High-temperature-resistant and stable heating wire as well as preparation method and application thereof

By applying an electric heat composite layer of conductive filler composition and a high-temperature resistant organic polymer on the heating wire, the problem of poor stability of existing heating wires in high-temperature environments is solved, and the conductive performance and heat resistance are improved. And reduces production costs and is suitable for the hotline field.

CN118921774AActive Publication Date: 2024-11-08YUNNAN JUSHENG ELECTRIC TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411207323.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-08
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The existing heating wires have poor stability in high-temperature environments, insufficient wear and heat resistance, resulting in uneven conductivity, short service life, and high production costs, which limits its application range.

Method used

The outer wall of the core wire is prepared by a high-temperature-resistant electrothermal composite layer composed of a conductive filler composition, a high-temperature-resistant organic polymer, a surface modifier and an aging-resistant additive. The high-temperature electric heating composite layer improves conductive properties and heat resistance stability, and reduces production costs by optimizing the ratio of conductive filler composition and resin.

Benefits of technology

The stable use of heating wire at -40 to 200°C was achieved. After 1000 cycles of heating tests, the resistance value change rate is less than 3%, the resistance value change rate is less than 5% at 200°C, and it has excellent conductivity and Flame retardant safety performance, suitable for industrial production and applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005021559640000131
    Figure BDA0005021559640000131
  • Figure BDA0005021559640000141
    Figure BDA0005021559640000141
  • Figure BDA0005021559640000142
    Figure BDA0005021559640000142
Patent Text Reader

Abstract

The invention relates to the technical field of polymer conductive fibers, in particular to a high-temperature-resistant and stable heating wire and a preparation method and application thereof. The high-temperature-resistant and stable heating wire comprises a core wire and a high-temperature-resistant electric heating composite layer, wherein the thickness of the high-temperature-resistant electric heating composite layer is 50-1500 microns; the resistivity of the high-temperature-resistant electric heating composite layer is 0.5 to 50 omega.cm; the high-temperature-resistant electric heating composite layer at least comprises a conductive filler composition, a high-temperature-resistant organic polymer, a surface modifier and an anti-aging additive, and the content of the conductive filler composition is 20-40wt%; and the high-temperature-resistant organic polymer is thermosetting high-temperature-resistant resin or thermoplastic high-temperature-resistant resin. The heating wire prepared in the invention can be stably used at-40 to 400 DEG C, and after 1000 times of cyclic heating tests, the change rate of the resistance value of the heating wire at 25 DEG C is lower than 3%, and the change rate of the resistance value at 400 DEG C is lower than 5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer conductive fibers, and in particular to a high temperature resistant and stable heating wire. Background Art

[0002] The heating wire has good electrical conductivity. After it is energized, it converts electrical energy into internal energy. The characteristic of releasing heat when the heating wire is energized makes it widely used in the field of heating and heat preservation. Common heating wires include metal alloy conductive wires, graphene carbon slurry wires, carbon fiber conductive wires, etc. Metal alloy conductive wires have good electrical conductivity and heat resistance, but their weight is heavy and their bending performance is biased, which limits their scope of application. Although the graphene carbon slurry wire is cheap and the production process is simple, its wear resistance is poor. During use, it is worn by foreign objects, causing the graphene to detach, resulting in the overall resistance uniformity deviation of the graphene carbon slurry wire, which limits its scope of application. The carbon fiber wire has good electrical conductivity and high temperature resistant stability, but its production process is high. High-performance carbon fiber conductive materials rely on imports, resulting in high overall costs, which are not suitable for large-scale commercial applications. In addition, the overall bending toughness of carbon fiber is relatively poorer than that of metal alloy wire, which limits its application and development. To this end, the inventor provides a high-temperature resistant and stable heating wire and a preparation method thereof. Summary of the invention

[0003] In order to solve the above technical problems, the present application provides a high temperature resistant and stable heating wire and a preparation method and application thereof.

[0004] The present application provides a high temperature resistant and stable heating wire, which is realized by the following technical solutions:

[0005] A high-temperature resistant and stable heating wire comprises a core wire and a high-temperature resistant electric heating composite layer coated on the outer wall of the core wire, wherein the high-temperature resistant electric heating composite layer is composited with a plated insulating layer; the thickness of the high-temperature resistant electric heating composite layer is 50-1500 μm; the resistivity of the high-temperature resistant electric heating composite layer is 0.5-50 Ω·cm; the high-temperature resistant electric heating composite layer contains at least a conductive filler composition, a high-temperature resistant organic polymer, a surface modifier, and an anti-aging additive, wherein the content of the conductive filler composition is 20-40wt%; the high-temperature resistant organic polymer is a thermosetting high-temperature resistant resin or a thermoplastic high-temperature resistant resin.

[0006] Preferably, the thermosetting high temperature resistant resin includes at least one of thermosetting polyphenylene sulfide resin PPS and thermosetting polyimide resin TPI; the thermoplastic high temperature resistant resin includes at least one of thermoplastic polyimide resin TPI, thermoplastic polyphenylene sulfide resin PPS, and thermoplastic fluorocarbon resin; the polytetrafluoroethylene resin includes at least one of polytetrafluoroethylene PTFE, polytrifluorochloroethylene PCTFE, polyvinylidene fluoride PVDF, ethylene-tetrafluoroethylene copolymer ETFE, and ethylene-trifluorochloroethylene copolymer ECTFE.

[0007] Preferably, the high temperature resistant electric heating composite layer is made of the following raw materials in percentage by mass: 20-40wt% conductive filler composition, 0.8-1wt% surface modifier, 0.8-1.6wt% anti-aging agent, 3-6wt% hyperbranched PPS resin, and the remainder is thermoplastic polyphenylene sulfide resin PPS.

[0008] Preferably, the high temperature resistant electric heating composite layer is made of the following raw materials in percentage by mass: 20-40wt% conductive filler composition, 1.2-1.8wt% surface modifier, 0.6-1.2wt% anti-aging agent, 4-8wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF.

[0009] Preferably, the conductive filler composition is made of the following raw materials in percentage by mass: 5-20wt% of flake graphite, 20-40wt% of nano-barium titanate, 1-5wt% of titanium diboride whiskers, 3-8wt% of titanium nitride, 5-20wt% of molybdenum disilicide nanosheets, 0-5wt% of graphene, and the balance is microcrystalline graphite.

[0010] The heating wire prepared in the present application can be used stably at -40 to 200°C, and after 1000 cycles of heating tests, the resistance value change rate of the heating wire at 25°C is less than 3%, and the resistance value change rate at 200°C is less than 5%.

[0011] Preferably, the surface modifier is composed of at least one of 3-isocyanate propyl triethoxy silane, γ-methacryloxypropyl trimethoxy silane, γ-glycidyloxypropyl trimethoxy silane, and γ-aminopropyl triethoxy silane in combination with a titanate coupling agent HY-201.

[0012] By adopting the above technical solution, the uniformity of the distribution of the conductive filler composition in the high temperature resistant organic polymer can be improved, thereby improving the conductive performance of the prepared heating wire, and at the same time improving the overall heat resistance stability and service life.

[0013] Preferably, the conductive filler composition is made of the following raw materials in percentage by mass: 10-12wt% of flake graphite, 32-36wt% of nano-barium titanate, 2-4wt% of titanium diboride whiskers, 5-6wt% of titanium nitride, 10-15wt% of molybdenum disilicide nanosheets, 0.5-2wt% of graphene, and the balance is microcrystalline graphite.

[0014] By optimizing the conductive filler composition, the conductivity of the resistance wire can be guaranteed while improving the heat resistance stability and reducing the production cost.

[0015] The present application provides a method for preparing a high temperature resistant and stable heating wire, which is achieved through the following technical solutions:

[0016] A method for preparing a high temperature resistant and stable heating wire comprises the following steps:

[0017] Step 1: Production of raw materials for preparing high temperature resistant electric heating composite layer:

[0018] When a thermosetting high temperature resistant resin is used in the high temperature resistant electric heating composite layer, the thermosetting high temperature resistant resin monomer is first reacted to a system viscosity of 6000-20000 mPa·s / 25°C, and then a conductive filler composition, a surface modifier, and an anti-aging additive are added in accurate amounts and mixed evenly to obtain a high temperature resistant electric heating slurry;

[0019] When a thermoplastic high temperature resistant resin is used in the high temperature resistant electric heating composite layer, the conductive filler composition, the thermoplastic high temperature resistant resin, the surface modifier, and the anti-aging additive are melt-extruded, wire-drawn, cooled, granulated, and dried to obtain a high temperature resistant electric heating masterbatch;

[0020] Step 2: When the high temperature resistant electric heating composite layer is made of high temperature resistant electric heating slurry, the core wire is immersed in the high temperature resistant electric heating slurry, and the core wire is pulled at a speed of 1-10 cm / s, so that the high temperature resistant electric heating slurry adheres to the outer wall of the core wire, and then the core wire is transferred to an oven for curing, that is, the high temperature resistant electric heating composite layer is compounded on the outer side of the core wire to obtain a finished heating wire;

[0021] When the high temperature resistant electric heating composite layer is made of high temperature resistant electric heating masterbatch, the molten extruded material obtained by melt-extruding the high temperature resistant electric heating masterbatch is attached to the outer surface of the core wire, and the finished heating wire can be obtained by water cooling, heat treatment and drying.

[0022] The preparation method of the heating wire in the present application is relatively simple, has low operating difficulty, and is easy to implement industrial production and manufacturing.

[0023] The high temperature resistant and stable heating wire in the present application is applied to the field of heating cables and has excellent high temperature resistant use stability.

[0024] In summary, this application has the following advantages:

[0025] 1. The heating wire prepared in this application can be used stably at -40 to 400°C, and after 1000 cycles of heating tests, the resistance value change rate of the heating wire at 25°C is less than 3%, and the resistance value change rate at 400°C is less than 5%.

[0026] 2. Doping a proper amount of graphene in the heating wire of the present application can improve the overall conductivity and effectively improve the overall flame retardant safety performance.

[0027] 3. The preparation method of the heating wire in this application is relatively simple, with low operating difficulty, and is easy to implement industrial production and manufacturing. DETAILED DESCRIPTION

[0028] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.

[0029] Example

[0030] A high temperature resistant and stable heating wire comprises a core wire and a high temperature resistant electric heating composite layer coated on the outer wall of the core wire, wherein the high temperature resistant electric heating composite layer is composited with a coated insulating layer. The thickness of the high temperature resistant electric heating composite layer is 50-1500μm, and the resistivity of the high temperature resistant electric heating composite layer is 0.5-50Ω·cm, that is, the thicker the thickness of the high temperature resistant electric heating composite layer, the better the conductivity of the prepared heating wire. The core wire can be selected according to the resistance requirements to select at least one of conductive or non-conductive chemical fiber wire, metal wire, alloy wire, carbon fiber wire, and conductive ceramic wire.

[0031] The high temperature resistant electric heating composite layer at least contains a conductive filler composition, a high temperature resistant organic polymer, a surface modifier, and an anti-aging additive, wherein the content of the conductive filler composition is 20-40wt%. The high temperature resistant organic polymer can be selected from a thermosetting high temperature resistant resin or a thermoplastic high temperature resistant resin, and the high temperature resistant organic polymer is selected according to different customer requirements for the heating wire.

[0032] The surface modifier is composed of at least one of 3-isocyanate propyl triethoxy silane, γ-methacryloxy propyl trimethoxy silane, γ-glycidyloxy propyl trimethoxy silane and γ-aminopropyl triethoxy silane and a titanate coupling agent HY-201.

[0033] The anti-aging agent is composed of at least one of silicon nitride and silicon dioxide, an antioxidant 1010, an antioxidant 168, and an anti-ultraviolet agent 326.

[0034] The conductive filler composition is made of the following raw materials in percentage by mass: 5-20wt% of flake graphite, 20-40wt% of nano barium titanate, 1-5wt% of titanium diboride whisker, 3-8wt% of titanium nitride, 5-20wt% of molybdenum disilicide nanosheets, 0-5wt% of graphene, and the balance is microcrystalline graphite.

[0035] Preferably, the conductive filler composition is made of the following raw materials in percentage by mass: 10-12wt% of flake graphite, 32-36wt% of nano-barium titanate, 2-4wt% of titanium diboride whiskers, 5-6wt% of titanium nitride, 10-15wt% of molybdenum disilicide nanosheets, 0.5-2wt% of graphene, and the balance is microcrystalline graphite.

[0036] A method for preparing a high temperature resistant and stable heating wire comprises the following steps:

[0037] Step 1, production of raw materials for preparing high temperature resistant electric heating composite layer: firstly react the thermosetting high temperature resistant resin monomer to a system viscosity of 6000-20000mPa·s / 25°C, then add the accurately measured conductive filler composition, surface modifier, and anti-aging additive and mix them evenly to obtain high temperature resistant electric heating slurry;

[0038] Step 2: immerse the core wire in the high temperature resistant electric heating slurry, pull the core wire at a speed of 1-10 cm / s, so that the high temperature resistant electric heating slurry adheres to the outer wall of the core wire, and then transfer it to an oven for curing, that is, compound a high temperature resistant electric heating composite layer on the outside of the core wire to obtain a finished heating wire.

[0039] Preferably, the high temperature resistant electric heating composite layer is made of the following raw materials in percentage by weight: 20-40wt% conductive filler composition, 1.2-1.8wt% surface modifier, 0.6-1.2wt% anti-aging agent, 4-8wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF.

[0040] Preferably, the high temperature resistant electric heating composite layer is made of the following raw materials in percentage by weight: 20-40wt% conductive filler composition, 0.8-1wt% surface modifier, 0.8-1.6wt% anti-aging agent, 3-6wt% hyperbranched PPS resin, and the remainder is thermoplastic polyphenylene sulfide resin PPS.

[0041] A method for preparing a high temperature resistant and stable heating wire comprises the following steps:

[0042] Step 1, production of raw materials for preparing high temperature resistant electric heating composite layer: melt extrusion of conductive filler composition, thermoplastic high temperature resistant resin, surface modifier, anti-aging additive, wire drawing, cooling, granulation, drying high temperature resistant electric heating masterbatch;

[0043] Step 2: melt-extrude the high-temperature resistant electrothermal masterbatch to obtain a molten extruded material, which is attached to the outer surface of the core wire, and then water-cooled, heat-treated and dried to obtain a finished heating wire.

[0044] The high temperature resistant and stable heating wire in the present application is applied to the field of heating cables and can replace expensive carbon fiber conductive wire products.

[0045] Embodiment 1: A high temperature resistant and stable heating wire comprises a core wire and a high temperature resistant electric heating composite layer coated on the outer wall of the core wire, wherein the high temperature resistant electric heating composite layer is composited with a 50nm coated insulating layer Al2O3 by a sol-gel method. The core wire is Japanese Kuraray Vectran 50D aramid wire.

[0046] The high temperature resistant electric heating composite layer is made of high temperature resistant electric heating masterbatch, and the high temperature resistant electric heating masterbatch is made of the following raw materials in percentage by weight: 20wt% conductive filler composition, 1.2wt% surface modifier, 1wt% anti-aging additive, 6wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF (Arkema 740 extrusion grade, France).

[0047] The surface modifier is composed of 3-isocyanate propyl triethoxysilane, γ-methacryloxypropyl trimethoxysilane, and titanate coupling agent HY-201 in a mass ratio of 4:3:3. The anti-aging additive is composed of nano silicon nitride, antioxidant 1010, antioxidant 168, and anti-ultraviolet agent 326 in a mass ratio of 5:4:1:5.

[0048] The conductive filler composition is made of the following raw materials in percentage by mass: 10wt% of flake graphite (brand: Yuchen Graphite, customized average particle size of 1μm), 30wt% of nano barium titanate (BT-2 high-purity nano electronic grade barium titanate BaTiO3, brand Wohai Chemical), 2wt% of titanium diboride whiskers, 5wt% of nano titanium nitride (brand Huaxiang, average particle size 700nm), 10wt% of molybdenum disilicide nanosheets (Xianfeng Nano's XF137 small-diameter thin-layer molybdenum disulfide nanosheets, sheet diameter: 20-500nm, thickness: 1-5nm), and the remainder is microcrystalline graphite (brand Jingao, 2000-mesh earthy graphite microcrystalline graphite powder).

[0049] Preparation method of titanium diboride whiskers: weigh 347g titanium dioxide, 204g boron oxide, 260g activated carbon, 63g sodium chloride as a whisker growth cosolvent, and 26g nickel as a whisker growth catalyst to mix to obtain a composite powder, put the composite powder into a cylinder ball mill with alumina balls for 8h and pass through a 100-mesh sieve, and then put it into a graphite reaction container with a cover at the end, a closed bottom, and a porous middle. The circular holes are evenly distributed on the outer wall of the graphite reaction container, with a diameter of about 10mm and a distance of about 20mm from the end; put the reaction container into a high-temperature sintering furnace for whisker cultivation, and the specific process is: the heating rate is 100℃ / min, argon atmosphere protection, and the temperature is kept at 1500℃ for 60min, and the required titanium diboride whisker material is synthesized after cooling to room temperature at a cooling rate of 10℃ / min.

[0050] A method for preparing a high temperature resistant and stable heating wire comprises the following steps:

[0051] Step 1, production of raw materials for preparing high-temperature resistant electric heating composite layer: placing a conductive filler composition, polyvinylidene fluoride PVDF resin, a surface modifier, dibutyl phthalate DBP, and an aging-resistant additive in a high-speed dispersion kettle and mixing at 400 rpn for 60 minutes, placing the resulting mixture in a twin-screw extruder, and melt-extrude at 240-260° C. The resulting molten extrudate is subjected to wire drawing, cooling, granulation, and drying to obtain a high-temperature resistant electric heating masterbatch with a particle size of 1.8-2.0 mm;

[0052] Step 2: Put the high temperature resistant electric heating masterbatch with a particle size of 1.8-2.0 mm obtained in step 1 into a twin-screw extruder, melt extrude at 240-260° C., and the obtained molten extrusion material is attached to the outer surface of the Vectran 50D aramid yarn. The pulling speed of the Vectran 50D aramid yarn is 1.2 m / s. The Vectran 50D aramid yarn with the high temperature resistant electric heating composite material attached to the outer surface is water-cooled for 15 seconds, sent to a 1200° C. oven for 30 minutes of heat treatment, and then sent to an 80° C. oven for 120 minutes of drying treatment. Finally, the high temperature resistant electric heating composite layer is compounded with a 50 nm coated insulating layer Al2O3 by a sol-gel method to obtain a finished heating wire. The thickness of the high temperature resistant electric heating composite layer is 927.5 μm. The resistivity of the high temperature resistant electric heating composite layer in the obtained finished heating wire is 39.41 Ω·cm, and its surface resistance is 6.94*10 14 Ω·cm, that is, the surface is insulated and has good thermal conductivity. The steady-state heating temperature of the finished heating wire can be controlled by controlling the voltage.

[0053] The difference between Example 2 and Example 1 is that the high temperature resistant electric heating masterbatch is made of the following raw materials in mass percentage: 30wt% conductive filler composition, 1.5wt% surface modifier, 1wt% anti-aging additive, 7.2wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 958.1μm, and the resistivity of the obtained finished heating wire is 27.25Ω·cm. The steady-state heating temperature of the finished heating wire can be controlled by controlling the voltage.

[0054] The difference between Example 3 and Example 1 is that the high temperature resistant electric heating masterbatch is made of the following raw materials in mass percentage: 35wt% conductive filler composition, 1.65wt% surface modifier, 1wt% anti-aging additive, 7.5wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 964.1μm, and the resistivity of the obtained finished heating wire is 22.49Ω·cm. The steady-state heating temperature of the finished heating wire can be controlled by controlling the voltage.

[0055] The difference between Example 4 and Example 1 is that the high temperature resistant electric heating masterbatch is made of the following raw materials in mass percentage: 40wt% conductive filler composition, 1.8wt% surface modifier, 1wt% anti-aging additive, 8wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 972.5μm, and the resistivity of the obtained finished heating wire is 18.25Ω·cm. The steady-state heating temperature of the finished heating wire can be controlled by controlling the voltage.

[0056] The difference between Example 5 and Example 1 is that the conductive filler composition is made of the following raw materials in mass percentage: 12wt% flake graphite, 35wt% nano barium titanate, 3.2wt% titanium diboride whisker, 5.4wt% nano titanium nitride, 15wt% molybdenum disilicide nanosheets, and the balance is microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 938.1μm, and the resistivity of the finished heating wire is 40.05Ω·cm.

[0057] The difference between Example 6 and Example 1 is that the conductive filler composition is made of the following raw materials in mass percentage: 12wt% flake graphite, 35wt% nano barium titanate, 3.2wt% titanium diboride whisker, 5.4wt% nano titanium nitride, 15wt% molybdenum disilicide nanosheets, 2wt% graphene, and the balance is microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 918.7μm, and the resistivity of the finished heating wire is 27.38Ω·cm.

[0058] The difference between Example 7 and Example 1 is that the conductive filler composition is made of the following raw materials in mass percentage: 5wt% flake graphite, 20wt% nano barium titanate, 1wt% titanium diboride whisker, 3wt% nano titanium nitride, 5wt% molybdenum disilicide nanosheets, 5wt% graphene, and the balance is microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 921.2μm, and the resistivity of the finished heating wire is 12.07Ω·cm.

[0059] The difference between Example 8 and Example 1 is that the conductive filler composition is made of the following raw materials in mass percentage: 20wt% flake graphite, 40wt% nano barium titanate, 5wt% titanium diboride whisker, 5wt% nano titanium nitride, 15wt% molybdenum disilicide nanosheets, and the balance is microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 940.4μm, and the resistivity of the finished heating wire is 44.29Ω·cm.

[0060] The difference between Example 9 and Example 1 is that the high temperature resistant electric heating masterbatch is made of the following raw materials in mass percentage: 40wt% conductive filler composition, 1.8wt% surface modifier, 1wt% anti-aging additive, 8wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF. The conductive filler composition is made of the following raw materials in mass percentage: 5wt% flake graphite, 20wt% nano barium titanate, 1wt% titanium diboride whisker, 3wt% nano titanium nitride, 5wt% molybdenum disilicide nanosheets, 5wt% graphene, and the balance is microcrystalline graphite.

[0061] The difference in the preparation method of the heating wire is: step 2, the high temperature resistant electric heating masterbatch with a particle size of 1.8-2.0 mm obtained in step 1 is put into a twin-screw extruder, melt-extruded at 240-260°C, and the obtained molten extrusion material is attached to the outer surface of the Vectran 50D aramid yarn. The pulling speed of the Vectran 50D aramid yarn is 4.0m / s. The Vectran 50D aramid yarn with the high temperature resistant electric heating composite material attached to the outer surface is water-cooled for 15s, sent to a 120°C oven for 30min heat treatment, and then sent to an 80°C oven for 120min drying treatment to obtain a finished heating wire. The thickness of the high temperature resistant electric heating composite layer is 208.4μm, and the resistivity of the finished heating wire is 15.30Ω·cm.

[0062] The difference between Example 10 and Example 9 is: Step 2, the high temperature resistant electric heating masterbatch with a particle size of 1.8-2.0 mm obtained in Step 1 is put into a twin-screw extruder, melt-extruded at 240-260°C, and the obtained molten extrusion material is attached to the outer surface of the Vectran 50D aramid yarn. The pulling speed of the Vectran 50D aramid yarn is 0.75m / s. The Vectran 50D aramid yarn with the high temperature resistant electric heating composite material attached to the outer surface is water-cooled for 15s, sent to a 1200°C oven for 30min heat treatment, and then sent to an 80°C oven for 120min drying treatment to obtain a finished heating wire. The thickness of the high temperature resistant electric heating composite layer is 1458.6μm, and the resistivity of the finished heating wire is 2.08Ω·cm.

[0063] The difference between Comparative Example 1 and Example 1 is that the high temperature resistant electric heating composite layer is made of a high temperature resistant electric heating masterbatch, and the high temperature resistant electric heating masterbatch is made of the following raw materials in mass percentage: 10wt% conductive filler composition, 1wt% surface modifier, 1wt% anti-aging additive, 5wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 909.8μm, and the resistivity of the finished heating wire is 87.35Ω·cm.

[0064] The difference between Comparative Example 2 and Example 1 is that the high temperature resistant electric heating composite layer is made of a high temperature resistant electric heating masterbatch, and the high temperature resistant electric heating masterbatch is made of the following raw materials in mass percentage: 50wt% conductive filler composition, 2wt% surface modifier, 1wt% anti-aging additive, 8wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 981.4μm, and the resistivity of the obtained finished heating wire is 15.51Ω·cm.

[0065] The difference between Comparative Example 3 and Example 1 is that the surface modifier is γ-methacryloxypropyltrimethoxysilane. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 965.1 μm, and the resistivity of the finished heating wire is 44.72 Ω·cm.

[0066] The difference between Comparative Example 4 and Example 1 is that the anti-aging additive is composed of antioxidant 1010, antioxidant 168, and anti-ultraviolet agent 326 in a mass ratio of 4:1:5. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 925.1 μm, and the resistivity of the finished heating wire is 40.19 Ω·cm.

[0067] The difference between Comparative Example 5 and Example 1 is that the conductive filler composition is made of 20wt% flake graphite and 80wt% microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 879.1μm, and the resistivity is 37.29Ω·cm.

[0068] The difference between Comparative Example 6 and Example 1 is that the conductive filler composition is made of 20wt% flake graphite, 10wt% molybdenum disilicide nanosheets and 70wt% microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 911.8μm, and the resistivity of the finished heating wire is 42.69Ω·cm.

[0069] The difference between Comparative Example 7 and Example 1 is that the conductive filler composition is made of 20wt% flake graphite, 5wt% nano silicon nitride and 75wt% microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 907.8μm, and the resistivity of the finished heating wire is 35.58Ω·cm.

[0070] The difference between Comparative Example 8 and Example 1 is that the conductive filler composition is made of 20wt% flake graphite, 20wt% nano-barium titanate, 10wt% molybdenum disilicide nanosheets and 50wt% microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 921.7μm, and the resistivity of the finished heating wire is 40.72Ω·cm.

[0071] The difference between Example 11 and Example 1 is that the high temperature resistant electric heating composite layer is made of the following raw materials in percentage by mass: 20wt% conductive filler composition, 0.8wt% surface modifier, 1.2wt% anti-aging agent, 4wt% hyperbranched PPS resin, and the remainder is thermoplastic polyphenylene sulfide resin PPS (Toray A504X90).

[0072] Preparation method of hyperbranched PPS resin: first, add 3,5-dichlorothiophenol 3,5-DB (2.5 g), anhydrous K2CO3 (3.350 g) and 20 mL anhydrous NMP (dried with anhydrous sodium sulfate to remove water) into a 100 mL three-necked flask equipped with a condenser and a magnet, evacuate and pass nitrogen three times, then heat the system in an oil bath under nitrogen flow, stir vigorously, heat to 150 ° C, continue to keep warm and react for 8 hours, cool to room temperature after the reaction, pour the product in the bottle into 75 mL of 6 mo l / L HCl solution, vigorously stirred for 2h, a large amount of precipitate was generated, the obtained precipitate was vacuum filtered, washed with a large amount of deionized water until the filtrate was colorless, vacuum filtered and separated, the product was vacuum dried at 40°C for 24h, and finally the dried product was dissolved with a small amount of tetrahydrofuran, added dropwise to 4 times the volume of anhydrous ethanol, and continued to stir for 1h to generate a large amount of precipitate, vacuum filtered again, and the filter cake was washed with a large amount of anhydrous ethanol until the filtrate was colorless, separated and dried to obtain an off-white powder product HPPS resin.

[0073] A method for preparing a high temperature resistant and stable heating wire comprises the following steps:

[0074] Step 1, production of raw materials for preparing high-temperature resistant electric heating composite layer: placing a conductive filler composition, a thermoplastic polyphenylene sulfide resin PPS, a surface modifier, a hyperbranched PPS resin, and an aging-resistant additive in a high-speed dispersion kettle and mixing them at 400 rpn for 60 minutes, placing the resulting mixture in a twin-screw extruder, and melt-extruded at 320-335°C, specifically, the feeding section temperature is 195°C, the barrel temperature is 300-335°C, the connector temperature is 320-335°C, and the die temperature is 300-320°C. The resulting molten extrudate is subjected to wire drawing, cooling, granulation, and drying to obtain a high-temperature resistant electric heating masterbatch with a particle size of 1.8-2.0 mm;

[0075] Step 2: Put the high temperature resistant electric heating masterbatch with a particle size of 1.8-2.0 mm obtained in step 1 into a twin-screw extruder, and melt extrude it at 320-335°C. Specifically, the temperature of the feeding section is 195°C, the temperature of the barrel is 300-335°C, the temperature of the connector is 320-335°C, and the temperature of the die is 300-320°C. The obtained molten extrusion material is attached to the outer surface of the Vectran 50D aramid yarn. The pulling speed of the Vectran 50D aramid yarn is 1.5m / s. After the 50D aramid yarn is cooled by water for 25 seconds, it is sent to a 1200℃ oven for heat treatment for 30 minutes and then sent to a 95℃ oven for drying for 120 minutes to obtain the finished heating wire. The thickness of the high-temperature resistant electric heating composite layer is 856.4μm. The resistivity of the obtained finished heating wire is 41.08Ω·cm. The steady-state heating temperature of the finished heating wire can be controlled by controlling the voltage.

[0076] The difference between Example 12 and Example 1 is that the high temperature resistant electric heating composite layer is made of the following raw materials in percentage by weight: 30wt% conductive filler composition, 1wt% surface modifier, 1.2wt% anti-aging additive, 5wt% hyperbranched PPS resin, and the remainder is thermoplastic polyphenylene sulfide resin PPS. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 860.5μm, and the resistivity of the finished heating wire is 32.45Ω·cm.

[0077] The difference between Example 13 and Example 1 is that the high temperature resistant electric heating composite layer is made of the following raw materials in percentage by weight: 40wt% conductive filler composition, 1wt% surface modifier, 1.2wt% anti-aging additive, 6wt% hyperbranched PPS resin, and the remainder is thermoplastic polyphenylene sulfide resin PPS. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 872.5μm, and the resistivity of the finished heating wire is 20.59Ω·cm.

[0078] The difference between Example 14 and Example 1 is that the conductive filler composition is made of the following raw materials in mass percentage: 12wt% flake graphite, 35wt% nano barium titanate, 3.2wt% titanium diboride whisker, 5.4wt% nano titanium nitride, 15wt% molybdenum disilicide nanosheets, and the balance is microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 867.1μm, and the resistivity of the finished heating wire is 41.74Ω·cm.

[0079] The difference between Example 15 and Example 1 is that the conductive filler composition is made of the following raw materials in mass percentage: 12wt% flake graphite, 35wt% nano barium titanate, 3.2wt% titanium diboride whisker, 5.4wt% nano titanium nitride, 15wt% molybdenum disilicide nanosheets, 2wt% graphene, and the balance is microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 875.1μm, and the resistivity of the finished heating wire is 28.74Ω·cm.

[0080] The difference between Example 16 and Example 1 is that the conductive filler composition is made of the following raw materials in mass percentage: 5wt% flake graphite, 20wt% nano barium titanate, 1wt% titanium diboride whisker, 3wt% nano titanium nitride, 5wt% molybdenum disilicide nanosheets, 5wt% graphene, and the balance is microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 867.9.5μm, and the resistivity of the finished heating wire is 13.56Ω·cm.

[0081] The difference between Comparative Example 9 and Example 1 is that the high temperature resistant electric heating composite layer is made of the following raw materials in mass percentage: 10wt% conductive filler composition, 0.8wt% surface modifier, 1.2wt% anti-aging additive, 4wt% hyperbranched PPS resin, and the remainder is thermoplastic polyphenylene sulfide resin PPS. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 867.2μm, and the resistivity of the finished heating wire is 93.75Ω·cm.

[0082] The difference between Comparative Example 10 and Example 1 is that the high temperature resistant electric heating composite layer is made of the following raw materials in mass percentage: 45wt% conductive filler composition, 0.8wt% surface modifier, 1.2wt% anti-aging additive, 6wt% hyperbranched PPS resin, and the remainder is thermoplastic polyphenylene sulfide resin PPS. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 877.5μm, and the resistivity of the finished heating wire is 17.41Ω·cm.

[0083] The difference between Comparative Example 11 and Example 1 is that the high temperature resistant electric heating composite layer is made of the following raw materials in mass percentage: 20wt% conductive filler composition, 0.8wt% surface modifier, 1.2wt% anti-aging additive, and the balance is thermoplastic polyphenylene sulfide resin PPS. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 938.4μm, and the resistivity of the finished heating wire is 52.08Ω·cm.

[0084] The difference between Comparative Example 12 and Example 1 is that the surface modifier is γ-methacryloxypropyltrimethoxysilane. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 879.5 μm, and the resistivity of the finished heating wire is 45.54 Ω·cm.

[0085] The difference between Comparative Example 13 and Example 1 is that the anti-aging additive is composed of antioxidant 1010, antioxidant 168, and anti-ultraviolet agent 326 in a mass ratio of 4:1:5. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 881.4 μm, and the resistivity of the finished heating wire is 41.64 Ω·cm.

[0086] The difference between Comparative Example 14 and Example 1 is that the conductive filler composition is made of 20wt% flake graphite and 80wt% microcrystalline graphite. The thickness of the high temperature resistant electric heating composite layer in the finished heating wire is 851.5μm, and the resistivity is 38.32Ω·cm.

[0087] Table 1: Test parameters of finished heating wires in Examples 1-10 and Comparative Examples 1-8

[0088]

[0089] It can be seen from Examples 1-10 and Comparative Examples 1-8 and Table 1 that the conductive filler composition compounded in the present application can give the heating wire good conductivity and high temperature resistant stability. The resistivity of the finished heating wire in the present application is 0.5-50Ω·cm. After 1000 cycles of heating tests, the resistance value change rate of the heating wire at 25°C is less than 3%, and the resistance value change rate at 200°C is less than 5%. It is used in the field of heating wires with PTC effect, and is specifically used in the insulation of oil pipelines.

[0090] It can be seen from Examples 1-10 and Comparative Examples 1-8 and Table 1 that the resistance stability of the finished heating wire obtained by using the composite surface modifier in the present application is better and the conductive filler composition is evenly dispersed to ensure the overall mechanical strength of the heating wire.

[0091] It can be seen from Examples 1-10 and Comparative Examples 1-8 and Table 1 that the resistance stability and heat stability of the finished heating wire obtained by using the compound anti-aging additive in the present application are better and it is convenient to reduce the thermal oxidation degradation of the resin processing plastic, thereby improving the overall high temperature resistance stability, service life and mechanical strength.

[0092] Table 2: Time-temperature parameter table of the finished heating wire in Example 1 at 110V voltage

[0093]

[0094] Table 3: Time-temperature parameter table of the finished heating wire in Example 9 at 110V voltage

[0095]

[0096] Table 4: Time-temperature parameter table of the finished heating wire in Example 10 at 36V voltage

[0097]

[0098] It can be seen from Example 1 and Examples 9-10 and Tables 2-4 that the heating wire of the product prepared in the present application can be used at 36-110V, the steady-state temperature is controlled at 200°C, and has excellent high-temperature resistance and stability.

[0099] Table 5: Test parameters of finished heating wires in Examples 11-16 and Comparative Examples 9-14

[0100]

[0101]

[0102] It can be seen from Examples 11-16 and Comparative Examples 9-14 and Table 5 that the conductive filler composition compounded in the present application can give the heating wire good conductivity and high temperature resistant stability. The resistivity of the finished heating wire in the present application is 0.5-50Ω·cm. After 1000 cycles of heating tests, the resistance value change rate of the heating wire at 25°C is less than 1.8%, and the resistance value change rate at 200°C is less than 3.5%.

[0103] Combining Examples 11-16 and Comparative Examples 9-14 and Table 2, it can be seen that the resistance stability of the finished heating wire obtained by using the surface modifier in the present application is better and the conductive filler composition is evenly dispersed to ensure the overall mechanical strength of the heating wire.

[0104] It can be seen from Examples 11-16 and Comparative Examples 9-14 and Table 2 that the resistance stability and heat stability of the finished heating wire obtained by using the anti-aging additive in the present application are better and it is convenient to reduce the thermal oxidation degradation of the resin processing plastic, thereby improving the overall high temperature resistance stability, service life and mechanical strength.

[0105] Table 6: Time-temperature parameter table of the finished heating wire in Example 16 at 72V voltage

[0106]

[0107] In summary, the heating wire prepared in the present application can be used stably at -40 to 200°C, and after 1000 cycles of heating tests, the resistance value change rate of the heating wire at 25°C is less than 3%, and the resistance value change rate at 200°C is less than 5%.

[0108] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high temperature resistant and stable heating wire, characterized in that: It comprises a core wire and a high temperature resistant electric heating composite layer coated on the outer wall of the core wire, wherein the high temperature resistant electric heating composite layer is composited with a plated insulating layer; the thickness of the high temperature resistant electric heating composite layer is 50-1500 μm; the resistivity of the high temperature resistant electric heating composite layer is 0.5-50 Ω·cm; the high temperature resistant electric heating composite layer contains at least a conductive filler composition, a high temperature resistant organic polymer, a surface modifier, and an anti-aging additive, wherein the content of the conductive filler composition is 20-40 wt%; the high temperature resistant organic polymer is a thermosetting high temperature resistant resin or a thermoplastic high temperature resistant resin.

2. A high temperature resistant and stable heating wire according to claim 1, characterized in that: The thermosetting high temperature resistant resin includes at least one of thermosetting polyphenylene sulfide resin PPS and thermosetting polyimide resin TPI; the thermoplastic high temperature resistant resin includes at least one of thermoplastic polyimide resin TPI, thermoplastic polyphenylene sulfide resin PPS and thermoplastic fluorocarbon resin; the polytetrafluoroethylene resin includes at least one of polytetrafluoroethylene PTFE, polytrifluorochloroethylene PCTFE, polyvinylidene fluoride PVDF, ethylene-tetrafluoroethylene copolymer ETFE and ethylene-trifluorochloroethylene copolymer ECTFE.

3. A high temperature resistant and stable heating wire according to claim 2, characterized in that: The high temperature resistant electric heating composite layer is made of the following raw materials in percentage by mass: 20-40wt% conductive filler composition, 0.8-1wt% surface modifier, 0.8-1.6wt% anti-aging additive, 3-6wt% hyperbranched PPS resin, and the remainder is thermoplastic polyphenylene sulfide resin PPS.

4. A high temperature resistant and stable heating wire according to claim 2, characterized in that: The high temperature resistant electric heating composite layer is made of the following raw materials in percentage by mass: 20-40wt% conductive filler composition, 1.2-1.8wt% surface modifier, 0.6-1.2wt% anti-aging additive, 4-8wt% dibutyl phthalate DBP, and the balance is polyvinylidene fluoride PVDF.

5. A high temperature resistant and stable heating wire according to claim 3 or 4, characterized in that: The surface modifier is composed of at least one of 3-isocyanate propyl triethoxy silane, γ-methacryloxy propyl trimethoxy silane, γ-glycidyloxy propyl trimethoxy silane and γ-aminopropyl triethoxy silane and a titanate coupling agent HY-201.

6. A high temperature resistant and stable heating wire according to claim 3 or 4, characterized in that: The anti-aging agent is composed of at least one of silicon nitride and silicon dioxide, antioxidant 1010, antioxidant 168, and anti-ultraviolet agent 326.

7. A high temperature resistant and stable heating wire according to claim 3 or 4, characterized in that: The conductive filler composition is made of the following raw materials in percentage by mass: 5-20wt% of flake graphite, 20-40wt% of nano barium titanate, 1-5wt% of titanium diboride whiskers, 3-8wt% of titanium nitride, 5-20wt% of molybdenum disilicide nanosheets, 0-5wt% of graphene, and the balance is microcrystalline graphite.

8. A high temperature resistant and stable heating wire according to claim 7, characterized in that: The conductive filler composition is made of the following raw materials in percentage by mass: 10-12wt% of flake graphite, 32-36wt% of nano barium titanate, 2-4wt% of titanium diboride whiskers, 5-6wt% of titanium nitride, 10-15wt% of molybdenum disilicide nanosheets, 0.5-2wt% of graphene, and the balance is microcrystalline graphite.

9. A method for preparing a high temperature resistant and stable heating wire according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Production of raw materials for preparing high temperature resistant electric heating composite layer: When a thermosetting high temperature resistant resin is used in the high temperature resistant electric heating composite layer, the thermosetting high temperature resistant resin monomer is first reacted to a system viscosity of 6000-20000 mPa·s / 25°C, and then a conductive filler composition, a surface modifier, and an anti-aging additive are added in accurate amounts and mixed evenly to obtain a high temperature resistant electric heating slurry; When a thermoplastic high temperature resistant resin is used in the high temperature resistant electric heating composite layer, the conductive filler composition, the thermoplastic high temperature resistant resin, the surface modifier, and the anti-aging additive are melt-extruded, wire-drawn, cooled, granulated, and dried to obtain a high temperature resistant electric heating masterbatch; Step 2: When the high temperature resistant electric heating composite layer is made of high temperature resistant electric heating slurry, the core wire is immersed in the high temperature resistant electric heating slurry, and the core wire is pulled at a speed of 1-10 cm / s, so that the high temperature resistant electric heating slurry adheres to the outer wall of the core wire, and then the core wire is transferred to an oven for curing, that is, the high temperature resistant electric heating composite layer is compounded on the outside of the core wire, and finally the high temperature resistant electric heating composite layer is compounded with a coated insulating layer to obtain a finished heating wire; When the high temperature resistant electric heating composite layer is made of high temperature resistant electric heating masterbatch, the molten extruded material obtained by melt-extruding the high temperature resistant electric heating masterbatch is attached to the outer surface of the core wire, and the finished heating wire can be obtained by water cooling, heat treatment and drying.

10. A high temperature resistant and stable heating wire according to any one of claims 1 to 8, applied to the field of heating cables with PTC effect.

Citation Information

Patent Citations

  • Electric heating wire with intelligent temperature control function and heating die assembly prepared by using electric heating wire

    CN116489838A

  • High-temperature-resistant low-expansion PI mold composite material for machining and preparation method thereof

    CN117089199A

  • Quick heating wire material with intelligent temperature control function and preparation method thereof

    CN118359900A

  • High-temperature-resistant graphene electrothermal coating and preparation method thereof

    CN118515994A

  • Graphene electrothermal material and application thereof

    WO2017114174A1