heat-fusible resin layer side of the outer packaging material in such a way that the surface of the barrier layer protective film is exposed. Specifically, in the above-mentioned Examples 1 to 4, as the heat-fusible resin layer, a heat-fusible resin layer with a hole of φ1 mm opened in such a way that the surface of the barrier layer protective film is exposed is used to make the outer packaging material. Each of these outer packaging materials is used as a test piece, and high pressure pressing (50 MPa) is applied in a state where a sulfide solid electrolyte (Li2S:P2S5=75:25, thickness 300μm) is arranged between the test piece and the lithium indium alloy (LiIn alloy). At this time, the sulfide solid electrolyte is arranged in a portion of the outer packaging material where a hole of φ1 mm is opened. In Examples 3 and 4, no barrier layer protective film is provided, so that the surface of the barrier layer is exposed. In this state, a voltage of 0.53V is applied between the barrier layer and the LiIn alloy of the test piece and left to stand for 1 hour. After 1 hour, the surface of the barrier layer at the portion of the test piece where the hole of φ1 mm was opened was observed with a microscope to confirm whether an alloy was formed on the surface of the barrier layer. The case where no alloy was formed on the surface of the barrier layer was evaluated as A, and the case where an alloy was formed on the surface of the barrier layer was evaluated as C. The results are shown in Table 2.

[0250] [Table 2]

[0251]

[0252] As described above, the present invention provides the following aspects of the invention.

[0253] Item 1. An all-solid battery outer packaging material for an all-solid battery containing a sulfide solid electrolyte material, the all-solid battery outer packaging material comprising a laminate having at least a substrate layer, a barrier layer and a heat-fusible resin layer in order from the outside, the all-solid battery outer packaging material being characterized in that: the hydrogen sulfide permeation amount of the resin constituting the heat-fusible resin layer is 1.0×10 -9 cc mm / cm 2 ·sec·cmHg or less.

[0254] Item 2. The all-solid-state battery outer casing material according to Item 1, wherein the thickness of the thermally fusible resin layer is 10 μm or more.

[0255] Item 3. The all-solid battery outer casing material according to Item 1 or 2, wherein the base layer comprises a polyester, an adhesive layer, and a polyamide in this order from the outside.

[0256] Item 4. The all-solid-state battery outer packaging material according to Item 1 or 2, wherein the base layer is composed of a single layer of a polyester resin.

[0257] Item 5. The all-solid battery outer casing material according to any one of Items 1 to 4, wherein the resin constituting the thermally fusible resin layer is a polyester or a fluororesin.

[0258] Item 6. The all-solid battery outer packaging material according to any one of Items 1 to 5, wherein the laminate has a barrier layer protective film formed on the surface of the barrier layer, and when the barrier layer protective film is analyzed using time-of-flight secondary ion mass spectrometry, the PO3 - The peak intensity P PO3 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO3 / CrPO4 In the range of 6 to 120.

[0259] Item 7. A total solid battery packaging body, characterized in that it is formed by molding the total solid battery outer packaging material according to any one of Items 1 to 6.

[0260] Item 8. An all-solid-state battery, wherein a battery element comprising at least a single cell is housed in a packaging body formed of an all-solid-state battery outer packaging material, wherein the single cell comprises a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer stacked between the positive electrode active material layer and the negative electrode active material layer, wherein the solid electrolyte layer comprises a sulfide solid electrolyte material, and the all-solid-state battery outer packaging material comprises a laminate having at least a substrate layer, a barrier layer, and a heat-fusible resin layer in this order from the outside, and the hydrogen sulfide permeability of the resin constituting the heat-fusible resin layer is 1.0×10 -9 cc mm / cm 2 ·sec·cmHg or less.

[0261] Item 9. A method for producing an outer packaging material for an all-solid-state battery, the outer packaging material for an all-solid-state battery being used for an all-solid-state battery containing a sulfide solid electrolyte material, the method comprising the step of laminating at least a substrate layer, a barrier layer, and a heat-fusible resin layer in order from the outside to obtain a laminate, wherein the hydrogen sulfide permeability of the resin constituting the heat-fusible resin layer is 1.0×10 -9 cc mm / cm 2 ·se c·cmHg or less.

[0262] Description of Reference Numerals

[0263] 1 substrate layer, 2 adhesive layer, 3 barrier layer, 3a, 3b barrier layer protective film, 4 heat-fusible resin layer, 5 adhesive layer, 10 outer packaging material for all-solid-state battery, 20 negative electrode layer, 21 negative electrode active material layer, 22 negative electrode collector, 30 positive electrode layer, 31 positive electrode active material layer, 32 positive electrode collector, 40 solid electrolyte layer, 50 single cell, 60 terminal, 70 all-solid-state battery.

Claims

1. An outer packaging material for an all-solid-state battery, which is used for an all-solid-state battery containing a sulfide solid electrolyte material, the outer packaging material for an all-solid-state battery being composed of a laminate having at least a substrate layer, a barrier layer and a heat-fusible resin layer in order from the outside, the outer packaging material for an all-solid-state battery being characterized in that: The heat-fusible resin layer includes at least one of polyester and fluororesin. The hydrogen sulfide permeation rate of the resin constituting the thermally fusible resin layer is 1.0×10 -9 cc mm / cm 2 ·sec·cmHg or less.

2. The outer packaging material for an all-solid-state battery according to claim 1, characterized in that: The thickness of the thermally fusible resin layer is 10 μm or more.

3. The outer packaging material for an all-solid-state battery according to claim 1 or 2, characterized in that: The base material layer has polyester, an adhesive layer, and polyamide in this order from the outside.

4. The outer packaging material for an all-solid-state battery according to claim 1 or 2, characterized in that: The substrate layer is composed of a single layer of polyester resin.

5. The all-solid battery outer packaging material according to any one of claims 1 to 4, characterized in that: The resin constituting the thermally fusible resin layer is polyester or fluororesin.

6. The all-solid battery outer packaging material according to any one of claims 1 to 5, characterized in that: The laminate has a barrier layer protection film formed on the surface of the barrier layer, When the barrier layer protective film was analyzed using time-of-flight secondary ion mass spectrometry, the PO3 - The peak intensity P PO3 Relative to CrPO4 - The peak intensity P CrPO4 Ratio P PO3 / CrPO4 In the range of 6 to 120.

7. A package for an all-solid-state battery, characterized in that: The all-solid-state battery packaging material is formed by molding the all-solid-state battery packaging material according to any one of claims 1 to 6.

8. An all-solid-state battery, wherein a battery element including at least a single cell is housed in a packaging body formed of an outer packaging material for an all-solid-state battery, wherein the single cell includes a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer stacked between the positive electrode active material layer and the negative electrode active material layer, wherein the all-solid-state battery is characterized in that: The solid electrolyte layer comprises a sulfide solid electrolyte material, The all-solid-state battery outer packaging material is composed of a laminate having at least a base layer, a barrier layer and a heat-fusible resin layer in order from the outside, The heat-fusible resin layer includes at least one of polyester and fluororesin. The hydrogen sulfide permeation rate of the resin constituting the thermally fusible resin layer is 1.0×10 -9 cc mm / cm 2 ·sec·cmHg or less.

9. A method for producing an outer packaging material for an all-solid-state battery, wherein the outer packaging material for an all-solid-state battery is used for an all-solid-state battery containing a sulfide solid electrolyte material, wherein the method for producing an outer packaging material for an all-solid-state battery is characterized by: The method comprises the steps of laminating at least a base material layer, a barrier layer and a heat-fusible resin layer in order from the outside to obtain a laminated body, The heat-fusible resin layer includes at least one of polyester and fluororesin. The hydrogen sulfide permeation rate of the resin constituting the thermally fusible resin layer is 1.0×10 -9 cc mm / cm 2 ·sec·cmHg or less.