Diaphragm and battery

By introducing specific compounds into the battery separator to form more ion channels, the safety hazards and insufficient cycling performance caused by excessive internal resistance of the battery are solved, and a battery with lower internal resistance, higher safety and longer life is achieved. .

CN118920020APending Publication Date: 2024-11-08ZHUHAI COSMX BATTERY CO LTD

Patent Information

Application Number
CN202411145462.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-07-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the high-speed cycle, existing batteries are prone to excessive temperature rise due to excessive battery internal resistance, causing safety accidents, such as fire or explosion, and insufficient circulation performance.

Method used

By introducing specific compounds into the separator, more ‘ion channels’ are formed to improve the wettability and conduction consistency of the separator, thereby reducing the internal resistance and safety risks of the battery.

Benefits of technology

It achieves lower internal resistance of the battery, improves cycle performance and safety, extends the battery life, shortens production time and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118920020A_ABST
    Figure CN118920020A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a diaphragm and a battery comprising the diaphragm. The diaphragm comprises a base material layer and a heat-resistant layer, the heat-resistant layer comprises ceramic particles and a first binder, the ceramic particles have a core-shell structure, a shell material of the ceramic particles comprises a first polymer, a first monomer has a structure represented by a formula (I) or a formula (II), R1 and R2 are respectively and independently selected from H,-CnNR3 and-CnNR4R5, and n is an integer of 0-4; nR3 is a 4-7-membered heterocyclic ring, R3 contains 0-2 oxygen atoms and / or 0-2 nitrogen atoms, and the balance is carbon atoms; a grafting group R6 exists or does not exist on R3, R6 is-CmOH, and m is an integer of 0-2; and R4 and R5 are respectively and independently aliphatic chains of C1-C4. The diaphragm can realize a lower ionic conductivity deviation ratio; and the battery has lower resistance, better cycle performance and higher safety. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a diaphragm and a battery comprising the diaphragm. Background Art

[0002] In recent years, batteries have been widely used in smart phones, tablets, smart wearables, power tools, electric vehicles, etc. With the widespread use of batteries, consumers' demands for battery life and application safety are increasing, which requires batteries to have a long cycle life and high safety performance.

[0003] At present, there are many potential safety hazards in the use of batteries. For example, after the battery has been used for a period of time, during the cycle process, especially the high-rate cycle process, the internal resistance of the battery is too high, causing the internal temperature of the battery to rise too high, which can easily lead to serious safety accidents, fires or even explosions.

[0004] Therefore, it is very important to invent a battery with lower internal resistance, which is safer and has better cycle performance. Summary of the invention

[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a diaphragm and a battery comprising the diaphragm. The diaphragm of the present invention has high wettability and can achieve a lower ion conductivity deviation ratio; the battery obtained by the diaphragm of the present invention has lower resistance, thus having better cycle performance and higher safety.

[0006] The inventors of the present invention have found that the internal resistance of the battery can be reduced by increasing the wettability of the separator.

[0007] After further in-depth research, the inventors of the present invention found that in order to increase the wettability of the diaphragm, the diaphragm can be modified with specific compounds to form more "ion channels" on the diaphragm instead of relying on the inherent pore structure in the diaphragm to conduct ions; these "ion channels" have a guiding effect on ions, thereby increasing the speed of ions passing through the diaphragm on the one hand, and on the other hand, improving the consistency of ions conducted by the diaphragm, making the ion conductivity on the diaphragm more uniform. After a lot of in-depth research, the inventors of the present invention screened out specific compounds that have a good modification effect on the diaphragm.

[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a membrane, wherein the membrane contains a first monomer and / or a first polymer, wherein the monomer of the first polymer is a first monomer;

[0009] The first monomer has a structure represented by formula (I) or formula (II),

[0010]

[0011] Among them, R 1 and R 2 Each independently selected from H, -C n NR 3 and -C n NR 4 R 5 , n is an integer from 0 to 4; NR 3 is a 4-7 membered heterocyclic ring, R 3 Contains 0-2 oxygen atoms and / or 0-2 nitrogen atoms, and the rest are carbon atoms; R 3 The presence or absence of a grafted group R 6 , R 6 For -C m OH, m is an integer from 0 to 2; R 4 and R 5 Each is independently a C1-C4 aliphatic chain.

[0012] A second aspect of the present invention provides a battery, wherein the separator of the battery is the separator described in the first aspect of the present invention.

[0013] Through the above technical solution, the present invention has at least the following advantages compared with the prior art:

[0014] (1) The diaphragm of the present invention has good wettability and fast ion conduction speed;

[0015] (2) The diaphragm of the present invention has good consistency in the conduction ions and a low deviation ratio of ionic conductivity;

[0016] (3) The internal current density of the battery of the present invention is consistent;

[0017] (4) The internal resistance of the battery of the present invention is low;

[0018] (5) The battery of the present invention has a high capacity retention rate and a long cycle life;

[0019] (6) The battery of the present invention has good safety performance;

[0020] (7) Due to the improvement of the wettability of the diaphragm, the aging time is also shortened, so that the production efficiency of the battery of the present invention is high and the production cost is low.

[0021] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0022] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0023] A first aspect of the present invention provides a membrane, wherein the membrane contains a first monomer and / or a first polymer, and the monomers of the first polymer include a first monomer;

[0024] The first monomer has a structure represented by formula (I) or formula (II),

[0025]

[0026]

[0027] Among them, R 1 and R 2 Each independently selected from H, -C n NR 3 and -C n NR 4 R 5 , n is an integer from 0 to 4; NR 3 is a 4-7 membered heterocyclic ring, R 3 Contains 0-2 oxygen atoms and / or 0-2 nitrogen atoms, and the rest are carbon atoms; R 3 The presence or absence of a grafted group R 6 , R 6 For -C m OH, m is an integer from 0 to 2; R 4 and R 5 Each is independently a C1-C4 aliphatic chain.

[0028] In the present invention, by adding the first monomer of the above-mentioned specific structure and / or the first polymer obtained by polymerization thereof into the separator, the separator can achieve a lower ion conductivity deviation ratio, better wettability and lower battery internal resistance than the prior art. In order to further improve the effect, one or more of the technical features can be further optimized.

[0029] The monomers of the first polymer may include a first monomer.

[0030] The first polymer can be obtained by polymerizing the first monomer, and the polymerization can be homopolymerization of the first monomer or copolymerization of the first monomer and other monomers. In a specific embodiment of the present invention, when other monomers are not mentioned, the first polymer refers to a polymer obtained by homopolymerization of the first monomer. However, it is understood that the polymer obtained by copolymerization of the monomers of conventional materials used in battery separators with the first monomer is also within the protection scope of the first polymer of the present invention.

[0031] The separator may contain only the first monomer, only the first polymer, or both the first monomer and the first polymer.

[0032] The first monomer has a structure of formula (I) or a structure of formula (II). As can be seen from the structural formula, the first monomer has two centrosymmetric benzene rings and at least four hydroxyl groups.

[0033] R 1 and R 2 The same or different, each independently selected from H, -C n NR 3 and -C n NR 4 R 5 .

[0034] Wherein, n represents the number of carbon atoms connecting the benzene ring and the nitrogen atom, and n can be an integer of 0-4 (such as 0, 1, 2, 3), preferably 1 or 2.

[0035] -C n NR 3 The N atom and R 3 The groups together form a ring structure, which can be a 4-7 membered heterocycle (such as a 4-membered, 5-membered, 6-membered, 7-membered) and is preferably a 5-membered heterocycle or a 6-membered heterocycle.

[0036] R 3 The group may be composed entirely of carbon atoms (excluding hydrogen atoms), or may contain 0-2 (eg, 0, 1, 2) oxygen atoms and / or 0-2 (eg, 0, 1, 2) nitrogen atoms.

[0037] In a specific embodiment, R 3 The radical consists of multiple carbon atoms and one oxygen atom.

[0038] In another specific embodiment, R 3 The radical is composed entirely of carbon atoms.

[0039] R 3 There may be no grafting groups.

[0040] According to a specific embodiment, R 3 There may also be a grafted group R 6 , R 6 For -C m OH, m is an integer of 0-2 (eg, 0, 1, 2).

[0041] Preferably, the grafting group R 6 The grafting site is NR 3 It is opposite to the N atom in the heterocyclic ring.

[0042] Listed, -C n NR 3 Including but not limited to the following structures:

[0043]

[0044] -C n NR 4 R 5 There is no ring structure in R 4 and R 5 The same or different, each independently being a C1-C4 fatty chain.

[0045] In a specific embodiment, R 4 and R 5 Each is independently selected from methyl and ethyl.

[0046] For example, the first monomer includes but is not limited to the following structure:

[0047]

[0048] Any position where the first monomer and / or the first polymer exists in the separator falls within the protection scope of the present invention.

[0049] According to a specific embodiment, the diaphragm includes a substrate layer and an optional heat-resistant layer and / or an optional adhesive layer (the term "optionally" means that it may or may not be present); the heat-resistant layer covers one side or both sides of the substrate layer; the adhesive layer covers the surface of the heat-resistant layer, and / or the adhesive layer covers the surface of the substrate layer. In one example, the diaphragm includes an adhesive layer, a heat-resistant layer, a substrate layer, a heat-resistant layer, and an adhesive layer arranged in sequence. In another example, the diaphragm includes an adhesive layer, a substrate layer, a heat-resistant layer, and an adhesive layer arranged in sequence.

[0050] At least one of the substrate layer, the heat-resistant layer and the adhesive layer contains the first monomer and / or the first polymer. The substrate layer, the heat-resistant layer and the adhesive layer may all contain the first monomer and / or the first polymer, or only one or more of them may contain the first monomer and / or the first polymer. Therefore, at least one of the substrate layer, the heat-resistant layer and the adhesive layer contains the first monomer and / or the first polymer, which falls within the protection scope of the present invention, can achieve the purpose of the present invention, and has a good technical effect. In this article, the term "a layer" refers to a layer rather than a type of layer. For example, when the adhesive layer contains the first monomer and / or the first polymer, it is not required to be contained in both the upper and lower adhesive layers.

[0051] In one example, at least the substrate layer contains the first monomer and / or the first polymer.

[0052] In one example, the substrate layer and the heat-resistant layer and / or the adhesive layer contain the first monomer and / or the first polymer.

[0053] In one example, the substrate layer contains the first monomer and / or the first polymer.

[0054] In one example, the heat-resistant layer contains the first monomer and / or the first polymer.

[0055] In one example, the coating layer contains the first monomer and / or the first polymer.

[0056] In one example, the substrate layer and the adhesive layer contain the first monomer and / or the first polymer.

[0057] In one example, the substrate layer and the heat-resistant layer contain the first monomer and / or the first polymer.

[0058] In one example, the heat-resistant layer and the adhesive layer contain the first monomer and / or the first polymer.

[0059] In one example, the substrate layer, the heat-resistant layer, and the adhesive layer all contain the first monomer and / or the first polymer.

[0060] In the same layer, the first monomer and / or the first polymer may contain only one structure, or may contain the first monomer and / or the first polymer of multiple structures.

[0061] The form in which the first monomer and / or the first polymer exist in the separator may not be particularly limited, and may exist in the separator in the form of, for example, doping (blending), grafting, partial coating, etc.

[0062] In a specific embodiment, the material of the substrate layer is a material obtained by grafting and modifying a base material with the first monomer.

[0063] In one example, relative to 100 parts by weight of the base material, the content of the first monomer can be 0.1-10 parts by weight (e.g., 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 parts by weight), preferably 0.5-5 parts by weight.

[0064] The matrix material may be a conventional material used as a diaphragm substrate in the art, for example, one or more selected from polyethylene, polypropylene, polyvinylidene fluoride, polyimide, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polynaphthalene system polymers, polyamide, poly(p-phenylene benzobisazole) and aramid.

[0065] In one example, the material of the substrate layer is obtained by the following grafting modification method:

[0066] (a1) subjecting the substrate material to a first plasma activation treatment;

[0067] (a2) subjecting the material obtained in step (a1) to a first oxygen treatment;

[0068] (a3) in a first solvent and under a protective atmosphere, subjecting the material obtained in step (a2) to a first contact reaction with the first monomer.

[0069] In step (a1), preferably, the conditions of the first plasma activation treatment include: a time of 3-10 min, preferably 5-8 min.

[0070] In step (a2), preferably, the first oxidation treatment process includes placing the material obtained in step (a1) in oxygen, and the control conditions include: temperature of 30-60°C, preferably 40-50°C; time of 100-250min, preferably 120-200min. After step (a2), a matrix material rich in peroxide is obtained.

[0071] In step (a3), the first contact reaction may include: immersing the material obtained in step (a2) in a solution containing a first monomer and a first solvent.

[0072] In step (a3), preferably, the conditions of the first contact reaction include: temperature of 50-80°C, preferably 55-65°C; time of 6-10h, preferably 7-9h.

[0073] In step (a3), preferably, the first solvent is selected from one or more of acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, cyclohexane, methanol, ethanol, isopropanol and water.

[0074] In this way, a substrate layer graft-modified with the first monomer according to a preferred embodiment can be obtained.

[0075] Other methods used by those skilled in the art to allow the first monomer to enter the substrate layer also fall within the protection scope of the present invention.

[0076] The thickness of the substrate layer can be 2-20 μm, for example, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 12 μm, 16 μm, 18 μm, or 20 μm.

[0077] The heat-resistant layer may also contain the first monomer and / or the first polymer. The first monomer and / or the first polymer may exist in the heat-resistant layer in various forms.

[0078] In a specific embodiment, the heat-resistant layer includes ceramic particles having a core-shell structure, wherein the shell material of the ceramic particles is the first polymer, and the core material of the ceramic particles is selected from one or more of aluminum oxide, boehmite, magnesium oxide, boron nitride and magnesium hydroxide.

[0079] The heat-resistant layer may also contain other conventional components, for example, the heat-resistant layer may also contain a first binder. The heat-resistant layer may be obtained by mixing the modified ceramic particles with the first binder, coating the mixture, and curing the mixture.

[0080] In one example, the shell material of the ceramic particle includes a homopolymer of the first monomer.

[0081] In one example, the shell material of the ceramic particle is a homopolymer of the first monomer.

[0082] Based on the total weight of the ceramic particles, the content of the shell material of the ceramic particles can be 5-50 weight % (for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50 weight %), and the content of the core material of the ceramic particles is 50-95 weight % (for example, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50 weight %).

[0083] According to a specific embodiment, based on the total weight of the ceramic particles, the content of the shell material of the ceramic particles is 15-25% by weight, and the content of the core material of the ceramic particles is 75-85% by weight.

[0084] According to a specific embodiment, the shell of the ceramic particle is prepared by the following method:

[0085] (b1) contacting the core material with the first monomer in a second solvent to obtain a solid-liquid mixture;

[0086] (b2) drying the solid-liquid mixture.

[0087] In step (b1), preferably, the second solvent is selected from one or more of acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, cyclohexane, methanol, ethanol, isopropanol and water.

[0088] In step (b1), in order to avoid loss during the process, the amount of the first monomer used can be excessive, that is, the amount of the first monomer used is more than the actual amount of shell formation, and the amount used can achieve the above core-shell ratio requirement.

[0089] In step (b1), the second contacting is, for example, stirring and mixing.

[0090] In step (b1), the first monomer in the solid-liquid mixture has been partially and / or completely polymerized. The solid-liquid mixture contains the first monomer and / or the first polymer.

[0091] In step (b2), the drying is, for example, vacuum heating drying or spray drying.

[0092] Thus, modified ceramic particles having a shell (the first monomer is homopolymerized into the shell) and a core structure are obtained.

[0093] The heat-resistant layer may further include a first binder.

[0094] Preferably, the first binder in the heat-resistant layer is selected from one or more of polytetrafluoroethylene, polyvinylidene fluoride, hexafluoropropylene-vinylidene fluoride copolymer, polyimide, polyacrylonitrile, polymethyl methacrylate, polyacrylic acid, and polyacrylate.

[0095] According to a specific embodiment, the heat-resistant layer is obtained by mixing modified ceramic particles with a first binder, coating and curing. According to the requirements for heat resistance, the content of the ceramic particles can be selected within a large range. Based on the total weight of the heat-resistant layer, the content of the ceramic particles can be 20-99% by weight, and the content of the first binder can be 1-80% by weight; preferably, the content of the ceramic particles can be 50-95% by weight, and the content of the first binder can be 5-50% by weight.

[0096] The first binder may not contain the first monomer and / or the first polymer.

[0097] The first binder may also contain the first monomer and / or the first polymer, which can be obtained by referring to the modification method of the second binder below.

[0098] The thickness of the heat-resistant layer may be 0.5-4 μm, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, or 4 μm.

[0099] The coating layer may also contain the first monomer and / or the first polymer, and the first monomer and / or the first polymer may exist in the coating layer in various forms.

[0100] In a specific embodiment, the coating layer is obtained by coating and curing a mixed slurry of a modified second binder and a third solvent (i.e., the coating layer includes the second binder and the third solvent), and the modified second binder is obtained by grafting the first monomer and / or the first polymer onto the base binder.

[0101] Preferably, the third solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, acetone and water.

[0102] Preferably, the usage ratio of the second binder to the third solvent is 1:(5-50), more preferably 1:(6-20).

[0103] In one example, the second binder is obtained by the following graft modification method:

[0104] (c1) subjecting the base binder to a second plasma activation treatment;

[0105] (c2) subjecting the material obtained in step (c1) to a second oxidation treatment;

[0106] (c3) in a fourth solvent and under a protective atmosphere, subjecting the material obtained in step (c2) to a third contact reaction with the first monomer.

[0107] In step (c1), preferably, the conditions of the plasma activation treatment include: a time of 3-10 min, preferably 5-8 min.

[0108] In step (c2), preferably, the second oxidation treatment process comprises placing the material obtained in step (c1) in oxygen, and the control conditions include: temperature of 30-60°C, preferably 40-50°C; time of 100-250min, preferably 120-200min. After this step (a2), a peroxide-rich base adhesive is obtained.

[0109] In step (c3), the third contact reaction may include: immersing the material obtained in step (c2) in a solution containing the first monomer and the fourth solvent.

[0110] In step (c3), preferably, the conditions of the third contact reaction include: temperature of 50-80°C, preferably 55-65°C; time of 6-10h, preferably 7-9h.

[0111] In step (c3), preferably, the fourth solvent is selected from one or more of acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone, cyclohexane, methanol, ethanol, isopropanol and water.

[0112] The base binder is, for example, one or more selected from polytetrafluoroethylene, polyvinylidene fluoride, hexafluoropropylene-vinylidene fluoride copolymer, polyimide, polyacrylonitrile, polymethyl methacrylate, polyacrylic acid and polyacrylate.

[0113] Preferably, relative to 100 parts by weight of the base binder, the amount of the first monomer is 0.1-20 parts by weight, more preferably 1-15 parts by weight, and further preferably 8-12 parts by weight.

[0114] The thickness of the adhesive layer may be 0.5-2 μm, for example, 0.5 μm, 1 μm or 2 μm.

[0115] The above exemplary embodiments respectively illustrate the modification methods of the substrate layer, the heat-resistant layer and the adhesive layer.

[0116] The content of the first monomer and / or the first polymer in the diaphragm can be selected in a large range according to the number of distribution layers and the required target. For example, relative to the total weight of the diaphragm, the content of the first monomer and / or the first polymer can be 0.1-20% by weight, preferably 0.5-10% by weight.

[0117] By introducing the first monomer / first polymer into the diaphragm, the ion channels of the diaphragm are increased, the consistency of ion conduction of the diaphragm is improved, the wettability of the diaphragm with the electrolyte is improved, and the speed and uniformity of ions passing through the diaphragm are accelerated.

[0118] A second aspect of the present invention provides a battery, wherein the separator of the battery is the separator described in the first aspect of the present invention.

[0119] The materials and preparation methods of the battery other than the battery separator can be carried out in accordance with the methods in the art, and can achieve the effects of reducing internal resistance, improving cycle performance and improving safety performance.

[0120] The battery is preferably a lithium-ion battery.

[0121] The battery further comprises a positive electrode sheet, a negative electrode sheet and a non-aqueous electrolyte.

[0122] The positive electrode sheet may be a conventional positive electrode sheet in the art, for example, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on one side or both sides of the surface of the positive electrode current collector.

[0123] The positive electrode active material layer may include a positive electrode active material, a conductive agent, and a binder.

[0124] In one example, the mixing mass ratio of the positive electrode active material, the conductive agent and the binder is (97-99):(0.5-1.5):(0.5-1.5).

[0125] In one embodiment, the positive electrode active material is selected from lithium cobalt oxide (LiCoO 2 ) or lithium cobalt oxide (LiCoO) doped with two or more elements of Al, Mg, Mn, Cr, Ti, and Zr. 2), the chemical formula of the lithium cobalt oxide doped and coated with two or more elements selected from Al, Mg, Mn, Cr, Ti, and Zr is Li x Co 1-y1-y2-y3-y4 A y1 B y2 C y3 D y4 O 2 ; 0.95≤x≤1.05, 0.01≤y1≤0.1, 0.01≤y2≤0.1, 0≤y3≤0.1, 0≤y4≤0.1, A, B, C, D are selected from two or more elements of Al, Mg, Mn, Cr, Ti, and Zr.

[0126] In one embodiment, the positive electrode active material is further selected from a ternary material (NCM or NCA) or a ternary material (NCM or NCA) doped with or coated with two or more elements of Al, Mg, W, Sr, Mo, and Zr, wherein the chemical formula of the ternary material doped with or coated with two or more elements of Al, Mg, W, Sr, Mo, and Zr is LiNi x Co y Mn z M 1-x-y-z O 2 ; 0.33≤x≤0.96, 0≤y≤0.33, 0.03≤Z≤0.33, 0≤1-xyz≤0.005, M is selected from two or more elements of Al, Mg, W, Sr, Mo and Zr.

[0127] In one embodiment, the positive electrode active material is further selected from lithium iron phosphate (LFP) or lithium iron phosphate (LFP) doped with or coated with two or more elements selected from Ti, W, V, Na, Mn, and Co. The chemical formula of the lithium iron phosphate doped with or coated with two or more elements selected from Ti, W, V, Na, Mn, and Co is LiFe x PN 1-x O 2 ; 0.095≤x≤1, 0.0001≤1-X≤0.005, N is selected from two or more elements of Ti, W, V, Na, Mn and Co.

[0128] In one example, the conductive agent in the positive electrode active material layer is selected from acetylene black.

[0129] In one example, the binder in the positive electrode active material layer is selected from polyvinylidene fluoride (PVDF).

[0130] The negative electrode sheet can be a conventional negative electrode sheet in the art. For example, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on one or both surfaces of the negative electrode current collector, and the negative electrode active material layer can include a negative electrode active material, a conductive agent, and a binder.

[0131] In one example, the negative electrode active material is selected from graphite.

[0132] In one example, the negative electrode active material also optionally contains SiO x / C or Si / C, where 0 < x < 2. For example, the negative electrode active material also contains 1-15 wt% SiO x / C or Si / C, exemplarily 1 wt.%, 2 wt.%, 5 wt.%, 8 wt.%, 10 wt.%, 12 wt.%, 15 wt.% or any point value within the range composed of any two of the foregoing numerical values.

[0133] Due to the inclusion of the separator described in the present invention, the internal resistance of the battery is reduced, thereby improving the long-term cycling performance and safety performance; and the required aging time is reduced, thus improving the production efficiency and reducing the cost.

[0134] The present invention will be described in detail below through examples. The examples described in the present invention are only a part of the examples of the present invention, rather than all the examples. All other examples obtained by those of ordinary skill in the art based on the examples in the present invention without creative efforts shall fall within the protection scope of the present invention.

[0135] Example I1

[0136] In this example, the first monomer having the structure shown in (I-1) is used for modification.

[0137] The separator is prepared according to the following steps.

[0138] (1) Modified substrate layer

[0139] After activating the matrix material polyolefin with a thickness of 5 μm by plasma treatment for 6 min, it is treated in oxygen at a temperature of 45 °C for 150 min to obtain a matrix material rich in peroxides; the matrix material rich in peroxides is soaked in a first monomer solution (the solvent is acetone, and the amount used makes the weight ratio of the first monomer to the matrix material 2:100), and under the presence of a protective atmosphere, the temperature is controlled at 60 °C and the reaction is carried out for 8 h to obtain a modified substrate layer.

[0140] (2) Modify ceramic particles and form a heat-resistant layer

[0141] The first monomer is dissolved in an acetone solvent by stirring to form an acetone solution containing the first monomer and the first polymer, and alumina ceramic particles are added to the acetone solution containing the first monomer and the first polymer, and stirred and mixed for 2 hours, so that the first monomer is polymerized into a shell on the surface of the ceramic particles; the obtained material is spray-dried to obtain modified ceramic particles. The shell-core weight ratio of the modified ceramic particles is 20:100.

[0142] The modified ceramic particles (60 wt %), polyvinylidene fluoride (PVDF) (40 wt %) and acetone were mixed and stirred to obtain a slurry.

[0143] The obtained slurry is applied to the upper and lower surfaces of the substrate layer, respectively, and cured to form a first heat-resistant layer and a second heat-resistant layer.

[0144] (3) Modification and formation of coating layer

[0145] After the coating material PVDF is activated by plasma treatment for 6 minutes, it is treated in oxygen at a temperature of 45°C for 150 minutes to obtain peroxide-rich PVDF; the peroxide-rich PVDF is immersed in a first monomer solution (the solvent is acetone, and the amount is used so that the weight ratio of the first monomer to the coating material is 10:100), and in the presence of protective gas, the temperature is controlled to 60°C, and after reacting for 8 hours, a modified PVDF is obtained. The modified PVDF and dimethylacetamide (DMAC) are stirred at a stirring speed of 1500 rpm for 120 minutes at a ratio of 6% solid content to obtain a slurry. The obtained slurry is coated on the surface of the first heat-resistant layer and the second heat-resistant layer to form a first coating layer and a second coating layer.

[0146] Finally, a diaphragm is obtained which comprises, from bottom to top, a first adhesive layer, a first heat-resistant layer, a substrate layer, a second heat-resistant layer and a second adhesive layer, and the thickness of each layer is 1 μm, 2 μm, 5 μm, 2 μm and 1 μm, respectively.

[0147] Comparative Example 1

[0148] The diaphragm prepared in this comparative example does not contain modified monomers.

[0149] The substrate layer uses a polyethylene substrate (denoted as D j );

[0150] A layer of alumina ceramic slurry is coated on both sides of the substrate layer to obtain a heat-resistant layer (denoted as D n ), the alumina ceramic slurry is prepared with reference to Example I1, except that the alumina ceramic is not modified;

[0151] A layer of rubber is applied to the upper and lower surfaces respectively to obtain a rubber coating layer (denoted as D t), the rubber compound was prepared with reference to Example I1, except that the PVDF was not modified.

[0152] Finally, a diaphragm is obtained which comprises, from bottom to top, a first adhesive layer, a first heat-resistant layer, a substrate layer, a second heat-resistant layer and a second adhesive layer, and the thickness of each layer is 1 μm, 2 μm, 5 μm, 2 μm and 1 μm, respectively.

[0153] Other embodiments

[0154] Each embodiment is carried out with reference to embodiment I1, except that the substrate layer, the heat-resistant layer and the adhesive layer respectively change the specific selection of the first monomer or do not modify it, as shown in Table 1.

[0155] Among them, Group I is used to represent the embodiments modified with the structural monomer of formula (I); Group II is used to represent the embodiments modified with the structural monomer of formula (II); Group III is used to represent the embodiments modified with the structural monomers of formula (I) and formula (II). These combinations are only for illustration, and the structural monomers of the present invention can be combined.

[0156] Table 1

[0157]

[0158]

[0159] The separators obtained in the examples were used to prepare batteries in the following manner:

[0160] (1) Preparation of positive electrode

[0161] The positive electrode active material LiCoO 2 , a binder polyvinylidene fluoride (PVDF), and a conductive agent acetylene black are mixed in a weight ratio of 98:1.0:1.0, N-methylpyrrolidone (NMP) is added, and the mixture is stirred under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on an aluminum foil with a thickness of 10 μm; the coated aluminum foil is baked in an oven with 5 different temperature gradients, and then dried in an oven at 120°C for 8 hours, and then rolled and cut to obtain the desired positive electrode sheet.

[0162] (2) Negative electrode preparation

[0163] 97% by weight of artificial graphite negative electrode material, 0.1% by weight of single-walled carbon nanotube (SWCNT) conductive agent, 0.8% by weight of conductive carbon black (SP) conductive agent, 1% by weight of sodium carboxymethyl cellulose (CMC) binder and 1.1% by weight of styrene-butadiene rubber (SBR) binder were made into slurry by a wet process, coated on the surface of 6 μm thick copper foil of the negative electrode current collector, and dried (temperature: 85°C, time: 5h), rolled and die-cut to obtain a negative electrode sheet.

[0164] (3) Preparation of non-aqueous electrolyte

[0165] In a glove box filled with argon (water content <10ppm, oxygen content <1ppm), ethylene carbonate (EC), propylene carbonate (PC) and propyl propionate (PP) are mixed in a mass ratio of 2:1.5:2, and 14wt.% of LiPF6 based on the total mass of the non-aqueous electrolyte and 5-60wt.% of ethyl propionate based on the total mass of the non-aqueous electrolyte are slowly added to the mixed solution, and the mixture is stirred to obtain a non-aqueous electrolyte.

[0166] (4) Diaphragm

[0167] The separators used were the separators obtained in the above-mentioned embodiments and comparative examples.

[0168] (5) Preparation of lithium-ion batteries

[0169] The positive electrode sheet, separator and negative electrode sheet prepared above are wound to obtain a bare cell without liquid injection; the bare cell is placed in an outer packaging foil, and the prepared electrolyte is injected into the dried bare cell. After vacuum packaging, standing, formation, secondary sealing, sorting and other processes, the desired lithium-ion battery is obtained.

[0170] Test Case

[0171] The obtained separator and battery were subjected to the following tests:

[0172] (1) Test the ionic conductivity of the diaphragm

[0173] The membranes obtained in the above examples and comparative examples were placed in an environment of (25±2)°C, and a circular sample with a diameter of 40 mm was prepared. The sample was placed in an electrolyte with an ion conductivity of 10±2ms / cm for 2 hours. A completely dried conductivity cell was taken and rinsed with electrolyte for 3 times, and then the standard electrolyte was added to the conductivity cell with a dropper, and a layer of the soaked membrane was clamped with tweezers and placed in the conductivity cell. The prepared sample was subjected to impedance testing using an electrochemical workstation, with a scanning frequency of 1KHz-100KHz. The impedance of 1 to 5 layers of the membrane was tested in sequence according to the above test method to obtain the ion conductivity of the membrane.

[0174] Record 100 sets of data and calculate the ion conductivity deviation ratio: ion conductivity deviation ratio (%) = maximum value / minimum value × 100%.

[0175] (2) Test the electrochemical performance of the battery

[0176] The batteries obtained in the above embodiments and comparative examples were placed in a (25±2)°C environment and left to stand for 2-3h. When the battery body reached (25±2)°C, the battery was charged at a 1C constant current with a cut-off current of 0.05C. After the battery was fully charged, it was left for 5min and then discharged at a 1C constant current to a cut-off voltage of 3.0V. The highest discharge capacity of the first three cycles was recorded as the initial capacity Q. When the number of cycles reached 1000, the last discharge capacity Q1 of the battery was recorded. The initial thickness T of the battery cell was recorded, and the thickness after 1000 cycles was recorded as T1. The recording results are shown in Table 2.

[0177] The calculation formula used is as follows: Capacity retention rate (%) = Q1 / Q×100%.

[0178] The obtained results are recorded in Table 2.

[0179] Table 2

[0180]

[0181]

[0182] *Comparative Example 1: When the battery made of conventional diaphragm was tested for battery capacity retention, the battery capacity retention rate dropped sharply to 60% after 608 cycles, and then the battery capacity retention rate dropped rapidly and could not complete the 1000-week test.

[0183] It can be seen from Table 2 that the ionic conductivity deviation ratio of the diaphragm of the embodiment is significantly reduced, and the capacity retention rate of the battery made of the diaphragm of the embodiment is significantly improved, indicating that the introduction of the first monomer and / or the first polymer of the present invention improves the consistency of the conductive ions of the diaphragm, reduces the internal resistance of the battery, increases the cycle life of the battery, and improves the safety performance of the battery.

[0184] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A diaphragm, characterized in that: The diaphragm comprises a substrate layer and a heat-resistant layer, the heat-resistant layer comprises ceramic particles and a first binder, the ceramic particles have a core-shell structure, the shell material of the ceramic particles comprises a first polymer, and the monomer of the first polymer comprises a first monomer; The first monomer has a structure represented by formula (I) or formula (II), Wherein, R1 and R2 are each independently selected from H, -C n NR3 and -C n NR4R5, n is an integer of 0-4; NR3 is a 4-7 membered heterocyclic ring, R3 contains 0-2 oxygen atoms and / or 0-2 nitrogen atoms, and the rest are carbon atoms; R3 may or may not have a grafted group R6, and R6 is -C m OH, m is an integer of 0-2; R4 and R5 are each independently a C1-C4 aliphatic chain.

2. The diaphragm according to claim 1, wherein n is 1 or 2; NR3 is a five-membered or six-membered heterocyclic ring, R3 contains 0-1 oxygen atoms, and the rest are carbon atoms; R3 may or may not have a grafted group R6, and R6 is OH; R4 and R5 are each independently selected from methyl and ethyl; Preferably, -C n NR3 is selected from the following structures:

3. The diaphragm according to claim 1, wherein The first monomer is selected from the following structures:

4. The diaphragm according to any one of claims 1 to 3, wherein: The diaphragm includes a substrate layer, a heat-resistant layer and an optional adhesive layer; the heat-resistant layer covers one side or both sides of the substrate layer; the adhesive layer covers the surface of the heat-resistant layer, and / or the adhesive layer covers the surface of the substrate layer.

5. The diaphragm according to claim 4, wherein At least one of the substrate layer and the adhesive layer contains the first monomer and / or the first polymer.

6. The diaphragm according to claim 4 or 5, wherein: The material of the substrate layer is a material obtained by grafting and modifying the base material with the first monomer; The matrix material is selected from one or more of polyethylene, polypropylene, polyvinylidene fluoride, polyimide, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polynaphthalene system polymer, polyamide, poly(p-phenylene benzobisazole) and aramid, etc.; And / or, based on 100 parts by weight of the base material, the content of the first monomer is 0.1-10 parts by weight.

7. The diaphragm according to claim 1, wherein The core material of the ceramic particles is selected from one or more of alumina, boehmite, magnesium oxide, boron nitride and magnesium hydroxide; Preferably, based on the total weight of the ceramic particles, the content of the shell material is 5-50% by weight, and the content of the core material is 50-95% by weight; And / or, based on the total weight of the heat-resistant layer, the content of the ceramic particles is 20-99% by weight, and the content of the first binder is 1-80% by weight.

8. The diaphragm according to claim 4 or 5, wherein: The coating layer includes a modified second binder and a third solvent, wherein the modified second binder is obtained by grafting the first monomer and / or the first polymer onto a base binder; Preferably, the third solvent is selected from one or more of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, acetone and water.

9. The diaphragm according to any one of claims 4 to 8, wherein: Relative to the total weight of the separator, the content of the first monomer and / or the first polymer is 0.1-20 wt %, preferably 0.5-10 wt %.

10. A battery, characterized in that: The separator of the battery is the separator according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Electrochemical cells with ionic sequestration provided by porous separators

    CN109804496A

  • Diaphragm and high-voltage battery comprising same

    CN111029514A

  • Binder and diaphragm, and preparation methods thereof

    CN112341961A

  • Lithium ion battery diaphragm and preparation method thereof

    CN112751141A

  • Diaphragm as well as preparation method and application thereof

    CN113904058A

Cited By

  • Separator, and electrochemical device and electronic device including same

    CN121261059A