Composition of plant-based wax

The shortage of petroleum wax alternatives is addressed by the use of plant-based wax and fibrillated cellulose compositions in paper and wood products, improving product performance and sustainability.

CN118922501APending Publication Date: 2024-11-08FINLAND CENTRAL LABORATORY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202380029212.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

There is a lack of alternatives to petroleum-derived waxes in the prior art, especially in the case of limited oil supply, and it is difficult to find alternatives to petroleum waxes for use in paper and wood products to improve their performance.

Method used

A composition containing plant-based waxes and fibrillated cellulose has been developed, which improves the performance of paper and wood products by forming a dispersion of wax particles in an aqueous medium for the replacement of traditional petroleum and synthetic waxes. .

Benefits of technology

The composition can improve barrier properties, moisture resistance, hydrophobicity and oleophobicity of paper and wood products, provide higher melting point and thermal stability, and has environmentally friendly and sustainable advantages due to the use of renewable materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922501A_ABST
    Figure CN118922501A_ABST
Patent Text Reader

Abstract

A composition, a method for making the composition, and a product comprising the composition are disclosed. The composition of the present invention is a dispersion comprising a plant-based wax and a fibrillated cellulose component. In addition, a solid wet product and uses of the composition are disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates generally to wax compositions. The present disclosure relates particularly, but not exclusively, to plant-based wax compositions containing fibrillated cellulose. Background Art

[0002] This section provides useful background information, but no admission is made that any of the techniques described herein represent prior art.

[0003] The prior art describes the use of petroleum-derived waxes and synthetic waxes for incorporation into emulsions and dispersions. Given that the worldwide supply of petroleum is limited and is being depleted, there is a recognized and long-standing need to find alternatives to petroleum-derived products (such as petroleum waxes) that are derived from limited natural resources that are in diminishing supply. It would be desirable to have waxes that could be obtained from renewable sources such as plants, rather than petroleum-based waxes.

[0004] Petroleum waxes such as paraffin wax and microcrystalline wax are widely used by themselves and in combination with asphalt emulsions, montan wax, polyvinyl alcohol copolymers, and other hydrophobic materials to improve product properties. Other waxes, such as synthetic waxes such as FischerTropsch, and polyethylene waxes have also been used for this purpose with mixed results.

[0005] Dispersions prepared using waxes are used in a variety of applications such as sizing and coating fibrous cellulosic products such as paper, corrugated containerboard, linerboard, kraft paper, boxboard, etc. to impart properties thereto.

[0006] The common first step in the process of preparing a wax emulsion or dispersion is to dissolve the wax and add enough base to saponify the desired number of functional groups on the wax. A surfactant is then added and the emulsion is allowed to form with good agitation.

[0007] Prior art has shown that microfibrillated cellulose has a unique ability to improve the stability of a variety of compositions.Microfibrillated cellulose has been used in compositions of the type used in, for example, foods, cosmetics, pharmaceuticals, and industrial products such as paints and drilling muds.

[0008] In nature, native cellulose is always in the form of microfibrils and is part of the plant cell wall structure. In the primary cell wall, especially in the parenchyma cells, cellulose microfibrils are randomly distributed and form a flexible membrane layer together with other polysaccharides such as pectin and hemicellulose. In the secondary cell wall, the microfibrils are usually highly aligned in the same direction and tightly bound to each other by hydrogen bonds and covalent lignin bridges, forming a very rigid structure.

[0009] Cellulose microfibrils located in primary or secondary cell walls are similar in structure. Two types of microfibrils are composed of highly aligned cellulose macromolecular chains, which form mechanically strong cellulose crystals with hydrogen-bonded parallel polymer chains. Microfibrils are generally considered to contain only few defects along their axes, although for the microfibrils obtained from secondary cell walls, the crystallinity variation between plant species is generally higher. It is generally understood that, depending on the plant species, 18, 24 or 36 cellulose chains form the smallest aligned structure, which is referred to as the cellulose elementary fibrils with several nanometer diameters and up to tens of micrometers of length.

[0010] An object of the present disclosure is to provide a composition that at least alleviates current problems encountered in conventional solutions. Summary of the invention

[0011] The attached claims define the scope of protection. Any examples or technical descriptions of devices, products and / or methods not covered by the claims in the specification and / or drawings are not provided as embodiments of the present invention, but are provided as background technology or examples useful for understanding the present invention.

[0012] The present inventors have unexpectedly discovered that plant-based waxes can be effectively used as replacements for conventional petroleum and synthetic waxes in a variety of applications.The present invention is directed to compositions comprising a plant-based wax and a fibrillated cellulose component which can be incorporated into a variety of paper, paperboard or wood products by conventional means.

[0013] According to a first exemplary aspect, there is provided a composition comprising:

[0014] plant-based waxes;

[0015] a fibrillated cellulose component; and

[0016] The composition is a dispersion of wax particles in an aqueous medium.

[0017] In one embodiment, the fibrillated cellulose component comprises fibrillated cellulose containing entangled cellulose microfibril aggregates comprising microfibrils and / or microfibril bundles smaller than 200 μm. Preferably, the fibrillated cellulose component is added as a suspension in an aqueous medium (eg water) during manufacture of the composition.

[0018] In one embodiment, the fibrillated cellulose comprises cellulose nanofibrils comprising nanofibrils and / or nanofibril bundles less than 200 μm, prepared by the method disclosed in the disclosed examples of WO 2022 / 003252A1, in particular Examples 1 and 3, or by the method provided in the disclosed examples of WO 2017 / 103329 A1, in particular Examples B and C.

[0019] In one embodiment, the fibrillated cellulose comprises cellulose nanofibrils having anionic or cationic groups attached to the surface, prepared by the method disclosed in WO2018 / 202955 (see specifically Examples 4-6 for anionization, and Examples 2-3 for cationization).

[0020] In one embodiment, the fibrillated cellulose comprises cellulose nanofibrils having phosphate, sulfate or hydroxypropyltrimethylammonium halide ether groups, the groups preferably being covalently attached to the cellulose.

[0021] In one embodiment, the fibrillated cellulose component is fibrillated parenchymal cellulose.

[0022] In the context of the present invention, the composition during its production is an emulsion, whereas the final product is a dispersion. In one embodiment, the dispersion is a colloidal dispersion.

[0023] In one embodiment, the plant-based wax comprises saponified triglycerides and / or partially saponified triglycerides. In one embodiment, the plant-based wax comprises triglycerides and / or partially saponified triglycerides, and the plant-based wax is preferably selected from the group consisting of palm wax, palm kernel wax, rapeseed wax, soy wax (soywax), corn wax, canola wax (canola wax), carnauba wax, candelilla wax, small crown coconut wax (ourieurywax), soy wax (soybean wax), coconut wax, cranberry wax (cranbe wax), sunflower wax, linseed wax, cottonseed wax, sugarcane wax, bayberry wax, peanut wax or a combination thereof.

[0024] In one embodiment, the plant-based wax comprises fully saponified triglycerides or fatty acids.

[0025] In one embodiment, the plant-based wax comprises partially hydrogenated tall oil acid, fully hydrogenated tall oil acid, crude tall oil, distilled tall oil, or any mixture thereof. The advantage of using such tall oil derived products is that it enables the saponification step to be omitted, and blends of such tall oil derived products with vegetable oils can be used as plant-based waxes. Furthermore, using these plant-based waxes, even completely wood-based paper products can be manufactured with good barrier properties.

[0026] In one embodiment, the plant-based wax comprises partially hydrogenated tall oil acid having an iodine value in the range of 45-65 g (I2) / 100 g, preferably 50-60 g (I2) / 100 g, more preferably about 54 g (I2) / 100 g, and most preferably about 54 g (I2) / 100 g.

[0027] In one embodiment, the vegetable based wax comprises partially hydrogenated tall oil acid having a melting point in the range of 50°C to 60°C, preferably 53°C to 55°C.

[0028] In one embodiment, the vegetable based wax is hydrogenated or partially hydrogenated.

[0029] In one embodiment, the fibrillated cellulose may contain other polysaccharides, such as pectin, hemicellulose and / or other soluble polysaccharides present in the cellulose raw material from which the fibrillated cellulose component is made. In one embodiment, no additional polysaccharides are added to the fibrillated cellulose component and / or composition.

[0030] Unless otherwise indicated, all percentage values ​​refer to weight percent (wt %) of dry product.

[0031] In one embodiment, the fibrillated cellulose component comprises cellulose in an amount of less than 70 wt%, preferably less than 65 wt%, of the dry matter of the fibrillated cellulose component, and hemicellulose in an amount of greater than 30 wt%, preferably greater than 35 wt%, of the dry matter of the fibrillated cellulose component. In one embodiment, the fibrillated cellulose component may additionally comprise starch.

[0032] In one embodiment the fibrillated cellulose component comprises cellulose in an amount less than 60 wt%, preferably less than 55 wt% of the dry matter of the fibrillated cellulose component, and hemicellulose in an amount greater than 40 wt%, preferably greater than 45 wt% of the dry matter of the fibrillated cellulose component.

[0033] In one embodiment the fibrillated cellulose component comprises cellulose in an amount less than 50 wt%, preferably less than 45 wt% of the dry matter of the fibrillated cellulose component and hemicellulose in an amount greater than 50 wt%, preferably greater than 55 wt% of the dry matter of the fibrillated cellulose component.

[0034] In one embodiment, the fibrillated cellulose component comprises cellulose in an amount preferably less than 25 wt% of the dry matter of the fibrillated cellulose component, and hemicellulose in an amount preferably greater than 50 wt% of the dry matter of the fibrillated cellulose component.

[0035] In one embodiment, the fibrillated cellulose component comprises cellulose in an amount preferably greater than 50 wt% of the dry matter of the fibrillated cellulose component, and hemicellulose in an amount preferably less than 50 wt% of the dry matter of the fibrillated cellulose component.

[0036] In one embodiment, in the fibrillated cellulose component, the amount of the fibrillated cellulose component is selected from the range of 50-70 wt% of the dry matter of the fibrillated cellulose component.

[0037] In one embodiment, the amount of hemicellulose in the fibrillated cellulose component is selected from the range of 30-50 wt% of the dry matter of the fibrillated cellulose component.

[0038] In one embodiment, in the fibrillated cellulose component, the amount of the fibrillated cellulose component is selected from the range of 50 wt% to 70 wt% of the dry matter of the fibrillated cellulose component, and the amount of hemicellulose is selected from the range of 30 wt% to 50 wt% of the dry matter of the fibrillated cellulose component.

[0039] In one embodiment, the composition comprises an additional anionic, cationic, zwitterionic, or amphiphilic surfactant or polymer, or a hydrophilic polymer of synthetic or natural origin.

[0040] In one embodiment, the composition comprises at least one complexing agent, such as ethylenediaminetetraacetic acid (EDTA) or at least one citrate.

[0041] In one embodiment, the composition further comprises a multivalent cation, preferably Zn 2+ Mg 2+ , Cu 2+ , Fe 2+ , Fe 3+ 、Al 3+ Sn 2+ , and Ca 2+ , a fatty acid salt of a polyvalent cation, or any combination thereof. By including a polyvalent cation or a fatty acid salt thereof, hydrophobicity and oleophobicity and / or antimicrobial or microbicidal properties can be increased. The polyvalent cation (e.g., Ca 2+) can be added under high shear mixing. 2+ ) is added to the composition. Preferably, the aqueous solution of multivalent cations is added to the composition under high shear mixing.

[0042] In one embodiment, the composition further comprises at least one thermoplastic polymer. Preferably, the thermoplastic polymer is selected to improve at least one of elasticity, thermoplasticity and heat sealability. Examples of suitable thermoplastic polymers include polyolefin dispersions, polyesters, polyamides, polycaprolactones, polylactic acid, ethylene copolymers, ethylene terpolymers, polyvinyl acetate latex, ethyl vinyl acetate latex, styrene butadiene latex, styrene acrylate latex, acrylate latex, methyl methacrylate latex, or any mixture thereof, or a copolymer or derivative thereof.

[0043] In one embodiment, the composition further comprises a synthetic wax, such as a polyolefin wax, a fatty amide wax, an amide wax, an inorganic modified wax, an oxidized polyethylene wax, or a combination thereof.

[0044] In one embodiment, the wax dispersion is prepared directly after hydrogenation of the oil.

[0045] In one embodiment, the wax composition comprises unhydrogenated vegetable triglycerides and / or unhydrogenated fatty acids, or combinations thereof.

[0046] In one embodiment, the composition further comprises at least one natural, synthetic or semi-synthetic polymer, such as carboxymethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, hydroxyethyl hydroxypropyl cellulose, quaternized hydroxyethyl cellulose, carboxymethyl starch, hydroxypropyl starch, hydroxypropyl methyl starch, hydroxyethyl starch, hydroxyethyl methyl starch, hydroxyethyl hydroxypropyl starch, hydroxypropyltrimethylammonium chloride starch, dextrin, starch, xanthan gum, guar gum, agar, alginate, tyloose, polyvinyl alcohol, polyacrylamide, vinyl acetate copolymer, or any combination thereof.

[0047] In one embodiment, the composition further comprises at least one nonionic surfactant, such as cetyl alcohol, stearyl alcohol, cetearyl alcohol, alcohol ethoxylates, polyethylene glycol ethers, polyoxyethylene alkyl ethers, secondary alcohol ethoxylates, polyoxyethylene alkyl ethers, polyalkyl glycol alkyl ethers, pentaerythritol esters, sugar esters of pentaerythritol, fatty acids, citric acid, fatty acid citrates, fatty alcohols, or any combination thereof.

[0048] In one embodiment, the composition further comprises at least one ionic surfactant comprising phosphates, sulfate sulfonates, sulfate carboxylates, such as sodium lauryl sulfate, ammonium lauryl sulfate, lauryl ether sulfate, lecithin, alkali metal salts of tall oil, or any combination thereof.

[0049] In one embodiment, the plant-based wax is substantially solid at room temperature.In a further embodiment, the melting point of the composition is above 30°C, preferably above 50°C, more preferably between 50°C and 90°C.

[0050] In one embodiment, the composition comprises a wax particle size of less than 20 μm, preferably between 0.1 μm and 10 μm, most preferably between 0.5 μm and 8 μm.

[0051] In one embodiment, the particle size of the wax particles in the composition is adjusted by the type and power of mixing. In one embodiment, the composition is subjected to high shear mixing.

[0052] In one embodiment, the dispersion of wax particles has a Brookfield viscosity of 10 cP to 6000 cP, measured at 50 rpm, spindle V-73, for a 20 wt% solution of dry matter of the composition in water.

[0053] In one embodiment, the composition is prepared as a solid wet product. This can be achieved by dehydration.

[0054] When applied to a product, the composition of the first aspect can improve one or more properties of the product, and when mixed with them, it can improve the processing properties of the composition. These properties include (non-exclusively) barrier properties, moisture resistance, water resistance, hydrophobicity, oleophobicity, durability, printing properties, inhibition of water absorption, and improved processing properties, such as higher melting point, lower viscosity, and thermal stability.

[0055] According to a second aspect, there is provided a solid wet product obtained by subjecting the composition of the first aspect to a powder preparation process.

[0056] In one embodiment, a solid wet product is obtained by cooling and optionally drying the composition. In one embodiment, the solid wet product has a water content of 30-80 wt% of the total weight of the solid wet product. In one embodiment, the solid wet product is a solidified dispersion. In one embodiment, the powder preparation method is granulation, grinding, granulation, cubicization, or any suitable technology to reduce the particle size. In one embodiment, the optional drying is selected from the group consisting of the following: freeze drying, freeze drying, vacuum drying, air drying, spray drying, atomization, evaporation, tray drying, flash drying, drum drying, fluidized bed drying, oven drying, conveyor belt drying, microwave drying, solar drying, or any combination thereof.

[0057] According to a third aspect, there is provided a method for preparing the composition of the first aspect, the method comprising:

[0058] Provides plant-based waxes;

[0059] providing a fibrillated cellulose component;

[0060] heating a plant-based wax and a fibrillated cellulose component;

[0061] adding a fibrillated cellulose component to a plant-based wax while continuously mixing;

[0062] The fibrillated cellulose component is mixed with a plant-based wax until a phase inversion occurs to obtain a dispersion composition of wax particles in an aqueous medium.

[0063] In one embodiment, the plant-based wax and fibrillated cellulose components are heated separately prior to mixing.

[0064] In one embodiment, when the plant-based wax is a blend of triglycerides with at least one of an acid, partially hydrogenated tall oil acid, fully hydrogenated tall oil acid, crude tall oil, and distilled tall oil, the step of providing the plant-based wax comprises heating and mixing to obtain a blend. One skilled in the art can use Example 12 as an indication to prepare any blend from the plant-based wax components described herein.

[0065] According to an alternative third aspect, there is provided a method for preparing the composition of the first aspect, the method comprising:

[0066] providing plant-based wax dispersions;

[0067] providing a fibrillated cellulose component; and

[0068] The fibrillated cellulose component is added to the dispersion with continued mixing to obtain a dispersion of wax particles in an aqueous medium.

[0069] In one embodiment, when the step of providing a plant-based wax dispersion is performed, the plant-based wax is heated under mixing, mixed with a solution of a polymer and / or a surfactant (which is preferably polyvinyl alcohol), then cooled, and subsequently high shear mixed. When this dispersion is mixed with a fibrillated cellulose component in the next step, a composition having good water barrier and oil barrier properties when used as a coating is obtained. In this method, an aqueous medium for the composition of the invention is provided by a solution of an added polymer, surfactant or fibrillated cellulose component. In one embodiment, the solution of the polymer and / or surfactant is in an aqueous phase or aqueous medium.

[0070] In one embodiment, an additional fibrillated cellulose component is added to the dispersion of wax particles in an aqueous medium.

[0071] In one embodiment, the fibrillated cellulose component is added to the plant-based wax in a continuous manner. In one embodiment, the fibrillated cellulose component is added to the plant-based wax in a gradual manner. In one embodiment, the fibrillated cellulose component is added to the plant-based wax all at once.

[0072] In one embodiment, the fibrillated cellulose component comprises entangled cellulose microfibril aggregates comprising microfibrils and / or microfibril bundles smaller than 200 μm.

[0073] In one embodiment, the method is performed using the emulsion transition point method.

[0074] In one embodiment, the solid wet product is a solid wet powder. In one embodiment, the solid wet product is redispersible by heating or diluting the solid wet product.

[0075] In one embodiment, the fibrillated cellulose comprises cellulose nanofibrils comprising nanofibrils and / or nanofibril bundles smaller than 200 μm.

[0076] In one embodiment, the fibrillated cellulose comprises cellulose nanofibrils having anionic or cationic groups attached to their surfaces.

[0077] In one embodiment, the fibrillated cellulose comprises cellulose nanofibrils having phosphate, sulfate or hydroxypropyltrimethylammonium halide ether groups.

[0078] According to a fourth aspect, there is provided a method for preparing a liquid dispersion, comprising providing the solid wet product of the second aspect, diluting the solid wet product in an aqueous medium, or heating the solid wet product to obtain a liquid dispersion.

[0079] In one embodiment, the method for preparing the liquid dispersion further comprises mixing the heated diluted solid wet product.

[0080] According to a fifth aspect, there is provided a coating formulation comprising the composition of the first aspect. In one embodiment, the formulation further comprises hot or cold soluble starch, other viscosity modifiers, pigments or fillers, such as clay, titanium dioxide, kaolinite, calcium carbonate, bentonite, talc, or any combination thereof.

[0081] In one embodiment, the composition of the present invention is used as an ingredient in a coating or adhesive formulation. In one embodiment, the coating or adhesive formulation further comprises at least one thermoplastic polymer in dissolved or latex form. In one embodiment, the coating or adhesive formulation forms a heat sealable layer after drying.

[0082] In one embodiment, the composition is used in a paper or paperboard coating process, such as spray coating, knife coating, rod coating, film coating or curtain coating. The coating can be applied on one side of the paper or paperboard, or on both sides to provide a coated paper or coated paperboard. The coating can include one or more layers.

[0083] In one embodiment, the composition is used as a coating for fruits, berries, vegetables or other edible substances to form an edible coating. In one embodiment, the composition is used as a coating or ingredient for various feed formulations such as feed pellets or granulated functional components such as vitamins.

[0084] According to a sixth aspect, there is provided an article, wherein the article comprises a cellulosic media, and wherein the article comprises at least one coating of the composition of the first aspect.

[0085] According to a seventh aspect, there is provided the use of the composition of the first aspect in sizing, internal sizing, paper coating, paperboard coating, barrier coating, hydrophobic coating, oleophobic coating, corrugated board production, gypsum board production, wood board production, hard or soft board production, laminated veneer lumber production, and / or particle board production.

[0086] In one embodiment, the composition comprising the plant-based wax and fibrillated cellulose component is used in paints, coatings and inks to meet a wide range of performance requirements. These performance requirements include imparting excellent rubbing resistance and toughness, scratch resistance, wear resistance, and blocking resistance, as well as sliding resistance and friction resistance.

[0087] Different non-binding example aspects and embodiments have been described above. The embodiments above are only used to explain selected aspects or steps that can be used in different embodiments. Certain embodiments may be presented only with reference to certain example aspects. It should be understood that the corresponding embodiments may also be applied to other example aspects. BRIEF DESCRIPTION OF THE DRAWINGS

[0088] Some exemplary embodiments will be described with reference to the accompanying drawings, in which:

[0089] Figure 1 A flow chart of the process steps for preparing a wax product is schematically shown.

[0090] Figure 2 The process setup for preparing MFC-stable wax dispersions is shown schematically.

[0091] Figure 3 Optical microscopy images of wax dispersions are shown.

[0092] Figure 4 Coating tests with wax dispersions on veneer-glued timber are shown. DETAILED DESCRIPTION

[0093] As used herein, the term "comprising" includes the broader meanings of "including," "containing," and "comprising," as well as the narrower expressions "consisting of" and "consisting only of.

[0094] In the following description, the same reference numerals denote the same elements or steps.

[0095] Composition of the present invention comprises plant-based wax and fibrillated cellulose component.Term wax is used to represent the solid material that is usually made up of hydrocarbon with C16-C28 carbon number scope.Usually identical compound can be called oil, and this depends on ambient temperature, the chain length of esterified fatty acid and their saturation or unsaturation.

[0096] The term "triglyceride" refers to fatty acid esters of glycerol. Generally, the greater the degree of saturation and the longer the chain length of the esterified acid, the higher the melting point of the triglyceride.

[0097] In the context of the present invention, a vegetable based wax is a wax derived from a plant, or an oil derived from a plant, which oil may be hydrogenated to give a vegetable based wax.

[0098] In the context of the present invention, the composition is an emulsion in the production process. In the context of the present invention, the final composition is a dispersion of wax particles in an aqueous medium at room temperature. An emulsion is a system of two immiscible liquids dispersed together containing droplets with high surface area.

[0099] In one embodiment, the dispersion is a colloidal dispersion.A colloidal dispersion consists of solid particles dispersed in a continuous liquid phase.

[0100] The choice of wax for a particular application is determined by whether it is liquid or solid at the temperature of the product with which it is used. Among the factors that determine whether a wax is liquid or solid at a given temperature are a variety of properties, such as the degree of saturation or unsaturation, or the length of the hydrocarbon chains of the wax components (primarily fatty acids).

[0101] In one embodiment, the plant based wax is substantially solid at room temperature.In one embodiment, the melting point of the composition is above 30°C, preferably above 50°C, more preferably between 50°C and 90°C.

[0102] Preferably, plant-based wax is obtained from at least one plant source. The wax obtained from plant sources is selected from the group consisting of the following: palm wax, palm kernel wax, rapeseed wax, soybean wax (soy wax), corn wax, canola wax (canola wax), carnauba wax, candelilla wax, small crown coconut wax (ourieury wax), soybean wax (soybeanwax), coconut wax, cranberry wax (cranbe wax), sunflower wax, linseed wax, cottonseed wax, sugarcane wax, bayberry wax, peanut wax or their combination. In these embodiments, the combination of wax can be used. These combinations can use one or more waxes. After normal refining processing by methods known in the art, use wax based on plant. For example, plant-based wax can be obtained by using aliphatic solvents to carry out solvent extraction to plant biomass. Other purification can include distillation, fractional crystallization, degumming, bleaching and / or steam stripping subsequently.

[0103] In one embodiment, the plant-based wax is partially or fully hydrogenated. The plant-based wax may include one or more different plant-based waxes. The plant-based wax may include only hydrogenated waxes. The plant-based wax may include one or more hydrogenated waxes combined with one or more non-hydrogenated waxes to obtain a partially hydrogenated plant-based wax component.

[0104] When hydrogenated to a high degree, the characteristics of the wax are changed, with high melting point, low viscosity and good hardness. Suitable hydrogenated wax has a fatty acid of the C16-C28 carbon number range. In addition, fatty acids can be obtained by the hydrolysis of natural triglycerides, for example, by alkaline hydrolysis, followed by purification methods known in the art, including distillation and steam stripping. The unsaturation (or saturation) of wax can be determined as an iodine value. The iodine value is expressed as the grams of iodine absorbed by 100 grams of wax. In one embodiment, the iodine value of the wax based on plants is 0.1-200, preferably 1-80, more preferably 1-40.

[0105] In one embodiment, the plant-based wax comprises fatty acid amides. The plant-based wax comprising triglycerides can be subjected to aminolysis. The aminolysis is performed by any known practice, such as using sodium methoxide as a catalyst and an organic amine at 100° C. to produce fatty acid amides.

[0106] In one embodiment, the composition further comprises. In one embodiment, the composition further comprises a polyvalent cation, preferably Zn 2+ Mg 2+ , Cu 2+ , Fe 2+ , Fe 3+ 、Al 3+ Sn 2+ , and Ca 2+At least one of, or any combination thereof. The hydrophobic and oleophobic properties of the wax composition can be adjusted with multivalent cations. The multivalent cations remove the excess negative charge present in the surfactant, thereby reducing their surface activity. This reduces the hydrophilicity of the surfactant in the composition, thereby increasing the hydrophobicity of the composition. The multivalent cations can be used as crosslinking agents between fatty acids in the composition, which improves the stability of the composition.

[0107] In one embodiment, the functional groups of the wax are saponified. The alkali used to saponify the functional groups of the wax includes potassium hydroxide (KOH), sodium hydroxide (NaOH), calcium hydroxide, sodium silicate and amines such as ammonia, diethylamine ("DEA") and other amine derivatives. Surfactants can be generated in situ during the saponification of the wax. Surfactants can be generated in the wax by saponifying the wax using, for example, potassium hydroxide.

[0108] Typically, waxes with a minimum saponification value of about 20 to 30 mg KOH / g wax can be easily emulsified. The saponification value or value represents the amount of KOH (in milligrams) that reacts with 1 gram of wax at elevated temperatures, and represents the amount of free carboxylic acid plus any esters that can be saponified. This value and the acid value described below provide an indication of the free carboxylic acid and ester content of the wax. ASTM D1387 (2019) is an example of how to determine the saponification value. ASTM D1386 (2016) represents a method for determining the acid value; the amount of KOH (in milligrams) required to neutralize 1 gram of wax indicates the amount of free carboxylic acid present.

[0109] The waxes of the present invention are highly functionalized with saponification values ​​of about 170 mgKOH / g to 220 mgKOH / g. The high saponification value allows the wax to be converted to an emulsion form, as opposed to petroleum and / or asphalt waxes, which are often first oxidized to functionalize the molecules to facilitate emulsification or dispersion. Since the waxes of the present invention do not require such processing, this also makes the present invention more economical than petroleum-derived waxes.

[0110] If the vegetable-based wax contains hydrogenated tall oil, it is not necessary to saponify the vegetable-based wax component, which typically contains partially saponified triglycerides, in the absence of hydrogenated tall oil. Thus, unsaponified triglycerides can be used in the vegetable-based wax as a blend with hydrogenated tall oil, rather than using at least partially saponified triglycerides alone.

[0111] In one embodiment, the compositions described herein can be formulated to have a certain ionic charge. The wax composition can include additional surfactants, which can be surfactants, or other surface-activated compounds. Additional surfactants can be cationic, nonionic or anionic, depending on the desired properties of the specific dispersion. In one embodiment, additional surfactants are additional surfactants. In one embodiment, additional surfactants can be biologically based surfactants, such as lecithin. Lecithin is an amphipathic surfactant. In another embodiment, additional surfactants can be synthetic surfactants.

[0112] Examples of suitable surfactants include alkyl ether carboxylates, alkyl sulfonates, sulfonated polyoxyethylated alcohols, sulfated or phosphated polyoxyethylated alcohols, polymerized ethylene oxide / propylene oxide / ethylene oxide, primary and secondary alcohol ethoxylates, alkyl glucosides and alkyl glycerides, fatty alcohols, cetyl alcohol, stearyl alcohol, cetearyl alcohol, oleyl alcohol, pentaerythritol, mixed esters of fatty acids, citric acid and fatty alcohols and / or mixed esters of fatty acids, methyl glucose and polyols, preferably glycerol or polyglycerol; sorbitan monoesters and diesters of saturated and unsaturated fatty acids and ethylene oxide addition products thereof; polyol esters, and in particular polyglycerol esters, fatty acid esters of sugar alcohols, alkyl glucosides and polyglucosides mixed esters, such as glyceryl stearate citrate and glyceryl stearate lactate, or any combination thereof.

[0113] Examples of particularly interesting surfactants include sodium lauryl sulfate, sodium stearate, sodium lauryl ether sulfate, sodium dioctyl sulfosuccinate, alkylbenzene sulfonates, lignin sulfonates, polyoxyethylene glycol octylphenol ethers, polyoxyethylene glycol alkylphenol ethers, polyoxyethylene glycol sorbitan alkyl esters, sorbitan alkyl esters, betaines, sultaines, ethoxylated nonylphenols, ethoxylated nonylphenol sulfates, ethoxylated lauryl alcohols, polyethylene glycols, polypropylene glycols, and copolymers or block copolymers and oligomers thereof, ethylene acid polymers such as ethylene acrylic acid copolymers or ethylene methacrylic acid copolymers, polysilicone / polyalkyl / polyether copolymers and corresponding derivatives, vinyl acetate, vinyl acrylate, methacrylate copolymers and esters, derivatized cellulose or starch ethers and esters, such as carboxymethyl, hydroxyethyl, hydroxypropyl ethers or mixed ethers of cellulose or starch, polysaccharides, more particularly xanthan gum, guar gum, agar and alginates, or any combination thereof.

[0114] The use of additional surfactants can replace the need for wax saponification, and when there is an additional surfactant in the composition, the plant-based wax can include unsaponified triglycerides, or it can include saponified and unsaponified triglycerides. Alternatively, the use of additional surfactants can supplement the saponification of the wax previously obtained. In one embodiment, the viscosity of the dispersion can be reduced by using additional surfactants.

[0115] In one embodiment, the wax dispersion has a positive surface charge or carries a cationic charge on the wax particle surface. In one embodiment, the positive or cationic surface charge realized by using a cationic surfactant. In one embodiment, the cationic surface charge is realized by using a cationic polymer such as cationic polyacrylamide, cationic starch or another cationic polymer that is applicable. In one embodiment, the cationic surface charge is realized by using cationic fibrillated cellulose.

[0116] In one embodiment, the composition described herein includes a wax particle size less than 20 μm. In one embodiment, the composition described herein includes a wax particle size preferably between 0.1 μm-10 μm. In one embodiment, the composition described herein includes a wax particle size most preferably between 0.5-8 μm. In another embodiment, the wax particles have a size of about 1-5 μm, or about 1.5-4.5 μm. The particle size of the wax particles in the composition can be adjusted by mechanical stirring or by a surfactant. The particle size of the wax particles in the composition can be adjusted by the type and power of mixing. When manufacturing a composition with a more limited wax particle size, in the manufacturing process of the composition, especially in the stage when the plant-based wax and the water containing the fibrillated cellulose component form an emulsion at a temperature higher than the wax melting point, suitable mixing power is required.

[0117] The slower or weaker the mixing, the larger the particle size of the wax particles in the composition. In one embodiment, the composition is subjected to high shear mixing, such as 17 kRPM and 10 kJ / dm 3Energy input, in order to obtain less wax particle size.In one embodiment, mix with the device that is suitable for this purpose.In one embodiment, the device that is suitable for purpose comprises batch mixer or online mixer, low shear or high shear mixer, static online mixer, agitator, disperser, grinder, pulverizer, granulator, homogenizer, rotor-stator mixer or grinder such as Ultra-Turrax, Silverson high shear online or batch mixer, from Masuko Supermass collision device of Masuko Sangyo, rotor-rotor mixer or grinder such as Atrex type device, high shear homogenizer such as Ariete type or Panda type, fluidizer, microfluidizer or large fluidizer such as microfluidizer and / or ultrasonic disintegrator or their combination in any from Microfluidics of GEA Niro-Soavi.In one embodiment, the granularity of wax particles in the composition can also be regulated by the amount of surfactant.

[0118] In one embodiment, the composition of the dispersion of wax particles has a Brookfield viscosity of 10 to 6000 cP, measured at 20 wt% dry matter of the composition in water, 50 rpm, spindle V-73.

[0119] In one embodiment, the composition includes a fibrillated cellulose component. The fibrillated cellulose component is a suspension comprising fibrillated cellulose and water, i.e., the fibrillated cellulose can provide an aqueous medium present in the composition. In one embodiment, the fibrillated cellulose component comprises cellulose microfibrils, cellulose microfibril aggregates and / or cellulose microfibril bundles. The fibrillated cellulose can be in the form of an expanded fibril network, in which individual microfibrils or microfibril bundles are still partially bound or entangled with each other, even after they have been subjected to homogenization. Such partially bound or entangled individual microfibrils and / or microfibril bundles can be referred to as cellulose microfibril aggregates. In one embodiment, the fibrillated cellulose component comprises entangled cellulose microfibril aggregates, which include microfibrils and / or microfibril bundles. The entangled cellulose microfibril aggregates are less than 200 μm.

[0120] In one embodiment, the fibrillated cellulose component is or it includes microfibrillated cellulose (MFC). In the context of the present invention, the term "microfibrillated" may also include nanofibrillated cellulose fibers or fiber fragments (NFC). Fibrillated cellulose can be separated from various cellulose raw materials. In one embodiment, fibrillated cellulose is derived from non-wood-based cellulose raw materials. In one embodiment, the fibrillated cellulose component is parenchyma cellulose. In one embodiment, the raw material of the fibrillated cellulose component is selected from beet pulp, dry beet pulp, wet beet pulp, beet grains, potato pulp, sweet potato, cassava pulp, bagasse pith, citrus peel, corn, fruit, vegetables, soybeans and any combination thereof. In one embodiment, the fibrillated cellulose component is manufactured according to the method provided in the disclosed embodiments of WO 2022 / 003252 A1 (especially in Examples 1 and 3) or the method provided in the disclosed embodiments of WO2017 / 103329A1 (especially in Examples B and C). In one embodiment, the fibrillated cellulose is obtained by mechanical treatment, such as homogenization or refining or grinding, without a previous treatment step of the cellulosic raw material selected from enzymatic modification, chemical modification or physical modification of the raw material.

[0121] In one embodiment, the fibrillated cellulose may contain other polysaccharides, such as pectin, hemicellulose and / or other soluble polysaccharides present in the cellulose raw material from which the fibrillated cellulose is made. The amount of other polysaccharides depends on the raw materials used and the separation method.

[0122] In one embodiment, the aspect ratio of the cellulose microfibrils is high. In one embodiment, the length of the microfibrils can be greater than 1 micron, and the number average diameter is generally less than 200nm, such as between 2nm and 100nm. The diameter of the microfibril bundles can be larger, but is generally less than 1μm. The smallest microfibrils are similar to the so-called elementary fibrils, and their diameter is generally 2nm to 12nm.

[0123] In one embodiment the fibrillated cellulose component has a Schopper-Riegler value of less than 20, preferably from 1 to 10, more preferably from 4 to 6, determined by EN ISO 5267-1 (1996).

[0124] The use of fibrillated cellulose in the composition has a number of benefits. Some of the benefits relate to the product obtained itself, but some of the benefits relate to the production method of the composition. The fibrillated cellulose reduces the viscosity of the intermediate phase at the emulsion transition point. Without the use of fibrillated cellulose in the emulsion preparation, the viscosity during the phase transition may increase to such an extent that mechanical mixing becomes difficult.

[0125] In terms of the benefits of fibrillated cellulose to the product, fibrillated cellulose stabilizes the composition by inhibiting agglomeration during aging by facilitating smaller wax particle size. Thus, fibrillated cellulose reduces ripening in the dispersion. The fibrillated cellulose component stabilizes the dispersion.

[0126] Can realize the stabilization of micron-level wax particles and nano-level wax particles with for example amphipathic surfactant or solid particles.The fibrillated cellulose component has stabilized the composition with its three-dimensional fibril network and interfacial energy.The particle size of wax particles, the surface characteristics of fibrillated cellulose component and liquid-liquid interfacial tension contribute to interfacial energy.The three-dimensional fibril network of fibrillated cellulose component prevents micron-level and nano-level droplet coalescence and stabilizes the interface between plant-based wax and aqueous medium.

[0127] The particle-particle interaction of the fibrillated cellulose component affects the stability of the composition. A higher number of interactions results in a mechanical barrier at the particle interface, which increases the stability of the composition. During the production process, the composition stabilized by the fibrillated cellulose component can be considered as a Pickering emulsion, wherein the stable feature is the interfacial energy and the emulsion is stabilized by the fibril network. In one embodiment, the hemicellulose included in the fibrillated cellulose component contributes to the stability of the composition. In another embodiment, stability can be provided by a combination of microfibrillated cellulose and a suitable polymer. In this specific embodiment, stability is achieved by spatial stabilization.

[0128] In addition, the fibrillated cellulose acts as an adhesion promoter in the composition. For example, if the composition is used to coat a substrate, the fibrillated cellulose increases the adhesion between the composition and the substrate and bonds the wax particles to the surface when drying. Therefore, the resulting coating is more durable.

[0129] The fibrillated cellulose component also acts as a retention agent in the composition. When applied in a wet state prior to filtration, the fibrillated cellulose improves the retention of the wax dispersion in the sizing of cellulose fiber-based materials by binding the dispersed wax particles to the cellulose pulp fibers.

[0130] In one embodiment, the composition further comprises an additional amount of microfibrillated cellulose. The additional microfibrillated cellulose increases the oleophobicity of the composition.

[0131] Figure 1A flow chart of the process steps of the method for producing a composition is schematically shown. The composition of the present invention includes a plant-based wax and a fibrillated cellulose component. Step 10 shows providing a plant-based wax and a fibrillated cellulose component. Both are described in more detail in the previous description. In step 20, both the plant-based wax and the fibrillated cellulose component are heated. The plant-based wax is heated to a temperature higher than its melting temperature. In step 30, the fibrillated cellulose component is added to the plant-based wax while continuously stirring. In step 30, the fibrillated cellulose component can be added to the plant-based wax quickly or slowly. In one embodiment, the fibrillated cellulose component is added to the plant-based wax in a continuous manner. In one embodiment, the fibrillated cellulose component is added to the plant-based wax in a gradual manner. In one embodiment, the fibrillated cellulose component is added to the plant-based wax all at once. In step 30, the composition is in the form of an oil-in-water emulsion.

[0132] exist Figure 1 In step 40, the fibrillated cellulose component and the plant-based wax are mixed until a phase change occurs. When a phase change occurs, a dispersion composition of wax particles in an aqueous medium is obtained. In one embodiment, the composition is produced by an emulsion transition point (EIP) method. In step 40, a phase change between an oil-in-water emulsion and an oil-in-water emulsion occurs at an emulsion transition point. In the emulsion transition point method, the oil-in-water emulsion obtained when the fibrillated cellulose component is added to the plant-based wax is transformed into an oil-in-water emulsion by a phase change through an interconversion process at an emulsion transition point. After step 40, the composition is in the form of a dispersion. Now the dispersion is liquid at room temperature. After step 40 (indicated in step 50 of the flow chart) the dispersion can be used in any suitable application.

[0133] exist Figure 1In step 60, an alternative to using a dispersion is provided. In an alternative embodiment, the method further includes subjecting the dispersion to a powder manufacturing process to obtain a solid wet product. The solid wet product is obtained to be easy to handle, for example, during storage and transportation. Compared with liquid dispersions, solid wet products are easier to package, store, transport, deliver and handle. The solid wet product contains water, so it is not anhydrous. After step 60, the solid wet product can be in the form of solid wet powder, solid wet granules, solid wet granules, solid wet cake or any combination thereof. The powder preparation method mentioned is granulation, grinding, granulation, forming blocks or any suitable technology to reduce particle size. In an optional embodiment, the composition is dried. In one embodiment, the optional drying is selected from the group consisting of the following: freeze drying, freeze drying, vacuum drying, air drying, spray drying, atomization, evaporation, tray drying, flash drying, drum drying, fluidized bed drying, oven drying, conveyor belt drying, microwave drying, solar drying or a combination thereof.

[0134] After step 60, the solid wet product can be diluted in an aqueous medium according to step 71, or heated according to step 72, to obtain a liquid dispersion. Therefore, in one embodiment, the solid wet product is redispersible. The redispersible solid wet product can be processed back into a dispersion. In step 80, the redispersed liquid dispersion is used in any suitable application. Obtaining a solid wet product and redispersing the solid wet product back into liquid form can be performed multiple times, and it is not limited to one cycle.

[0135] Figure 2 A process configuration 100 for preparing a microfibrillated cellulose (MFC) stabilized wax dispersion according to an exemplary embodiment is schematically shown.

[0136] exist Figure 2 The tank 101 includes a polyvalent cation such as Ca 2+ Tank 102 comprises water. Tank 103 comprises a fibrillated cellulose component, preferably a microfibrillated cellulose component, which is heated to an elevated temperature, such as 80° C. Tank 104 comprises a plant-based wax, which is heated to an elevated temperature, such as 90° C. In tank 104, the wax is saponified, such as with potassium hydroxide.

[0137] Mixing in process configuration 100 may be performed by individual mixers located in the tanks. For example, tanks 105, 106, and 108 may be equipped with individual mixers. Alternatively, mixing in process configuration 100 may be performed via inline mixers 107 between the tanks. Material from any one tank may be directed through inline mixer 107 to enhance agitation.

[0138] In tank 105, the saponified oil from tank 104 is mixed with the fibrillated cellulose component from tank 103. In this step, the mixing can be adjusted to obtain the desired wax particle size. In tank 106, the mixture of heated wax and heated fibrillated cellulose component is mixed with water from tank 102. In tank 108, the mixture containing heated wax, heated fibrillated cellulose and water from tank 106 is mixed with water containing divalent cations (such as Ca 2+) from tank 101. 2+ The product is stored and cooled in tank 108.

[0139] In one embodiment, the equipment used to prepare the composition is capable of agitation of the reactants to achieve adequate mixing and has appropriate temperature control to maintain adequate heating and cooling of the reagents and products.

[0140] exist Figure 2 , valve 110 (110a, 110b, 110c, 110d, 110e, 110f) controls the flow between the tanks. Preferably, valve 110 is a three-way valve. In one embodiment, the valves can be individually controllable. Pump 111 (111a, 111b) pumps the process material to the desired tank. Process configuration 100 implements a continuous process configuration. Tanks 105, 106 and 107 can be connected in series directly or with a buffer tank (not shown). By adding pumps and in-line mixers, these process steps can be run simultaneously.

[0141] Optionally, valve 110 and pump 111 allow bypass. Thus, if necessary, any previously mentioned tank can be bypassed and certain process steps can be skipped. In addition, valve 110 and pump 111 enable certain components of the composition to be completely omitted.

[0142] In one embodiment, the process steps are performed in the order indicated in any aspect, embodiment, or claim. In another embodiment, any process step specified to be performed on a product or intermediate obtained in a previous process step is performed directly on the product or intermediate, i.e., without additional, optional or auxiliary processing steps that may chemically and / or physically change the product or intermediate between two consecutive steps.

[0143] A coating formulation comprising the above composition is provided. In one embodiment, the composition is used as a component of a coating formulation. In one embodiment, the formulation further comprises hot or cold soluble starch, other viscosity modifiers, pigments or fillers, such as clay, titanium dioxide, kaolinite, calcium carbonate, bentonite, talc, or any combination thereof. In one embodiment, the formulation may further comprise a defoamer, a pH adjuster, or any combination thereof.

[0144] In one embodiment, the composition is used as an ingredient in a coating or adhesive formulation. In one embodiment, the coating or adhesive formulation further comprises at least one thermoplastic polymer in dissolved or latex form. In one embodiment, the coating or adhesive formulation forms a heat sealable layer after drying.

[0145] In one embodiment, the composition is used in a paper or paperboard coating process, such as spray coating, knife coating, rod coating, film coating or curtain coating.

[0146] In one embodiment, the composition is used as a coating for fruits, berries, vegetables or other edible substances to form an edible coating. The edible coating protects the product and prevents drying out during storage.

[0147] In one embodiment, the composition is used as a coating or ingredient for various feed formulations such as feed pellets or granulated functional components, such as vitamins. The composition is used in applications to protect materials from exposure to water, oil or oxygen. The composition can be applied to pellets, particles or the like by conventional coating methods. The use of the composition prevents drying during storage.

[0148] Articles comprising the compositions of the present invention are provided. In one embodiment, the articles comprise a cellulosic medium, such as paper, paperboard, wood, pulp, or a starch-based medium. The articles comprise at least one coating of the composition of the first aspect comprising a plant-based wax and a fibrillated cellulose component. Use of the composition improves the properties of the articles, such as barrier properties, moisture and water resistance, hydrophobicity, oleophobicity, durability, printing properties, and inhibition of water absorption.

[0149] In one embodiment, coating with the composition of the first aspect and subsequent drying of the article is performed at a temperature below the melting point of the wax.In one embodiment, coating with the composition of the first aspect and / or subsequent drying of the article is performed at a temperature above the melting point of the wax.

[0150] In one embodiment, the article can be a disposable product, such as a food service or packaging article, or a continuous use product. In one embodiment, the article is biodegradable.

[0151] In one embodiment, the process of the invention is an industrial process. In another embodiment, an industrial process may exclude small scale processes, such as laboratory scale processes that cannot be scaled up to a scale for industrial use.

[0152] In one embodiment, the process of the invention is a continuous process. In another embodiment, the process of the invention is a semi-continuous process. According to one embodiment, the process of the invention comprises batch process steps.

[0153] In another aspect, there is provided a method for making a dispersion, the method comprising:

[0154] blending hydrogenated tall oil and hydrogenated vegetable oil, preferably rapeseed oil, by mixing and heating to provide a liquefied wax blend;

[0155] Providing a dispersion of MFC (microfibrillated cellulose) in water;

[0156] The emulsion was prepared by pouring a dispersion of MFC in water into the wax blend under high shear mixing;

[0157] diluting the emulsion into a cold water-based solution containing polyvinyl alcohol; and

[0158] Optionally, CaCl2 is added along with high shear mixing.

[0159] The obtained dispersion can be used as a hydrophobic coating.

[0160] In another aspect, there is provided a method for making a dispersion, the method comprising:

[0161] providing a hydrogenated molten vegetable wax, preferably rapeseed wax;

[0162] Providing a dispersion of MFC in water;

[0163] providing a water-based solution comprising polyvinyl alcohol;

[0164] blending hydrogenated molten vegetable wax with a water-based solution comprising polyvinyl alcohol under high shear mixing to obtain a wax dispersion;

[0165] diluting the wax dispersion with cold water under high shear mixing; and

[0166] The wax dispersion was mixed with the dispersion of MFC in water under high shear mixing.

[0167] The dispersion has good water barrier and oil barrier properties.

[0168] In another aspect, there is provided a method for making a dispersion, the method comprising:

[0169] providing a hydrogenated molten vegetable wax, preferably rapeseed wax;

[0170] providing a water-based solution containing polyvinyl alcohol and MFC;

[0171] An emulsion is prepared by pouring a water-based solution containing polyvinyl alcohol and MFC into hydrogenated molten vegetable wax and mixing by using high shear mixing;

[0172] The emulsion is diluted with cold water containing polyvinyl alcohol and mixed by high shear mixing to provide a wax dispersion.

[0173] The obtained wax dispersion has good water and oil barrier properties.

[0174] Embodiments and implementations are further disclosed in the following numbered clauses:

[0175] Item 1. A composition comprising: a plant-based wax; a fibrillated cellulose component; and wherein the composition is a dispersion of wax particles in an aqueous medium.

[0176] Item 2. The composition described in Item 1, wherein the fibrillated cellulose comprises entangled cellulose microfibril aggregates, the cellulose microfibril aggregates comprising microfibrils and / or microfibril bundles smaller than 200 μm.

[0177] Item 3. The composition of Item 1 or 2, wherein the plant-based wax comprises triglycerides and / or partially saponified triglycerides, and the plant-based wax is preferably selected from the group consisting of palm wax, palm kernel wax, rapeseed wax, soy wax, corn wax, canola wax, carnauba wax, candelilla wax, ourieury wax, soybean wax, coconut wax, cranberry wax, sunflower wax, linseed wax, cottonseed wax, sugarcane wax, bayberry wax, peanut wax, or a combination thereof.

[0178] Item 4. The composition of any one of Items 1-3, wherein the fibrillated cellulose component is fibrillated parenchyma cellulose.

[0179] Item 5. The composition of any one of Items 1-4, wherein the fibrillated cellulose component comprises cellulose in an amount less than 70 wt% of the dry matter of the fibrillated cellulose component, and hemicellulose in an amount greater than 30 wt% of the dry matter of the fibrillated cellulose component.

[0180] Item 6. The composition of any one of Items 1 to 5, wherein the composition further comprises a polyvalent cation, preferably Zn 2+ Mg 2+ , Cu 2+ , Fe 2+ , Fe 3+ 、Al 3+ Sn 2+ , or Ca 2+ , or fatty acid salts of polyvalent cations.

[0181] Item 7. The composition of any one of Items 1-6, wherein the composition comprises a wax particle size of less than 20 μm, preferably between 0.1-10 μm, and most preferably between 0.5-8 μm.

[0182] Item 8. The composition of any one of Items 1-7, wherein the plant-based wax is hydrogenated or partially hydrogenated.

[0183] Item 9. The composition of any one of Items 1-8, wherein the dispersion of wax particles has a Brookfield viscosity of 10 cP to 6000 cP, measured at 50 rpm, spindle V-73, for a 20 wt % aqueous solution of the dry matter of the composition.

[0184] Item 10. A solid wet product obtained by subjecting the composition described in any one of Items 1 to 9 to a powder preparation method.

[0185] Item 11. A method for preparing a composition described in any one of Items 1-9, comprising: providing a plant-based wax; providing a fibrillated cellulose component; heating the plant-based wax and the fibrillated cellulose component; adding the fibrillated cellulose component to the plant-based wax while continuously mixing; mixing the fibrillated cellulose component and the plant-based wax until a phase transition occurs to obtain a dispersion composition of wax particles in an aqueous medium.

[0186] Item 12. The method according to Item 11, wherein the method is carried out using an emulsion transition point method.

[0187] Item 13. A method for preparing a liquid dispersion, comprising: providing the solid wet product of Item 10; diluting the solid wet product in an aqueous medium, or heating the solid wet product, to obtain a liquid dispersion.

[0188] Item 14. A coating composition comprising the composition of any one of items 1 to 9.

[0189] Item 15. An article, wherein the article comprises a cellulosic media, and wherein the article comprises at least one coating of the composition of any of items 1-9.

[0190] Item 16. Use of the composition described in any one of Items 1-9 in sizing, internal sizing, paper coating, cardboard coating, barrier coating, hydrophobic coating, oleophobic coating, corrugated board production, gypsum board production, wood board production, hard or soft board production, laminated veneer lumber production, and / or particle board production.

[0191] Example

[0192] The following examples are provided to better illustrate the claimed invention. They should not be construed as limiting the scope of the invention as determined by the claims. To the extent that specific materials are mentioned, they are for illustrative purposes only and are not intended to limit the present invention. Those skilled in the art may use or develop equivalent means or materials without exerting creative ability and without departing from the scope of the present invention. It should be understood that many changes may be made in the process described herein while remaining within the scope of the present invention. All exemplary materials and parameters used in the following examples are compatible with the methods and products specified in the independent claims. Any non-essential features disclosed in the examples or embodiments herein may be included in the methods or products of the independent claims without adding new content.

[0193] In the context of the present invention, the composition during its production is an emulsion, whereas the final product is a dispersion.

[0194] Example 1

[0195] The following is a method for preparing a composition comprising hydrogenated rapeseed wax and beet microfibrillated cellulose (MFC). Beet microfibrillated cellulose (MFC) was produced according to the method provided in the disclosed examples of WO 2022 / 003252 A1, in particular in Sample 3C of Example 3.

[0196] Referring to Tables 1a and 1b, entry A: A dispersion was prepared using hydrogenated rapeseed wax having a melting point of 68°C and a theoretical triglyceride composition of 90% stearic acid, 7% palmitic acid by adding the aqueous phase containing MFC (preheated to 80°C) to the molten wax phase at once or at a rate of 50 g / ml while stirring. Foaming was avoided by adjusting the stirrer to avoid stirring air into the system. The surfactant was generated in situ in the oil phase by potassium hydroxide saponification.

[0197] With reference to Tables 1a and 1b, Item B: Wax (300 g) was weighed in a 1L glass beaker and allowed to melt at 100°C. To the liquefied wax, 6.0 g of potassium hydroxide, KOH, (50%) solution was added and allowed to stir at 90°C for 60 minutes. In a separate beaker, a 1.5% dispersion of beet MFC (173 g) was heated to 80°C and the pH was adjusted to 11. An emulsion was prepared by pouring the aqueous phase containing MFC into the wax in one go and mixing for 30 seconds using a high shear mixer (17000 rpm, 180 W). The obtained emulsion was diluted with water (20°C) to obtain the compositions shown in Tables 1a and 1b.

[0198] With respect to Tables 1a and 1b, Item C: Wax (381 g) was weighed in a glass beaker and allowed to melt at 100°C. To the liquefied wax was added 30.5 g of KOH (50%) solution and allowed to stir at 90°C for 90 minutes. In a separate beaker, a 3% beet MFC dispersion (255 g) was heated to 80°C. An emulsion was prepared by pouring the aqueous phase into the oil phase at a rate of about 50 g / min while stirring with a propeller mixer at 500 rpm and allowing to mix for 5 minutes. 381 g of water (20°C) was added and allowed to mix. CaCl 2 The dispersion was further diluted with a solution of (7.15 g, 77%) dissolved in 990 g of water and mixed with a high shear mixer (17000 rpm, 180 W) to obtain the compositions shown in Tables 1a and 1b. A reference sample without sugar beet MFC was prepared as described above (Tables 1a and 1b, entry A), but high shear blending was used due to the extremely high viscosity of the emulsion transition point.

[0199] These examples show that the use of sugar beet MFC during the emulsification process reduces the wax particle size. It also reduces the viscosity near the emulsion transition point. The dispersion obtained has hydrophobic properties and, in the presence of multivalent salts, oleophobic properties can also be obtained.

[0200] Table 1a. Dispersions obtained from hydrogenated rapeseed wax.

[0201]

[0202] Table 1b. Dispersions obtained from hydrogenated rapeseed wax.

[0203]

[0204]

[0205] Example 2

[0206] The following is a method for preparing a composition comprising hydrogenated palm wax and beet microfibrillated cellulose (MFC). Beet microfibrillated cellulose (MFC) was prepared according to the method provided in the disclosed examples of WO 2022 / 003252 A1, in particular in Sample 3C of Example 3.

[0207] Hydrogenated palm wax having a melting point of 58° C. and a theoretical triglyceride composition of 54% stearic acid, 43% was used to produce the dispersion.

[0208] With respect to Tables 2a and 2b, Item A: Wax (400 g) was weighed in a glass beaker and allowed to melt at 100°C. 32 g of KOH (50%) solution was added to the liquefied wax and allowed to stir at 90°C for 60 minutes. In a separate beaker, a 3% beet MFC dispersion (233 g) was heated to 80°C. An emulsion was prepared by pouring the aqueous phase into the oil phase at a rate of about 50 g / min while stirring with a propeller mixer at 500 rpm and allowing to mix for 5 minutes. 405 g of water (20°C) was added and allowed to mix. 400 g of the obtained dispersion was taken and mixed with CaCl 2 A solution of (2.8 g, 77%) dissolved in 400 g of water was diluted and mixed with a high shear mixer (17000 rpm, 180 W) to obtain the compositions shown in Tables 2a and 2b.

[0209] With respect to Tables 2a and 2b, Item B: Wax (300 g) was weighed in a glass beaker and allowed to melt at 100°C. To the liquefied wax, 24.0 g of a KOH (50%) solution was added and allowed to stir at 90°C for 60 minutes. In a separate beaker, a 3% beet MFC dispersion (173 g) was heated to 80°C. An emulsion was prepared by pouring the aqueous phase into the oil phase at once and mixing with a propeller mixer at 500 rpm and allowing to mix for 5 minutes. Then 300 g of water (20°C) was added and allowed to mix. The pH of the resulting dispersion was then adjusted to 11 with KOH. 457 g of the obtained dispersion was taken and diluted with a solution of sodium dodecyl sulfate (SDS) (4.0 g, 99%) dissolved in 280 g of water and mixed with a high shear mixer (17000 rpm, 180 W) to obtain the compositions shown in Tables 2a and 2b.

[0210] These examples show that palm oil wax can be used instead of rapeseed oil wax with similar results. The dispersion obtained has hydrophobic properties and in the presence of multivalent salts, oleophobic properties can also be obtained. If necessary, additional surfactants such as sodium dodecyl sulfate (SDS) can be used to reduce the viscosity of the dispersion.

[0211] Table 2a. Dispersions obtained from hydrogenated palm oil wax.

[0212]

[0213] Table 2b. Dispersions obtained from hydrogenated palm oil wax.

[0214] entry Particle size (max) μm Hydrophobic Oleophobic Viscosity after 2 weeks A 10 yes yes 2800 B 10 yes yes 2030

[0215] Example 3

[0216] An example of induced solidification of a wax dispersion containing hydrogenated palm oil and beet microfibrillated cellulose (MFC) to obtain a solid wet product is given below. Beet microfibrillated cellulose (MFC) was prepared according to the disclosed examples of WO 2022 / 003252 A1, especially the method provided in Sample 3C of Example 3

[0217] About Table 3a and 3b, Item A: Hydrogenated palm oil wax (400 g) was weighed in a glass beaker and allowed to melt at 100°C. To the liquefied wax, 16.0 g of KOH (50%) solution was added and allowed to stir at 90°C for 60 minutes. In a separate beaker, 3% beet MFC dispersion (230 g) was heated to 80°C. An emulsion was prepared by pouring the aqueous phase containing MFC into the wax at one time and mixing for 30 seconds using a high shear mixer (17000 rpm, 180 W). Then 305 g of water was added to the dispersion and continued to mix for 60 seconds using a high shear mixer (17000 rpm, 180 W), at which time a low viscosity dispersion was obtained. The dispersion was cooled to 20°C in a water bath and allowed to solidify to obtain the compositions shown in Tables 3a and 3b. Solid wet wax can be easily made into a free-flowing non-sticky powder.

[0218] With respect to Tables 3a and 3b, Item B: Hydrogenated palm oil wax (400 g) was weighed in a glass beaker and allowed to melt at 100°C. 32.0 g of KOH (50%) solution was added to the liquefied wax and allowed to stir at 90°C for 60 minutes. In a separate beaker, a 4% beet MFC dispersion (230 g) was heated to 80°C. An emulsion was prepared by pouring the aqueous phase containing MFC into the wax in one go and mixing for 30 seconds using a high shear mixer (17000 rpm, 180 W). CaCl was then added to the dispersion. 2 A solution of (7.5 g 77%) in 336 g water was prepared and mixing was continued for 60 seconds with a high shear mixer (17000 rpm, 180 W) at which time a low viscosity dispersion was obtained. The dispersion was cooled to 20° C. in a water bath and allowed to solidify to obtain the compositions shown in Tables 3a and 3b. The solidified hard wet wax can be easily made into a free-flowing, non-sticky powder.

[0219] These examples show that dispersions can be formulated to cure quickly by adjusting the wax particle size, surfactant and amount of MFC. In addition, the particle size of the wax particles can be adjusted by surfactant (saponification ratio) and mixing methods during emulsification. The dispersion has hydrophobic properties and, in the presence of multivalent salts, oleophobic properties can also be obtained.

[0220] Table 3a. Solidified dispersions obtained from hydrogenated palm oil wax.

[0221]

[0222]

[0223] Table 3b. Solidified dispersions obtained from hydrogenated palm oil wax.

[0224] entry Particle size (max) μm Hydrophobic Oleophobic Curing time A 2.5 yes no 10min B 2.5 yes yes 30min

[0225] Figure 3 An optical microscopic image of the obtained wax dispersion prepared with MFC at 40 times magnification is provided. Figure 3 The upper image in provides the low shear mixing obtained from Example 1, Entry C. Figure 3 The bottom image in provides the high shear mixed dispersion from Example 3, Entry B. Figure 3 The scale bar in is 10 μm.

[0226] Example 4

[0227] The following provides for the storage and redispersion of the powdered solid wet product by heating.

[0228] The solidified wax dispersion from Example 3, Entry A, comminuted into a free-flowing powder form was stored for 1 month after which heating in an 80°C water bath returned the material to a low viscosity liquid dispersion having the original properties as before solidification.

[0229] These examples show that the powdered wet dispersion has a long shelf life and can be converted to liquid form simply by heating. In addition, the powdered material can be conveniently transported and stored in the form of bags.

[0230] Example 5

[0231] Storage and redispersion of the powdered solid wet product by dilution is provided below.

[0232] The solidified wax dispersion from Example 3 Entry A, crushed into a free-flowing powder, was stored for 1 month after which it was diluted to 20 wt% and dispersed using a high shear mixer (17000 rpm, 180 W) for 60 seconds, returning the material to a low viscosity liquid dispersion with initial properties as before solidification.

[0233] These examples show that the powdered wet dispersion has a longer shelf life and can be made into a liquid dispersion form by dilution. In addition, the powdered material can be conveniently transported and stored in the form of bags.

[0234] Example 6

[0235] Various analytical methods for wax dispersions are provided below.

[0236] The viscosity of the samples was measured by a Brookfield DV3T viscometer (RV-Torque range, Brookfield Engineering Laboratories, Middleboro, USA) equipped with a blade geometry (V-73). The formulated samples were measured at a shear rate of 50 rpm.

[0237] The pH of the samples was measured using a Hach Pocket Pro plus pH meter. Optical microscopy images were acquired using 10x and 40x magnification and cross-polarization with a Nikon Eclipse E200 microscope equipped with a Canon EOS100D camera.

[0238] The hydrophobic / oleophobic properties of the dispersion coated foil panels (Rochcoat GC2) were determined by placing a drop of rapeseed oil or water and observing the stability after 30 minutes.

[0239] Example 7

[0240] The following provides coating tests of the composition according to the present invention on veneer glued wood.

[0241] The hydrophobization of veneer glued wood (LVL) was performed by applying a wax dispersion according to the dispersion provided in Example 1C to a cross-sectional cut of veneer glued wood. The dispersion was allowed to dry at room temperature. The dry coating was tested as is (A) and polished by a cloth (B). A drop of water was placed on top of the coating. The water drop did not penetrate the wood, but evaporated within a few hours. The reference untreated LVL cross-sectional cut absorbed water within a few seconds.

[0242] Figure 4 Results of coating tests with wax dispersions on the cut side of veneer glued timber are presented. Figure 4 In the examples, water drops are on A) coated layer B) coated, polished layer and REF) uncoated veneer glued wood. These examples show that the developed wax can be used to make wood hydrophobic and that the surface texture can be easily polished.

[0243] Example 8

[0244] A paper coating having a composition according to the invention is provided below.

[0245] Dispersion coating of paper substrates was demonstrated using an Elcometer 4340 draw-down coater using two different wax dispersions. The paper substrate (i.e. base paper) was 300 g / m 2 Basis weight of UPM Fine uncoated wood-free paper. The process details are summarized in Table 4.

[0246] The coating dispersions were prepared from the wax dispersions of Example 1, entry C or Example 2, entry A by diluting the corresponding dispersion to an aqueous dispersion with a dry matter content of 15 wt %. The coating dispersions were easily applied with a coater and a smooth coating layer was obtained. The coated substrate was dried at a temperature below the melting point of the wax (66° C. or 56° C.) or at a higher temperature well above the melting point (80° C.). Two different coating weight levels were tested, 10 to 11 g / m 2 or 5 to 7 g / m 2 .

[0247] The coating conditions for the coating experiments shown in Table 4 were a temperature of 23° C. and normal indoor humidity. The test conditions for the experiments shown in Table 4 were a temperature of 23° C. and a humidity of 50% RH. The gram weight was measured according to ISO 536:19 (2019).

[0248] Table 4. Details of coating experiments.

[0249]

[0250] Example 9

[0251] An analysis of the coated paper from Example 8 is provided below.

[0252] The water absorption and surface properties of the coated paper in Example 8 were analyzed by different methods, see Table 5. The surface energy and contact angle were measured with FIBROETIX. Obviously, the dispersion coating with the wax used makes the base paper hydrophobic, and the characteristic Cobb60 value is significantly reduced for all test points. In addition, the paper surface becomes more hydrophobic as the water contact angle increases and the surface energy increases. Carrying out the drying stage at a temperature below the melting point of the corresponding wax seems to have a slight effect on the functionality, because the Cobb60 value is generally lower than that of the samples dried at an elevated temperature (80°C). The same trend can also be seen for the surface energy and contact angle. However, for the test points where the drying temperature exceeds the melting temperature, the results are also very good.

[0253] Table 5. Summary of water absorption and surface properties of the test points.

[0254]

[0255] Example 10

[0256] The following provides an application of internal sizing using the composition according to the present invention.

[0257] Internal sizing of cellulose pulp sheets was demonstrated with the wax dispersion in Example 2, Item A. Cellulose sheets were prepared according to method ISO 5269-1:2005 by using a mixture of 70% bleached birch pulp (SR38) and 30% bleached pine pulp (SR32) and 0.01% retention agent (Fennopol K3400P). The total dosage of the wax dispersion was 1.0% (calculated on dry basis). The wax dispersion was added together with the retention agent to a thin stock of pulp fibers. The mixture obtained was filtered and dried according to the standards. The characteristic values ​​of the reference and wax dispersion treated sheets are shown in Table 6.

[0258] The wax dispersion treated pulp sheets clearly show much lower water absorption compared to the reference sheets, which is shown as Cobb 60 values ​​in Table 6.

[0259] Table 6. Summary of internal sizing experiments.

[0260]

[0261] *Water passes through the sample.

[0262] Embodiment 11

[0263] The use of the composition according to the invention in gypsum board is provided below.

[0264] Gypsum hemihydrate, water, and wax emulsion (10% dry matter content) were mixed in different ratios, keeping the ratio of gypsum to water constant in view of the water in the wax emulsion. The gypsum was first mixed with the water, and then the wax emulsion was mixed into the plaster. Table 7 shows the compositions. 0.75 g of the plaster samples were molded in paper cups, hardened for 1 h at room temperature, then baked at 90° C. for 2 h and finally dried overnight at 60° C. in a convection oven.

[0265] Table 7. Composition

[0266] Wax content in dry mortar Wax dispersion (10%) water <![CDATA[CaSO 4 Hemihydrate]]> Total wet weight 0.0% 0 40 60 100 1.0% 7.1 33 60 100

[0267] Water absorption was tested by immersing the sample in water for 2 hours, quickly wiping the loose water from the surface with a paper towel and measuring the change in mass. With the addition of 1.0% wax, a 20% reduction in water absorption was observed.

[0268] Example 12

[0269] The hydrogenation of tall oil acid was carried out as follows: 100 g of distilled tall oil acid (acid value (ASTM D465), 196 mgKOH / g and iodine value (ASTM D5768), 153 g (I2) / 100 g) was charged into a two-necked round bottom flask and 2.00 grams of catalyst (10% palladium on carbon) was added and mixed using a magnetic stirrer. The mixture was flushed first with argon and then with hydrogen and the temperature was raised to 150° C. using an oil bath. The hydrogenation was allowed to proceed at atmospheric pressure for 4 days, after which the mixture was flushed with argon. The catalyst was removed by vacuum filtration of the molten mixture through 415 filter paper and then through 589 / 3 filter paper. The hydrogenated tall oil acid obtained (yield 90 g) had an iodine value of 54 g (I2) / 100 g and a melting point of 53° C.-55° C.

[0270] A blend of hydrogenated tall oil and hydrogenated rapeseed oil was prepared as follows: rapeseed wax (42.7 g) and tall oil wax (2.3 g) were weighed in a glass beaker and allowed to melt at 100°C. To the liquefied wax blend, 0.9 g of KOH (50%) solution was added and allowed to stir at 90°C for 60 minutes. In a separate beaker, 1.5% (26 g) of beet MFC dispersion (prepared according to WO 2022 / 003252, in particular Sample 3C of Example 3) was heated to 80°C. An emulsion was prepared by pouring the aqueous phase containing MFC into the wax at one time and mixing for 60 seconds using a high shear mixer (Ultra-Turrax 12 krpm). The obtained emulsion was diluted and cooled by pouring it into 137 g of cold water containing 0.13% polyvinyl alcohol (Kuraray, Poval 8-88), and allowed to stir. CaCl was then added 2 (2.94%, 13.5 g) solution while high shear mixing (17000 rpm, 180 W) to obtain fatty calcium salt. The obtained dispersion can be used as a hydrophobic coating.

[0271] Example 13 - Order of adding MFC

[0272] Hydrogenated rapeseed wax (300 g) was weighed in a glass beaker and allowed to melt at 100°C. To the liquefied wax was added 0.27 g of citric acid hydrate followed by 24.0 g of KOH (50%) solution and allowed to stir at 90°C for 120 minutes. In a separate beaker, 173 g of a 3% solution of polyvinyl alcohol (Poval 8-88) was heated to 80°C. A wax dispersion was prepared by pouring the polymer solution into the wax in one go and mixing using a high shear mixer (Ultra-Turrax 12 krpm) for 60 seconds and further diluting with cold water (2330 g) containing 0.129% polyvinyl alcohol (Poval 8-88) and high shear mixing (17000 rpm, 180 W) for 60 seconds. The wax dispersion obtained had a maximum particle size of 3 μm and a concentration of about 11%. To 2584 g of the obtained dispersion was added CaCl under high shear mixing. 2 1.06%, 363g of solution.

[0273] To 200 g of the obtained wax dispersion, 16.2 g of 7% microfibrillated cellulose (prepared according to WO2017 / 103329, see Example E, sample 202.2) was added and mixed with high shear mixing to obtain a wax dispersion containing microfibrillated cellulose having good water and oil barrier properties.

[0274] Example 14 - Order of adding MFC

[0275] Hydrogenated rapeseed wax (300 g) was weighed in a glass beaker and allowed to melt at 100° C. 0.27 g of citric acid hydrate was added to the liquefied wax, followed by 24.0 g of KOH (50%) solution, and allowed to stir at 90° C. for 120 minutes. In a separate beaker, 173 g of a 3% polyvinyl alcohol solution (Poval 8-88) and 1% microfibrillated cellulose (prepared according to WO 2017 / 103329, see Example E, Sample 202.2) were heated to 80° C. The emulsion was prepared by pouring the aqueous phase immediately into the wax and mixing using a high shear mixer (17000 rpm, 180 W) for 60 seconds, and further diluted with cold water (2300 g) containing 0.129% of polyvinyl alcohol (Poval 8-88) and high shear mixing (17000 rpm, 180 W) for 60 seconds to obtain a wax dispersion with a maximum particle size of 3 μm and a concentration of about 11%. To 2580 g of the obtained dispersion was added CaCl under high shear mixing. 2 1.06%, 360 g of solution. The wax dispersion obtained gave good water and oil barrier properties.

[0276] Embodiment 15

[0277] Various additives were tested on the wax dispersion to study their effect on enhancing the oil barrier properties while maintaining the original water resistance. The wax dispersion was prepared by a standard protocol with a maximum particle size of 2 μm and a concentration of 10 wt %:

[0278] Briefly, 200 g of wax dispersion was weighed in a PP container and the additives (Table 1) were mixed under magnetic stirring for a few minutes, followed by high shear mixing (17000 rpm 180w) 3 times with an interval of 10 seconds. For coating tests, the obtained wax mixture was applied on a box plate to obtain 5-10 g / m 2 The samples were placed in an oven at 109°C for 1-2 minutes and then allowed to cool to room temperature. A drop of water or rapeseed oil was placed on the coating and allowed to sit for 30 minutes before visual inspection. All additives tested gave both oil and water resistance. Adding clay or talc is also useful for increasing the dry matter content of the wax mixture.

[0279] Table 1. Various additives tested and their dry composition in the mixture. MFC: microfibrillated cellulose from alkali treated, washed and bleached beet pulp (prepared according to WO2017 / 103329, see Example E, sample 202.2). CNF: cellulose nanofibrils from sulphate derived dissolving pulp (prepared according to WO2018 / 202955, Example 6, sample SUL-2), POVAL: polyvinyl alcohol (Kuraray Poval 8-88). Talc: Elementis Finntalc C15; Kaolin: Imerys Argirec B24.

[0280] entry wax Additive 1 Additive 1 Additive 2 Additive 2 A 99.0% POVAL 1.0% - - B 98.4% CNF 1.6% - - C 94.8% MFC 5.2% - - D 67.6% MFC 1.7% talc 30.7% E 36.8% CNF 0.3% Kaolin 62.9%

[0281] The foregoing description has been provided by way of specific embodiments and non-limiting examples of embodiments, which are comprehensive and informative descriptions of the best modes currently contemplated by the inventors for carrying out the invention. However, it should be clear to those skilled in the art that the invention is not limited to the details of the embodiments provided above, but may be implemented in other embodiments or in different combinations of embodiments using equivalent means without departing from the characteristics of the invention.

Claims

1. A composition comprising: Plant-based waxes; and a fibrillated cellulose component; and The composition is a dispersion of wax particles in an aqueous medium.

2. The composition according to claim 1, wherein the fibrillated cellulose component comprises entangled cellulose microfibril aggregates comprising microfibrils and / or microfibril bundles smaller than 200 μm.

3. The composition according to claim 1 or 2, wherein the plant-based wax comprises triglycerides and / or partially saponified triglycerides, and the plant-based wax is preferably selected from the group consisting of palm wax, palm kernel wax, rapeseed wax, soy wax, corn wax, canola wax, carnauba wax, candelilla wax, cocoa wax, soy wax, coconut wax, cranberry wax, sunflower wax, linseed wax, cottonseed wax, sugarcane wax, bayberry wax, peanut wax or a combination thereof.

4. The composition of claim 1 or 2, wherein the plant-based wax comprises partially hydrogenated tall oil acid or fully hydrogenated tall oil acid.

5. The composition of any one of claims 1-4, wherein the plant-based wax is a blend comprising: triglycerides, preferably selected from the group consisting of palm wax, palm kernel wax, rapeseed wax, soy wax, corn wax, canola wax, carnauba wax, candelilla wax, cocoa wax, soy wax, coconut wax, cranberry wax, sunflower wax, linseed wax, cottonseed wax, sugar cane wax, bayberry wax, peanut wax, or combinations thereof, or any mixture thereof; and At least one of fatty acids, partially hydrogenated tall oil acid, fully hydrogenated tall oil acid, crude tall oil, and distilled tall oil.

6. The composition according to any one of claims 1 to 5, wherein the fibrillated cellulose component is fibrillated parenchyma cellulose.

7. A composition according to any one of claims 1-6, wherein in the fibrillated cellulose component, the amount of cellulose is selected in the range of 50wt% to 70wt% of the dry matter of the fibrillated cellulose component, and the amount of hemicellulose is selected in the range of 30wt% to 50wt% of the dry matter of the fibrillated cellulose component.

8. The composition according to any one of claims 1 to 7, wherein The composition further comprises a multivalent cation, preferably Zn 2+ Mg 2+ , Cu 2+ , Fe 2+ , Fe 3+ 、Al 3+ Sn 2+ , Ca 2+ , fatty acid salts of multivalent cations, or at least one of any combination thereof.

9. The composition according to any one of claims 1 to 8, wherein the composition comprises wax particles having a size less than 20 μm, preferably between 0.1 and 10 μm, most preferably between 0.5 and 8 μm.

10. The composition according to any one of claims 1 to 9, wherein The composition further comprises at least one of the following: a. thermoplastic polymer, polyolefin dispersion, polyester, polyamide, polycaprolactone, polylactic acid, ethylene copolymer, ethylene terpolymer, polyvinyl acetate latex, ethyl vinyl acetate latex, styrene butadiene latex, styrene acrylate latex, acrylate latex, methyl methacrylate latex, or any mixture, copolymer or derivative thereof; b. synthetic wax, polyolefin wax, fatty amide wax, amide wax, inorganic modified wax, oxidized polyethylene wax, or any combination thereof; c. natural, synthetic or semi-synthetic polymers, carboxymethyl cellulose, hydroxypropyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, hydroxyethyl hydroxypropyl cellulose, quaternized hydroxyethyl cellulose, carboxymethyl starch, hydroxypropyl starch, hydroxypropyl methyl starch, hydroxyethyl starch, hydroxyethyl methyl starch, hydroxyethyl hydroxypropyl starch, hydroxypropyltrimethylammonium chloride starch, dextrin, starch, xanthan gum, guar gum, agar, alginate, tyloose, polyvinyl alcohol, polyacrylamide, vinyl acetate copolymers, or any combination thereof; d. nonionic surfactants, cetyl alcohol, stearyl alcohol, cetearyl alcohol, alcohol ethoxylates, polyethylene glycol ethers, polyoxyethylene alkyl ethers, secondary alcohol ethoxylates, polyoxyethylene alkyl ethers, polyalkyl glycol alkyl ethers, esters of pentaerythritol, sugar esters of pentaerythritol, fatty acids, citric acid, fatty acid citrates, fatty alcohols, or any combination thereof; and / or e. Ionic surfactants comprising phosphates, sulfate sulfonates, sulfate carboxylates, sodium lauryl sulfate, ammonium lauryl sulfate, lauryl ether sulfate, lecithin, alkali metal salts of tall oil, or any combination thereof.

11. A solid wet product obtained by subjecting a composition according to any one of claims 1 to 10 to a powder preparation process.

12. A method for preparing a composition according to any one of claims 1 to 10, comprising: Provides plant-based waxes; providing a fibrillated cellulose component; heating the plant-based wax and the fibrillated cellulose component; adding the fibrillated cellulose component to the plant-based wax while continuously mixing; as well as The fibrillated cellulose component and the plant-based wax are mixed until a phase inversion occurs to obtain a dispersion of wax particles in an aqueous medium.

13. A method for preparing a composition according to any one of claims 1 to 10, comprising: Providing a dispersion of a plant-based wax; providing a fibrillated cellulose component; as well as The fibrillated cellulose component is added to the dispersion while continuing mixing to obtain a dispersion of wax particles in an aqueous medium.

14. A method for preparing a liquid dispersion, comprising: Providing a solid wet product according to claim 11; and The solid wet product is diluted in an aqueous medium, or the solid wet product is heated, to obtain the liquid dispersion.

15. A coating formulation comprising the composition according to any one of claims 1 to 10.

16. An article, wherein the article comprises a cellulosic media, and wherein the article comprises at least one coating of the composition of any one of claims 1-10.

17. A food wrapper comprising at least one layer of the composition according to claims 1-10 on at least one side.

18. Use of the composition according to any one of claims 1 to 10 in sizing, internal sizing, paper coating, board coating, barrier coating, hydrophobic coating, oleophobic coating, corrugated board production, gypsum board production, wood board production, hardboard production, softboard production, veneer glued wood production, and / or particle board production.

Citation Information

Cited By

  • Energy storage phase change thermal insulation foam material and preparation method thereof

    CN119875190A

  • Energy storage phase change thermal insulation foam material and preparation method thereof