Surface coated cutting tool
Patent Information
- Application Number
- CN202380029564.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-08
AI Technical Summary
[0006] The present invention was completed in view of the above-mentioned circumstances and solutions, and its purpose is to provide a method that regulates the uniformity of the coating layer so that multiple cutting tips of the same shape all have sufficient and uniform coating even in high-speed intermittent cutting. Long life cladding tool.
Smart Images

Figure CN118922265A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a surface-coated cutting tool (hereinafter, sometimes referred to as a coated tool). This application claims priority based on Japanese patent application No. 2022-56507 filed on March 30, 2022. All the contents described in the Japanese patent application are incorporated into this specification by reference. Background Art
[0002] As a cutting tool, there is known a coated tool in which a coating layer is formed on the surface of a base such as tungsten carbide (hereinafter referred to as WC)-based cemented carbide.
[0003] Furthermore, in order to ensure that the plurality of cutting edges provided in the coated tool have uniform cutting performance, efforts have been made to make the composition of the coating layer uniform.
[0004] For example, Patent Document 1 describes a chemical vapor deposition device that can form a coating layer with uniform composition on multiple substrates placed on a fixture. By using this device for film formation, a coated tool can be obtained, wherein the coating layer formed on the substrate on the inner side of the fixture and the substrate on the outer side of the fixture has a small difference in average Al or Ti content and a uniform composition.
[0005] Patent Document 1: Japanese Patent Publication No. 2017-20111 Summary of the invention
[0006] The present invention is completed in view of the above situation and scheme, and its purpose is to provide a coated tool with a predetermined uniformity of the coating layer so that multiple cutting tips of the same shape all have sufficient and uniform service life even in high-speed intermittent cutting.
[0007] Regarding the surface-coated cutting tool according to the embodiment of the present invention,
[0008] A substrate and a coating layer arranged on the substrate,
[0009] (a) the coating layer comprises a composite nitride layer or a composite carbonitride layer of Al and Ti having grains with a NaCl-type face-centered cubic structure,
[0010] (b) The tool has a plurality of cutting tips of the same shape, and in the back surfaces of all the cutting tips, the composite nitride layer or composite carbonitride layer of Al and Ti is (Al x Ti 1-x )(C y N 1-y )(Average content of x avg is 0.60 or more and 0.95 or less, and the average content of y avgis greater than 0.0000 and less than 0.0050),
[0011] (c) In each flank of all the cutting tips, the grains having the NaCl-type face-centered cubic structure included in the coating layer have 200 diffraction lines measured using an X-ray diffraction device, and the average value of the intensity values of the 200 diffraction lines is set as I avg (200), and its standard deviation is set to σ I(200) When I(200) / I avg (200) satisfies 0.00 or more and 0.20 or less,
[0012] (d) In each of the above-mentioned cutting edges, the thickness of the coating layer on a line 100 μm away from the cutting edge ridgeline in the flank direction is defined as Lm, and the average value of the Lm in all the cutting edges is defined as Lm. avg , the standard deviation is set to σ L When L / L avg Satisfy 0.00 or more and 0.20 or less,
[0013] (e) In each flank surface of all the cutting tips, the composite nitride layer or composite carbonitride layer of Al and Ti includes columnar crystals, and the maximum value x of x in the columnar crystals is max *The average value of x max and the minimum value x of x min *The average value of x min Satisfy 0.02≤x max -x min The area ≤0.40.
[0014] Furthermore, the surface-coated cutting tool according to the above-mentioned embodiment may satisfy one or more of the following items (1) to (5).
[0015] (1) The average value TC of the texture coefficient TC(200) of the grains having the NaCl type face-centered cubic structure included in the coating layer in each flank surface of all the cutting tips avg (200) satisfies 1.0 or more and 6.0 or less.
[0016] (2) In each of all the cutting tips, the average value of the texture coefficient TC(200) of the grains having the NaCl type face-centered cubic structure included in the coating layer is set to TC avg (200), and its standard deviation is set to σ TC(200) When TC(200) / TC avg (200) is greater than or equal to 0.00 and less than or equal to 0.10.
[0017] (3) In each flank surface of all the cutting edges, a region having a variation in the content of Al and Ti included in the cladding layer accounts for 70% by area or more in a longitudinal section of the cladding layer.
[0018] (4) In each of the coating layers of all the cutting tips, the average grain width W of the columnar crystals of the composite nitride layer or composite carbonitride layer of Al and Ti is greater than 0.10 μm and less than 1.20 μm, and the average aspect ratio A thereof is greater than 2.0 and less than 10.0.
[0019] (5) The composite nitride layer or composite carbonitride layer of Al and Ti contains chlorine, and the content ratio thereof is 0.005 atomic % or more and 0.500 atomic % or less.
[0020] The coating layer of the surface-coated cutting tool has excellent uniformity, and all cutting edges thereof also exhibit excellent heat crack resistance and chipping resistance in high-speed intermittent cutting of alloy steel, carbon steel, and cast iron. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a cross-sectional view schematically illustrating an example of a cutting edge ridgeline portion on a cutting edge of an insert.
[0022] Figure 2 This is a diagram schematically illustrating an example of a corner portion of a cutting edge on a cutting edge of an insert.
[0023] Figure 3 It is a schematic plan view showing an example of the arrangement of gas supply pipes of a chemical vapor deposition apparatus for manufacturing a surface-coated cutting tool according to the present embodiment.
[0024] Figure 4 Yes means Figure 3 A schematic diagram of the side of the device.
[0025] Figure 5 This is a schematic diagram of a chemical vapor deposition apparatus for producing a surface-coated cutting tool of a comparative example.
[0026] Figure 6 yes Figure 5 A schematic diagram of a cross section of a gas supply pipe of the device. DETAILED DESCRIPTION
[0027] When a coated tool is subjected to high-speed intermittent cutting, if the coating layer is non-uniform, that is, the coating layer has non-uniform thickness, composition, etc., the non-uniform portion becomes a starting point for damage, causing thermal cracking and chipping. In particular, when a coated tool has multiple cutting tips, if the coating layers of each cutting tip are non-uniform, the cutting performance of the cutting tips will vary, resulting in differences in durability.
[0028] The present inventors have studied the variation in cutting performance and the difference in durability of each cutting tip. As a result, they have obtained the following findings:
[0029] In a coating layer having a composite nitride or composite carbonitride of Al and Ti (hereinafter, the composite nitride and composite carbonitride may be collectively referred to as AlTiCN), when grains with a {111} plane preferential orientation and grains with a {100} plane preferential orientation are mixed, or,
[0030] If there are grains with {100} plane preferential orientation that are easy to include hexagonal grains in the grain boundaries, the growth rate of the grains varies depending on the orientation and crystal system. Therefore, when one coated tool has multiple cutting edges,
[0031] The uniformity of the thickness, orientation, and crystallinity of the coating layer decreases for each cutting edge, causing variations in cutting performance and durability.
[0032] On the other hand, the present inventors have studied film formation using the vapor deposition device described in the aforementioned Patent Document 1. As a result, they have found that even when the vapor deposition device is used, in a coated tool having a plurality of cutting tips including the aforementioned coating layer with different grain growth rates, the thickness, orientation, and uniformity of crystallinity of the coating layer on the plurality of flank surfaces cannot be made sufficiently equal. In other words, they have found that when the coated tool is used for high-speed intermittent cutting of carbon steel, cast iron, or alloy steel, the generation of a cutting tip having a shorter service life than other cutting tips among the plurality of cutting tips cannot be suppressed, and uniform durability cannot be obtained in some cases.
[0033] Based on this understanding, the inventors believe that in order to obtain uniform heat crack resistance and chipping resistance for a coated tool having multiple cutting tips (the multiple cutting tips have a coating layer including grains with different growth rates) in high-speed intermittent cutting of carbon steel, cast iron, and alloy steel, it is indispensable to specifically stipulate the allowable limits (allowable degree of non-uniformity) of the uniformity of the thickness, orientation, and crystallinity of the coating layer on the back face. Therefore, an in-depth study was conducted on the allowable limits of the uniformity of the thickness and orientation of the coating layer on the back face of the multiple cutting tips, and insights related to the allowable limits were obtained. Furthermore, when a coated tool having multiple cutting tips including a coating layer with different growth rates of the aforementioned grains is provided for high-speed intermittent cutting of carbon steel, cast iron, and alloy steel, insights related to the physical properties required of the coating layer are also obtained.
[0034] Hereinafter, embodiments of the present invention will be described in detail.
[0035] In the present specification and claims, when "L~M" (L and M are both numerical values) is used to express a numerical range, it has the same meaning as "above L and below M", and the range includes an upper limit M and a lower limit L. When only the unit of the upper limit M is recorded, the units of the upper limit M and the lower limit L are the same.
[0036] First, the terms related to the coated tool of the present embodiment are defined.
[0037] The high-speed intermittent cutting process referred to in this specification refers to a cutting process that is higher than the cutting speed usually performed by those skilled in the art, and is a process in which the cutting tool tip repeatedly cuts and idles.
[0038] In the description of this specification and claims, a longitudinal section refers to a section perpendicular to the surface of the substrate when the blade is treated as a flat surface while ignoring the micro-concave and convex surfaces on the surface of the substrate. In addition, in this specification, the surface of the substrate refers to the average line (straight line) of the interface roughness between the substrate and the coating layer in the observation image of the longitudinal section. And, the direction perpendicular to the average line is set as the direction perpendicular to the substrate (thickness direction of the coating layer).
[0039] Even when the substrate has a curved surface like a drill, if the tool diameter is sufficiently large relative to the thickness of the coating, the surface of the substrate can be determined by the same method because the interface between the coating and the substrate in the measurement area is approximately flat.
[0040] In the present specification and claims, the cutting edge refers to the portion that actually comes into contact with a workpiece during cutting.
[0041] 1. Coating layer
[0042] The coating layer of this embodiment includes an AiTiCN layer. This layer will be described in detail below.
[0043] (1) NaCl-type face-centered cubic grains
[0044] When a plurality of cutting tips of the same shape are included in a coated tool, in the back faces of all the cutting tips, the AlTiCN layer included in the coating layer preferably includes grains of NaCl type face-centered cubic structure. Moreover, in all the plurality of cutting tips, the area ratio of the grains having the NaCl type face-centered cubic structure in the longitudinal section of the coating layer on the back face is preferably 50 area % or more, and more preferably 70 area % or more. The reason is that although the aforementioned problem can be solved when the area ratio is 50 area % or more, if it is less than 70 area %, the hardness becomes low and the wear resistance sometimes becomes insufficient. In addition, all the grains may be of NaCl type face-centered cubic structure (may be 100 area %).
[0045] Whether there are grains of NaCl-type face-centered cubic structure constituting the AlTiCN layer can be confirmed by, for example, measuring the X-ray diffraction pattern by micro-area X-ray diffraction measurement (example of measurement conditions: Cu-Kα rays, output 50 kV, 22 mA, step size 0.02 mm, scanning step time 300 sec, detection distance 150 mm, collimator diameter 100 μmΦ) based on the presence or absence of X-ray diffraction peaks appearing between the diffraction angles of the same crystal plane represented by JCPDS00-038-1420 cubic TiN and JCPDS00-046-1200 cubic AlN, respectively (e.g., 36.66 to 38.53°, 4359 to 44.77°, 61.81 to 65.18°).
[0046] Furthermore, whether or not there are grains of a NaCl face-centered cubic structure constituting the AlTiCN layer can also be confirmed by combining a method for determining the area ratio of grains of a NaCl face-centered cubic structure constituting the AlTiCN layer described below. The measurement location is preferably an observation field near a measurement location (within a radius of 50 μm from the measurement location) where the average value (Lm) of the thickness of the AlTiCN layer of the flank face described later is determined for each cutting tip.
[0047] The procedure for measuring the area ratio of the NaCl-type face-centered cubic grains is as follows.
[0048] First, the grain boundaries are determined. That is, the longitudinal section is polished to obtain the surface polished surface, and the crystal orientation analysis device attached to the transmission electron microscope (TEM) is used to irradiate the surface polished surface with electron beams inclined, for example, by 0.5 degrees or more and 1.0 degrees or less relative to the normal direction of the surface polished surface by precession motion (Pression), and the electron beams are scanned at arbitrary beam diameters and intervals at each measurement point to continuously measure the electron diffraction pattern.
[0049] Furthermore, by analyzing each measurement point, the presence or absence of the NaCl type face-centered cubic structure and its crystal orientation can be determined. Furthermore, for example, for an observation field set to a width of 2000 nm and a height including the entire thickness of the coating layer, the grain boundary is determined as described below.
[0050] In addition, the conditions for obtaining the electron diffraction pattern used in the measurement are, for example, an acceleration voltage of 200 kV, a camera length of 20 cm, a beam size of 2.4 nm, and a measurement step of 10.0 nm in the horizontal and vertical directions. At this time, the measured crystal orientation is the orientation obtained by discretely investigating on the measurement surface, and the orientation distribution of the entire measurement surface is obtained by representing the area up to the middle between adjacent measurement points with its measurement results. In addition, as an area represented by a measurement point (hereinafter sometimes referred to as a pixel), a square area can be exemplified.
[0051] When there is a crystal orientation angle difference of 5 degrees or more between adjacent pixels in the pixel, or when only one of the adjacent pixels shows a NaCl-type face-centered cubic structure, the edge of the region where these pixels are connected is regarded as a grain boundary. And, the region surrounded by the edge serving as the grain boundary is defined as one grain.
[0052] However, a single pixel having an orientation difference of 5 degrees or more with all adjacent pixels or having no adjacent measurement points with a NaCl-type face-centered cubic structure is not considered a grain, but a region connected to two or more pixels is considered a grain. In this way, grain boundaries are determined to identify grains.
[0053] The area ratio of the grains with the NaCl face-centered cubic structure is calculated as the ratio of the total area of the determined grains with the NaCl face-centered cubic structure to the total area of the observation field. The same measurement is performed on each cutting tip in five or more observation fields, and the average value of the measurement results of all the cutting tips is set as the area ratio of the grains with the NaCl face-centered cubic structure constituting the AlTiCN layer.
[0054] (2) Composition of AlTiCN layer
[0055] In each of the flank surfaces of all the cutting tips, the AlTiCN layer is preferably (Al x Ti 1-x )(C y N 1-y )(Average content of x avg is 0.60 or more and 0.95 or less, and the average content of y avg is greater than 0.0000 and less than 0.0050).
[0056] x avg The reason for setting this range is that if x avg If x is less than 0.60, the heat crack resistance will decrease, which is not preferred. avg If y is greater than 0.95, the wear resistance will decrease, which is not preferred. avg The reason for setting the average content x in this range is that the lubricity is improved, the impact during cutting is alleviated, and the chipping resistance is improved. avg When it is 0.75 or more and 0.95 or less, the above-mentioned characteristics can be exhibited more excellently.
[0057] x related to the average content of AlTiCN layer avg ,y avg It can be obtained as follows: The measurement location is preferably an observation field near a measurement position (within a radius of 50 μm from the measurement position) where the average value (Lm) of the thickness of the AlTiCN layer of the flank surface described later is obtained for each cutting edge.
[0058] The content (x) of Al in the total amount of Al and Ti can be obtained by, for example, irradiating electron beams from the surface side of the longitudinal section of the surface of the coating layer by using an electron probe microanalyzer (EPMA) near the measurement position of the longitudinal section where the surface is polished, and averaging the analysis results of 10 characteristic X-rays obtained. Alternatively, the polished surface near the measurement position of the longitudinal section of the coating layer can be irradiated with electron beams from the longitudinal section using energy dispersive X-ray spectroscopy (EDS), and the analysis results of the composition of Al and Ti obtained by performing ray analysis in the thickness direction of the layer can be used to obtain the content (x) of Al in the total amount of Al and Ti.
[0059] Regarding the C content (y), for example, a 70 μm×70 μm area of the polished surface of the coating layer parallel to the surface of the substrate near the measurement position is measured by secondary ion mass spectrometry (SIMS) in the depth direction to obtain the average value. In addition, regarding these average values, multiple locations (for example, three locations) are measured in the coating layer on all cutting edges of the same shape in one coated tool, and the average value of all these measurement results is taken as y. avg .
[0060] In addition, (Al x Ti 1-x ) and (C y N 1-y ) is not particularly limited. x Ti 1-x ) is set to 1, and (C y N 1-y ) is preferably 0.8 or more and 1.2 or less. The reason is that if (Al x Ti 1-x ) and (C y N 1-y ) is within the above range, the aforementioned purpose can be achieved more effectively.
[0061] In addition, even if the AlTiCN layer includes a trace amount of inevitable impurities (impurities not intentionally included) such as oxygen, it does not hinder the achievement of the aforementioned purpose.
[0062] (3) Average and standard deviation of the 200-degree diffraction line intensity of grains with NaCl-type face-centered cubic structure in the AlTiCN layer
[0063] In each flank of all cutting tips, the grains having the NaCl type face-centered cubic structure included in the coating layer measured using an X-ray diffraction device have 200 diffraction lines, and the average value of the intensity values of the 200 diffraction lines is set as I avg (200), and its standard deviation is set to σ I(200) When I(200) / I avg (200) is preferably greater than or equal to 0.00 and less than or equal to 0.20.
[0064] The reason for this is that since the average value of the 200 diffraction line intensity values has no deviation, that is, the standard deviation σ is preferably 0 (none), so σ I(200) / I(200) has a lower limit of 0.00. On the other hand, if σ I(200) / I avgWhen (200) is greater than 0.20, the uniformity of crystallinity and orientation of each blade tip is reduced, thereby reducing the uniformity of heat crack resistance and chipping resistance during high-speed intermittent cutting. Here, the 200 diffraction line refers to the reflection indexed as 200 when performing XRD analysis.
[0065] The average value of 200 diffraction line intensity values of the grains having NaCl-type face-centered cubic structure is avg (200) and its standard deviation σ I(200) For example, it can be obtained for each cutting tip in the following manner. The X-ray diffraction pattern is measured by micro-area X-ray diffraction measurement (example of measurement conditions: Cu-Kα ray, output 50kV, 22mA, step size 0.02mm, scanning step time 300sec, detection distance 150mm, collimator diameter 100μmΦ), and the 200 diffraction line intensity value is obtained. In this way, I(200) is obtained for each cutting tip, and the average value is taken to obtain I avg (200).
[0066] The measurement position was a line segment of 500 μm selected from the blade edge line and the line segment was parallelly moved by 100 μm in the flank direction near the center.
[0067] Here, if n is the number of cutting edges of the same shape, the standard deviation σ I(200) It can be calculated by the following [Formula 1].
[0068] [Mathematical formula 1]
[0069]
[0070] (4) Average and standard deviation of the thickness of the AlTiCN layer on the back face
[0071] For each of the cutting edges, the average thickness Lm of the AlTiCN layer on a line 100 μm away from the cutting edge ridgeline in the flank direction was determined, and the average value of Lm was defined as L avg And the standard deviation of Lm is σ L When σ L / L avg Satisfies 0.00 or more and 0.20 or less.
[0072] L avg The L is preferably 1.0 μm or more and 20.0 μm or less. The reason is that if it is within this range, the wear resistance can be fully ensured and excellent chipping resistance can be obtained. avg When the thickness is 3.0 μm or more and 15.0 μm or less, the above-mentioned characteristics can be exhibited more excellently.
[0073] The reason is that, since L is preferred avg No deviation, that is, standard deviation σ L is 0 (none), so σ L / L avg The lower limit is 0.00. On the other hand, if σ L / L avg When the ratio is greater than 0.20, the coating layer thickness distribution occurs due to the difference in film forming speed, and the uniformity of the heat crack resistance and chipping resistance provided during high-speed intermittent cutting is reduced.
[0074] Here, the cutting edge line portion on the cutting edge refers to Figure 1 As shown, when the front cutting edge 1 and the back cutting edge 2 are respectively fitted with a straight line (hereinafter sometimes referred to as a fitting straight line), in an area separated from the straight line and connected to the starting point of the bending (i.e., the area on the surface of the covering layer from the bending point of the front cutting edge to the bending point of the back cutting edge), the point on the surface of the covering layer closest to the intersection of the fitting straight line (the portion indicated by the dotted arrow) is the point.
[0075] In this embodiment, a coated tool including a plurality of cutting tips of the same shape is taken as an object, and among all the cutting tips, the average thickness Lm of the coating layer on a line 100 μm away from the ridgeline of the cutting tip in the back face direction and the average value Lm of the Lm are calculated as follows: avg and standard deviation σ L .
[0076] like Figure 2 As shown, when viewed from the front cutting edge 1, the cutting edge ridge portion is the cutting edge ridge 3 of the main cutting edge. The line 100 μm away from the cutting edge ridge portion in the back cutting edge direction refers to a straight line that passes through a point 100 μm away from the back cutting edge direction from any point on the cutting edge ridge 3 of the main cutting edge as a starting point and is parallel to the cutting edge ridge 3 of the main cutting edge.
[0077] Specifically, in Figure 2 A line segment of 500 μm is selected from the blade edge line 3, and a plurality of points on the line segment which is parallelly moved 100 μm in the direction of the back face and spaced apart by a predetermined length are selected to measure the thickness of the coating layer and obtain the average value Lm.
[0078] Here, the plurality of points on the line segment that are spaced apart by a predetermined length may be, for example, four points spaced apart by 30 μm, but the present invention is not limited thereto, and it is preferred to select more measurement points. In this way, Lm is calculated for each cutting edge, and L is calculated by taking the average value. avg .
[0079] When measuring the thickness, a sample for observing the longitudinal section of the coating layer is prepared using an ion beam cross section polisher (CP) or the like, and the cross section is observed using a scanning electron microscope (SEM).
[0080] Here, if n is the number of cutting blade tips of the same shape, the standard deviation σ L It can be calculated by the following [Formula 2].
[0081] [Mathematical formula 2]
[0082]
[0083] In addition, in the case where there are multiple cutting tips of the same shape with acute corners and obtuse corners in a coated tool, if either one satisfies the requirements described in this specification and claims, it is treated as a surface coated cutting tool of the present invention.
[0084] In addition, for a circular blade, when the cutting tip exists along the outer periphery of the circle, for example, two points can be selected: an arbitrary point on the circumference and a point located 180 degrees rotated relative to the point with the center of the circle as the starting point, and they can be regarded as cutting tips of the same shape, and the above-mentioned standard deviation can be calculated.
[0085] (5) Including columnar crystals, including the content changes of Al and Ti, and the maximum value of x max and the minimum value x min and the area ratio S of the region with this change
[0086] Preferably, in each flank of all cutting tips, the AlTiCN layer includes columnar crystals, including a variation in the content of Al and Ti, wherein the maximum value x of the content (ratio) x of Al in the total amount of Ti and Al in the variation in the content is max and the minimum value x min Satisfy 0.02≤x max -x min ≤0.40. In addition, the columnar crystal refers to a crystal having an aspect ratio A (defined later) of 1.5 or more in the crystal grains of the AlTiCN layer.
[0087] If x max -x min Within this range, the heat crack resistance and chipping resistance of the coated tool will be improved. However, if it is less than 0.02, the improvement is insufficient, and if it is greater than 0.40, the intragranular distortion of the grains constituting the AiTiCN layer is too large, and the heat crack resistance and chipping resistance of the coated tool will be reduced.
[0088] In addition, in each flank of all cutting tips, the area including the content variation of Al and Ti (described in detail later) preferably exists at 50% by area or more, and more preferably exists at 70% by area or more in the longitudinal section of the AlTiCN layer. The reason is that although the aforementioned problem can be solved when the area including the content variation of Al and Ti is 50% by area or more, if it is less than 70% by area, the heat crack resistance and chipping resistance of the coated tool provided during high-speed intermittent cutting may be reduced. The area including the content variation of Al and Ti may be 100% by area in the longitudinal section of the coating layer.
[0089] In each cutting edge, the maximum value x of the content of Al in the total amount of Ti and Al is obtained when the content of Al and Ti varies. max and the minimum value x min The area ratio of the region including the changes in the Al and Ti contents in the coating layer can be calculated, for example, as follows.
[0090] The longitudinal section of the cladding layer was observed at an appropriate magnification of 160,000 to 320,000 times using an energy dispersive X-ray spectrometer attached to a scanning transmission electron microscope (STEM).
[0091] Furthermore, in the longitudinal section of the coating layer, in the entire rectangular observation field whose width in the direction parallel to the surface of the substrate is set to be greater than 2 μm and includes the entire thickness of the coating layer, the content x of Al in the total amount of Ti and Al where the contents of Al and Ti vary is calculated.
[0092] The observation field is preferably near the measurement position (within a circle with a radius of 50 μm from the measurement position) where the average value (Lm) of the thickness of the AlTiCN layer on the flank surface of each cutting edge is obtained.
[0093] For each grain (columnar crystal) of the NaCl face-centered cubic structure and the hexagonal crystal structure in the entire observation field, the distribution of the content x of Al in the total amount of Ti and Al is calculated, and the maximum value x is max * and minimum value x min *All relative to their average value x avg * When a difference of ±1% or more occurs, it is determined that the crystal grain contains changes in the contents of Al and Ti.
[0094] That is, the region including the variation of the content of Al and Ti refers to the region where the grains determined to include the variation of the content of Al and Ti are collected (totaled). max * and minimum value xmin *The average value of each is set to the maximum value x in a certain cutting tip max , minimum value x min .
[0095] Furthermore, it is more preferable that in a region including a variation in the content of Al and Ti, relative to the average value x avg * The region where a difference of +1% or more occurs (region with high Al content) and the region where a difference of -1% or more occurs (region with low Al content) are distributed in a mesh, layer or granular form. Furthermore, it is more preferred that the minimum value of the distance between the outer edges of the regions with high Al content separated by the regions with low Al content or the outer edges of the regions with low Al content separated by the regions with high Al content is 1 nm or more and less than 50 nm.
[0096] The reason is that if the minimum value of the interval of change in the content of Al and Ti is within this range, the heat crack resistance and chipping resistance of the coated tool will be improved, but if it is less than 1nm, the improvement in heat crack resistance is insufficient, and if it is greater than 50nm, the improvement in chipping resistance is sometimes insufficient.
[0097] The ratio of the total area of the grains determined to include the changes in the Al and Ti contents in the observation field is defined as the area ratio of the region including the changes in the Al and Ti contents in the coating layer.
[0098] (6) The average value of the texture coefficient TC(200) avg (200))
[0099] When the texture coefficient TC(200) of the grains having the NaCl type face-centered cubic structure on a line 100 μm away from the ridgeline of the cutting tip in the direction of the back face is obtained for each of the cutting tips, the average value TC avg (200) satisfies 1.0 or more and 6.0 or less.
[0100] The reason is that if TC avg If (200) is less than 1.0, the heat crack resistance of each cutting edge provided during high-speed intermittent cutting may be reduced. avg The larger (200) is, the better the heat crack resistance is, and the maximum value of 6.0 is defined as the maximum value. avg When (200) is 1.0 or more and 3.4 or less, the balance between heat crack resistance and wear resistance is excellent. avg When (200) is greater than 3.5 and less than or equal to 6.0, the heat crack resistance is excellent.
[0101] (7) Deviation of texture coefficient TC(200)
[0102] σ TC(200) / TC avg (200) more preferably satisfies 0.00 or more and 0.10 or less. The reason is that if σ TC(200) / TC avg When (200) is larger than 0.10, the uniformity of heat crack resistance and chipping resistance of each cutting edge provided during high-speed intermittent cutting may be reduced.
[0103] The texture coefficient TC(200) is calculated as follows.
[0104] That is, when a plurality of cutting tips are included in one coated tool, a line segment of 500 μm is selected from the edge line of the cutting tip in each cutting tip, and the center of the line segment moved parallel to the back face direction by 100 μm is set as the measurement position. At this measurement position, an X-ray diffraction pattern is measured by micro-area X-ray diffraction measurement (example of measurement conditions: Cu-Kα ray, output 50 kV, 22 mA, detection distance 150 mm, collimator diameter 100 μmΦ).
[0105] When the 200 diffraction line of the grains having the NaCl type face-centered cubic structure can be visually identified, the texture coefficient TC(200) is calculated, and the average value of each cutting edge is set as TC avg (200), find their respective standard deviations σ TC ( 200 ) .
[0106] Here, the texture coefficient TC(200) is defined as follows. That is,
[0107] TC(200)={I(200) / I0(200)}×[(1 / 6)×Σ{I(hkl) / I0(hkl)}] -1 ,
[0108] Each cutting tip is measured and the average value is TC avg (200).
[0109] In addition, as described below:
[0110] I(200): measured value of the X-ray diffraction peak intensity in the 200 diffraction line;
[0111] I0(200): average value of the standard X-ray diffraction peak intensity in the 200 diffraction line of the AlN crystal plane recorded in JCPDS card 00-046-1200;
[0112] ∑(I(hkl) / I0(hkl): the total value of ([measured value of X-ray diffraction peak intensity] / [average value of standard diffraction peak intensity of AlN listed on the ICDD card]) values of each diffraction line of 111, 200, 220, 311, 222, and 400.
[0113] (8) Average particle width and average aspect ratio of columnar crystals
[0114] More preferably, the AlTiCN layer includes columnar crystals on the flank surfaces of all the cutting edges, the columnar crystals having an average grain width W of 0.1 μm to 2.0 μm in longitudinal section and an average aspect ratio A of 2.0 to 10.0.
[0115] The reasons are as follows: if the average particle width W is less than 0.1 μm, abnormal damage may be easily caused due to the decrease in plastic deformation resistance and oxidation resistance caused by the increase in grain boundaries, while if the average particle width W is greater than 2.0 μm, the toughness may be easily reduced due to the presence of coarsely grown particles.
[0116] In addition, if the average aspect ratio A is less than 2.0, the shear stress generated on the surface of the AlTiCN layer during cutting causes the interface to easily become a starting point for damage, which may sometimes cause chipping. In addition, if the average aspect ratio A is greater than 10.0, tiny chipping occurs on the tip of the blade during cutting. When a notch is generated in the adjacent columnar crystal structure, the resistance to the shear stress generated on the surface of the AlTiCN layer is likely to decrease, the columnar crystal structure breaks, and the damage continues to progress, which may sometimes cause larger chipping.
[0117] Next, a method for calculating the average grain width W and the average aspect ratio A of the crystal grains having the NaCl type face-centered cubic structure of each cutting edge will be described.
[0118] First, a longitudinal section of the AlTiCN layer is ground by the aforementioned method.
[0119] The observation field is near the measurement position (within a circle with a radius of 50 μm from the measurement position) where the average value (Lm) of the thickness of the AlTiCN layer on the back face of each cutting tip mentioned above is calculated, and is preferably set to a rectangle including the entire thickness of the coating layer and having a size including 20 or more grains with a NaCl face-centered cubic structure.
[0120] As described above, the grain boundary is determined to identify the grain. Next, image analysis is performed to measure the maximum length H of the grain ik in a direction perpendicular to the surface of the substrate (the surface of the substrate is treated as a flat surface) at a certain blade edge k. ik, the maximum length of the grain ik in the direction parallel to the matrix, that is, the particle width W ik and the area S of the grain ik ik The aspect ratio of grain ik is A ik Calculated as A ik =H ik / W ik .
[0121] <Average particle width W>
[0122] For each blade tip k, the particle widths (W1 to W2) measured for 20 or more crystals in the observation field are calculated by [Mathematical Formula 3]. j , 1≤i≤jk, jk is the number of grains at each cutting edge. jk≥20) is area-weighted averaged to be the average grain width Wk of a certain cutting edge k. In addition, jk can be the same number in all cutting edges.
[0123] [Mathematical formula 3]
[0124]
[0125] <Average aspect ratio>
[0126] In addition, for each blade edge k, the aspect ratio A is calculated for 20 or more crystals in the observation field according to the above definition. jk (1≤i≤jk, jk≥20), and the average aspect ratio Ak of a certain cutting edge k is obtained by performing area-weighted averaging using [Formula 4].
[0127] [Formula 4]
[0128]
[0129] (9) Chlorine content ratio
[0130] The AlTiCN layer may contain chlorine (Cl), and when containing chlorine (Cl), the average content ratio thereof is preferably greater than 0.005 atomic % and less than 0.500 atomic %. Here, the average chlorine content ratio is defined as follows:
[0131] (The number of atoms of Cl) / (the number of atoms of Cl+the number of atoms of Al+the number of atoms of Ti+the number of atoms of C+the number of atoms of N)×100.
[0132] The reason why the average content ratio when chlorine is contained is set to the above range is that if it is within this range, the lubricity can be reliably improved without reducing the toughness of the AlTiCN layer.
[0133] The average chlorine content in the AlTiCN layer is determined as follows. For example, an electron beam microanalyzer (Electron-Probe-Micro-Analyser: EPMA) is used to irradiate the longitudinal section of the polished surface with electron beams, and the chlorine content is determined based on the analysis results of the obtained characteristic X-rays. The observation field is preferably near the measurement position (within a circle with a radius of 50 μm from the measurement point) where the average value (Lm) of the thickness of the AlTiCN layer on the back face of each cutting tip is determined. In the coating layer on all cutting tips of the same shape existing in a coated tool, multiple locations (for example, three locations) are observed separately to determine the average chlorine content of each cutting tip.
[0134] 2. Other layers
[0135] 2-1. Lower layer
[0136] Although only the AlTiCN layer has sufficient durability, a lower layer may be provided between the AlTiN layers adjacent to the substrate, the lower layer being composed of one or more Ti compound layers among the Ti nitride layer, carbide layer, and carbonitride layer (the composition of these layers is not limited to the stoichiometric composition. Layers of all known compositions may also be used), and having a total average thickness of 0.1 μm or more and 2.0 μm or less. The lower layer improves the adhesion between the AlTiCN layer and the substrate.
[0137] 2-2. Upper layer
[0138] An upper layer may be provided on the upper part of the AlTiCN layer, and the upper layer is composed of a Ti compound layer, an aluminum oxide layer, and one or more Ti nitride layers, a carbide layer, a carbonitride layer, and an oxide layer (the composition of these layers is not limited to the stoichiometric composition. Layers of all known compositions may also be used), and has a total average thickness of 0.1 μm or more and 4.0 μm or less. The upper layer brings durability.
[0139] It is preferred that both the lower layer and the upper layer be formed according to the method for producing the AlTiCN layer described later, so as to eliminate the variation among the cutting edges.
[0140] 2-3. Non-intentional layer
[0141] Furthermore, due to fluctuations in gas pressure and temperature in the film forming apparatus when the film forming gas is switched, unintentional layers other than the AlTiCN layer, the lower layer, and the upper layer may be formed.
[0142] 3. Matrix
[0143] (1) Material
[0144] If the substrate is a substrate known in the past as such a substrate, any substrate may be used as long as it does not hinder the achievement of the aforementioned purpose. Examples thereof include WC-based cemented carbide (in addition to WC, Co, and further alloys formed by adding carbonitrides of Ti, Ta, Nb, etc.), cermets (ceramics with TiC, TiN, TiCN as the main components), ceramics (titanium carbide, silicon carbide, silicon nitride, aluminum nitride, aluminum oxide), and cBN sintered bodies.
[0145] (2) Shape
[0146] The shape of the base body is not particularly limited as long as it is a shape used as a cutting tool, and examples thereof include the shape of an insert and the shape of a drill.
[0147] 4. Manufacturing method
[0148] The AlTiCN layer according to the present embodiment can be produced using, for example, the following film-forming gas and film-forming apparatus.
[0149] (1) Composition of film-forming gas, etc.
[0150] The reaction gas composition and the like are exemplified as follows: The gas composition is a composition obtained by taking the sum of the compositions of the gas group A and the gas group B as 100% by volume, and is hereinafter referred to as %.
[0151] Gas Group A:
[0152] Gas composition: TiCl4: 0.07-0.40%, AlCl3: 0.20-1.29%, N2: 0.0-10.0%, C2H4: 0.0-0.5%, H2: the rest
[0153] Gas Group B:
[0154] Gas composition NH3: 1.00~4.40%, H2: 25.0~35.0%
[0155] Reaction atmosphere pressure: 4.0~5.0kPa
[0156] Reaction atmosphere temperature: 700~850℃
[0157] Supply cycle: 1.00~5.00 seconds
[0158] Gas supply time per cycle: 0.15 to 0.25 seconds
[0159] Phase difference between the supply of gas group A and the supply of gas group B: 0.10 to 0.20 seconds
[0160] The film-forming gas composition, reaction atmosphere pressure, reaction atmosphere temperature, supply cycle, gas supply time per cycle, and the phase difference between the supply of gas group A and the supply of gas group B are set values.
[0161] (2) Film forming device
[0162] As a film forming device, there can be exemplified a device having Figure 3 and Figure 4 The film forming device is a film forming device with a gas ejection tube 7 shown. The film forming device is a film forming device for a coated tool having four cutting edges, and the film forming gas is ejected at the same time toward the back tool surface having four surfaces in such a way that any part of the cutting edge is at the same distance from the front end (gas supply part) of the gas ejection tube of the film forming device.
[0163] In addition, the substrate 6 is placed on a plate-shaped fixture (not shown), and the gas is ejected in four directions in the space between the gas ejection pipes. Furthermore, when forming a film on the cutting tip on the lower side of the substrate, for example, a spacer is provided between the plate-shaped fixture and the substrate to form a gap, and the distance between any part of the cutting edge and the front end of the gas supply pipe of the film forming device can be arranged in the same manner.
[0164] The above description includes the following additional features.
[0165] (Note 1)
[0166] A surface-coated cutting tool comprises a substrate and a coating layer arranged on the substrate, characterized in that:
[0167] (1) The coating layer comprises a composite nitride layer or a composite carbonitride layer of Al and Ti having grains with a NaCl-type face-centered cubic structure,
[0168] (2) The tool has a plurality of cutting tips of the same shape, and in the back surfaces of all the cutting tips, the composite nitride layer or composite carbonitride layer of Al and Ti is (Al x Ti 1-x )(C y N 1-y )(Average content of x avg is 0.60 or more and 0.95 or less, and the average content of y avg is greater than 0.0000 and less than 0.0050),
[0169] (3) In each flank of all the cutting tips, the grains having the NaCl-type face-centered cubic structure included in the coating layer have 200 diffraction lines measured using an X-ray diffraction device, and the average value of the intensity value of the 200 diffraction lines is set to I(200), and the standard deviation thereof is set to σ I(200) WhenI(200) / I(200) satisfies 0.00 or more and 0.20 or less,
[0170] (4) In each of the above-mentioned cutting edges, the thickness of the coating layer on a line 100 μm away from the cutting edge ridgeline in the flank direction is defined as Lm, and the average value of the Lm of all the cutting edges is defined as Lm. avg , the standard deviation is set to σ L When L / L avg Satisfy 0.00 or more and 0.20 or less,
[0171] (5) In each flank surface of all the cutting tips, the composite nitride layer or composite carbonitride layer of Al and Ti includes columnar crystals having a maximum value x of x in the columnar crystals. max *The average value of x max and the minimum value x of x min *The average value of x min Satisfy 0.02≤x max -x min The area ≤0.40.
[0172] (Note 2)
[0173] The surface-coated cutting tool according to Supplement 1 is characterized in that, in each flank of all the cutting tips, the average value TC of the texture coefficient TC(200) of the grains having the NaCl-type face-centered cubic structure in the coating layer is avg (200) satisfies 1.0 or more and 6.0 or less.
[0174] (Note 3)
[0175] The surface-coated cutting tool according to Supplement 1 or Supplement 2 is characterized in that, in each flank of all the cutting tips, the average value of the texture coefficient TC(200) of the grains having the NaCl face-centered cubic structure included in the coating layer is set to TC avg (200), and its standard deviation is set to σ TC(200) When TC(200) / TC avg (200) satisfies 0.00 or more and 0.10 or less.
[0176] (Note 4)
[0177] A surface-coated cutting tool according to any one of Supplementary Notes 1 to 3, characterized in that, in each flank of all the cutting tips, a region having a variation in the content of Al and Ti included in the coating layer accounts for 70% by area or more in the longitudinal section of the coating layer.
[0178] (Note 5)
[0179] A surface-coated cutting tool according to any one of Notes 1 to 4, characterized in that, in each back face of all the cutting tips, the average particle width W of the columnar crystals including the composite nitride layer or composite carbonitride layer of Al and Ti in the coating layer is greater than 0.10 μm and less than 1.20 μm, and its average aspect ratio A is greater than 2.0 and less than 10.0.
[0180] (Note 6)
[0181] The surface-coated cutting tool according to any one of Supplementary Notes 1 to 5, wherein the composite nitride layer or composite carbonitride layer of Al and Ti contains chlorine, and the content ratio thereof is 0.005 atomic % or more and 0.500 atomic % or less.
[0182] (Note 7)
[0183] The surface-coated cutting tool according to any one of Supplementary Notes 1 to 6, wherein the region having the varying contents of Al and Ti is distributed in a mesh, layer or granular form.
[0184] (Note 8)
[0185] The surface-coated cutting tool according to any one of Supplementary Notes 1 to 7, characterized in that a lower layer is provided between the composite nitride layer or composite carbonitride layer of Al and Ti and the substrate.
[0186] (Note 9)
[0187] The surface-coated cutting tool according to any one of Supplementary Notes 1 to 8, characterized in that an upper layer is provided on the upper portion of the composite nitride layer or composite carbonitride layer of Al and Ti.
[0188] Example
[0189] Next, examples are described.
[0190] Here, as an embodiment of the coated tool of the present invention, a coated tool suitable for a blade cutting tool using WC-based cemented carbide as the material of the substrate is described, but the material of the substrate is also applicable even if the other materials described above are used, and the shape of the substrate is also applicable to drills and end mills.
[0191] As raw material powders, WC powder, TiC powder, ZrC powder, TaC powder, NbC powder, Cr3C2 powder, TiN powder and Co powder were prepared, and these raw material powders were blended according to the blending composition shown in Table 1.
[0192] Wax was further added and mixed in acetone using a ball mill for 24 hours. After reduced pressure drying, the pressed green body was pressed at a pressure of 98 MPa into a specified shape. The green body was vacuum sintered in a vacuum of 5 Pa and at a temperature of 1420°C for 1 hour to produce WC-based cemented carbide substrates A to C having a blade shape (four cutting tips) of SEMT13T3AGSN manufactured by Mitsubishi Materials Corporation after sintering, and WC-based cemented carbide substrates D to F having a blade shape (four cutting tips) of ISO specification CNMG120412.
[0193] Next, on the surfaces of these substrates A to F, Figure 3 and Figure 4 In the film forming apparatus with the configuration of the gas ejection pipe shown in , AlTiCN layers were formed by CVD method according to the film forming conditions shown in Table 2, and Examples 1 to 27 shown in Tables 7 and 8 were obtained. In addition, regarding the average thickness Lm of the coating layer on a line 100 μm away from the cutting edge line portion in the back face direction, four points separated by 30 μm were selected as the aforementioned multiple points separated by a predetermined length to measure the thickness of the coating layer, and the average value Lm was calculated. Lm was calculated for all cutting edges, and the average value Lm was calculated by taking the average value. avg .
[0194] In addition, Examples 1 to 27 have a lower layer or a lower layer and an upper layer as shown in Table 4, and these layers are formed under the film forming conditions shown in Table 3.
[0195] For comparison, a film forming apparatus ( Figure 5 , Figure 6 ), an AlTiCN layer was formed by CVD using formation symbols a~j representing the film forming conditions shown in Table 5, and Comparative Examples 1~15 shown in Tables 7 and 8 were obtained.
[0196] Here, Comparative Examples 1 to 15 have a lower layer or a lower layer and an upper layer as shown in Table 6, and these layers were formed under the film forming conditions shown in Table 3.
[0197] As Figure 5 In the film forming apparatus shown, the diameter of the Bell-type reaction vessel 11 is 250 mm and the height is 750 mm. As the external heating heater 12, a heater capable of heating the inside of the reaction vessel 11 from 700°C to 1050°C is used. As the tray, a ring-shaped fixture 13 with an outer diameter of 220 mm and a center hole with a diameter of 65 mm formed in the center is used. The substrates are placed on the outer peripheral side of the fixture, and the substrates A to F are placed at intervals of 20 mm along the radial direction of the fixture 13 and at approximately equal intervals along the circumferential direction of the fixture 13.
[0198] Gas supply pipe 14 uses Figure 6 The structure shown in the figure is formed by Figure 5 , Figure 6 The gas supply pipe 14 is rotated around the rotating shaft 16 shown in FIG. 5. In addition, as shown in Table 5, the gas ejection ports provided in the gas supply pipe 14 and adjacent to each other in the circumferential direction are as follows: Figure 6 As shown, the gas group A outlet and the gas group B outlet each have one hole (the outlet 18) or two holes (the outlet 19 and the outlet 20). When the outlet of the outlet group belonging to the same gas group flow section has two holes (the outlet 19 and the outlet 20), as shown in FIG. Figure 6 As shown, their relative positions are determined by their angle α.
[0199] In addition, the gas group A nozzle and the gas group B nozzle which are adjacent to each other in the circumferential direction are arranged relative to each other. Figure 5 A group of spaces 15 between the trays on which the substrates are placed is provided, and the flow rates of the gases of the gas group A and the gas group B ejected from each tray are supplied at the flow rates of the gases described in Table 5.
[0200] Generally, the chemical vapor deposition device used in the manufacture of surface-coated cutting tools is as described above. Figure 5 , Figure 6 In order to make the device as in this embodiment, the gas supply pipe is arranged in the center of the reaction container. Figure 3 , Figure 4 The device structure illustrated in the example requires significant design changes to the branch of the gas supply pipe and the fixture for mounting the substrate. Figure 3 , Figure 4 Although the film formation mode on one substrate is exemplified in FIG, by mounting a jig of this structure in the height direction, it is possible to form a coating layer on a plurality of tools.
[0201] Tables 7, 8, 9 and 10 show the composition of Examples 1 to 27 and Comparative Examples 1 to 15, the area ratio of the NaCl face-centered cubic structure, the average thickness of the back tool face, the changes in the Al and Ti contents, the texture coefficient of the back tool face, the average grain size, and the aspect ratio.
[0202] The measured value k of each cutting tip is distinguished by numbers 1 to 4.
[0203] [Table 1]
[0204]
[0205] [Table 2]
[0206]
[0207] [Table 3]
[0208]
[0209] [Table 4]
[0210]
[0211] In Table 4, "-" indicates that the corresponding layer does not exist.
[0212]
[0213] In Table 5, "Spout Angle" means Figure 6 The “-” in α means that no angle is formed because there is only one ejection port.
[0214] [Table 6]
[0215]
[0216] In Table 6, "-" indicates that the corresponding layer does not exist.
[0217]
[0218] In Table 7, in the column "Are there 70 area % or more of NaCl-type face-centered cubic grains in all cutting tips?", "○" indicates compliance, and "×" indicates that in one or more cutting tips, the number of NaCl-type face-centered cubic grains is 50 area % or more and less than 70 area %.
[0219] In other columns, "○" indicates compliance with the items described in the columns, and "×" indicates noncompliance with the items described in the columns.
[0220] [Table 8]
[0221]
[0222] In Table 8, regarding "whether all cutting edges are 70 area % or more", "○" indicates compliance, "×" indicates that one or more cutting edges are 50 area % or more and less than 70 area %, and "-" indicates that measurement is impossible.
[0223] In the column "Does it exist in all cutting edges?", "○" indicates compliance, "×" indicates noncompliance, and "-" indicates that it cannot be measured.
[0224] [Table 9]
[0225]
[0226] In Table 9, "the presence of mesh, layer, and granular" means "the presence of mesh, layer, and granular in a region including the variation of Al and Ti contents, relative to the average value x avg *The regions producing a difference of +1% or more (regions with high Al content) and the regions producing a difference of -1% or more (regions with low Al content) are distributed in a mesh, layer or granular form, "○" indicates distribution, "-" indicates no distribution, and "the minimum value of the interval between the outer edges of each region" means "the minimum value of the interval between the outer edges of the high Al content region separated by the low Al content region or the minimum value of the interval between the outer edges of the low Al content region separated by the high Al content region".
[0227] In the column "Are the values 0.02 or more and 0.40 or less in all cutting edges?", "○" indicates compliance, "×" indicates noncompliance, and "-" in other columns indicates that measurement was not possible.
[0228] [Table 10]
[0229]
[0230] In Table 10, TC under the TC(200) column i (where i = 1 to 4) is TC i (200), σ TC is TC(200) .
[0231] In addition, "○" indicates compliance, "×" indicates non-compliance, and "-" indicates that measurement was not possible.
[0232] Next, for the aforementioned embodiments 1 to 9 and comparative examples 1 to 5, the aforementioned various substrates A to C (SEMT13T3AGSN shape) were all clamped with only one single-edged cutting tool at the front end of an alloy steel tool with a tool diameter of 80 mm using a fixed fixture, and cutting test 1 as dry high-speed end milling cutter cutting and center tool cutting of carbon steel as shown below was implemented.
[0233] For all four cutting edges of each tool base, the flank wear width of the cutting edge was measured every 1 minute of cutting, and the cutting time when the flank wear width became 0.2 mm or more, which is the life judgment standard, was measured as the time to reach the life. And the average value and standard deviation were calculated. The results of cutting test 1 are shown in Table 11.
[0234] Cutting test 1: Dry high-speed face milling and center tool cutting
[0235] Tool diameter: 80mm, single-edge cutting
[0236] Workpiece: JIS S45C block with a width of 60 mm and a length of 200 mm
[0237] Rotation speed: 1393 / min
[0238] Cutting speed: 350m / min
[0239] Cutting depth: 2.0mm
[0240] Feed per blade: 0.2mm / blade
[0241] (Usually the cutting speed is 200m / min)
[0242] [Table 11]
[0243]
[0244] In Table 11, the cutting time to reach the life (minutes) indicates the time (minutes) to reach the life due to chipping before the flank wear width reaches the above-mentioned width.
[0245] In addition, for the aforementioned embodiments 10 to 18 and comparative examples 6 to 10, the aforementioned various coated substrates D to F (ISO specification CNMG120412 shape) were all threadedly fastened to the front end of the alloy steel turning tool with a fixing clamp, and the cutting test 2 shown below for dry high-speed intermittent cutting of ductile iron was carried out.
[0246] The flank wear width of the cutting edge was measured for each 0.5-minute cutting at the acute corners of the upper and lower surfaces of each tool base and at all four cutting tips, and the cutting time at which the flank wear width became 0.3 mm or more, which is a life judgment standard, was measured as the time to reach the life. The average value and standard deviation were calculated. The results of cutting test 2 are shown in Table 12.
[0247] Cutting test 2: Dry high-speed interrupted cutting
[0248] Workpiece: JIS FCD700 round bar with four longitudinal grooves at equal intervals in the length direction
[0249] Cutting speed: 400m / min
[0250] Cutting depth: 1.0mm
[0251] Feed rate: 0.2mm / rev
[0252] (Usually the cutting speed is 150-200m / min)
[0253] [Table 12]
[0254]
[0255] In Table 12, the cutting time to reach the life (minutes) indicates the time (minutes) to reach the life due to chipping before the flank wear width reaches the above-mentioned width.
[0256] In addition, regarding the aforementioned embodiments 19 to 27 and comparative examples 11 to 15, the aforementioned various substrates A to C (SEMT13T3AGSN shape) were all clamped with only one single-edged cutting tool at the front end of an alloy steel tool with a tool diameter of 80 mm using a fixed fixture, and the cutting test 3 shown below, which included dry high-speed end milling cutter cutting and center tool cutting of alloy steel, was implemented.
[0257] For all four tool tips of each tool base, the flank wear width of the cutting edge was measured every 0.5 minutes of cutting, and the cutting time when the flank wear width became 0.2 mm or more, which is the life judgment standard, was measured as the time to reach the life. And the average value and standard deviation were calculated. The results of cutting test 3 are shown in Table 13.
[0258] Cutting test 3: Dry high-speed face milling and center tool cutting
[0259] Tool diameter: 80mm, single-edge cutting
[0260] Workpiece: JIS SCM440 block material with a width of 60 mm and a length of 200 mm
[0261] Rotation speed: 1592 / min
[0262] Cutting speed: 400m / min
[0263] Cutting depth: 2.0mm
[0264] Feed per blade: 0.2mm / blade
[0265] (Usually the cutting speed is 200m / min)
[0266] [Table 13]
[0267]
[0268] In Table 13, the cutting time to reach the life (minutes) indicates the time (minutes) to reach the life due to chipping before the flank wear width reaches the above-mentioned width.
[0269] According to the results shown in Tables 11, 12 and 13, since the AlTiCN layer in each cutting tip of Examples 1 to 27 has uniform thickness and structure, each cutting tip has excellent resistance to heat cracking and chipping. Therefore, even when used for high-speed intermittent cutting of carbon steel, cast iron and alloy steel, no heat cracking or chipping will occur in any cutting tip, and excellent wear resistance will be exhibited for a long time.
[0270] In contrast, according to the results shown in Tables 11, 12 and 13, since the thickness and structure of the AlTiCN layer between the cutting tips in Comparative Examples 1 to 15 are uneven and the heat cracking resistance and chipping resistance are also uneven, when used for high-speed intermittent cutting of carbon steel, cast iron and alloy steel, the four cutting tips of each tool have shortened service life, the average value of the time to reach the service life is shortened, and the deviation of the time to reach the service life (standard deviation / average value) is increased.
[0271] Therefore, it can be said that any of the examples has a longer average service life than any of the comparative examples, and the variation is smaller, and exhibits uniform and excellent cutting performance.
[0272] The embodiments disclosed above are merely illustrative in all aspects and are not restrictive. The scope of the present invention is expressed by the claims rather than the embodiments described above, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0273] Description of Reference Numerals
[0274] 1 Rake face
[0275] 2 Flank
[0276] 3. The main cutting edge of the cutting edge
[0277] 4. The cutting edge of the secondary cutting edge
[0278] 5 Cutting corners
[0279] 6 Matrix
[0280] 7 Gas outlet pipe
[0281] 8 Gas Group A
[0282] 9 Gas Group B
[0283] 11. Reaction vessel
[0284] 12 External Heater
[0285] 13. Fixture
[0286] 14 Gas supply pipe
[0287] 15 Space between pallets
[0288] 16 Rotation axis
[0289] 17 Gas Group A and Gas Group B
[0290] 18~20 ejection holes
Claims
1. A surface-coated cutting tool comprising a substrate and a coating layer disposed on the substrate, characterized in that: (a) the coating layer comprises a composite nitride layer or a composite carbonitride layer of Al and Ti having grains with a NaCl-type face-centered cubic structure, (b) The tool has a plurality of cutting tips of the same shape, and in the back surfaces of all the cutting tips, the composite nitride layer or composite carbonitride layer of Al and Ti is (Al x Ti 1-x )(C y N 1-y ), where the average content of x is avg is 0.60 or more and 0.95 or less, and the average content of y avg is greater than or equal to 0.0000 and less than or equal to 0.0050, (c) In each flank of all the cutting tips, the grains having the NaCl-type face-centered cubic structure included in the coating layer have 200 diffraction lines measured using an X-ray diffraction device, and the average value of the intensity value of the 200 diffraction lines is set to I(200), and the standard deviation thereof is set to σ I(200) When I(200) / I(200) satisfies 0.00 or more and 0.20 or less, (d) In each of the above-mentioned cutting edges, the thickness of the coating layer on a line 100 μm away from the cutting edge ridgeline in the flank direction is defined as Lm, and the average value of the Lm in all the cutting edges is defined as Lm. avg , the standard deviation is set to σ L When L / L avg Satisfy 0.00 or more and 0.20 or less, (e) In each flank surface of all the cutting tips, the composite nitride layer or composite carbonitride layer of Al and Ti includes columnar crystals, and the maximum value x of x in the columnar crystals is max *The average value of x max and the minimum value x of x min *The average value of x min Satisfy 0.02≤x max -x min The area ≤0.
40.
2. The surface-coated cutting tool according to claim 1, characterized in that: The average value TC of the texture coefficient TC(200) of the grains having the NaCl type face-centered cubic structure included in the coating layer in each flank surface of all the cutting tips is avg (200) satisfies 1.0 or more and 6.0 or less.
3. The surface-coated cutting tool according to claim 1 or 2, characterized in that: In each flank of all the cutting tips, the average value of the texture coefficient TC(200) of the grains having the NaCl type face-centered cubic structure included in the coating layer is set to TC avg (200), and its standard deviation is set to σ TC(200) When TC(200) / TC avg (200) satisfies 0.00 or more and 0.10 or less.
4. The surface-coated cutting tool according to claim 1, characterized in that: In each flank surface of all the cutting tips, a region having a variation in the content of Al and Ti included in the cladding layer accounts for 70% by area or more in a longitudinal section of the cladding layer.
5. The surface-coated cutting tool according to claim 1, characterized in that: In each flank of all the cutting tips, the average grain width W of the columnar crystals of the composite nitride layer or composite carbonitride layer of Al and Ti included in the coating layer is greater than 0.10 μm and less than 1.20 μm, and the average aspect ratio A is greater than 2.0 and less than 10.
0.
6. The surface-coated cutting tool according to claim 1, characterized in that: The composite nitride layer or composite carbonitride layer of Al and Ti contains chlorine, and the content ratio thereof is 0.005 atomic % or more and 0.500 atomic % or less.
Citation Information
Patent Citations
Chemical vapor deposition apparatus and chemical vapor deposition method
JP2017020111A