Method for eliminating plate edge bubbles after high-speed material electroplating
By introducing laser drilling and optimized electroplating processes into optical module products, the problems of loose dielectric layer structure and bubbles at the board edge have been solved, improving interlayer bonding and product reliability while maintaining optimized production costs.
Patent Information
- Application Number
- CN202411054140.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In existing technologies, excessive removal of adhesive from the dielectric layer material at the board edge after plasma adhesive removal in optical module products leads to a loose dielectric layer structure, and bubbles appear at the board edge after chemical copper plating and electroplating.
By introducing laser drilling technology at the edge of the PCB board and filling the copper with solid copper during the copper plating process, combined with optimized development, acid etching, film removal and electroplating processes, the bonding strength of the copper teeth is ensured, thus solving the problem of bubbling at the board edge.
It significantly improves interlayer tensile strength, solves the problems of loose dielectric layer structure and bubble at the edge of the board in traditional methods, while maintaining optimized production costs and product reliability.
Smart Images

Figure CN118921858A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical module product manufacturing, and in particular to a method for eliminating board edge blistering after high-speed material electroplating. Background Art
[0002] Conventional design and manufacturing solutions for optical module products (such as Figure 2 ), based on the traditional copper window opening + laser hole opening process, due to the problem of edge retention of photosensitive dry film, the board edge cannot be completely covered, resulting in the exposure of the dielectric layer material after acid etching. Since the optical module product needs to reduce signal loss and achieve efficient signal transmission, high-frequency + high-speed materials need to be selected. Due to the characteristics of high-frequency and high-speed materials, it is impossible to solve the residual glue at the bottom of the laser hole through a single chemical (permanganate) degumming. Plasma degumming needs to be added after laser hole opening. The plasma degumming process is through the high-speed impact of physical charged particles + chemical cross-linking and etching (such as Figure 3 ), remove the glue and roughen the surface of the dielectric layer at the same time, so as to improve the bonding strength of the subsequent copper deposition;
[0003] However, due to the difference in debonding rate between the laser hole and the open area at the edge of the board, the SEM (scanning electron microscope) 5000x image after plasma debonding clearly shows that the dielectric layer material at the edge of the board is over-debonded after plasma debonding (e.g. Figure 4-6 ) causes the dielectric layer structure to become loose; bubbles appear at the edge of the board after chemical copper deposition + electroplating (such as Figure 4-6 ). Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a method for eliminating bubbles at the edge of a board after high-speed material electroplating, which solves the problem in the background technology that excessive degumming of the dielectric layer material at the edge of the board after plasma degumming leads to a loose dielectric layer structure, and bubbles appear at the edge of the board after chemical copper deposition + copper electroplating.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: a method for eliminating blistering at the edge of a plate after high-speed material electroplating, the steps of which are as follows:
[0006] S01: Paste photosensitive film; press photosensitive dry film on the surface of high-frequency ultra-low copper foil on the upper surface of copper-containing substrate;
[0007] S02: Dry film exposure and development: UV light is irradiated to the dry film in the non-circuit area by an exposure machine to cause polymerization reaction, and then the dry film that has not undergone polymerization reaction is removed by a developer;
[0008] S03: Acid etching: By acid etching, the copper at the position not covered by the photosensitive film will be etched;
[0009] S04: Stripping: Use the stripping solution to peel off the dry film layer. At this time, the high-frequency ultra-low copper tooth copper foil laser hole opening is completed;
[0010] S05: Laser drilling: Use laser drilling technology to make high-frequency ultra-low copper teeth copper foil and laser blind holes between dielectric layers;
[0011] S06: Hole filling electroplating: Copper is plated on the laser hole and the surface by hole filling electroplating to connect the high-frequency ultra-low copper foil and dielectric layer circuit.
[0012] Preferably, before laminating the photosensitive dry film in S01, the surface of the high-frequency ultra-low copper foil needs to be cleaned; the photosensitive film is cut to a suitable size and accurately aligned with the surface of the high-frequency ultra-low copper foil to ensure full coverage, and the photosensitive dry film needs to be preheated before laminating;
[0013] It is beneficial to improve the adhesion of high-frequency ultra-low copper foil and reduce the generation of bubbles.
[0014] Preferably, the developer type in S02 is an alkaline aqueous solution, and tetramethylammonium hydroxide (TMAH) is selected as the developer of the positive photoresist. The development temperature is controlled at 21-23°C with an error of ±0.5°C. After the development is completed, it is immediately rinsed with deionized water to remove all residual chemicals, and necessary drying treatment is performed.
[0015] Preferably, the exposure dose calculation method of the exposure machine in S02 is:
[0016] E=I×t
[0017] Where: E is the exposure dose (mJ / cm2); I is the light intensity (mW / cm2); t is the exposure time (s); the light intensity calculation method is: P is the power of the light source (W); A is the area of the exposure area (m2); the exposure time t is calculated as: Accurately calculating the exposure machine parameters helps to fully initiate the polymerization reaction initiated by the photosensitizer in the dry film; avoid insufficient exposure dose, incomplete polymerization reaction, and insufficient or uneven pattern adhesion after development; and avoid excessive exposure dose, which leads to excessive cross-linking of the dry film and affects subsequent development and etching steps.
[0018] Preferably, the acidic etching solution in S03 includes: ferric chloride; which can effectively react with copper to dissolve it; the chemical composition of the ferric chloride etching solution includes ferric chloride itself, ferric dichloride and free hydrochloric acid;
[0019] Hydrochloric acid: Hydrochloric acid plays a role in maintaining the pH value of the solution and promoting the dissolution of copper in the etching solution.
[0020] The addition of hydrochloric acid can inhibit the hydrolysis of ferric chloride and increase the etching rate;
[0021] Sodium chloride or ammonium chloride: as an auxiliary component of the etching solution, it helps to improve etching efficiency and etching quality;
[0022] Ammonium persulfate: Ammonium persulfate can act as an oxidant to participate in the etching reaction and increase the etching rate.
[0023] Preferably, the film stripping temperature in S04 is controlled between 50° C. and 55° C.; and the optimal film stripping time is determined through a film stripping experiment.
[0024] Preferably, the drilling process in S05 is carried out in a nitrogen or argon atmosphere to reduce the possibility of material oxidation. Preferably, after drilling in S05, the PCB is immersed in a cleaning solution containing a cleaning agent, and the residual glue on the hole wall is peeled off by the cavitation effect generated by ultrasound; the frequency of the ultrasound is 100kHz-250kHz, the power is 15-25W / L, the temperature of the cleaning solution is 40℃-60℃, and a thorough cleaning and activation treatment is performed before electroplating to ensure that the hole wall surface is clean and enhance the adhesion of the coating.
[0025] Preferably, the electroplating current density in S06 is controlled within the range of 2-5A / dm2 to achieve good coating quality and deposition rate; the temperature of the electroplating solution is controlled within the range of 20-40°C, too high a temperature may cause decomposition of the additive, while too low a temperature may slow down the electroplating rate and affect the coating quality; the pH value of the electroplating solution is maintained between 7.5-8.5 to ensure the stability of the electroplating process and the uniformity of the coating.
[0026] Proper stirring can also help maintain a uniform distribution of copper ions in the electroplating solution and avoid uneven plating due to concentration gradients.
[0027] The present invention provides a method for eliminating blistering at the edge of a plate after high-speed material electroplating. It has the following beneficial effects:
[0028] This method is based on eliminating blistering on the edge of the board after high-speed material electroplating. By introducing laser drilling technology in the copper-free area of the PCB edge and filling solid copper during the copper plating process, it not only significantly improves the interlayer tensile strength, but also cleverly solves the problem of insufficient gripping force between the traditional electroplating layer and the dielectric layer due to the lack of copper teeth. At the same time, it has high adaptability and flexibility, and can easily adjust the number of laser holes according to the size of the copper-free area on the edge of the board to meet different structural strength requirements.
[0029] In addition, since this added laser hole copper plating process is perfectly synchronized with the existing laser opening process flow, it does not bring additional production steps, thus maintaining the optimization of production costs; this innovative approach not only improves the reliability and durability of the product, but also reflects the improvement of performance through technological innovation without increasing costs.
[0030] The invention solves the problem that the dielectric layer material at the edge of the board is excessively debonded after plasma debonding, resulting in a loose dielectric layer structure, and bubbles appear at the edge of the board after chemical copper deposition + electroplating. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the process of the present invention;
[0032] Figure 2 This is a schematic diagram of a conventional design solution for optical module products;
[0033] Figure 3 It is a schematic diagram of the glue removal principle;
[0034] Figure 4 This is a schematic diagram of the hole after conventional glue removal;
[0035] Figure 5 This is a schematic diagram of the board edge after conventional degumming;
[0036] Figure 6 This is a schematic diagram of bubbles on the edge of the plate after copper plating;
[0037] Figure 7 This is a schematic diagram of the improved board edge of the present invention;
[0038] Figure 8 This is a schematic diagram of the board edge of the conventional method;
[0039] Fig. 9 It is a schematic diagram of the principle of the present invention. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] See also Figure 1 The embodiment of the present invention provides a technical solution: a method for eliminating blistering at the edge of a plate after high-speed material electroplating, the steps of which are as follows:
[0042] S01: Pasting photosensitive film; Pressing photosensitive dry film on the surface of high-frequency ultra-low copper foil on the copper-containing substrate; S02: Exposure and development of dry film; Exposure machine irradiates ultraviolet light to the dry film in non-circuit area to make it polymerize, and then removes the dry film that has not polymerized by developing developer; S03: Acid etching; The copper in the position not covered by the photosensitive film will be etched by acid etching; S04: Stripping; The dry film layer is peeled off by using stripping solution, and the window opening of the high-frequency ultra-low copper foil laser hole is completed at this time; S05: Laser drilling; Laser drilling process is used to make laser blind holes between high-frequency ultra-low copper foil and dielectric layer; S06: Hole filling electroplating; The laser hole and surface are plated with copper by hole filling electroplating to connect the high-frequency ultra-low copper foil and dielectric layer circuit.
[0043] In S01, before laminating the photosensitive dry film, the surface of the high-frequency ultra-low copper foil needs to be cleaned to ensure that the surface is clean, free of oil, fingerprints and dust; the photosensitive film is cut to a suitable size and accurately aligned with the surface of the high-frequency ultra-low copper foil to ensure full coverage. The photosensitive dry film needs to be preheated before laminating; this is beneficial to improve the adhesion of the high-frequency ultra-low copper foil and reduce the generation of bubbles.
[0044] The developer type in S02 is an alkaline aqueous solution. Tetramethylammonium hydroxide (TMAH) is selected as the developer of positive photoresist. The development temperature is controlled at 21°C with an error of ±0.5°C. After the development is completed, it is immediately rinsed with deionized water to remove all residual chemicals, and necessary drying treatment is performed.
[0045] The acidic etching solution in S03 includes: ferric chloride; it can effectively react with copper and dissolve it; the chemical composition of ferric chloride etching solution includes ferric chloride itself, ferric chloride and free hydrochloric acid; hydrochloric acid: hydrochloric acid plays a role in maintaining the pH value of the solution and promoting the dissolution of copper. The addition of hydrochloric acid can inhibit the hydrolysis of ferric chloride and increase the etching rate; sodium chloride or ammonium chloride: as an auxiliary component of the etching solution, it helps to improve the etching efficiency and improve the etching quality; ammonium persulfate: ammonium persulfate can participate in the etching reaction as an oxidant to increase the etching rate.
[0046] In S04, the stripping temperature is controlled between 50℃; and the best stripping time is determined through the stripping experiment. The stripping experiment method is as follows: a: Prepare samples; prepare several PCB board samples of the same material and thickness to ensure that they have a consistent dry film layer; determine the variable in the experiment, the variable is the stripping time; set up one or more control groups, use the known stripping time as a benchmark to compare the experimental results; formulate a series of different stripping times, starting from 10 seconds, and gradually increase the time interval by 10 seconds each time; ensure that all other conditions except the stripping time remain constant, including the temperature, concentration, and stirring speed of the stripping solution;
[0047] b: Conduct experiments; process PCB samples according to different stripping times; ensure that the immersion time of each board in the stripping solution is precisely controlled; take out the PCB at each time point, observe the removal of the dry film, and record it; use a microscope or other detection tools to evaluate the removal effect of the dry film; pay attention to whether there is any dry film residue that has not been completely removed or damage caused by excessive stripping;
[0048] c: Data analysis: Analyze the experimental data to find out the best time period for dry film removal. The best film removal time should be the time point when the dry film is completely removed and the copper foil surface is not damaged. In order to verify the consistency of the results, repeat the experiment on the best film removal time.
[0049] The drilling process in S05 is carried out under nitrogen or argon atmosphere to reduce the possibility of material oxidation.
[0050] After drilling in S05, the PCB is immersed in a cleaning solution containing a cleaning agent, and the residual glue on the hole wall is peeled off by the cavitation effect generated by ultrasound; the frequency of the ultrasound is 100kHz, the power is 15W / L, the temperature of the cleaning solution is 40°C, and a thorough cleaning and activation treatment is performed before electroplating to ensure that the hole wall surface is clean and enhance the adhesion of the coating.
[0051] In S06, the electroplating current density is controlled at 2A / dm2 to achieve good coating quality and deposition rate; the temperature of the electroplating solution is controlled at 20°C. Too high a temperature may cause the additive to decompose, while too low a temperature may slow down the electroplating rate and affect the coating quality; the pH value of the electroplating solution is maintained at 7.5 to ensure the stability of the electroplating process and the uniformity of the coating. Appropriate stirring can also help maintain the uniform distribution of copper ions in the electroplating solution to avoid uneven coating caused by concentration gradients. Design of adding laser holes on the edge of the board ( Figure 7 ) scheme and conventional design ( Figure 8 ) compared to the previous method, the problem of completely relying on the bonding strength between the electroplated copper layer and the dielectric material is solved by adding laser holes between the upper and lower plates and filling the holes with electroplating ( Fig. 9 ), the metal copper in the laser hole strengthens the tensile strength between the board layers, effectively solving the problems of bubbling and delamination at the edge of the board.
[0052] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.
[0053] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for eliminating blistering on the edge of a plate after high-speed material electroplating, characterized in that: The steps are as follows: S01: Paste photosensitive film; press photosensitive dry film on the surface of high-frequency ultra-low copper foil on the upper surface of copper-containing substrate; S02: Dry film exposure and development: UV light is irradiated to the dry film in the non-circuit area by an exposure machine to cause polymerization reaction, and then the dry film that has not undergone polymerization reaction is removed by a developer; S03: Acid etching: By acid etching, the copper at the position not covered by the photosensitive film will be etched; S04: Stripping: Use the stripping solution to peel off the dry film layer. At this time, the high-frequency ultra-low copper tooth copper foil laser hole opening is completed; S05: Laser drilling: Use laser drilling technology to make high-frequency ultra-low copper teeth copper foil and laser blind holes between dielectric layers; S06: Hole filling electroplating: Copper is plated on the laser hole and the surface by hole filling electroplating to connect the high-frequency ultra-low copper foil and dielectric layer circuit.
2. According to claim 1, a method for eliminating board edge blistering after high-speed material electroplating, characterized in that: In the S01, before laminating the photosensitive dry film, the surface of the high-frequency ultra-low copper foil needs to be cleaned; the photosensitive film is cut to a suitable size and accurately aligned with the surface of the high-frequency ultra-low copper foil to ensure full coverage. The photosensitive dry film needs to be preheated before laminating.
3. According to claim 1, a method for eliminating board edge blistering after high-speed material electroplating, characterized in that: The developer in S02 is an alkaline aqueous solution, and tetramethylammonium hydroxide (TMAH) is selected as the developer of the positive photoresist. The developing temperature is controlled at 21-23° C. with an error of ±0.5° C.; After development, rinse immediately with deionized water to remove any residual chemicals and dry as necessary.
4. According to claim 1, a method for eliminating board edge blistering after high-speed material electroplating, characterized in that: The method for calculating the exposure dose of the exposure machine in S02 is: E=I×t Where: E is the exposure dose (mJ / cm2); I is the light intensity (mW / cm2); t is the exposure time (s); the light intensity calculation method is: P is the power of the light source (W); A is the area of the exposure area (m2); the exposure time t is calculated as:
5. According to claim 1, a method for eliminating board edge blistering after high-speed material electroplating, characterized in that: The acidic etching solution in the S03 includes: ferric chloride, hydrochloric acid, sodium chloride or ammonium chloride, and ammonium persulfate.
6. According to claim 1, a method for eliminating board edge blistering after high-speed material electroplating, characterized in that: In S04, the film stripping temperature is controlled between 50° C. and 55° C., and the optimal film stripping time is determined through a film stripping experiment.
7. According to claim 1, a method for eliminating board edge blistering after high-speed material electroplating, characterized in that: The drilling process in S05 is performed under a nitrogen or argon atmosphere to reduce the possibility of material oxidation.
8. The method for eliminating blistering at the edge of a plate after high-speed material electroplating according to claim 1, characterized in that: After drilling in S05, the PCB is immersed in a cleaning solution containing a cleaning agent, and the residual glue on the hole wall is peeled off by the cavitation effect generated by ultrasound; the frequency of the ultrasound is 100kHz-250kHz, the power is 15-25W / L, the temperature of the cleaning solution is 40℃-60℃, and a thorough cleaning and activation treatment is performed before electroplating to ensure that the hole wall surface is clean and enhance the adhesion of the coating.
9. The method for eliminating board edge blistering after high-speed material electroplating according to claim 1, characterized in that: The electroplating current density in S06 is controlled within the range of 2-5A / dm2; the temperature of the electroplating solution is controlled within the range of 20-40°C; and the pH value of the electroplating solution is maintained between 7.5-8.5 to ensure the stability of the electroplating process and the uniformity of the coating.
Citation Information
Patent Citations
Electronic product window and manufacturing method thereof and electronic product
CN101686618A
Manufacturing method of step circuit board and the step circuit board
CN108696995A
Fabrication method for PCB with metal half holes in board edge
CN108738248A
Laser drilling device for LCP flexible circuit board
CN110337188A
Conductive hole and preparation method and application thereof