Water-absorbent resin composition, method for producing same, absorbent body, and absorbent article

By combining surface-crosslinked water-absorbing resin particles with specific chelating agents, the problems of easy gel deterioration and difficulty in reducing gel strength under ultraviolet radiation are solved, achieving gel stability and easy separation, which is suitable for sanitary materials.

CN118922246APending Publication Date: 2024-11-08SUMITOMO SEIKA CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380029507.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing absorbent resins are prone to gel deterioration during use, leading to reduced absorbency. Furthermore, the release of water-soluble substances during gel decomposition may cause skin rashes, and ultraviolet radiation is not effective in reducing gel strength.

Method used

A composition comprising surface-crosslinked water-absorbing resin particles and a chelating agent is used. The iron(III) chelate stability constant of the chelating agent is above 16 log KML and below 24 log KML, and the number of carboxyl groups is above 4 and below 10. This composition improves the stability of the gel and makes it easy to separate after ultraviolet irradiation.

Benefits of technology

It maintains the stability of the gel in sanitary materials, while effectively separating the water-absorbing resin composition after ultraviolet irradiation, improving workability and reducing the leaching of water-soluble substances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005054747080000381
    Figure BDA0005054747080000381
  • Figure HDA0005054747090000011
    Figure HDA0005054747090000011
  • Figure HDA0005054747090000012
    Figure HDA0005054747090000012
Patent Text Reader

Abstract

Provided is a water-absorbent resin composition which, in a sanitary material, has both the gel stability of the water-absorbent resin composition when worn normally and the high workability when the water-absorbent resin composition is subjected to a separation treatment after ultraviolet irradiation as a waste treatment means. A water-absorbent resin composition containing water-absorbent resin particles and a chelating agent, in which the water-absorbent resin particles have been subjected to a surface crosslinking treatment, the iron (III) chelate stability constant of the chelating agent is from 16 logKML to 24 logKML (inclusive), and the number of carboxyl groups is from 4 to 10 (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a water-absorbent resin composition and a method for producing the same, an absorbent body and an absorbent article, and more particularly to a water-absorbent resin composition constituting an absorbent body suitable for use in sanitary materials such as disposable diapers, sanitary napkins and incontinence pads, a method for producing the water-absorbent resin composition, an absorbent body and an absorbent article. Background Art

[0002] In recent years, water-absorbent resins have been widely used in the field of sanitary materials such as diapers, sanitary napkins, and incontinence pads.

[0003] As such a water-absorbing resin, a cross-linked product of a partially neutralized salt polymer of acrylic acid has excellent water absorption performance. In addition, since acrylic acid as a raw material is easily available industrially, it has many advantages such as stable quality, can be produced at low cost, and is unlikely to become corrupted or deteriorated. Therefore, it is considered to be a preferred water-absorbing resin. Prior art literature Patent Literature

[0004] Patent Document 1: Japanese Patent Application Publication No. 2005-29751 Summary of the invention Technical problem to be solved by the invention

[0005] The gel produced by the water-absorbent resin by absorbing body fluids such as human urine usually deteriorates over time, so its absorbency decreases. In addition, if the gel deteriorates further, the water-absorbent resin itself partially decomposes, so that water-soluble solutes are dissolved from the gel. When a product using the water-absorbent resin is used in contact with the human body, the dissolved water-soluble solutes adhere to the skin and may cause rashes, etc. (see Patent Document 1). Therefore, in sanitary materials, the water-absorbent resin is required to have gel stability when normally worn.

[0006] In addition, absorbent articles such as disposable diapers, sanitary napkins, and incontinence pads are mainly composed of an absorbent body arranged in the center to absorb and retain body fluids such as urine and menstrual blood excreted from the body, a liquid-permeable surface sheet (top sheet) arranged on the side in contact with the body, and a liquid-impermeable back sheet (back sheet) arranged on the opposite side in contact with the body. The absorbent body is usually composed of hydrophilic fibers such as pulp and a water-absorbent resin.

[0007] When discarding a used absorbent article, in the method of separating the water-absorbent resin from the absorbent body, it is considered to use some means to appropriately reduce the gel strength of the water-absorbent resin, thereby facilitating the separation of the gel from other materials (hydrophilic fibers, etc.) contained in the absorbent body and improving the workability. As such means, ultraviolet irradiation, addition of a gel deterioration accelerator, etc. are used.

[0008] However, if the gel stability of the water-absorbent resin is improved, there is a problem that the gel strength is less likely to decrease even if ultraviolet irradiation or the like is used.

[0009] Under such circumstances, a main object of the present invention is to provide a water-absorbent resin composition having both gel stability of the water-absorbent resin composition when normally worn in sanitary materials and high handleability when the water-absorbent resin composition is separated after ultraviolet irradiation as a disposal means. Technical solutions for solving technical problems

[0010] The present inventors have conducted intensive research to solve the above technical problems. As a result, they have found that the above technical problems can be solved by using a water-absorbent resin composition comprising water-absorbent resin particles subjected to surface crosslinking treatment and a chelating agent, thereby satisfying the prescribed iron (III) chelate stability constant and number of carboxyl groups as a chelating agent. The present invention was completed based on such findings and further intensive research.

[0011] That is, the present invention provides an invention having the following configuration. Item 1. A water-absorbent resin composition comprising water-absorbent resin particles and a chelating agent, The water-absorbent resin particles are surface cross-linked. The chelating agent has an iron (III) chelate stability constant of 16 log KML or more and 24 log KML or less, and has a carboxyl group number of 4 or more and 10 or less. Item 2. The water-absorbent resin composition according to Item 1, wherein the degree of change in gel strength after UV irradiation is 40% or more. (Gel strength change after UV irradiation) From the initial value of the gel strength (gel strength (A)) and the value of the gel strength after ultraviolet irradiation (gel strength (C)) obtained in the following steps 1 and 2, the change (%) of the gel strength after UV irradiation was calculated by the following formula. Change in gel strength after UV irradiation (%) = [(gel strength (A) - gel strength (C)) / gel strength (A)] × 100 (Initial value of gel strength (gel strength (A)) The swollen gel prepared in the following step 1 was allowed to stand at 25±2°C and 50±10% relative humidity for 60 minutes after preparation, and then the gel strength (initial value of gel strength) was measured in the following step 2. The gel strength value at this time was recorded as gel strength (A). (Value of gel strength after ultraviolet irradiation (gel strength (C)) The swollen gel prepared by the following step 1 is allowed to stand at a temperature of 37±2°C and a relative humidity of 60±10% for 14 hours after preparation. Then, the swollen gel after standing is placed directly below the light source of the ultraviolet irradiation device in an environment of a temperature of 25±2°C and a relative humidity of 50±10%. At this time, the distance between the surface of the swollen gel and the light source is set to 7 cm. After shielding the entire device with a box, the swollen gel in the beaker is irradiated with ultraviolet rays of a wavelength of 254nm for 150 minutes. After ultraviolet irradiation, the gel strength is measured by the following step 2. The value of the gel strength at this time is recorded as the gel strength (C). Step 1 (Preparation of swollen gel) 39.0 g of artificial urine was measured in a beaker with an internal volume of 100 mL, and a magnetic stirrer was placed on the beaker, which was rotated at 600 rpm. Next, 1.00 g of the water-absorbent resin composition was placed in the stirring beaker, and the mixture was stirred until the vortex disappeared and the liquid surface became horizontal, thereby preparing a swollen gel as a measurement sample. Immediately after the swollen gel was prepared, the beaker containing the swollen gel was covered with plastic wrap. Step 2 (Determination of gel strength) Gel strength value (N / m 2 ) is measured using a curd meter according to the conditions of temperature and standing time for the initial value of the gel strength (gel strength (A)) and the value of the gel strength after ultraviolet irradiation (gel strength (C)). Item 3. The water-absorbent resin composition according to Item 1 or 2, wherein the content of the chelating agent is 0.001 parts by mass or more and 2 parts by mass or less relative to 100 parts by mass of the water-absorbent resin particles. Item 4. The water-absorbent resin composition according to any one of Items 1 to 3, wherein the water-absorbent resin composition has a physiological saline water retention capacity of 25 g / g or more and 60 g / g or less. Item 5. The water-absorbent resin composition according to any one of Items 1 to 4, wherein the water-absorbent resin composition has a physiological saline water absorption capacity of 5 ml / g or more and 40 ml / g or less under a load of 4.14 kPa. Item 6. An absorbent body comprising the water-absorbent resin composition according to any one of Items 1 to 5. Item 7. An absorbent article comprising the absorbent body according to Item 6. Item 8. A method for producing a water-absorbent resin composition, the method according to any one of Items 1 to 5, comprising the following steps: a step of mixing the water-absorbing resin particles before surface cross-linking and the chelating agent, and / or a step of mixing the water-absorbing resin particles after surface cross-linking and the chelating agent. Effects of the Invention

[0012] According to the present invention, it is possible to provide a water-absorbent resin composition which has both gel stability of the water-absorbent resin composition when normally worn in sanitary materials and high workability when the water-absorbent resin composition is separated after ultraviolet irradiation as a disposal means. Furthermore, according to the present invention, it is possible to provide a method for producing the water-absorbent resin composition, an absorbent body and an absorbent article using the water-absorbent resin composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 Schematic diagram of the device for measuring the water absorption of physiological saline under a load of 4.14 kPa. Figure 2 This is a schematic diagram of a measuring apparatus used for measuring gel strength. DETAILED DESCRIPTION

[0014] In this specification, the term "comprising" includes "consisting essentially of" and "consisting of". In addition, in this specification, "(meth)acrylic acid" means "acrylic acid or methacrylic acid", and "(meth)acrylate" means "acrylate or methacrylate". It should be noted that "water-soluble" means showing a solubility of 5% by mass or more in water at 25°C.

[0015] In addition, in this specification, the numerical value connected by "to" means the numerical range including the numerical values ​​before and after "to" as the lower limit and upper limit. When multiple lower limits and multiple upper limits are described separately, any lower limit and upper limit can be selected and connected by "to".

[0016] 1. Water-absorbent resin composition The water-absorbent resin composition of the present invention is characterized in that it is a water-absorbent resin composition comprising water-absorbent resin particles and a chelating agent, the water-absorbent resin particles are subjected to surface crosslinking treatment, the iron (III) chelate stability constant of the chelating agent is 16 log KML or more and 24 log KML or less, and the number of carboxyl groups is 4 or more and 10 or less (hereinafter, the chelating agent satisfying this characteristic is sometimes referred to as "chelating agent A"). The water-absorbent resin composition of the present invention having such characteristics has both gel stability when normally worn in sanitary materials and high operability when the water-absorbent resin composition is separated after ultraviolet irradiation as a waste treatment means. The water-absorbent resin composition of the present invention is described in detail below.

[0017] (Chelating Agent) The iron (III) chelate stability constant of the chelating agent A contained in the water-absorbent resin composition of the present invention is 16 log KML to 24 log KML, and the number of carboxyl groups is 4 to 10. As the iron (III) chelate stability constant of the chelating agent, a literature value can be used.

[0018] From the viewpoint of more appropriately exerting the effect of the present invention, the iron (III) chelate stability constant of the chelating agent A is preferably 16 logKML or more, more preferably 18 logKML or more, further preferably 19 logKML or more, further preferably 19.5 logKML or more, and preferably 24 logKML or less, more preferably 22 logKML or less, more preferably 21 logKML or less, further preferably 20.4 logKML or less, and the preferred range is 16 to 24 logKML, 19 to 21 logKML, 19.5 to 20.4 logKML, etc.

[0019] The number of carboxyl groups of the chelating agent A contained in the water-absorbent resin composition of the present invention is 4 to 10. From the viewpoint of more appropriately exerting the effects of the present invention, the number of carboxyl groups of the chelating agent is preferably 4 to 10, more preferably 4 to 6, further preferably 4 to 5, and further preferably 4.

[0020] As the chelating agent A contained in the water-absorbent resin composition of the present invention, preferred specific examples include ethylenediamine-N,N′-disuccinic acid, glycol ether diaminetetraacetic acid, etc. The chelating agent A may exist in the form of a salt. As salts, sodium salts, potassium salts, etc. may be mentioned. The chelating agent contained in the water-absorbent resin composition of the present invention may be only one kind, or may be two or more kinds. In addition, in the water-absorbent resin composition of the present invention, other chelating agents different from the chelating agent A (that is, chelating agents that do not satisfy the characteristics that the iron (III) chelate stability constant is greater than 16logKML and less than 24logKML, and the number of carboxyl groups is greater than 4 and less than 10) may be included, or may not be included. As other chelating agents, known chelating agents added to water-absorbent resins can be used. From the viewpoint of more appropriately exerting the effects of the present invention, the proportion of the chelating agent A in the chelating agent contained in the water-absorbent resin composition of the present invention is preferably 60 mass % or more, more preferably 70 mass % or more, further preferably 80 mass % or more, further preferably 90 mass % or more, further preferably 95 mass % or more, further preferably 100 mass % (that is, the chelating agent contained in the water-absorbent resin composition of the present invention is only the chelating agent A).

[0021] In the water-absorbent resin composition of the present invention, the content of the chelating agent A is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and is preferably 2 parts by mass or less, more preferably 1 part by mass or less, with a preferred range being 0.001 to 2 parts by mass, 0.01 to 1 part by mass, etc., based on 100 parts by mass of the water-absorbent resin particles.

[0022] The chelating agent A is preferably present on at least one of the surface and the interior of the water-absorbing resin particles treated with surface crosslinking, and more preferably at least on the surface. For example, by mixing the water-absorbing resin particles treated with surface crosslinking with the chelating agent A in a solid phase, the chelating agent A can be present on the surface of the water-absorbing resin particles treated with surface crosslinking to such an extent that the effect of the present invention can be exhibited. In addition, the water-absorbing resin composition of the present invention can be prepared by mixing the water-absorbing resin particles treated with surface crosslinking in a state where the chelating agent A is dissolved or dispersed in a liquid medium such as an aqueous liquid. In addition, the interior of the water-absorbing resin particles treated with surface crosslinking may contain the chelating agent A.

[0023] Next, the water-absorbent resin particles contained in the water-absorbent resin composition of the present invention will be described in detail.

[0024] (Water-absorbent resin particles) The water-absorbent resin particles contained in the water-absorbent resin composition of the present invention are formed by crosslinking a polymer of a water-soluble ethylenically unsaturated monomer, that is, a crosslinked polymer having a structural unit derived from a water-soluble ethylenically unsaturated monomer. In addition, the water-absorbent resin particles are surface crosslinked. It should be noted that the surface processing method can be, for example, the method described in the <Surface Crosslinking Step> described later.

[0025] From the viewpoint of more appropriately exerting the effects of the present invention, the physiological saline water retention capacity of the water-absorbent resin particles is preferably 20 g / g or more, more preferably 25 g / g or more, and even more preferably 30 g / g or more, and is preferably 60 g / g or less, more preferably 55 g / g or less, and even more preferably 50 g / g or less, and the preferred range is 25 to 60 g / g, 30 to 50 g / g, etc.

[0026] In addition, from the viewpoint of more appropriately exerting the effects of the present invention, the water absorption amount of physiological saline under a load of 4.14 kPa of the water-absorbent resin particles is preferably 5 ml / g or more, more preferably 10 ml / g or more, and even more preferably 15 ml / g or more, and is preferably 40 ml / g or less, more preferably 35 ml / g or less, and even more preferably 30 ml / g or less, and the preferred range is 5 to 40 ml / g, 10 to 30 ml / g, etc.

[0027] The physiological saline water retention capacity and the physiological saline water absorption capacity under a load of 4.14 kPa of the water-absorbent resin particles are values ​​measured by the methods described in Examples.

[0028] The water-absorbent resin is usually in a granular form. From the viewpoint of avoiding local absorption in the absorbent article and appropriately exerting the effect of the present invention, the median particle size of the water-absorbent resin particles is preferably 150 μm or more, 200 μm or more, 250 μm or more, 280 μm or more, 300 μm or more, or 350 μm or more. In addition, from the viewpoint of making the touch in the absorbent article comfortable and appropriately exerting the effect of the present invention, the median particle size is preferably 850 μm or less, 600 μm or less, 550 μm or less, 500 μm or less, 450 μm or less, or 400 μm or less. That is, the median particle size is preferably 150 to 850 μm, more preferably 200 to 600 μm, further preferably 250 to 500 μm, further preferably 300 to 450 μm, and further preferably 320 to 400 μm. The water-absorbent resin composition of the present invention preferably has a median particle size of 150 to 850 μm, more preferably 200 to 600 μm, further preferably 250 to 500 μm, further preferably 300 to 450 μm, and further preferably 320 to 400 μm.

[0029] It should be noted that the water-absorbent resin particles may be in a form of agglomeration of fine particles (primary particles) in addition to the form of each being composed of a single particle. Examples of the shape of the primary particles include a roughly spherical shape, an irregularly shaped broken shape, a plate shape, etc. In the case of primary particles produced by reversed phase suspension polymerization, examples include a roughly spherical single particle shape having a smooth surface shape such as a true sphere, an ellipsoidal sphere, etc.

[0030] The median particle size of the water-absorbing resin particles can be measured using a JIS standard sieve, and specifically, is a value measured by the method described in Examples.

[0031] The polymerization method of the water-soluble ethylenically unsaturated monomer can use aqueous solution polymerization, emulsion polymerization, reversed phase suspension polymerization, etc. as representative polymerization methods. In the aqueous solution polymerization method, the water-soluble ethylenically unsaturated monomer aqueous solution is stirred and heated as needed to perform polymerization. In addition, in the reversed phase suspension polymerization method, the water-soluble ethylenically unsaturated monomer is heated in a hydrocarbon dispersion medium under stirring to perform polymerization.

[0032] An example of a method for producing the water-absorbing resin particles will be described below.

[0033] As a specific example of the method for producing water-absorbent resin particles, there can be mentioned a method comprising a step of performing polymerization in the presence of a radical polymerization initiator and a step of surface crosslinking the hydrogel obtained by the polymerization in the presence of a surface crosslinking agent in a method for producing water-absorbent resin particles by reverse phase suspension polymerization of a water-soluble ethylenically unsaturated monomer in a hydrocarbon dispersion medium. In addition, in the method for producing water-absorbent resin particles of the present invention, an internal crosslinking agent may be added to the water-soluble ethylenically unsaturated monomer as needed to form a hydrogel having an internal crosslinked structure.

[0034] <Polymerization process> [Water-soluble ethylenically unsaturated monomer] Examples of water-soluble ethylenically unsaturated monomers include (meth)acrylic acid (in this specification, "acrylic acid" and "methacrylic acid" are collectively referred to as "(meth)acrylic acid", and the same applies hereinafter) and salts thereof; 2-(meth)acrylamide-2-methylpropanesulfonic acid and salts thereof; nonionic monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, 2-hydroxyethyl(meth)acrylate, N-hydroxymethyl(meth)acrylamide, and polyethylene glycol mono(meth)acrylate; amino group-containing unsaturated monomers such as N,N-diethylaminoethyl(meth)acrylate, N,N-diethylaminopropyl(meth)acrylate, and diethylaminopropyl(meth)acrylamide, and quaternary ammonium compounds thereof. Among these water-soluble ethylenically unsaturated monomers, (meth)acrylic acid or salts thereof, (meth)acrylamide, and N,N-dimethylacrylamide are preferred, and (meth)acrylic acid and salts thereof are more preferred from the viewpoint of easy industrial availability. In addition, these water-soluble ethylenically unsaturated monomers may be used alone or in combination of two or more.

[0035] Among them, acrylic acid and its salts are widely used as raw materials for water-absorbent resin particles. These acrylic acid and / or its salts are sometimes copolymerized with the above-mentioned other water-soluble ethylenically unsaturated monomers and used. In this case, acrylic acid and / or its salts are preferably used as the main water-soluble ethylenically unsaturated monomer in an amount of 70 to 100 mol % relative to the total water-soluble ethylenically unsaturated monomers.

[0036] The water-soluble ethylenically unsaturated monomer can be dispersed in a hydrocarbon dispersion medium in the form of an aqueous solution and provided for reverse suspension polymerization. The water-soluble ethylenically unsaturated monomer can improve the dispersion efficiency in the hydrocarbon dispersion medium by forming an aqueous solution. The concentration of the water-soluble ethylenically unsaturated monomer in the aqueous solution is preferably in the range of 20% by mass to below the saturated concentration. In addition, as the concentration of the water-soluble ethylenically unsaturated monomer, it is more preferably 55% by mass or less, further preferably 50% by mass or less, and further preferably 45% by mass or less. On the other hand, as the concentration of the water-soluble ethylenically unsaturated monomer, it is more preferably 25% by mass or more, further preferably 30% by mass or more, and further preferably 35% by mass or more.

[0037] When the water-soluble ethylenically unsaturated monomer has an acid group such as (meth) acrylic acid, 2-(meth) acrylamide-2-methylpropanesulfonic acid, etc., a monomer whose acid group is pre-neutralized by an alkaline neutralizer may be used as required. As such an alkaline neutralizer, alkali metal salts such as sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, etc.; ammonia, etc. may be cited. In addition, in order to simplify the neutralization operation, these alkaline neutralizers may be used in the form of aqueous solutions. It should be noted that the above-mentioned alkaline neutralizers may be used alone or in combination of two or more.

[0038] The degree of neutralization of the water-soluble ethylenically unsaturated monomer by the alkaline neutralizing agent is preferably 10 to 100 mol %, more preferably 30 to 90 mol %, further preferably 50 to 85 mol %, and further preferably 70 to 80 mol % relative to all acid groups of the water-soluble ethylenically unsaturated monomer.

[0039] [Free Radical Polymerization Initiator] Examples of the radical polymerization initiator added in the polymerization step include persulfates such as potassium persulfate, ammonium persulfate, and sodium persulfate; peroxides such as methyl ethyl ketone peroxide, methyl isobutyl ketone peroxide, di-tert-butyl peroxide, tert-butyl isopropyl peroxide, tert-butyl peracetate, tert-butyl peroxyisobutyrate, tert-butyl peroxypivalate, and hydrogen peroxide; and 2,2′-azobis(2-amidinopropane) dihydrochloride, 2,2′-azobis[2-(N-phenylamidino)propane] Azo compounds such as dihydrochloride, 2,2′-azobis[2-(N-allylamidinyl)propane] dihydrochloride, 2,2′-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} dihydrochloride, 2,2′-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2′-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide], 4,4′-azobis(4-cyanovaleric acid), etc. Among these free radical polymerization initiators, potassium persulfate, ammonium persulfate, sodium persulfate, and 2,2′-azobis(2-amidinopropane) dihydrochloride are preferred from the viewpoint of easy availability and easy handling. These free radical polymerization initiators may be used alone or in combination of two or more. Furthermore, the above-mentioned radical polymerization initiator may be used in combination with a reducing agent such as sodium sulfite, sodium hydrogen sulfite, ferrous sulfate, and L-ascorbic acid to be used as a redox polymerization initiator.

[0040] The amount of the radical polymerization initiator used is, for example, 0.00005 to 0.01 mol per 1 mol of the water-soluble ethylenically unsaturated monomer. By satisfying such an amount, a rapid polymerization reaction can be avoided and the polymerization reaction can be terminated at an appropriate time.

[0041] [Internal crosslinking agent] Examples of the internal crosslinking agent include a crosslinking agent capable of crosslinking the polymer of the water-soluble ethylenically unsaturated monomer used, for example, (poly)ethylene glycol [the expression "(poly)" indicates the case where the prefix "poly" is present and the case where "poly" is not present. [hereinafter the same], unsaturated polyesters obtained by reacting diols, triols and other polyols such as (poly)propylene glycol, 1,4-butanediol, 1,6-hexanediol, trimethylolpropane and (poly)glycerol with unsaturated acids such as (meth)acrylic acid, maleic acid and fumaric acid; bisacrylamides such as N,N-methylenebisacrylamide; di(meth)acrylates or tri(meth)acrylates obtained by reacting polyepoxide with (meth)acrylic acid; di(meth)acrylic acid urethanes obtained by reacting polyisocyanates such as toluene diisocyanate and hexamethylene diisocyanate with hydroxyethyl (meth)acrylate; compounds having two or more polymerizable unsaturated groups such as allylated starch, allylated cellulose, diallyl phthalate, N,N′,N″-triallyl isocyanurate and divinylbenzene; (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, (poly)glycerol diglycidyl ether ethers, such as diglycidyl compounds, triglycidyl compounds, such as polyglycidyl compounds; epihalohydrin compounds such as epichlorohydrin, epibromohydrin, α-methyl epichlorohydrin; compounds having two or more reactive functional groups such as isocyanate compounds such as 2,4-toluene diisocyanate and hexamethylene diisocyanate; oxetane compounds such as 3-methyl-3-oxetane methanol, 3-ethyl-3-oxetane methanol, 3-butyl-3-oxetane methanol, 3-methyl-3-oxetane ethanol, 3-ethyl-3-oxetane ethanol, 3-butyl-3-oxetane ethanol, etc. Among these internal crosslinking agents, it is preferred to use polyglycidyl compounds, and it is more preferred to use diglycidyl ether compounds, and it is preferred to use (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, and (poly)glycerol diglycidyl ether. These internal crosslinking agents can be used alone or in combination of two or more.

[0042] The amount of the internal crosslinking agent used is preferably 0.000001 to 0.02 mol, more preferably 0.00001 to 0.01 mol, further preferably 0.00001 to 0.005 mol, and further preferably 0.00005 to 0.002 mol, based on 1 mol of the water-soluble ethylenically unsaturated monomer.

[0043] [Hydrocarbon dispersion medium] As hydrocarbon dispersion medium, for example, there can be mentioned: aliphatic hydrocarbons having 6 to 8 carbon atoms such as n-hexane, n-heptane, 2-methylhexane, 3-methylhexane, 2,3-dimethylpentane, 3-ethylpentane, and n-octane; alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, cyclopentane, methylcyclopentane, trans-1,2-dimethylcyclopentane, cis-1,3-dimethylcyclopentane, and trans-1,3-dimethylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene. Among these hydrocarbon dispersion mediums, n-hexane, n-heptane, and cyclohexane are preferably used from the viewpoint of being easily available industrially, having stable quality, and being inexpensive. These hydrocarbon dispersion mediums can be used alone or in combination of two or more. It should be noted that as an example of a mixture of hydrocarbon dispersion mediums, even if a commercial product such as Exxsol heptane (manufactured by Exxon Mobil: hydrocarbons containing 75 to 85% by mass of heptane and its isomers) is used, suitable results can be obtained.

[0044] The amount of the hydrocarbon dispersion medium used is preferably 100 to 1500 parts by mass, more preferably 200 to 1400 parts by mass, relative to 100 parts by mass of the water-soluble ethylenically unsaturated monomer in the first stage, from the viewpoint of uniformly dispersing the water-soluble ethylenically unsaturated monomer and facilitating the control of the polymerization temperature. It should be noted that, as described later, the reversed phase suspension polymerization is carried out in one stage (single stage) or in multiple stages of two or more stages, and the first stage polymerization mentioned above refers to the first stage polymerization reaction in the single stage polymerization or the multistage polymerization (hereinafter the same).

[0045] [Dispersion stabilizer] (Surfactant) In the reverse phase suspension polymerization, a dispersion stabilizer may be used to improve the dispersion stability of the water-soluble ethylenically unsaturated monomer in the hydrocarbon dispersion medium. As the dispersion stabilizer, a surfactant may be used.

[0046] As surfactant, for example, sucrose fatty acid ester, polyglycerol fatty acid ester, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene glycerol fatty acid ester, sorbitol fatty acid ester, polyoxyethylene sorbitol fatty acid ester, polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene castor oil, polyoxyethylene hydrogenated castor oil, alkyl allyl formaldehyde condensation polyoxyethylene ether, polyoxyethylene polyoxypropylene block copolymer, polyoxyethylene polyoxypropylene alkyl ether, polyethylene glycol fatty acid ester, alkyl glucoside, N-alkyl glucamide, polyoxyethylene fatty acid amide, polyoxyethylene alkylamine, the phosphoric acid ester of polyoxyethylene alkyl ether, the phosphoric acid ester of polyoxyethylene alkyl allyl ether etc. can be used. Among these surfactants, from the dispersion stability aspect of monomer, sorbitan fatty acid ester, polyglycerol fatty acid ester, sucrose fatty acid ester are particularly preferably used. These surfactants can be used alone, or two or more can be used in combination.

[0047] The amount of the surfactant used is preferably 0.1 to 30 parts by mass, more preferably 0.3 to 20 parts by mass, based on 100 parts by mass of the water-soluble ethylenically unsaturated monomer in the first stage.

[0048] (Polymer dispersant) Furthermore, as a dispersion stabilizer used in the reverse phase suspension polymerization, a polymeric dispersant may be used together with the above-mentioned surfactant.

[0049] Examples of the polymer dispersant include maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-modified EPDM (ethylene-propylene-diene terpolymer), maleic anhydride-modified polybutadiene, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, maleic anhydride-butadiene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, oxidized ethylene-propylene copolymer, ethylene-acrylic acid copolymer, ethyl cellulose, ethyl hydroxyethyl cellulose, etc. Among these polymer dispersants, maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, maleic anhydride-modified ethylene-propylene copolymer, maleic anhydride-ethylene copolymer, maleic anhydride-propylene copolymer, maleic anhydride-ethylene-propylene copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, oxidized polyethylene, oxidized polypropylene, oxidized ethylene-propylene copolymer, etc. are particularly preferably used from the perspective of monomer dispersion stability. These polymer dispersants may be used alone or in combination of two or more.

[0050] The amount of the polymer dispersant used is preferably 0.1 to 30 parts by mass, more preferably 0.3 to 20 parts by mass, based on 100 parts by mass of the water-soluble ethylenically unsaturated monomer in the first stage.

[0051] [Other ingredients] In the method for producing water-absorbent resin particles, other components may be added to the aqueous solution containing the water-soluble ethylenically unsaturated monomer as necessary to carry out reverse phase suspension polymerization. As other components, various additives such as a thickener and a chain transfer agent may be added.

[0052] As an example, a thickener may be added to an aqueous solution containing a water-soluble ethylenically unsaturated monomer to perform reversed phase suspension polymerization. By adjusting the viscosity of the aqueous solution by adding a thickener, the median particle size obtained in the reversed phase suspension polymerization can be controlled.

[0053] As thickeners, for example, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, carboxymethyl cellulose, polyacrylic acid, polyacrylic acid (partially) neutralized product, polyethylene glycol, polyacrylamide, polyethylene imine, dextrin, sodium alginate, polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene oxide, etc. It should be noted that if the stirring speed during polymerization is the same, there is a tendency that the higher the viscosity of the aqueous solution of the water-soluble ethylenically unsaturated monomer, the larger the primary particles and / or secondary particles of the obtained particles.

[0054] [Inverse suspension polymerization] When reverse phase suspension polymerization is performed, for example, a monomer aqueous solution containing a water-soluble ethylenically unsaturated monomer is dispersed in a hydrocarbon dispersion medium in the presence of a dispersion stabilizer. At this time, the dispersion stabilizer (surfactant or polymer dispersant) may be added before or after the monomer aqueous solution is added, provided that the dispersion stabilizer is added before the polymerization reaction is started.

[0055] Among them, it is preferred to disperse the monomer aqueous solution and then disperse the surfactant in the hydrocarbon dispersion medium in which the polymer dispersant is dispersed, and then perform polymerization, from the viewpoint of easily reducing the amount of the hydrocarbon dispersion medium remaining in the obtained water-absorbing resin particles.

[0056] Such reversed phase suspension polymerization may be carried out in one stage or in two or more stages, but is preferably carried out in two or three stages from the viewpoint of improving productivity.

[0057] When carrying out reversed-phase suspension polymerization with multistages more than 2 stages, after carrying out the reversed-phase suspension polymerization of the first stage, in the reaction mixture obtained by the first stage polyreaction, add water-soluble ethylenically unsaturated monomers and mix, carry out the reversed-phase suspension polymerization after the second stage with the method identical with the first stage.In the reversed-phase suspension polymerization of each stage after the second stage, preferably except water-soluble ethylenically unsaturated monomers, the amount of the water-soluble ethylenically unsaturated monomers that free radical polymerization initiator adds during the reversed-phase suspension polymerization of each stage after the second stage is used as a benchmark, in the scope of the molar ratio of each above-mentioned component relative to water-soluble ethylenically unsaturated monomers, add, carry out reversed-phase suspension polymerization.It should be explained that in the polymerization after the second stage, as required, internal crosslinking agent can also be added in the water-soluble ethylenically unsaturated monomers.

[0058] The reaction temperature of the polymerization reaction is preferably 20 to 110° C., more preferably 40 to 90° C., from the viewpoint of rapidly advancing the polymerization and shortening the polymerization time to improve economic efficiency, and easily removing the polymerization heat to smoothly advance the reaction.

[0059] <Surface cross-linking process> Next, the water-absorbent resin particles of the present invention are obtained by adding a surface crosslinking agent to a hydrogel having an internal crosslinking structure obtained by polymerizing a water-soluble ethylenically unsaturated monomer and performing crosslinking (surface crosslinking reaction). The surface crosslinking reaction is preferably performed in the presence of a surface crosslinking agent after the water-soluble ethylenically unsaturated monomer is polymerized. In this way, after the polymerization, the hydrogel having an internal crosslinking structure is subjected to a surface crosslinking reaction, so that the crosslinking density near the surface of the water-absorbent resin particles can be increased, and water-absorbent resin particles having improved various properties such as water absorption capacity under load can be obtained.

[0060] Examples of the surface cross-linking agent include compounds having two or more reactive functional groups. For example, polyols such as ethylene glycol, propylene glycol, 1,4-butanediol, diethylene glycol, triethylene glycol, trimethylolpropane, glycerol, polyoxyethylene glycol, polyoxypropylene glycol, and polyglycerol can be mentioned; polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerol diglycidyl ether, (poly)glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and (poly)glycerol polyglycidyl ether can be mentioned; halogenated epoxy compounds such as epichlorohydrin, epibromohydrin, and α-methylepichlorohydrin can be mentioned; isocyanate compounds such as 2,4-toluene diisocyanate and hexamethylene diisocyanate can be mentioned; 3-methyl-3-hydroxymethyloxetane, 3-ethyl-3-hydroxymethyloxetane, 3-butyl-3-hydroxymethyloxetane, 3-methyl-3-hydroxyethyloxetane Oxetane compounds such as cyclobutane, 3-ethyl-3-hydroxyethyloxetane, and 3-butyl-3-hydroxyethyloxetane; oxazoline compounds such as 1,2-ethylenebisoxazoline; carbonate compounds (e.g., alkylene carbonate) such as ethylene carbonate, propylene carbonate, 4,5-dimethyl-1,3-dioxolane-2-one, 4,4-dimethyl-1,3-dioxolane-2-one, 4-ethyl-1,3-dioxolane-2-one, 4-hydroxymethyl-1,3-dioxolane-2-one, 1,3-dioxane-2-one, 4-methyl-1,3-dioxane-2-one, 4,6-dimethyl-1,3-dioxane-2-one, and 1,3-dioxolane-2-one; hydroxyalkylamide compounds such as bis[N,N-di(β-hydroxyethyl)]adipamide. Among these surface crosslinking agents, preferred are polyglycidyl compounds such as (poly)ethylene glycol diglycidyl ether, (poly)glycerol diglycidyl ether, (poly)glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, (poly)propylene glycol polyglycidyl ether, and (poly)glycerol polyglycidyl ether; and carbonate compounds (e.g., alkylene carbonates) such as ethylene carbonate, propylene carbonate, 4,5-dimethyl-1,3-dioxolane-2-one, 4,4-dimethyl-1,3-dioxolane-2-one, 4-ethyl-1,3-dioxolane-2-one, 4-hydroxymethyl-1,3-dioxolane-2-one, 1,3-dioxane-2-one, 4-methyl-1,3-dioxane-2-one, 4,6-dimethyl-1,3-dioxane-2-one, and 1,3-dioxolane-2-one. These surface cross-linking agents may be used alone or in combination of two or more.

[0061] The amount of the surface crosslinking agent used is preferably 0.00001 to 0.01 mol, more preferably 0.00005 to 0.005 mol, and even more preferably 0.0001 to 0.002 mol, based on 1 mol of the total amount of the water-soluble ethylenically unsaturated monomers used in the polymerization.

[0062] As a method for adding the surface crosslinking agent, the surface crosslinking agent can be added as it is or as an aqueous solution. If necessary, it can also be added in the form of a solution using a hydrophilic organic solvent as a solvent. Examples of hydrophilic organic solvents include: lower alcohols such as methanol, ethanol, n-propanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; ethers such as diethyl ether, dioxane, and tetrahydrofuran; amides such as N,N-dimethylformamide; sulfoxides such as dimethyl sulfoxide, etc. These hydrophilic organic solvents can be used alone, in combination of two or more, or as a mixed solvent with water.

[0063] The surface crosslinking agent can be added after the polymerization reaction of the water-soluble ethylenically unsaturated monomer is almost completely completed. It is preferably added in the presence of 1 to 400 parts by mass of water relative to 100 parts by mass of the water-soluble ethylenically unsaturated monomer, more preferably in the presence of 5 to 200 parts by mass of water, further preferably in the presence of 10 to 100 parts by mass of water, and further preferably in the presence of 20 to 60 parts by mass of water. It should be noted that the amount of water refers to the total amount of water contained in the reaction system and the water used as needed when adding the surface crosslinking agent.

[0064] The reaction temperature in the surface crosslinking reaction is preferably 50 to 250° C., more preferably 60 to 180° C., further preferably 60 to 140° C., and further preferably 70 to 120° C. The reaction time in the surface crosslinking reaction is preferably 1 to 300 minutes, and more preferably 5 to 200 minutes.

[0065] <Drying process> After the above-mentioned reversed phase suspension polymerization, a drying step may be included in which water, hydrocarbon dispersion medium, etc. are removed by distillation by applying energy such as heat from the outside. In the case of dehydrating the hydrogel after the reversed phase suspension polymerization, the system in which the hydrogel is dispersed in the hydrocarbon dispersion medium is heated, thereby temporarily distilling water and the hydrocarbon dispersion medium out of the system by azeotropic distillation. At this time, if only the hydrocarbon dispersion medium removed by distillation is returned to the system, continuous azeotropic distillation can be performed. In this case, the temperature in the system during drying is maintained below the temperature of azeotropy with the hydrocarbon dispersion medium, so it is preferred from the viewpoint of not easily causing the resin to deteriorate. Next, water and hydrocarbon dispersion medium are removed by distillation to obtain water-absorbent resin particles. By controlling the treatment conditions of the drying step after the polymerization and adjusting the dehydration amount, the various properties of the obtained water-absorbent resin particles can be controlled.

[0066] In the drying process, the drying treatment by distillation may be carried out under normal pressure or under reduced pressure. In addition, from the viewpoint of improving the drying efficiency, it may be carried out under a stream of nitrogen or the like. When the drying treatment is carried out under normal pressure, the drying temperature is preferably 70 to 250° C., more preferably 80 to 180° C., further preferably 80 to 140° C., and further preferably 90 to 130° C. In addition, when the drying treatment is carried out under reduced pressure, the drying temperature is preferably 40 to 160° C., and more preferably 50 to 110° C.

[0067] The water content of the water-absorbing resin particles obtained by the production method of the present invention is preferably 20 mass % or less, more preferably 15 mass % or less, further preferably 10 mass % or less, and preferably in the range of 1 to 10 mass %.

[0068] It should be noted that when a surface crosslinking step using a surface crosslinking agent is performed after polymerization of the monomers by reverse phase suspension polymerization, the drying step using distillation is performed after the surface crosslinking step is completed. Alternatively, the surface crosslinking step and the drying step may be performed simultaneously.

[0069] The water-absorbent resin composition of the present invention may contain additives according to the purpose. Examples of such additives include inorganic powders, surfactants, oxidants, reducing agents, free radical chain inhibitors, antioxidants, antibacterial agents, and the like. For example, by adding 0.05 to 5 parts by mass of amorphous silica as an inorganic powder relative to 100 parts by mass of the water-absorbent resin particles, the fluidity of the water-absorbent resin composition can be further improved. It should be noted that the additive is preferably hydrophilic or water-soluble.

[0070] In the water-absorbent resin composition of the present invention, the content of the water-absorbent resin particles (excluding additives) is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more.

[0071] From the viewpoint of more appropriately exerting the effects of the present invention, the physiological saline water retention capacity of the water-absorbent resin composition is preferably 25 g / g or more, more preferably 30 g / g or more, and is preferably 60 g / g or less, more preferably 55 g / g or less, and further preferably 50 g / g or less. Preferred ranges are 25 to 60 g / g, 30 to 50 g / g, and the like.

[0072] In addition, from the viewpoint of more appropriately exerting the effects of the present invention, the water-absorbent resin composition preferably has a physiological saline water absorption capacity of 5 ml / g or more under a load of 4.14 kPa, more preferably 10 ml / g or more, and even more preferably 15 ml / g or more, and is preferably 40 ml / g or less, more preferably 35 ml / g or less, and even more preferably 30 ml / g or less, and the preferred range is 5 to 40 ml / g, 10 to 30 ml / g, and the like.

[0073] The physiological saline water retention capacity and the physiological saline water absorption capacity under a load of 4.14 kPa of the water-absorbent resin composition are values ​​measured by the methods described in Examples, respectively.

[0074] From the viewpoint of more appropriately exerting the effects of the present invention, the water absorption rate of the water-absorbent resin composition by a vortex method is preferably 60 seconds or less, more preferably 50 seconds or less, and even more preferably 40 seconds or less, and is preferably 1 second or more, more preferably 3 seconds or more, and even more preferably 10 seconds or more, and the preferred range is 1 to 60 seconds, 3 to 40 seconds, etc.

[0075] The water absorption rate of the water-absorbent resin composition by a vortex method is a value measured by the method described in Examples.

[0076] In addition, the water-absorbent resin composition of the present invention has a "soluble component eluted one hour after a degradation test" evaluated by the method described in Examples, preferably 20% by mass or less, more preferably 14% by mass or less, and preferably 0% by mass or more, more preferably 1% by mass or more, and preferably in the range of 0 to 20% by mass, 1 to 14% by mass, etc.

[0077] In addition, from the viewpoint of gel stability when the sanitary material is usually worn, the "initial value of gel strength" of the water-absorbent resin composition of the present invention evaluated by the method described in the Examples is preferably 5000 N / m 2 More than 6000 N / m 2 More than, more preferably 6500N / m 2 It should be noted that the upper limit of the initial value of the gel strength is, for example, 20000 N / m 2 .

[0078] In addition, from the viewpoint of gel stability when the sanitary material is usually worn, the water-absorbent resin composition of the present invention preferably has a "gel strength after standing at 37° C. for 14 hours" evaluated by the method described in the Examples of 4000 N / m 2 More than 4500 N / m 2 More than, more preferably 5000N / m 2It should be noted that the upper limit of the gel strength is, for example, 20000 N / m 2 .

[0079] In addition, from the viewpoint of gel stability when the sanitary material is normally worn, the "gel strength variation" of the water-absorbent resin composition of the present invention evaluated by the method described in the Examples is preferably 40% or less, more preferably 35% or less, and even more preferably 30% or less. The lower limit of the gel strength variation is, for example, 0%.

[0080] In addition, from the viewpoint of workability when the water-absorbent resin composition is separated from sanitary materials after being irradiated with ultraviolet rays as a disposal means, the water-absorbent resin composition of the present invention preferably has a "gel strength after standing at 37° C. for 14 hours and then irradiated with ultraviolet rays" evaluated by the method described in the Examples of 7000 N / m 2 Below, more preferably 6000N / m 2 Below, more preferably 4000N / m 2 Below, in addition, preferably 0N / m 2 More than 500 N / m 2 More preferably 1000 N / m 2 above.

[0081] In addition, from the viewpoint of workability when the water-absorbent resin composition is separated from sanitary materials after ultraviolet irradiation as a disposal means, the "degree of change in gel strength after UV irradiation" of the water-absorbent resin composition of the present invention evaluated by the method described in the Examples is preferably 40% or more, more preferably 45% or more, and even more preferably 50% or more, and is preferably 100% or less, more preferably 95% or less, and even more preferably 90% or less. Preferred ranges are 40 to 100% by mass, 40 to 90% by mass, etc.

[0082] The method for producing the water-absorbent resin composition of the present invention is not particularly limited, and can be appropriately produced by a method for producing the water-absorbent resin composition having the following steps, wherein the steps are a step of mixing the water-absorbent resin particles before surface crosslinking with the chelating agent, and / or a step of mixing the water-absorbent resin particles after surface crosslinking with the chelating agent. That is, the step of mixing the water-absorbent resin particles with the chelating agent may be a step of mixing the water-absorbent resin particles before surface crosslinking with the chelating agent, and then subjecting the water-absorbent resin particles to surface crosslinking treatment, or a step of mixing the water-absorbent resin particles with the chelating agent after subjecting the water-absorbent resin particles to surface crosslinking treatment, or a step of mixing the water-absorbent resin particles before surface crosslinking with the chelating agent, and then subjecting the water-absorbent resin particles to surface crosslinking treatment, and then subjecting the water-absorbent resin particles after surface crosslinking treatment to the chelating agent. The water-absorbent resin particles and the chelating agent are as described above.

[0083] In addition, as described above, the mixing of the water-absorbing resin particles and the chelating agent can be appropriately performed by, for example, mixing them in a solid phase state.

[0084] 2. Absorbents and absorbent articles The water-absorbent resin composition of the present invention constitutes an absorbent body used in sanitary materials such as sanitary products and disposable diapers, and is suitable for use in absorbent articles including the absorbent body.

[0085] Here, the absorbent using the water-absorbent resin composition of the present invention includes the water-absorbent resin composition of the present invention. The absorbent may further include hydrophilic fibers. As the structure of the absorbent, there can be cited a sheet structure in which the water-absorbent resin composition is fixed on a non-woven fabric or between a plurality of non-woven fabrics, a mixed dispersion obtained by mixing the water-absorbent resin composition and the hydrophilic fibers in a uniform composition, a sandwich structure in which the water-absorbent resin composition is sandwiched between layered hydrophilic fibers, and a structure in which the water-absorbent resin composition and the hydrophilic fibers are wrapped with tissue paper. It should be noted that other components may be added to the absorbent, such as adhesive adhesives such as heat-fusible synthetic fibers, hot-melt adhesives, and adhesive emulsions for improving the shape-retaining performance of the absorbent.

[0086] The content of the water-absorbent resin composition in the absorbent body is preferably 5 to 100% by mass, more preferably 10 to 95% by mass, further preferably 20 to 90% by mass, and further preferably 30 to 80% by mass.

[0087] Examples of hydrophilic fibers include cellulose fibers such as cotton pulp, mechanical pulp, chemical pulp, and semi-chemical pulp obtained from wood, artificial cellulose fibers such as rayon and cellulose acetate, and fibers containing hydrophilized synthetic resins such as polyamide, polyester, and polyolefin. The average fiber length of the hydrophilic fibers is usually 0.1 to 10 mm, or 0.5 to 5 mm.

[0088] The absorbent article of the present invention can be prepared by holding an absorbent body using the water-absorbent resin composition of the present invention between a liquid-permeable sheet (top sheet) through which liquid can pass and a liquid-impermeable sheet (back sheet) through which liquid cannot pass. The liquid-permeable sheet is arranged on the side in contact with the body, and the liquid-impermeable sheet is arranged on the opposite side in contact with the body.

[0089] Examples of liquid-permeable sheets include air-through, spunbond, chemically bonded, needle-punched nonwoven fabrics and porous synthetic resin sheets made of fibers such as polyethylene, polypropylene, and polyester. Examples of liquid-impermeable sheets include synthetic resin films made of resins such as polyethylene, polypropylene, and polyvinyl chloride. Example

[0090] The present invention will be described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.

[0091] The water-absorbent resin particles obtained in the following preparation examples and the water-absorbent resin compositions obtained in the examples and comparative examples were evaluated by the following various tests. Unless otherwise specified, the measurements were performed under an environment of a temperature of 25±2° C. and a humidity of 50±10%.

[0092] [Manufacturing of water-absorbent resin particles] <Production Example 1> A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and a volume of 2 L and equipped with two stages of stirring blades having four inclined blades with a blade diameter of 5 cm was prepared as a reflux cooler, a dropping funnel, a nitrogen inlet pipe, and a stirrer. In this flask, 293 g of n-heptane as a hydrocarbon dispersion medium was taken, 0.736 g of maleic anhydride-modified ethylene-propylene copolymer (Mitsui Chemicals, Inc., HI-WAX 1105A) as a polymer dispersant was added, and the temperature was raised to 80° C. while stirring to dissolve the dispersant, and then cooled to 50° C. On the other hand, 92.0 g (1.03 mol) of an 80.5 mass % aqueous solution of acrylic acid as a water-soluble ethylenically unsaturated monomer was taken in a beaker having an internal volume of 300 mL, and 147.7 g of a 20.9 mass % aqueous solution of sodium hydroxide was added dropwise while cooling with ice water. After 75 mol % neutralization, 0.092 g of hydroxyethyl cellulose (Sumitomo Seika Co., Ltd., HEC AW-15F) as a thickener, 0.0736 g (0.272 mmol) of potassium persulfate as a water-soluble free radical polymerization agent, and 0.010 g (0.057 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare an aqueous liquid of the first stage. Then, the aqueous liquid prepared as above was added to a separable flask and stirred for 10 minutes. Then, a surfactant solution of 0.736 g of HLB3 sucrose stearate (Mitsubishi Chemical Foods Co., Ltd., Ryoto Sugar Ester S-370) dissolved in 6.62 g of n-heptane as a surfactant was further added to a 20 mL-tube bottle. The system was fully substituted with nitrogen while the stirrer speed was set to 550 rpm for stirring. The flask was immersed in a 70°C water bath for heating and polymerization was carried out for 60 minutes to obtain a first-stage polymerization slurry.

[0093] On the other hand, in another beaker having an internal volume of 500 mL, 128.8 g (1.43 mol) of an 80.5 mass % aqueous solution of acrylic acid as a water-soluble ethylenically unsaturated monomer was taken, and while cooling with ice water, 159.0 g of a 27 mass % aqueous solution of sodium hydroxide was added dropwise, and after 75 mol % neutralization, 0.103 g (0.381 mmol) of potassium persulfate as a water-soluble free radical polymerization initiator and 0.0116 g (0.067 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare an aqueous liquid of the second stage.

[0094] While stirring with the stirrer set at 1000 rpm, the separable flask system was cooled to 27°C, and then the total amount of the second-stage aqueous liquid was added to the first-stage polymerization slurry liquid. After the system was purged with nitrogen for 30 minutes, the flask was immersed in a 70°C water bath again to raise the temperature, and a polymerization reaction was carried out for 60 minutes to obtain a hydrogel polymer.

[0095] Then, the flask was immersed in an oil bath set at 125° C., and 251.7 g of water was discharged to the outside of the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, 4.42 g (0.507 mmol) of a 2% by mass aqueous solution of ethylene glycol diglycidyl ether as a surface crosslinking agent was added to the flask, and the mixture was kept at 83° C. for 2 hours.

[0096] Then, the n-heptane was evaporated and dried at 125°C, and the mixture was passed through a sieve with a mesh size of 850 μm, thereby obtaining 220.2 g of water-absorbent resin particles (1). The water-absorbent resin particles (1) had a water retention capacity of 40 g / g in physiological saline, a water absorption capacity of 15 mL / g in physiological saline under a load of 4.14 kPa, a water content of 8% by mass, and a median particle size of 370 μm.

[0097] [Production of water-absorbent resin composition] <Example 1> 0.1 parts by mass of ethylenediamine-N,N′-disuccinic acid (EDDS·4H, iron (III) chelate stability constant: 20.1 [logKML], number of carboxyl groups in molecule: 4) was added as a chelating agent in the form of powder to 100 parts by mass of the water-absorbent resin particles (1) obtained in Production Example 1, and mixed for 30 minutes using a crossrotary mixer manufactured by Meiwa Industry Co., Ltd. (conditions: revolution speed 50 rpm, rotation speed 50 rpm). Furthermore, 0.5 parts by mass of amorphous silica (Tokusil NP-S manufactured by Rikantō Chemical Co., Ltd.) was mixed to 100 parts by mass of the water-absorbent resin particles (1), thereby obtaining a water-absorbent resin composition (1).

[0098] <Example 2> 20 g of the water-absorbent resin particles (1) obtained in Production Example 1 were weighed into a round-bottomed cylindrical separable flask having an inner diameter of 11 cm and equipped with an anchor-type stirring blade made of fluororesin. Next, a chelating agent aqueous solution prepared by adding 0.143 g of ion-exchanged water to 0.057 g of a 35% by mass aqueous solution of trisodium ethylenediamine-N,N′-disuccinate (EDDS·3Na, iron (III) chelate stability constant: 20.1 [logKML], number of carboxyl groups in the molecule: 4) was added dropwise into the separable flask using a Pasteur pipette while stirring at 300 rpm, and stirred for 10 minutes to obtain a mixture. The mixture was heated at 100° C. for 30 minutes, and then 0.5 parts by mass of amorphous silica (Tokusil NP-S manufactured by Rikantō Chemical Co., Ltd.) was mixed with 100 parts by mass of the water-absorbent resin particles (1) to obtain a water-absorbent resin composition (2).

[0099] <Example 3> In Example 1, except that 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H) was replaced with 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (GEDTA, iron (III) chelate stability constant: 20.5 [logKML], number of carboxyl groups in the molecule: 4), the same operation as in Example 1 was carried out to obtain a water-absorbent resin composition (3).

[0100] <Comparative Example 1> In Example 2, the same operation as in Example 2 was carried out except that 0.044 g of a 45% by mass aqueous solution of pentasodium diethylenetriaminepentaacetate (DTPA·5Na, iron (III) chelate stability constant: 28.6 [logKML], number of carboxyl groups in the molecule: 5) was used instead of 0.057 g of a 35% by mass aqueous solution of ethylenediamine-N,N′-disuccinate trisodium (EDDS·3Na) and the amount of ion exchange water was changed from 0.143 g to 0.156 g to prepare a chelating agent aqueous solution.

[0101] <Comparative Example 2> In Example 1, the same operation as in Example 1 was carried out, except that 0.1 mass part of ethylenediaminetetramethylenephosphonic acid dihydrate (EDTMP·2H2O, iron (III) chelate stability constant: 19.6 [logKML], number of carboxyl groups in the molecule: 0) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H). A water-absorbent resin composition (5) was obtained.

[0102] <Comparative Example 3> In Example 1, the same operation as in Example 1 was carried out, except that 0.1 mass part of hydroxyethylenediaminetriacetic acid (EDTA-OH, iron (III) chelate stability constant: 19.8 [logKML], number of carboxyl groups in the molecule: 3) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H). To obtain a water-absorbent resin composition (6).

[0103] <Comparative Example 4> In Example 2, the same operation as in Example 2 was carried out except that 0.050 g of 40% by mass of trisodium N-methylglycine diacetate (MGDA·3Na, iron (III) chelate stability constant: 16.5 [logKML], number of carboxyl groups in the molecule: 3) was used instead of 0.057 g of 35% by mass of ethylenediamine-N,N′-disuccinate trisodium (EDDS·3Na) aqueous solution and the amount of ion exchange water was changed from 0.143 g to 0.150 g to prepare a chelating agent aqueous solution. A water-absorbent resin composition (7) was obtained.

[0104] <Comparative Example 5> A water-absorbent resin composition (8) was obtained by the same operation as in Example 2 except that 0.043 g of a 47% by mass aqueous solution of tetrasodium L-glutamic acid diacetate (GLDA·4Na, iron (III) chelate stability constant: 15.2 [logKML], number of carboxyl groups in the molecule: 4) was used instead of 0.057 g of a 35% by mass aqueous solution of ethylenediamine-N,N′-disuccinate trisodium (EDDS·3Na) and the amount of ion-exchanged water was changed from 0.143 g to 0.157 g.

[0105] <Comparative Example 6> In Example 1, the same operation as in Example 1 was carried out, except that 0.1 mass part of iminodisuccinic acid (IDS, iron (III) chelate stability constant: 13.9 [logKML], number of carboxyl groups in the molecule: 4) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H). A water-absorbent resin composition (9) was obtained.

[0106] <Comparative Example 7> In Example 2, the same operation as in Example 2 was carried out except that 0.050 g of a 40 mass % sodium polyaspartate (molecular weight 2000-3000, iron (III) chelate stability constant: 18.5 [logKML], number of carboxyl groups in the molecule: 14 or more) aqueous solution was used instead of 0.057 g of a 35 mass % ethylenediamine-N,N′-disuccinate trisodium (EDDS·3Na) aqueous solution and the amount of ion exchange water was changed from 0.143 g to 0.150 g to prepare a chelating agent aqueous solution.

[0107] <Comparative Example 8> In Example 2, the same operation as in Example 2 was carried out except that 0.040 g of a 50 mass % aqueous solution of tetrasodium 3-hydroxy-2,2′-iminodisuccinate (HIDS, iron (III) chelate stability constant: 15.0 [logKML], number of carboxyl groups in the molecule: 4) was used instead of 0.057 g of a 35 mass % aqueous solution of ethylenediamine-N,N′-disuccinic acid·trisodium (EDDS·3Na) and the amount of ion exchange water was changed from 0.143 g to 0.160 g to prepare a chelating agent aqueous solution.

[0108] <Comparative Example 9> In Example 1, the same operation as in Example 1 was carried out, except that 0.1 mass part of L(+)-disodium tartrate dihydrate (iron (III) chelate stability constant: 18.1 [logKML], number of carboxyl groups in the molecule: 2) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H). A water-absorbent resin composition (12) was obtained.

[0109] <Comparative Example 10> In Example 1, except that 0.1 mass part of trisodium citrate dihydrate (iron (III) chelate stability constant: 11.9 [logKML], number of carboxyl groups in the molecule: 3) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H), the same operation as in Example 1 was carried out to obtain a water-absorbent resin composition (13).

[0110] <Comparative Example 11> In Example 1, except that 0.1 mass part of pyridine-2,6-dicarboxylic acid (iron (III) chelate stability constant: 10.9 [logKML], number of carboxyl groups in the molecule: 2) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H), the same operation as in Example 1 was carried out to obtain a water-absorbent resin composition (14).

[0111] <Comparative Example 12> In Example 1, the same operation as in Example 1 was carried out, except that 0.1 mass part of ethylenediaminetetraacetic acid (EDTA, iron (III) chelate stability constant: 25.1 [logKML], number of carboxyl groups in the molecule: 4) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H). A water-absorbent resin composition (15) was obtained.

[0112] <Comparative Example 13> In Example 1, except that 0.1 mass part of triethylenetetraaminehexaacetic acid (TTHA, iron (III) chelate stability constant: 26.8 [logKML], number of carboxyl groups in the molecule: 6) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H), the same operation as in Example 1 was carried out to obtain a water-absorbent resin composition (16).

[0113] <Comparative Example 14> In Example 1, except that 0.1 mass part of sodium gluconate (iron (III) chelate stability constant: 37.2 [logKML], number of carboxyl groups in the molecule: 1) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H), the same operation as in Example 1 was carried out to obtain a water-absorbent resin composition (17).

[0114] <Comparative Example 15> In Example 1, except that 0.1 mass part of sodium glucoheptonate dihydrate (iron (III) chelate stability constant: 38.3 [logKML], number of carboxyl groups in the molecule: 1) was used instead of 0.1 mass part of ethylenediamine-N,N′-disuccinic acid (EDDS·4H), the same operation as in Example 1 was carried out to obtain a water-absorbent resin composition (18).

[0115] <Example 4> In Example 2, the same operation as in Example 2 was carried out except that ion exchange water was not used and the amount of 35 mass % ethylenediamine-N,N′-disuccinate trisodium (EDDS·3Na) aqueous solution as the chelating agent aqueous solution was changed to 0.2 g to obtain a water-absorbent resin composition (19).

[0116] <Example 5> A round-bottomed cylindrical separable flask with an inner diameter of 11 cm and a volume of 2 L and equipped with two stages of stirring blades having four inclined blades with a blade diameter of 5 cm was prepared as a reflux cooler, a dropping funnel, a nitrogen inlet pipe, and a stirrer. In this flask, 293 g of n-heptane as a hydrocarbon dispersion medium was taken, 0.736 g of maleic anhydride-modified ethylene-propylene copolymer (Mitsui Chemicals, Inc., HI-WAX 1105A) as a polymer dispersant was added, and the temperature was raised to 80° C. while stirring to dissolve the dispersant, and then cooled to 50° C. On the other hand, 92.0 g (1.03 mol) of an 80.5 mass % aqueous solution of acrylic acid as a water-soluble ethylenically unsaturated monomer was taken in a beaker having an internal volume of 300 mL, and 147.7 g of a 20.9 mass % aqueous solution of sodium hydroxide was added dropwise while cooling with ice water. After 75 mol % neutralization, 0.092 g of hydroxyethyl cellulose (Sumitomo Seika Co., Ltd., HEC AW-15F) as a thickener, 0.0736 g (0.272 mmol) of potassium persulfate as a water-soluble free radical polymerization agent, and 0.010 g (0.057 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare an aqueous liquid of the first stage. Then, the aqueous liquid prepared as above was added to a separable flask and stirred for 10 minutes. Then, a surfactant solution of 0.736 g of HLB3 sucrose stearate (Mitsubishi Chemical Foods Co., Ltd., Ryoto Sugar Ester S-370) dissolved in 6.62 g of n-heptane as a surfactant was further added to a 20 mL-tube bottle. The system was fully substituted with nitrogen while the stirrer speed was set to 550 rpm for stirring. The flask was immersed in a 70°C water bath for heating and polymerization was carried out for 60 minutes to obtain a first-stage polymerization slurry.

[0117] On the other hand, in another beaker having an internal volume of 500 mL, 128.8 g (1.43 mol) of an 80.5 mass % aqueous solution of acrylic acid as a water-soluble ethylenically unsaturated monomer was taken, and while cooling with ice water, 159.0 g of a 27 mass % aqueous solution of sodium hydroxide was added dropwise, and after 75 mol % neutralization, 0.103 g (0.381 mmol) of potassium persulfate as a water-soluble free radical polymerization initiator and 0.0116 g (0.067 mmol) of ethylene glycol diglycidyl ether as an internal crosslinking agent were added and dissolved to prepare an aqueous liquid of the second stage.

[0118] While stirring with the stirrer set at 1000 rpm, the separable flask system was cooled to 27°C, and then the total amount of the second-stage aqueous liquid was added to the first-stage polymerization slurry liquid. After the system was purged with nitrogen for 30 minutes, the flask was immersed in a 70°C water bath again to raise the temperature, and a polymerization reaction was carried out for 60 minutes to obtain a hydrogel polymer.

[0119] Then, the flask was immersed in an oil bath set at 125°C, and 176.6g of water was discharged to the outside of the system by azeotropic distillation of n-heptane and water while refluxing n-heptane. Then, a chelating agent aqueous solution prepared by adding 1.281g of ion exchange water to 0.189g of 35% by mass ethylenediamine-N,N′-disuccinate trisodium aqueous solution was added under stirring. Then, 76.4g of water was discharged to the outside of the system by azeotropic distillation of n-heptane and water again while refluxing n-heptane. Then, 4.42g (0.507 mmol) of 2% by mass ethylene glycol diglycidyl ether aqueous solution as a surface crosslinking agent was added to the flask and kept at 83°C for 2 hours.

[0120] Then, n-heptane was evaporated and dried at 125°C, and the mixture was passed through a sieve with a mesh size of 850 μm, thereby obtaining 225.7 g of water-absorbent resin particles. 0.5 parts by mass of amorphous silica (Tokusil NP-S, manufactured by Riantong Chemical Co., Ltd.) was mixed with 100 parts by mass of the obtained water-absorbent resin particles, thereby obtaining 226.8 g of a water-absorbent resin composition (20). The water retention capacity of the water-absorbent resin composition (20) was 41 g / g in physiological saline, the water absorption capacity of physiological saline under a load of 4.14 kPa was 11 mL / g, the water content was 8% by mass, and the median particle size was 361 μm.

[0121] <Example 6> In Example 5, the same operation as in Example 5 was carried out except that the amount of 35 mass % ethylenediamine-N,N′-disuccinate trisodium (EDDS·3Na) aqueous solution added to the hydrogel polymer of the second stage was changed from 0.189 g to 0.063 g, the amount of ion exchange water used was changed from 1.281 g to 0.427 g to prepare a chelating agent aqueous solution, and the amount of water discharged to the outside of the system by azeotropic distillation of n-heptane and water was changed from 76.4 g to 75.5 g, thereby obtaining 231.1 g of a water-absorbent resin composition (21). The water-absorbent resin composition (21) had a water retention capacity of 39 g / g in physiological saline, a water absorption capacity of 19 mL / g in physiological saline under a load of 4.14 kPa, a water content of 9 mass %, and a median particle size of 372 μm.

[0122] <Comparative Example 16> In Example 2, the same operation as in Example 2 was carried out except that 0.175 g of a 40 mass % aqueous solution of trisodium N-methylglycine diacetate (MGDA·3Na, iron (III) chelate stability constant: 16.5 [logKML], number of carboxyl groups in the molecule: 3) was used instead of 0.057 g of a 35 mass % aqueous solution of ethylenediamine-N,N′-disuccinate trisodium (EDDS·3Na) and the amount of ion exchange water was changed from 0.143 g to 0.025 g to prepare a chelating agent aqueous solution. A water-absorbent resin composition (22) was obtained.

[0123] <Comparative Example 17> In Comparative Example 16, the same operation as in Comparative Example 16 was carried out except that ion exchange water was not used and the amount of 40 mass % N-methylglycine diacetate trisodium (MGDA·3Na) aqueous solution as the chelating agent aqueous solution was changed to 0.425 g, thereby obtaining a water-absorbent resin composition (23).

[0124] <Example 7> The same operation as in Example 5 was carried out except that the amount of water discharged to the outside of the system by azeotropic distillation of n-heptane and water was changed from 76.4 g to 65.5 g, thereby obtaining 227.9 g of a water-absorbent resin composition (24). The water-absorbent resin composition (24) had a water retention capacity of 35 g / g in physiological saline, a water absorption capacity of 28 mL / g in physiological saline under a load of 4.14 kPa, a water content of 7% by mass, and a median particle size of 353 μm.

[0125] <Example 8> The same operation as in Example 5 was carried out except that the amount of water discharged to the outside of the system by azeotropic distillation of n-heptane and water was changed from 76.4 g to 78.6 g, thereby obtaining 229.2 g of a water-absorbent resin composition (25). The water-absorbent resin composition (25) had a water retention capacity of 46 g / g in physiological saline, a water absorption capacity of 10 mL / g in physiological saline under a load of 4.14 kPa, a water content of 8% by mass, and a median particle size of 351 μm.

[0126] [Evaluation of water-absorbent resin particles] <Water retention of saline solution> A cotton bag (cotton broad No. 60, 100 mm wide x 200 mm long) weighing 2.0 g of water-absorbent resin particles was placed in a 500 mL beaker. 500 g of a 0.9 mass % sodium chloride aqueous solution (physiological saline) was poured into the cotton bag containing the water-absorbent resin particles at once so as not to form a lump, and the upper part of the cotton bag was tied with an elastic band and left to stand for 30 minutes to swell the water-absorbent resin particles. After 30 minutes, the cotton bag was dehydrated for 1 minute using a dehydrator (manufactured by KOKUSAN Co., Ltd., product number: H-122) set to a centrifugal force of 167 G, and the mass Wd (g) of the cotton bag including the swollen gel after dehydration was measured. The same operation was performed without adding water-absorbent resin particles, and the empty mass We (g) of the cotton bag when wet was measured, and the water retention of the physiological saline was calculated according to the following formula. Water retention of saline solution (g / g) = [Wd-We] / 2.0

[0127] <Water absorption of physiological saline solution under 4.14kPa load> 4.14kPa water absorption of physiological saline under load (water absorption under load) Figure 1 The measurement is performed using a measuring device schematically shown in the figure. The measurement is performed twice on a type of water-absorbent resin particles, and the average value is obtained. The measuring device comprises a burette portion 1, a fixture 3, a catheter 5, a stand 11, a measuring table 13, and a measuring portion 4 placed on the measuring table 13. The burette portion 1 comprises: a burette 21 with a scale recorded thereon, a rubber stopper 23 that tightly covers the opening at the upper portion of the burette 21, a stopcock 22 connected to the front end of the lower portion of the burette 21, and an air introduction tube 25 and a stopcock 24 connected to the lower portion of the burette 21. The burette portion 1 is fixed by the fixture 3. The flat measuring table 13 has a through hole 13a with a diameter of 2 mm formed in the center thereof, and is supported by a stand 11 with a variable height. The through hole 13a of the measuring table 13 and the stopcock 22 of the burette portion 1 are connected via a catheter 5. The inner diameter of the catheter 5 is 6 mm.

[0128] The measuring section 4 includes a cylinder 31 made of organic glass, a polyamide net 32 ​​bonded to one opening of the cylinder 31, and a weight 33 movable in the cylinder 31 in the vertical direction. The cylinder 31 is placed on the measuring table 13 via the polyamide net 32. The inner diameter of the cylinder 31 is 20 mm. The mesh of the polyamide net 32 ​​is 75 μm (200 mesh). The weight 33 has a diameter of 19 mm and a mass of 119.6 g. As described later, it is possible to apply a load of 4.14 kPa (0.6 psi) to the water-absorbent resin particles 10a uniformly arranged on the polyamide net 32.

[0129] First, close the stopcock 22 and stopcock 24 of the burette part 1, and inject 0.9 mass % physiological saline adjusted to 25° C. into the burette 21 from the upper opening of the burette 21. Next, after sealing the upper opening of the burette 21 with the rubber stopper 23, open the stopcock 22 and stopcock 24. Fill the interior of the catheter 5 with 0.9 mass % saline 50 in such a way that bubbles do not enter. The height of the measuring table 13 is adjusted so that the height of the water surface of the 0.9 mass % saline solution reaching the through hole 13a is the same as the height of the upper surface of the measuring table 13. After adjustment, read the height of the water surface of the 0.9 mass % saline 50 in the burette 21 using the scale of the burette 21, and use its position as the zero point (the reading value at 0 seconds).

[0130] In the measuring section 4, 0.10 g of the water-absorbent resin particles 10a were evenly arranged on the polyamide mesh 32 in the cylinder 31, a weight 33 was arranged on the water-absorbent resin particles 10a, and the cylinder 31 was set so that the center thereof coincided with the catheter opening in the center of the measuring table 13. The amount of physiological saline reduced in the burette 21 (i.e., the amount of physiological saline absorbed by the water-absorbent resin particles 10a) Wc (mL) after 60 minutes from the time when the water-absorbent resin particles 10a began to absorb the physiological saline from the catheter 5 was read, and the physiological saline absorption capacity of the water-absorbent resin particles 10a under a load of 4.14 kPa was calculated by the following formula. 4.14 kPa water absorption capacity of physiological saline under load (mL / g) = Wc (mL) / mass of water-absorbent resin particles (g)

[0131] <Median particle size (particle size distribution)> 10 g of water-absorbent resin particles were sieved using an ultrasonic vibration sieve measuring device (Robot Shifter RPS-01, manufactured by Seishin Enterprise Co., Ltd.), sieves with mesh sizes of 850 μm, 600 μm, 500 μm, 425 μm, 300 μm, 250 μm and 180 μm according to the JIS standard, and a receiving plate. The mass percentage of the particles remaining on each sieve relative to the total mass was calculated. The mass percentage of the particles remaining on each sieve was accumulated in order from the particles with the largest particle size, and the relationship between the mesh size of the sieve and the cumulative value of the mass percentage of the particles remaining on the sieve was plotted on a logarithmic probability paper. By connecting the plots on the probability paper with a straight line, the particle size corresponding to the cumulative mass percentage of 50% was obtained, and it was taken as the median particle size.

[0132] <Water content> 2.0 g of water-absorbent resin particles are placed in an aluminum foil box (No. 8) that has been pre-made to a constant weight (W1 (g)). The mouth of the aluminum foil box is gently closed, and the total mass W2 (g) of the aluminum foil box containing the sample is accurately weighed. The above-mentioned aluminum foil box containing the sample is dried for 2 hours in a hot air dryer (manufactured by ADVANTEC, model: FV-320) with the internal temperature set to 105°C. The dried aluminum foil box containing the sample is cooled to room temperature in the dryer. The total mass W3 (g) of the aluminum foil box containing the sample after cooling is measured. The moisture content of the sample is calculated according to the following formula. Water content [mass %] = [{(W2-W1)-(W3-W1)} / (W2-W1)] × 100

[0133] [Evaluation of water-absorbent resin composition] <Water retention of saline solution> The physiological saline water retention capacity of the water absorbent resin composition was measured in the same manner as the physiological saline water retention capacity of the water absorbent resin particles.

[0134] <Water absorption of physiological saline solution under 4.14kPa load> The physiological saline water absorption under a load of 4.14 kPa of the water absorbent resin composition was measured in the same manner as the physiological saline water absorption under a load of 4.14 kPa measured for the water absorbent resin particles.

[0135] <Measurement of water absorption rate by vortex method> In a constant temperature water bath, 50±0.1 g of physiological saline solution adjusted to 25±0.2°C was weighed in a 100 mL beaker and stirred with a magnetic stirrer ( The water-absorbent resin composition was stirred at a speed of 600 rpm to generate a vortex. 2.0 ± 0.002 g of the water-absorbent resin composition was added to the physiological saline at once, and the time (seconds) from the addition of the water-absorbent resin composition to the moment when the vortex on the liquid surface converged was measured, and the time was taken as the water absorption rate of the water-absorbent resin composition. The water absorption rate is also expressed as the vortex method or vortex time.

[0136] <Median particle size (particle size distribution)> The median particle size (particle size distribution) of the water-absorbent resin composition is measured in the same manner as the median particle size (particle size distribution) measured for the above-mentioned water-absorbent resin particles.

[0137] <Water content> The water content of the water absorbent resin composition was measured in the same manner as the water content of the water absorbent resin particles.

[0138] <Soluble components dissolved in 1 hour after degradation test> The soluble components dissolved out one hour after the degradation test were measured according to the following procedure. The "soluble content dissolved in one hour" in the present invention refers to the water-soluble content when the 0.90 mass % sodium chloride aqueous solution is changed to an aqueous solution in which L-ascorbic acid is mixed in the 0.90 mass % sodium chloride aqueous solution (deterioration test solution) according to the Ext (water-soluble content) measurement method specified in ERT 470.2-02, and then stirred for one hour after standing at 60°C for 2 hours. That is, 200.0 g of an aqueous solution containing 0.05 mass % L-ascorbic acid and 0.90 mass % sodium chloride (deterioration test solution / mixture of 0.10 g of L-ascorbic acid and 199.90 g of 0.90 mass % sodium chloride aqueous solution) is measured in a 250 ml plastic container with an inner lid and an outer lid equipped with a rotor of 35 mm in length, and then 1.00 g of the water-absorbent resin composition is added to the aqueous solution, and the container is sealed with the inner lid and the outer lid. Then, the container is left standing for 2 hours in a thermostat adjusted to 60±2°C. After 2 hours, the container was taken out from the thermostat and stirred at room temperature for 1 hour using a stirrer (rotation speed of about 500 rpm). The water-soluble components of the water-absorbent resin composition were extracted by the above operation. After stirring, the extract as the above aqueous solution was filtered with a piece of filter paper (manufactured by ADVANTEC Toyo Co., Ltd.; product name: JIS P 3801 No. 2 / thickness 0.26 mm, retention particle size 5 μm), and 50.0 g of the obtained filtrate was used as the measurement liquid. Next, the above measurement liquid was titrated with 0.1N-NaOH aqueous solution to pH 10, and then titrated with 0.1N-HCl aqueous solution to pH 2.7. The titration amount at this time was determined as [NaOH] ml and [HCl] ml. In addition, the water-absorbent resin composition was not added, and only 200.0 g of the deterioration test liquid was used, and the same operation was performed to determine the empty titration amount ([b2NaOH] ml and [b2HCl] ml). The soluble component dissolved in one hour was calculated according to the following formula from the titration amount and the average molecular weight of the monomers. Soluble component dissolved in 1 hour [mass %] = 0.1 × average molecular weight of monomer × 200 × 100 × ([HCl] - [b2HCl]) / 1000 / 1.0 / 50.0

[0139] <Test of gel absorbing artificial urine> Using artificial urine, a test of gel (swollen gel) formed by water absorption of the water-absorbent resin composition was conducted. It should be noted that, as described in detail below, the evaluation of gel strength after standing at 37°C for 14 hours was used as an indicator for evaluating stability during normal use. Then, the evaluation of gel strength after standing at 37°C for 14 hours and further irradiation with ultraviolet rays was performed as an indicator for evaluating gel separation during disposal.

[0140] (Preparation of artificial urine) Artificial urine of the following composition was prepared. Urea: 20.0g Sodium chloride: 8.0g Calcium chloride dihydrate: 0.3g Magnesium sulfate heptahydrate: 0.8 g L(+)-ascorbic acid: 0.2 g Ion exchange water: 970.9g

[0141] (Preparation of swollen gel) 39.0 g of the artificial urine was weighed into a beaker with an internal volume of 100 mL (opening inner diameter: 51 mm), and a magnetic stirrer (8 mmφ×30 mm, without ring) was placed on a magnetic stirrer (manufactured by Iuchi: HS-30D), and the magnetic stirrer was rotated at 600 rpm. Next, 1.00 g of the water-absorbent resin composition was placed into the stirring beaker, and the mixture was stirred until the vortex disappeared and the liquid surface became horizontal, thereby preparing a swollen gel as a measurement sample. After the swollen gel was prepared, the beaker containing the swollen gel was immediately covered with a plastic wrap (manufactured by Mitsubishi Chemical Corporation, DIAWRAP).

[0142] (Determination of gel strength) The gel strength after standing for a specified time under various temperature conditions was measured using Figure 2 The measurement principle is shown in the apparatus for carrying out the measurement. Figure 2The device shown is composed of a support portion 50a, a movable platen 60, a driving portion 70 for driving the movable platen 60, and a measuring portion 80. In the support portion 50a, a stand 53 is fixed to the upper part of a pillar 52 erected on the support platform 51. The movable platen 60 is mounted on the pillar 52 in a manner that it can move up and down. The movable platen 60 can carry a measurement sample (gel) 61. A pulse motor 71 is mounted on the stand 53, and the movable platen 60 is moved up and down via a wire 73 by rotating a pulley 72. In the measuring portion 80, a pressure-sensitive shaft 84 is mounted on a force sensor 81 for measuring strain caused by deformation via a precision spring 82 and a connecting shaft 83. The reel pressure-sensitive shaft 84 has a disk at the front end. The diameter of the disk can be changed according to the measurement conditions. A counterweight 90 can be mounted on the upper part of the reel pressure-sensitive shaft 84. The working principle of the device for measuring the gel strength is as follows. The precision spring 82 is fixed to the load cell 81 (stress detector) at the top, and the pressure-sensitive shaft 84 with a disk is connected at the bottom, and a specified counterweight 90 is placed on it and suspended vertically. The movable platen 60 carrying the test sample 61 is raised at a constant speed by the rotation of the pulse motor 71. A constant speed load is applied to the sample 61 via the precision spring 82, and the strain caused by the deformation is measured by the load cell 81 to measure the hardness. The gel strength value (N / m2) is measured using a curdmeter (Asuka Machine Manufacturing, Curdmeter-MAX, Model: ME-500) with the disk of the pressure-sensitive shaft. The measurement was performed with a load of 400 g, a speed of 7 sec / inch, and a viscous mode setting.

[0143] (Initial value of gel strength) After the preparation, the swollen gel was allowed to stand for 60 minutes in an environment of 25±2°C and 50±10% relative humidity, and then the gel strength (initial value of gel strength) was measured by the method described in (Measurement of gel strength). The gel strength value at this time was recorded as gel strength (A).

[0144] (Gel strength after standing for 14 hours at 37°C) After the preparation, the swollen gel was left to stand for 14 hours in a constant temperature and humidity chamber (LHU-113 manufactured by ESPEC Co., Ltd.) set at a temperature of 37±2°C and a relative humidity of 60±10%, and then the gel strength was measured by the method described in the above (Measurement of gel strength). The gel strength value at this time was recorded as gel strength (B).

[0145] (Evaluation of gel strength change and gel stability) The gel strength change (%) was calculated from the initial value of the gel strength (gel strength (A)) and the gel strength (B) by the following formula. The lower the gel strength change, the higher the gel stability. The stability of the gel was determined based on the value of the gel strength change using the following criteria. Gel strength change (%) = [(gel strength (A) - gel strength (B)) / gel strength (A)] × 100

[0146] <Criteria for judging gel stability> Gel strength variation less than 40%: Good Gel strength variation of 40% or more: Poor

[0147] (Gel strength after standing at 37°C for 14 hours and further UV irradiation) After preparation, the swollen gel was allowed to stand for 14 hours in a constant temperature and humidity machine (LHU-113 manufactured by ESPEC Co., Ltd.) set at a temperature of 37±2°C and a relative humidity of 60±10%. Then, the swollen gel after standing was placed in a beaker (the covering plastic wrap was removed) and placed directly below the light source of an ultraviolet irradiation device (SPECTROLINE manufactured by SPECTRONICS, model: XX-15NF) at a temperature of 25±2°C and a relative humidity of 50±10%. At this time, the distance between the surface of the swollen gel and the light source was 7 cm. After shielding the light by covering the entire device with a box, the swollen gel in the beaker was irradiated with ultraviolet rays of a wavelength of 254 nm for 150 minutes. After ultraviolet irradiation, the gel strength was measured by the method described in the above (Measurement of gel strength). The value of the gel strength at this time was referred to as the gel strength (C).

[0148] (Evaluation of gel strength change and gel separation after UV irradiation) The change in gel strength after UV irradiation (%) was calculated by the following formula based on the initial value of the obtained gel strength (gel strength (A)) and the value of the gel strength after UV irradiation (gel strength (C)). The greater the change in gel strength after UV irradiation, the softer the gel. Based on the value of the change in gel strength after UV irradiation, the ease of gel separation operation was determined using the following criteria. Change in gel strength after UV irradiation (%) = [(gel strength (A) - gel strength (C)) / gel strength (A)] × 100

[0149] <Criteria for judging gel separation properties> The gel strength change after UV irradiation is less than 40%: bad Gel strength change after UV irradiation is 40% or more: Good

[0150] [Table 1]

[0151] Notes to Table 1: 1) Tongren Chemistry. 2018. Product Catalog. 31st Edition. 268-269. 2) Isabel SS Pinto, Isabel FF Neto, Helena MVM Soares. 2014. Biodegradable chelating agents for industrial, domestic, and agricultural applications-a review. Environ Sci Pollut Res. 21. 11893-11906. 3) Takashi Minoura. 1984. Chelating agent industry. Synthetic Organic Chemistry. 42(2). 165-169. 4) LANXESS. 2005. BAYPURE GENERAL PRODUCTIMFORMATION. 10. 19. 5) R. M. Smith, A. E. Martell. 1995. Critical Stability Constants. 3rd Edition. Plenum Press.

[0152] In the water-absorbent resin compositions of Examples 1 to 8, in addition to the surface-crosslinked water-absorbent resin particles, a chelating agent having an iron (III) chelate stability constant of 16 log KML or more and 24 log KML or less and a carboxyl group number of 4 or more and 10 or less is used as a chelating agent. The water-absorbent resin compositions of Examples 1 to 8 have both the gel stability of the water-absorbent resin composition when normally worn in sanitary materials and the high operability when the water-absorbent resin composition is separated after ultraviolet irradiation as a waste treatment means. In particular, the water-absorbent resin compositions of Examples 1 to 2 and 4 to 8 have moderate gel strength after UV irradiation and are particularly excellent in operability during separation. Description of Reference Numerals

[0153] 1 Burette section 3. Fixture 4 Measurement unit 5 Catheter 10a Water-absorbent resin particles 11 racks 13. Measuring table 13a Through hole 15 Nylon mesh 21 Burette 22 Plug 23 Rubber stopper 24 Plug 25 Air inlet pipe 31 Cylinder 32 Polyamide mesh 33 Counterweight.

Claims

1. A water-absorbent resin composition, characterized in that Contains water-absorbent resin particles and a chelating agent, The water-absorbent resin particles are surface cross-linked. The iron (III) chelate stability constant of the chelating agent is 16 log KML or more and 24 log KML or less, and the number of carboxyl groups is 4 or more and 10 or less.

2. The water-absorbent resin composition according to claim 1, wherein The change in gel strength of the water-absorbent resin composition after UV irradiation is 40% or more, Regarding the change in gel strength after UV irradiation: From the initial value of the gel strength (gel strength (A)) and the value of the gel strength after ultraviolet irradiation (gel strength (C)) obtained by the following steps 1 and 2, the change (%) of the gel strength after UV irradiation is calculated by the following formula: Change in gel strength after UV irradiation (%) = [(gel strength (A) - gel strength (C)) / gel strength (A)] × 100 About the initial value of gel strength (gel strength (A)): The swollen gel prepared by the following step 1 is allowed to stand at a temperature of 25±2° C. and a relative humidity of 50±10% for 60 minutes after preparation, and then the gel strength (initial value of the gel strength) is measured by the following step 2; the gel strength value at this time is recorded as gel strength (A). The value of gel strength after ultraviolet irradiation (gel strength (C)): The swollen gel prepared by the following step 1 is allowed to stand at a temperature of 37±2°C and a relative humidity of 60±10% for 14 hours after preparation; then, the swollen gel after standing is placed directly under the light source of an ultraviolet irradiation device at a temperature of 25±2°C and a relative humidity of 50±10%; at this time, the distance between the surface of the swollen gel and the light source is 7 cm; after covering the entire device with a box to block light, the swollen gel in the beaker is irradiated with ultraviolet rays of a wavelength of 254nm for 150 minutes; after irradiating with ultraviolet rays, the gel strength is measured by the following step 2; the value of the gel strength at this time is recorded as the gel strength (C), Step 1, preparation of swelling gel: 39.0 g of artificial urine was measured in a beaker with an internal volume of 100 mL, and a magnetic stirrer was placed in it and arranged on a magnetic stirrer, and the magnetic stirrer was rotated at 600 rpm; then, 1.00 g of the water-absorbent resin composition was placed in the stirring beaker, and the stirring was continued until the vortex disappeared and the liquid surface became horizontal, thereby preparing a swollen gel as a measurement sample; immediately after the swollen gel was prepared, the beaker containing the swollen gel was covered with a plastic wrap, Step 2, i.e. determination of gel strength: Gel strength value (N / m 2 ) Using a curd meter, the initial value of the gel strength (gel strength (A)) and the value of the gel strength after ultraviolet irradiation (gel strength (C)) were measured under the conditions of temperature and standing time.

3. The water-absorbent resin composition according to claim 1 or 2, wherein The content of the chelating agent is 0.001 parts by mass or more and 2 parts by mass or less relative to 100 parts by mass of the water-absorbing resin particles.

4. The water-absorbent resin composition according to claim 1 or 2, wherein The water-absorbent resin composition has a physiological saline water retention capacity of 25 g / g or more and 60 g / g or less.

5. The water-absorbent resin composition according to claim 1 or 2, wherein The water-absorbent resin composition has a physiological saline water absorption capacity of 5 ml / g or more and 40 ml / g or less under a load of 4.14 kPa.

6. An absorbent body, characterized in that: The absorbent body comprises the water-absorbent resin composition according to claim 1 or 2.

7. An absorbent article, characterized in that: The absorbent article includes the absorbent body according to claim 6.

8. The method for producing a water-absorbent resin composition according to claim 1 or 2, wherein: have: A step of mixing the water-absorbing resin particles before surface cross-linking and the chelating agent; and / or A step of mixing the surface-crosslinked water-absorbing resin particles and the chelating agent.

Citation Information

Patent Citations

  • Water-absorbing resin composition

    JP2005029751A