Resin composition, prepreg, resin sheet, laminate, metal foil-clad laminate, and printed wiring board
By using a resin composition with a surface coating of titanium oxide and thermosetting compounds, the water absorption rate is controlled, solving the problems of high-frequency signal transmission loss and poor manufacturability. This results in an insulating layer with high dielectric constant and low dielectric loss tangent, improving the moisture absorption, heat resistance, and reliability of printed circuit boards.
Patent Information
- Application Number
- CN202380029150.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-08
AI Technical Summary
In existing technologies, high-frequency electrical signal transmission suffers from high loss, deterioration of dielectric properties, and poor manufacturability. Furthermore, printed circuit boards are prone to voids and interlayer delamination during reflow soldering.
A specific resin composition is used, including a surface-coated titanium oxide and a thermosetting compound, to control the water absorption rate to below 0.40%. A surface treatment agent is used to improve dispersibility and adhesion, forming an insulating layer with a high dielectric constant and a low dielectric loss tangent.
An insulating layer with high dielectric constant and low dielectric loss tangent is achieved, which has excellent moisture absorption and heat resistance and low coefficient of thermal expansion, avoiding voids and interlayer delamination during reflow soldering and improving the reliability of printed circuit boards.
Smart Images

Figure BDA0005052281700000041 
Figure BDA0005052281700000042 
Figure BDA0005052281700000043
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, a prepreg, a resin sheet, a laminate, a metal foil-clad laminate and a printed circuit board. Background Art
[0002] In recent years, the signal band of information communication equipment such as PHS and mobile phones, and the CPU clock time of computers have reached the GHz band and are being high-frequencyized. The dielectric loss of an electrical signal is proportional to the square root of the relative dielectric constant of the insulating layer forming the circuit, the dielectric loss tangent, and the product of the frequency of the electrical signal. Therefore, the higher the frequency of the signal used, the greater the dielectric loss will become. Since the increase in dielectric loss will attenuate the electrical signal and damage the reliability of the signal, in order to suppress this situation, the insulating layer needs to select a material with a small dielectric constant and dielectric loss tangent.
[0003] On the other hand, the insulating layer of the high-frequency circuit has requirements such as the formation of a delay circuit, impedance integration of the circuit board in the low-impedance circuit, densification of the wiring pattern, and composite circuitization with a built-in capacitor in the substrate itself, and sometimes there is a situation where the insulating layer is required to have a high dielectric constant. Therefore, some people have proposed electronic components using an insulating layer with a high dielectric constant and a low dielectric loss tangent (for example, patent document 1). The insulating layer with a high dielectric constant and a low dielectric loss tangent is formed by dispersing fillers such as ceramic powder and metal powder that has been subjected to insulation treatment in a resin.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2000-91717 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] However, in order to increase the relative dielectric constant of the insulating layer, it is required to mix a filler with a high relative dielectric constant, but at the same time, the dielectric loss tangent also increases, so there is a problem that the transmission loss of high-frequency signals increases.
[0009] In addition, if the filler and the resin are highly hygroscopic, there is a problem that the dielectric properties and manufacturability of the printed wiring board are deteriorated.
[0010] In addition, if the insulating layer has low hygroscopic heat resistance, the moisture contained in the insulating layer will evaporate during reflow soldering, thereby generating voids, which will cause interlayer delamination during the manufacture of laminated boards. Therefore, in the field of electronic materials that require high reliability, an insulating layer with excellent hygroscopic heat resistance is required.
[0011] Furthermore, if the insulating layer has a low glass transition temperature (Tg) and a high thermal expansion coefficient, warping and interface peeling may occur during the manufacture of the laminate. Therefore, it is also important for the resin composition used in a printed circuit board or the like that the insulating layer obtained has a high glass transition temperature and a low thermal expansion coefficient.
[0012] The present invention is made to solve the above-mentioned problems, and its purpose is to provide a resin composition suitable for producing an insulating layer of a printed wiring board having a high dielectric constant and a low dielectric loss tangent, excellent moisture absorption heat resistance, a high glass transition temperature, and a low thermal expansion coefficient, and a prepreg, a resin sheet, a laminate, a metal foil-clad laminate, and a printed wiring board obtained by using the resin composition.
[0013] Solutions for solving problems
[0014] The present inventors have conducted intensive studies to solve the above-mentioned problems of the prior art and, as a result, have found that a specific resin composition can solve the above-mentioned problems, thereby completing the present invention.
[0015] That is, the present invention is as follows.
[0016] [1] A resin composition comprising a surface-coated titanium oxide (A) and a thermosetting compound (B), wherein the water absorption calculated by the following formula (i) is 0.40% or less.
[0017] Water absorption (%) = [(M2-M1) / M1] × 100… (i)
[0018] (In formula (i), M1 represents: a prepreg having a thickness of 0.1 mm obtained by laminating two sheets of the resin composition impregnated and coated on an E glass cloth having a thickness of 0.094 mm and then heating and drying at 130° C. for 3 minutes, and applying a surface pressure of 30 kgf / cm 2 and temperature 220 ℃ for 120 minutes of vacuum pressing, laminated molding, the laminated plate obtained by drying at 150 ℃ for 1 hour, the mass (g) of the dried laminated plate (a); M2 represents: the mass (g) of the dried laminated plate (a) after moisture absorption treatment at 85 ℃ and 85% RH for 168 hours)
[0019] [2] The resin composition according to [1], wherein the surface-covering titanium oxide (A) has an organic layer and / or an inorganic oxide layer on the surface of titanium oxide particles.
[0020] [3] The resin composition according to [2], wherein the surface-covering titanium oxide (A) further has the organic layer on the surface of the inorganic oxide layer.
[0021] [4] The resin composition according to [2] or [3], wherein the total amount of the organic layer and the inorganic oxide layer is 0.1 to 10% by mass relative to 100% by mass of the surface-covering titanium oxide (A).
[0022] [5] The resin composition according to any one of [2] to [4], wherein the inorganic oxide layer is one or more selected from the group consisting of a layer containing silicon dioxide, a layer containing zirconium oxide, and a layer containing aluminum oxide.
[0023] [6] The resin composition according to any one of [2] to [5], wherein the organic layer is a layer surface-treated with an organic silicon compound.
[0024] [7] The resin composition according to [6], wherein the organosilicon compound includes one or more selected from the group consisting of a silane coupling agent, an organosilane, and an organopolysiloxane.
[0025] [8] The resin composition according to any one of [2] to [7], wherein the content of the titanium oxide in the surface-covering titanium oxide (A) is 90 to 99.9% by mass relative to 100% by mass of the surface-covering titanium oxide (A).
[0026] [9] The resin composition according to any one of [1] to [8], wherein the content of the surface-covering titanium oxide (A) is 50 to 500 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.
[0027]
[10] The resin composition according to any one of [1] to [9], wherein the thermosetting compound (B) comprises one or more selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, cyanate compounds, phenol compounds, alkenyl-substituted nadic imide compounds, oxetane resins, benzoxazine compounds, and compounds having a polymerizable unsaturated group.
[0028]
[11] The resin composition according to
[10] , wherein the maleimide compound comprises one or more selected from the group consisting of bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, a maleimide compound represented by the following formula (1), and a maleimide compound represented by the following formula (2).
[0029]
[0030] (In formula (1), R 1Each independently represents a hydrogen atom or a methyl group, and n1 is an integer of 1 to 10.
[0031]
[0032] (In formula (2), R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, and n2 is an average value and represents 1<n2≤5. )
[0033]
[12] The resin composition according to
[10] or
[11] , wherein the epoxy compound comprises one or more selected from the group consisting of biphenyl aralkyl epoxy resins, naphthalene epoxy resins, and naphthylene ether epoxy resins.
[0034]
[13] The resin composition according to any one of
[10] to
[12] , wherein the modified polyphenylene ether compound includes a compound represented by the following formula (3).
[0035]
[0036] (In formula (3), X represents an aromatic group, -(YO) m - represents a polyphenylene ether portion; R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group; m represents an integer of 1 to 100, n represents an integer of 1 to 6, and q represents an integer of 1 to 4.
[0037]
[14] The resin composition according to any one of
[10] to
[13] , wherein the cyanate compound comprises one or more selected from the group consisting of phenol novolac type cyanate compounds, naphthol aralkyl type cyanate compounds, naphthylene ether type cyanate compounds, xylene resin type cyanate compounds, bisphenol M type cyanate compounds, bisphenol A type cyanate compounds, diallyl bisphenol A type cyanate compounds, bisphenol E type cyanate compounds, bisphenol F type cyanate compounds, biphenyl aralkyl type cyanate compounds, and prepolymers or polymers of these cyanate compounds.
[0038]
[15] The resin composition according to any one of [1] to
[14] , further comprising a filler (C) different from the surface-coating titanium oxide (A).
[0039]
[16] The resin composition according to
[15] , wherein the filler (C) comprises one or more selected from the group consisting of silica, alumina, barium titanate, strontium titanate, calcium titanate, aluminum nitride, boron nitride, boehmite, aluminum hydroxide, zinc molybdate, silicone rubber powder, and silicone composite powder.
[0040]
[17] The resin composition according to
[15] or
[16] , wherein the content of the filler (C) is 50 to 300 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.
[0041]
[18] The resin composition according to any one of [1] to
[17] , which is used for a printed wiring board.
[0042]
[19] A prepreg comprising a substrate and the resin composition according to any one of [1] to
[18] impregnated or coated on the substrate.
[0043]
[20] A resin sheet comprising the resin composition according to any one of [1] to
[18] .
[0044]
[21] A laminate comprising at least one selected from the group consisting of the prepreg described in
[19] and the resin sheet described in
[20] .
[0045]
[22] A metal foil-clad laminate comprising the laminate according to
[21] and a metal foil disposed on one or both surfaces of the laminate.
[0046]
[23] A printed wiring board comprising an insulating layer and a conductor layer disposed on one or both surfaces of the insulating layer, wherein the insulating layer contains a cured product of the resin composition according to any one of [1] to
[18] .
[0047] Effects of the Invention
[0048] According to the resin composition of the present invention, there can be provided a resin composition suitable for use in manufacturing an insulating layer of a printed circuit board having a high dielectric constant and a low dielectric loss tangent and having excellent moisture absorption heat resistance, a high glass transition temperature, and a low thermal expansion coefficient, and a prepreg, a resin sheet, a laminate, a metal foil-clad laminate, and a printed circuit board obtained using the resin composition. DETAILED DESCRIPTION
[0049] The following is a detailed description of a method for implementing the present invention (hereinafter referred to as "this embodiment"). The following this embodiment is an example for illustrating the present invention and is not intended to limit the present invention to the following content. The present invention can be implemented by appropriately deforming within the scope of its purpose.
[0050] In the present embodiment, unless otherwise specified, "resin solid content" or "resin solid content in the resin composition" refers to the resin component after removing the surface-coated titanium oxide (A), filler (C), additives (silane coupling agent, wetting dispersant, curing accelerator, and other components), and solvent (solvent) in the resin composition. "100 parts by mass of the total resin solid content" or "100 parts by mass of the total resin solid content in the resin composition" means that the total of the resin component after removing the surface-coated titanium oxide (A), filler (C), additives (silane coupling agent, wetting dispersant, curing accelerator, and other components), and solvent (solvent) in the resin composition is 100 parts by mass.
[0051] [Resin composition]
[0052] The resin composition of the present embodiment contains a surface-covered titanium oxide (A) and a thermosetting compound (B), and the water absorption calculated by the following formula (i) is 0.40% or less;
[0053] Water absorption (%) = [(M2-M1) / M1] × 100… (i)
[0054] In formula (i), M1 represents: a prepreg having a thickness of 0.1 mm obtained by laminating two sheets of E glass cloth having a thickness of 0.094 mm by impregnation and coating the resin composition, and then heating and drying at 130°C for 3 minutes, and applying a surface pressure of 30 kgf / cm 2 and temperature 220°C for 120 minutes of vacuum pressing to perform lamination molding, and the obtained laminated plate is dried at 150°C for 1 hour, and the mass (g) of the dried laminated plate (a); M2 represents: the mass (g) of the dried laminated plate (a) after moisture absorption treatment at 85°C and 85%RH for 168 hours. It should be noted that the specific measurement and calculation method of water absorption can also refer to the examples.
[0055] According to the resin combination of the present embodiment, it is possible to provide a cured product with high dielectric constant and low dielectric loss tangent, and with excellent moisture absorption heat resistance, high glass transition temperature, and low thermal expansion coefficient. That is, by using the resin combination of the present embodiment, it is possible to suitably manufacture a cured product with high dielectric constant and low dielectric loss tangent, and with excellent moisture absorption heat resistance, high glass transition temperature, and low thermal expansion coefficient prepreg, resin sheet, plywood, metal foil-covered plywood, and printed circuit board. Therefore, the resin combination of the present embodiment can be more suitably used to manufacture the insulating layer of a printed circuit board.
[0056] Especially, the inventors have found that, by using a resin composition containing a surface-covered titanium oxide (A) and a thermosetting compound (B) in the insulating layer of a printed circuit board, and the water absorption calculated by using a specific formula (i) is less than 0.40%, the amount of moisture contained in the insulating layer can be appropriately suppressed during reflow soldering, so it is not easy to produce a gap, and when manufacturing a laminate, it is not easy to cause interlayer peeling. Therefore, according to the present embodiment, a printed circuit board with excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature and excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained. Its reason has not yet been determined, but the inventors infer as follows. Usually, the water absorption of laminates is not only affected by the internal structure of the cured product of the resin composition, but also by the amount of functional groups remaining when not participating in the curing reaction. Therefore, if there are a large number of unreacted functional groups in the insulating layer, functional groups from the resin component after hydrolysis, there will be a tendency for the insulating layer to become higher water absorption. On the other hand, if only reducing these functional groups and increasing the crosslinking density is considered, stress relaxation of the insulating layer will be hindered and the desired physical properties cannot be obtained. However, since the amount of these functional groups is appropriately controlled, the insulating layer whose water absorption is less than 0.40% calculated by the specific formula (i) is not easy to produce voids during reflow soldering and is not easy to cause poor curing. Therefore, it is speculated that the obtained insulating layer can obtain the desired properties. However, the reason is not limited to this.
[0057] From the perspective of obtaining a cured product of a resin composition having a higher dielectric constant and a lower dielectric loss tangent, and having better moisture absorption heat resistance, a higher glass transition temperature, and a lower thermal expansion coefficient, the water absorption calculated using the above formula (i) is preferably 0.39% or less, and more preferably 0.38% or less. In addition, the lower limit of the water absorption is not particularly limited, and is, for example, 0.01% or more.
[0058] The specific method for measuring the water absorption is described in the Examples.
[0059] <Surface coating with titanium oxide (A)>
[0060] The resin composition of the present embodiment contains a surface-coated titanium oxide (A).
[0061] The surface-coated titanium oxide (A) preferably has an organic layer and / or an inorganic oxide layer on the surface of the titanium oxide particles (hereinafter referred to as "titanium oxide particles" or "core particles") that serve as the core of the surface-coated titanium oxide (A). The surface-coated titanium oxide (A) may be used alone or in combination of two or more surface-coated titanium oxides having different particle sizes and surface states.
[0062] From the viewpoint of dispersibility, the average particle size (D50) of the surface-covered titanium oxide (A) is preferably 0.1 to 5 μm, and more preferably 0.15 to 1 μm. It should be noted that in this specification, the average particle size (D50) refers to the value when the volume of a predetermined amount of powder put into a dispersion medium is accumulated from small particles and reaches 50% of the total volume by measuring the particle size distribution using a laser diffraction-scattering particle size distribution measuring device. The average particle size (D50) can be obtained by measuring the particle size distribution using a laser diffraction-scattering method and calculating it. The specific measurement method can be referred to in the examples.
[0063] The shape of the surface-coated titanium oxide (A) is not particularly limited, and may be scaly, spherical, plate-like, or irregular in shape. The shape is preferably spherical in view of having better dispersibility with the thermosetting compound (B) described later, obtaining a resin composition having better hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature, and better dielectric properties (high dielectric constant and low dielectric loss tangent) when cured, and obtaining an insulating layer with more suitable surface hardness.
[0064] The relative dielectric constant of the surface-coated titanium oxide (A) is preferably more than 20, more preferably more than 25. If the relative dielectric constant is more than 20, there is a tendency to obtain an insulating layer with a high relative dielectric constant. It should be noted that the relative dielectric constant of the surface-coated titanium oxide (A) in the present embodiment is a value at 10 GHz measured using a cavity resonator method. In the present embodiment, the relative dielectric constant of the surface-coated titanium oxide (A) can be calculated using the Bruggeman formula (composite rule).
[0065] The dielectric loss tangent of the surface-coated titanium oxide (A) is preferably less than 0.01, more preferably less than 0.008. If the dielectric loss tangent is less than 0.01, there is a tendency to obtain an insulating layer with a low dielectric loss tangent. In addition, in the present embodiment, the dielectric loss tangent of the surface-coated titanium oxide (A) is the value at 10 GHz measured using a cavity resonance method. In the present embodiment, the dielectric loss tangent of the surface-coated titanium oxide (A) can be calculated using Bruggeman's formula (composite rule).
[0066] From the viewpoint that the water absorption of the resin composition can be further suppressed, the adhesion with the resin component can be further improved, the aggregation of the surface-covered titanium oxide (A) in the resin composition can be further alleviated, the dispersibility can be further improved, and a cured product having excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent moisture absorption and heat resistance can be obtained, the total amount (covering amount) of the organic layer and the inorganic oxide layer in the surface-covered titanium oxide (A) is preferably 0.1 to 10% by mass, more preferably 1 to 8% by mass, and even more preferably 1 to 4% by mass relative to 100% by mass of the surface-covered titanium oxide (A).
[0067] From the viewpoint that the water absorption of the resin composition can be further suppressed, the adhesion with the resin component can be further improved, the aggregation of the surface-covering titanium oxide (A) in the resin composition can be further alleviated, the dispersibility can be further improved, and a cured product having excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent moisture absorption heat resistance can be obtained, the content of titanium oxide in the surface-covering titanium oxide (A) is preferably 90 to 99.9% by mass, more preferably 92 to 99% by mass, and further preferably 96 to 99% by mass relative to 100% by mass of the surface-covering titanium oxide (A).
[0068] Examples of the core particles include titanium monoxide (TiO), titanium trioxide (Ti 2 O 3 ) and titanium dioxide (TiO 2 ) etc. Among them, titanium dioxide is preferred. Titanium dioxide preferably has a rutile or anatase crystal structure, and more preferably has a rutile crystal structure.
[0069] From the viewpoint of dispersibility, the average particle size (D50) of the core particles is preferably 0.10 to 0.45 μm, and more preferably 0.15 to 0.25 μm. In the present embodiment, the average particle size (D50) of the core particles is obtained from the average value of the particle sizes of primary particles based on single particles.
[0070] Surface-coated titanium oxide (A) can be obtained by using a surface treatment agent to cover an organic layer or an inorganic oxide layer on the surface of core particles. In addition, on the surface of the organic layer or inorganic oxide layer covering the surface of the core particles, it is also possible to use a surface treatment agent to further cover the organic layer and / or the inorganic oxide layer. Considering the water absorption of the resin composition that is more suppressed, the adhesion with the resin component is further improved, the aggregation of the surface-coated titanium oxide (A) in the resin composition is more relaxed, the dispersibility is further improved, the viewpoint of the cured product with excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent hygroscopic heat resistance can be obtained, the surface-coated titanium oxide (A) preferably has an organic layer further on the surface of the inorganic oxide layer covering the surface of the core particles. As a covering method, inorganic treatment and organic treatment can be cited. Surface treatment agent can be used alone 1, or more than 2 can be used in combination.
[0071] As the surface treatment agent used for inorganic treatment, for example, oxygen-containing acids (such as silicic acid and aluminic acid) of metals such as aluminum, silicon, zirconium, tin, titanium, antimony, zinc, cobalt and manganese, metal salts of oxygen-containing acids (such as sodium silicate and sodium aluminate), oxides, hydroxides and hydrated oxides, etc. The surface-covered titanium oxide (A) obtained by inorganic treatment has an inorganic oxide layer on the surface of the titanium oxide particles, the surface of the inorganic oxide layer, or the surface of the organic layer described later.
[0072] As the surface treatment agent used for organic treatment, for example, organic silicon compounds such as organic silane, silane coupling agent and organic polysiloxane; organic titanium compounds such as titanium coupling agent; organic substances such as organic acid, polyol and alkanolamine, etc. The surface-coated titanium oxide (A) obtained by organic treatment has an organic layer on the surface of titanium oxide particles, the surface of the organic layer, or the surface of the inorganic oxide layer.
[0073] Examples of the organosilane include alkoxysilanes such as n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, octyltrimethoxysilane, decyltrimethoxysilane, 3-chloropropyltriethoxysilane, phenyltriethoxysilane and trifluoropropyltrimethoxysilane.
[0074] Examples of the silane coupling agent include aminosilanes such as 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane; epoxysilanes such as 3-glycidoxypropyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; methacrylic silanes such as 3-(methacryloxypropyl)trimethoxysilane; vinylsilanes such as vinyltrimethoxysilane, vinyltriethoxysilane, and vinyltrichlorosilane; and mercaptosilanes such as 3-mercaptopropyltrimethoxysilane.
[0075] As the organopolysiloxane, silicone oil is preferred from the viewpoint of being able to form a more uniform organic layer. Examples of the silicone oil include alkyl silicone, alkyl hydrogen silicone, alkoxy silicone and modified silicone.
[0076] As an example of the alkyl silicone, dimethyl silicone is mentioned.
[0077] Examples of the alkyl hydrogen silicone include methyl hydrogen silicone and ethyl hydrogen silicone.
[0078] As the alkoxy silicone, an organosilicon compound containing an alkoxysilyl group in which an alkoxy group is directly bonded to a silicon atom or is bonded to a silicon atom via a divalent hydrocarbon group is preferred. As such an organosilicon compound, for example, a linear, cyclic, network, and partially branched linear organopolysiloxane can be cited. Among them, a linear organopolysiloxane is preferred, and an organopolysiloxane having a molecular structure in which an alkoxy group is directly bonded to the organosilicon main chain is more preferred. As the alkoxy silicone, for example, a methoxy silicone and an ethoxy silicone can be cited.
[0079] Examples of the modified silicone include amino-modified silicone, epoxy-modified silicone, and mercapto-modified silicone.
[0080] Examples of the titanium coupling agent include isopropyl triisostearoyl titanate, isopropyl dimethacryloyl isostearyl titanate, and isopropyl tridodecylbenzenesulfonyl titanate.
[0081] Examples of the organic acid include adipic acid, terephthalic acid, lauric acid, myristic acid, palmitic acid, stearic acid, polyhydroxystearic acid, oleic acid, salicylic acid, malic acid, maleic acid, and metal salts thereof.
[0082] Examples of the polyol include trimethylolethane, trimethylolpropane, di(trimethylol)propane, ethoxylated trimethylolpropane, and pentaerythritol.
[0083] Examples of the alkanolamine include monoethanolamine, monopropanolamine, diethanolamine, dipropanolamine, triethanolamine, and tripropanolamine.
[0084] From the viewpoint of having better dispersibility with the thermosetting compound (B), obtaining a resin composition having better moisture absorption heat resistance, low thermal expansion coefficient, high glass transition temperature and better dielectric properties (high dielectric constant and low dielectric loss tangent) when cured, and further obtaining an insulating layer with more suitable surface hardness, the surface-coated titanium oxide (A) preferably has an inorganic oxide layer on the surface of the titanium oxide particles, and the inorganic oxide layer is one or more selected from the group consisting of a layer containing silicon dioxide, a layer containing zirconium oxide, and a layer containing aluminum oxide. More preferably, the inorganic oxide layer is one or more selected from the group consisting of a layer containing silicon dioxide and a layer containing aluminum oxide.
[0085] The surface-coated titanium oxide (A) may also have two or more inorganic oxide layers. When having two or more inorganic oxide layers, it is preferably configured as follows: the inorganic oxide layer located near the titanium oxide particle side can mainly further suppress the water absorption caused by the core particle, i.e., the titanium oxide particle, and the inorganic oxide layer located far from the titanium oxide particle side can mainly improve the adhesion with the resin component, the aggregation relaxation of the surface-coated titanium oxide (A) in the resin composition, and the dispersibility.
[0086] From such a viewpoint, when the surface-covered titanium oxide (A) has two or more inorganic oxide layers, it is preferred that the inorganic oxide layer located on the side close to the core particle is one or more selected from the group consisting of a layer containing silicon dioxide and a layer containing zirconium oxide, and the inorganic oxide layer located on the side away from the core particle is a layer containing aluminum oxide, and it is more preferred that the inorganic oxide layer located on the side close to the core particle is a layer containing silicon dioxide, and the inorganic oxide layer located on the side away from the core particle is a layer containing aluminum oxide.
[0087] From the viewpoint of being able to further suppress the water absorption of the resin composition and having excellent heat resistance of the cured product, the total amount of the inorganic oxide layer is preferably 0.1 to 10 mass %, more preferably 0.3 to 7.5 mass %, further preferably 0.4 to 5.0 mass %, and further preferably 0.5 to 4.0 mass %, relative to 100 mass % of the surface-covered titanium oxide (A).
[0088] The inorganic oxide layer has the effect of suppressing the water absorption of the core particles, i.e., titanium oxide. On the other hand, silicon dioxide, zirconium oxide, and aluminum oxide, which are inorganic oxides, are hydrated inorganic substances, so there is a tendency that the water absorption rate is higher among the inorganic oxides and the water evaporates easily in the reflow soldering. The evaporated water can become the cause of the voids in the insulating layer. From such a viewpoint, the surface-coated titanium oxide (A) preferably has an organic layer on the surface of the inorganic oxide layer. The organic layer can further reduce the water absorption of the core particles, i.e., titanium oxide and the inorganic oxide layer, and further suppress the water absorption of the resin composition. Therefore, the evaporation of water from the insulating layer can be suppressed in the reflow soldering. In addition, the organic layer can also play the effect of making the aggregation of the surface-coated titanium oxide (A) in the resin composition more moderate and improving the dispersibility.
[0089] The organic layer is preferably a layer surface-treated with an organic silicon compound from the viewpoint of further alleviating aggregation of the surface-coating titanium oxide (A) in the resin composition, further improving dispersibility, and reducing the water absorption of the laminate due to better water repellency.
[0090] As the organosilicon compound, it is preferred to include more than one selected from the group consisting of a silane coupling agent, an organosilane, and an organopolysiloxane. By using these surface treatment agents to carry out surface treatment, the obtained organic layer becomes a layer with a siloxane structure. The layer with a siloxane structure has the tendency to further alleviate the aggregation of the surface-covered titanium oxide (A) in the resin composition, further improve dispersibility, and reduce the water absorption rate of the laminate due to more excellent water repellency. In addition, from the viewpoint of being able to form a layer with a more uniform siloxane structure and further exerting the above-mentioned effect, the organopolysiloxane is preferably silicone oil, and among the silicone oils, dimethyl silicone is more preferably used. It should be noted that if the organic layer becomes a layer with a siloxane structure at this time, a surface treatment agent other than the above-mentioned can also be used.
[0091] From the viewpoint of further alleviating aggregation of the surface-covering titanium oxide (A) in the resin composition and further improving dispersibility, the total amount of the organic layer is preferably 0.1 to 10% by mass, more preferably 0.5 to 7.5% by mass, further preferably 0.6 to 6.0% by mass, and further preferably 0.7 to 5.0% by mass, relative to 100% by mass of the surface-covering titanium oxide (A).
[0092] When the surface-coated titanium oxide (A) has an inorganic oxide layer and an organic layer, the covering layer of the surface-coated titanium oxide (A) can also be a 2-layer structure of an inorganic oxide layer and an organic layer. By being set to such a layer structure, the catalytic activity (such as photocatalytic activity and metal catalytic activity) of titanium oxide can be exerted and the effect of water repellency. At this time, as an inorganic oxide layer, it is preferably selected from one or more of the group consisting of a layer comprising silicon dioxide, a layer comprising zirconium oxide, and a layer comprising aluminum oxide, from the viewpoint of further improving the affinity with the resin and further suppressing the catalytic activity of titanium oxide, more preferably a layer comprising aluminum oxide. From the viewpoint of excellent heat resistance and chemical stability, the organic layer preferably has a siloxane structure. By using such a surface-covered titanium oxide (A), the water absorption of the resin composition can be further suppressed, and the adhesion with the resin component can be further improved. The aggregation of the surface-covered titanium oxide (A) in the resin composition can be further alleviated, and the dispersibility with the thermosetting compound (B) can be further improved. A resin composition having further excellent moisture absorption heat resistance, a low thermal expansion coefficient, and a high glass transition temperature during curing, as well as further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained, and an insulating layer having a more suitable surface hardness can be obtained.
[0093] Such a surface-coated titanium oxide (A) can be a commercially available product, and examples of the commercially available product include R-22L, R-11P, and R-39 (these are trade names, Sakai Chemical Industry Co., Ltd.).
[0094] When the surface-covered titanium oxide (A) has an inorganic oxide layer and an organic layer, it is preferred that the inorganic oxide layer located near the core particle side is a layer comprising silicon dioxide, and the inorganic oxide layer is a layer comprising aluminum oxide, and the organic layer located at the farthest side from the core particle is a layer having a siloxane structure. By using such a surface-covered titanium oxide (A), the water absorption of the resin composition can be further suppressed, and the adhesion with the resin component can be further improved, and the aggregation of the surface-covered titanium oxide (A) in the resin composition can be further alleviated, and the thermosetting compound (B) has further good dispersibility, and a resin composition having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature, and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when curing, and then an insulating layer with further suitable surface hardness can be obtained.
[0095] As such a surface-coating titanium oxide (A), a commercially available product can be used. Examples of the commercially available product include CR-63 (trade name, Ishihara Sangyo Co., Ltd.).
[0096] The content of the surface-coated titanium oxide (A) is preferably 50 to 500 parts by mass, more preferably 60 to 450 parts by mass, and further preferably 70 to 400 parts by mass relative to a total of 100 parts by mass of the resin solid component in the resin composition. By making the content of the surface-coated titanium oxide (A) within the above range, there is a tendency to obtain a resin composition having further good dispersibility with the thermosetting compound (B), further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature, and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when cured, and further to obtain an insulating layer having a further suitable surface hardness.
[0097] <Thermosetting compound (B)>
[0098] The resin composition of the present embodiment contains a thermosetting compound (B).
[0099] The thermosetting compound (B) is not particularly limited as long as it is a thermosetting compound or resin. The thermosetting compound or resin may be used alone or in combination of two or more.
[0100] From the viewpoint of having further good dispersibility with the surface-covered titanium oxide (A), and obtaining a resin composition having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature, and more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when cured, the thermosetting compound (B) preferably includes one or more thermosetting compounds or resins (hereinafter also referred to as "thermosetting resins") selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, cyanate compounds, phenol compounds, alkenyl substituted nadic imide compounds, oxetane resins, benzoxazine compounds, and compounds having polymerizable unsaturated groups. These thermosetting resins can be used alone or in combination of two or more.
[0101] From the viewpoint of having further good dispersibility with the surface-covered titanium oxide (A), and being able to obtain a resin composition having further excellent moisture absorption heat resistance, low thermal expansion coefficient, and high glass transition temperature when cured, as well as further excellent dielectric properties (high dielectric constant and low dielectric loss tangent), the thermosetting compound (B) more preferably contains one or more selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, cyanate compounds, phenol compounds, and compounds having a polymerizable unsaturated group, and more preferably one or more selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, and cyanate compounds.
[0102] Surface-coated titanium oxide (A) can suitably suppress the electrophilicity produced by Lewis acidity possessed by titanium oxide by being covered by the surface. Therefore, in resin combination, even if surface-coated titanium oxide (A) and thermosetting compound (B) are close, the polymerization of thermosetting compound (B) will not be carried out intentionally, and poor curing can be prevented. In addition, surface-coated titanium oxide (A) can also suitably suppress the hydrolysis for thermosetting compound (B) by being covered by the surface, and therefore the amount of unreacted functional groups in the insulating layer can be reduced. Therefore, according to the resin combination of the present embodiment, the amount of moisture contained in the insulating layer during reflow can be suitably suppressed, so it is not easy to produce space, and when the manufacture of laminated board, it is not easy to cause interlayer peeling. From the viewpoint of further suppressing the progress of polymerization and hydrolysis, thereby obtaining a resin composition having further excellent moisture absorption heat resistance, low thermal expansion coefficient, and high glass transition temperature, as well as further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when cured, the thermosetting compound (B) further preferably contains one or more selected from the group consisting of maleimide compounds and cyanate ester compounds.
[0103] From the viewpoint of further well dispersing the surface-coated titanium oxide (A) and obtaining a resin composition having further excellent moisture absorption heat resistance, low thermal expansion coefficient, high glass transition temperature and dielectric properties (low dielectric loss tangent) when cured, the mass ratio of the surface-coated titanium oxide (A) to the thermosetting compound (B) (surface-coated titanium oxide (A): thermosetting compound (B)) is preferably 30:70 to 90:10, more preferably 35:65 to 85:15, and even more preferably 40:60 to 80:20.
[0104] (Maleimide compound)
[0105] From the viewpoint of the resin composition of the surface-covered titanium oxide (A) further well dispersed, can obtain when solidifying, there is further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent), the resin composition of the present embodiment preferably includes maleimide compounds. In addition, from the aspect of the inhibition effect of the polymerization based on the surface-covered titanium oxide (A) more significantly obtained and hydrolyzed, also preferably maleimide compounds. And then, if resin composition contains maleimide compounds, the water absorption of resin composition can be further suppressed, there is the adhesion with the surface-covered titanium oxide (A) more improved, can more relax the aggregation of the surface-covered titanium oxide (A) in the resin composition, improve dispersibility more, can obtain the tendency of the cured product with excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent hygroscopic heat resistance.
[0106] If the maleimide compound is a compound having one or more maleimide groups in one molecule, a known maleimide compound can be used appropriately, and its type is not particularly limited. The number of maleimide groups in one molecule of the maleimide compound is 1 or more, preferably 2 or more. One maleimide compound can be used alone, or two or more maleimide compounds can be used in combination.
[0107] Examples of the maleimide compound include N-phenylmaleimide, N-hydroxyphenylmaleimide, bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane, bis(3,5-dimethyl-4-maleimidephenyl)methane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, bis(3,5-diethyl-4-maleimidephenyl)methane, the maleimide compound represented by formula (1), the maleimide compound represented by formula (2), prepolymers of these maleimide compounds, and prepolymers of the above maleimide compounds and amine compounds.
[0108] Among them, the maleimide compound preferably contains one or more selected from the group consisting of bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, the maleimide compound represented by formula (1) and the maleimide compound represented by formula (2), and more preferably contains one or more selected from the group consisting of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane and the maleimide compound represented by formula (2), from the viewpoint that the surface-coated titanium oxide (A) is further well dispersed, a resin composition having further excellent moisture absorption heat resistance, low thermal expansion coefficient, and high glass transition temperature during curing, and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained, and further an insulating layer having further suitable surface hardness can be obtained. Furthermore, when the resin composition contains these maleimide compounds, there is a tendency that the water absorption of the resin composition is further suppressed, the adhesion with the surface-coated titanium oxide (A) is further improved, the aggregation of the surface-coated titanium oxide (A) in the resin composition can be further alleviated, the dispersibility is further improved, and a cured product having excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent moisture absorption heat resistance can be obtained.
[0109]
[0110] In formula (1), R 1 Each independently represents a hydrogen atom or a methyl group, and n1 is an integer of 1-10.
[0111]
[0112] In formula (2), R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, and n2 is an average value and 1 <n2≤5。
[0113] The content of the maleimide compound is preferably 10 to 85 parts by mass, more preferably 15 to 80 parts by mass, further preferably 20 to 75 parts by mass, further preferably 25 to 70 parts by mass, and further preferably 20 to 60 parts by mass relative to a total of 100 parts by mass of the resin solid component in the resin composition. By making the content of the maleimide compound within the above range, there is a tendency that the surface-coated titanium oxide (A) is further well dispersed, a resin composition having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature, and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when curing, and an insulating layer having further suitable surface hardness can be obtained. By setting the content of the maleimide compound within the above range, there is a tendency that the water absorption of the resin composition can be further suppressed, the adhesion with the surface-coated titanium oxide (A) can be further improved, the aggregation of the surface-coated titanium oxide (A) in the resin composition can be further alleviated, the dispersibility can be further improved, and a cured product having excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent moisture absorption heat resistance can be obtained.
[0114] The maleimide compound may be a commercial product or a product manufactured by a known method. Examples of commercial products of the maleimide compound include BMI-70, BMI-80 and BMI-1000P (the above are trade names, K.I. Chemical Industry Co., Ltd.); BMI-3000, BMI-4000, BMI-5100, BMI-7000 and BMI-2300 (the maleimide compound represented by the above formula (1), wherein R 1 All of them are hydrogen atoms, and n1 is an integer of 1 to 5) (the above are trade names, Yamato Chemical Industry Co., Ltd.); MIR-3000-70MT (trade name, the maleimide compound represented by the above formula (2), in which R 2 All are hydrogen atoms, n2 is an average value, and 1<n2≤5. Nippon Kayaku Co., Ltd.) etc.
[0115] (Epoxides)
[0116] From the viewpoint of the resin composition of the surface-covered titanium oxide (A) further well dispersed, having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when solidified, the resin composition of the present embodiment preferably contains epoxy compounds. And then, if the resin composition contains epoxy compounds, there is the tendency of the cured product that can suppress the water absorption of the resin composition more, improve the adhesion with the surface-covered titanium oxide (A), alleviate the aggregation of the surface-covered titanium oxide (A) in the resin composition more, improve dispersibility more, obtain excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent hygroscopic heat resistance.
[0117] If the epoxy compound is a compound having one or more epoxy groups in one molecule, a known epoxy compound can be used appropriately, and its type is not particularly limited. The number of epoxy groups per one molecule of the epoxy compound is 1 or more, preferably 2 or more. The epoxy compound can be used alone or in combination of two or more.
[0118] As the epoxy compound, conventionally known epoxy compounds and epoxy resins can be used. For example, biphenyl aralkyl epoxy resins, naphthalene epoxy resins, binaphthalene epoxy resins, multifunctional phenol epoxy resins, naphthylene ether epoxy resins, phenol aralkyl epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, xylene novolac epoxy resins, naphthalene skeleton modified novolac epoxy resins, dicyclopentadiene novolac epoxy resins, biphenyl novolac epoxy resins, phenol aralkyl novolac epoxy resins, naphthol aralkyl novolac epoxy resins, aralkyl novolac epoxy resins, aromatic hydrocarbon formaldehyde epoxy compounds, anthraquinone epoxy compounds, anthracene epoxy resins, naphthol aralkyl novolac epoxy resins, Oxygen compounds, dicyclopentadiene type epoxy resins, Xylok type epoxy compounds, bisphenol A type epoxy resins, bisphenol E type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol A novolac type epoxy resins, phenol type epoxy compounds, biphenyl type epoxy resins, aralkyl novolac type epoxy resins, triazine skeleton epoxy compounds, triglycidyl isocyanurate, alicyclic epoxy resins, polyol type epoxy resins, glycidyl amine, glycidyl ester resins, compounds obtained by epoxidizing double bonds of compounds containing double bonds such as butadiene, and compounds obtained by reacting hydroxyl-containing silicone resins with epichlorohydrin, etc.
[0119] Among them, from the viewpoint of making the surface-covered titanium oxide (A) further well dispersed, having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) resin composition when curing, epoxy compound preferably includes more than one selected from the group consisting of biphenyl aralkyl epoxy resin, naphthalene type epoxy resin and naphthylene ether type epoxy resin, more preferably including naphthalene type epoxy resin.And then, if resin composition contains these epoxy compounds, there is the tendency of the cured product that can suppress the water absorption of resin composition more, the adhesion with the surface-covered titanium oxide (A) is further improved, the aggregation of the surface-covered titanium oxide (A) in the resin composition can be further eased, dispersibility can be further improved, and excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent hygroscopic heat resistance can be obtained.
[0120] As the naphthalene type epoxy resin, commercially available products may be used, and examples thereof include EPICLON (registered trademark) EXA-4032-70M and EPICLON (registered trademark) HP-4710 (these are trade names, manufactured by DIC Corporation).
[0121] Relative to the total 100 parts by mass of the resin solids in the resin composition, the content of epoxy compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and further preferably 10 to 30 parts by mass. By making the content of epoxy compound in the above-mentioned range, there is a tendency of more excellent adhesion and flexibility. By making the content of epoxy compound in the above-mentioned range, there is a tendency of more suppressing the water absorption of the resin composition, improving the adhesion with the surface-covered titanium oxide (A), alleviating the aggregation of the surface-covered titanium oxide (A) in the resin composition, improving dispersibility, obtaining a cured product with excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent hygroscopic heat resistance.
[0122] (Modified polyphenylene ether compound)
[0123] From the viewpoint of the resin composition of the surface-covered titanium oxide (A) further well dispersed, the dielectric properties (high dielectric constant and low dielectric loss tangent) further excellent in the time of solidification, the resin composition of the present embodiment preferably includes a modified polyphenylene ether compound. In addition, if the resin composition contains a modified polyphenylene ether compound, there is the tendency of the cured product that can suppress the water absorption of the resin composition more, improve the adhesion of the surface-covered titanium oxide (A) more, relax the aggregation of the surface-covered titanium oxide (A) in the resin composition more, improve dispersibility more, obtain excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent hygroscopic heat resistance.
[0124] In this specification, the "modification" of the modified polyphenylene ether compound means that part or all of the ends of the polyphenylene ether compound are substituted with reactive functional groups such as carbon-carbon unsaturated double bonds. For the modified polyphenylene ether compound, as long as part or all of the ends of the polyphenylene ether compound are modified, known ones can be used appropriately without particular limitation. The modified polyphenylene ether compound can be used alone or in combination of two or more.
[0125] Examples of the polyphenylene ether compound as the modified polyphenylene ether compound include polymers containing at least one structural unit selected from the group consisting of the structural unit represented by formula (4), the structural unit represented by formula (5), and the structural unit represented by formula (6).
[0126]
[0127] In formula (4), R 8 , R 9 , R 10 and R 11 Each independently represents an alkyl group having 6 or less carbon atoms, an aryl group, a halogen atom or a hydrogen atom.
[0128]
[0129] In formula (5), R 12 , R 13 , R 14 , R 18 , R 19 Each independently represents an alkyl group having 6 or less carbon atoms or a phenyl group. 15 , R 16 , R 17 Each independently represents a hydrogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group.
[0130]
[0131] In formula (6), R20 , R 21 , R 22 , R 23 , R 24 , R 25 , R 26 , R 27 Each independently represents a hydrogen atom, an alkyl group having no greater than 6 carbon atoms, or a phenyl group. -A- represents a linear, branched, or cyclic divalent hydrocarbon group having no greater than 20 carbon atoms.
[0132] Examples of -A- in formula (6) include divalent organic groups such as methylene, ethylidene, 1-methylethylidene, 1,1-propylidene, 1,4-phenylenebis(1-methylethylidene), 1,3-phenylenebis(1-methylethylidene), cyclohexylidene, phenylmethylene, naphthylmethylene, and 1-phenylethylidene, but are not limited thereto.
[0133] Preferred modified polyphenylene ether compounds include, for example, polyphenylene ether compounds in which a part or all of the terminals are modified with functional groups such as vinylbenzyl groups or other ethylenically unsaturated groups, epoxy groups, amino groups, hydroxyl groups, mercapto groups, carboxyl groups, methacryl groups, and silyl groups.
[0134] As a modified polyphenylene ether compound having a hydroxyl group at the end, SA90 (trade name, SABIC INNOVATIVE PLASTICS CO., LTD.) etc. are mentioned, for example.
[0135] As a modified polyphenylene ether compound having a methacryloyl group at the end, SA9000 (trade name, SABIC INNOVATIVE PLASTICS CO., LTD.) etc. are mentioned, for example.
[0136] The method for producing the modified polyphenylene ether compound is not particularly limited as long as the effects of the present invention can be obtained. For example, the modified polyphenylene ether compound can be produced by the method described in Japanese Patent No. 4591665.
[0137] The modified polyphenylene ether compound more preferably includes a modified polyphenylene ether compound having an ethylenically unsaturated group at the terminal. Examples of the ethylenically unsaturated group include alkenyl groups such as vinyl, allyl, acryloyl, methacryloyl, propenyl, butenyl, hexenyl, and octenyl; cycloalkenyl groups such as cyclopentenyl and cyclohexenyl; and alkenylaryl groups such as vinylbenzyl and vinylnaphthyl. Among them, vinylbenzyl is preferred.
[0138] The terminal ethylenically unsaturated group may be one or more and may be the same functional group or different functional groups.
[0139] From the viewpoint that the surface-covered titanium oxide (A) is further well dispersed, and a resin composition having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when solidified, the modified polyphenylene ether compound having an ethylenically unsaturated group at the end is preferably a compound shown in formula (3). In addition, if the resin composition contains the compound shown in formula (3), there is a tendency that the water absorption of the resin composition can be further suppressed, the adhesion with the surface-covered titanium oxide (A) can be further improved, the aggregation of the surface-covered titanium oxide (A) in the resin composition can be further alleviated, the dispersibility can be further improved, and the cured product having excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent hygroscopic heat resistance can be obtained.
[0140]
[0141] In formula (3), X represents an aromatic group, -(YO) m - represents a polyphenylene ether moiety. 1 , R 2 , R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group. m represents an integer of 1 to 100, n represents an integer of 1 to 6, and q represents an integer of 1 to 4. m is preferably an integer of 1 to 50, and more preferably an integer of 1 to 30. In addition, n is preferably an integer of 1 to 4, and more preferably 1 or 2, and 1 is ideal. In addition, q is preferably an integer of 1 to 3, and more preferably 1 or 2, and 2 is ideal.
[0142] Examples of the aromatic group represented by X in formula (3) include a group obtained by removing q hydrogen atoms from one ring structure selected from a benzene ring structure, a biphenyl ring structure, an indene ring structure, and a naphthalene ring structure (e.g., a phenylene group, a biphenylene group, an indenylene group, and a naphthylene group). Among them, a biphenylene group is preferred.
[0143] Here, the aromatic group represented by X may include a diphenyl ether group in which an aryl group is bonded via an oxygen atom, a benzophenone group in which an aryl group is bonded via a carbonyl group, a 2,2-diphenylpropane group in which an aryl group is bonded via an alkylene group, and the like.
[0144] In addition, the aromatic group may be substituted with a common substituent such as an alkyl group (preferably an alkyl group having 1 to 6 carbon atoms, particularly a methyl group), an alkenyl group, an alkynyl group, a halogen atom, etc. However, since the aromatic group is substituted on the polyphenylene ether portion via an oxygen atom, the limit of the number of common substituents depends on the number of polyphenylene ether portions.
[0145] As the polyphenylene ether portion in formula (3), the structural unit represented by formula (4), the structural unit represented by formula (5), and the structural unit represented by formula (6) can be used. Among them, it is more preferable to contain the structural unit represented by formula (4).
[0146] In addition, as the modified polyphenylene ether compound represented by formula (3), the number average molecular weight is preferably 500 or more and 7000 or less. In addition, a modified polyphenylene ether compound having a minimum melt viscosity of 50000 Pa·s or less in formula (3) can be used. From the viewpoint that the surface-coated titanium oxide (A) is further well dispersed, and a resin composition having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature, as well as further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained during curing, a modified polyphenylene ether compound having a number average molecular weight of 1000 or more and 7000 or less and a minimum melt viscosity of 50000 Pa·s or less in formula (3) is more preferred.
[0147] The number average molecular weight is measured using a gel permeation chromatograph according to a predetermined method. The number average molecular weight is more preferably 1,000 or more and 3,000 or less.
[0148] The minimum melt viscosity is measured using a dynamic viscoelasticity measuring apparatus according to a predetermined method. The minimum melt viscosity is more preferably 500 Pa·s or more and 50000 Pa·s or less.
[0149] As the modified polyphenylene ether compound, in the formula (3), a compound represented by the following formula (7) is preferred.
[0150]
[0151] In formula (7), X is an aromatic group, -(YO) m - each represents a polyphenylene ether moiety, and m represents an integer of 1 to 100. m is preferably an integer of 1 to 50, and more preferably an integer of 1 to 30.
[0152] X, -(YO) in formula (7) m -, and m have the same meanings as in formula (3).
[0153] Preferably, X in formula (3) and formula (7) is formula (8), formula (9) or formula (10), and -(YO) in formula (3) and formula (7) m -and-(OY) m - a structure in which the compounds of formula (11) or formula (12) are arranged, or a structure in which the compounds of formula (11) and formula (12) are arranged in blocks or randomly.
[0154]
[0155] In formula (9), R 28 , R 29 , R 30 and R 31 Each independently represents a hydrogen atom or a methyl group. -B- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.
[0156] As specific examples of -B-, the same ones as the specific examples of -A- in formula (6) can be mentioned.
[0157]
[0158] In the formula (10), -B- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.
[0159] As specific examples of -B-, the same ones as the specific examples of -A- in formula (6) can be mentioned.
[0160]
[0161] The method for producing the modified polyphenylene ether compound having the structure represented by formula (7) is not particularly limited, and it can be produced, for example, by vinylbenzyl etherifying the terminal phenolic hydroxyl group of a bifunctional phenylene ether oligomer obtained by oxidative coupling of a bifunctional phenol compound and a monofunctional phenol compound.
[0162] In addition, such modified polyphenylene ether compounds can use commercially available products, for example, OPE-2St1200 (in formula (7), X in -(OXO)- is the structure represented by formula (8), and -(OY)- and -(YO)- are polymerized from the structure of formula (11)) and OPE-2st2200 (in formula (7), X in -(OXO)- is the structure represented by formula (8), and -(OY)- and -(YO)- are polymerized from the structure of formula (11)) (the above are trade names, Mitsubishi Gas Chemical Co., Ltd.) can be preferably used.
[0163] Relative to a total of 100 parts by mass of the resin solids in the resin composition, the content of the modified polyphenylene ether compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and further preferably 10 to 30 parts by mass. By making the content of the modified polyphenylene ether compound within the above range, there is a tendency for low dielectric loss tangent and reactivity to be further improved. By making the content of the modified polyphenylene ether compound within the above range, there is a tendency for the water absorption of the resin composition to be further suppressed, the adhesion to the surface-coated titanium oxide (A) to be further improved, the aggregation of the surface-coated titanium oxide (A) in the resin composition to be further alleviated, the dispersibility to be further improved, and the cured product with excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent hygroscopic heat resistance to be obtained.
[0164] (Cyanate ester compound)
[0165] From the viewpoint of the resin composition of the surface-covered titanium oxide (A) further well dispersed, the resin composition of the present embodiment preferably includes cyanate compounds, and has further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when solidified. In addition, from the aspect of the inhibition effect of the polymerization and hydrolysis obtained significantly based on the surface-covered titanium oxide (A), cyanate compounds are also preferred. And then, if resin composition includes cyanate compounds, there is the tendency of the cured product that can suppress the water absorption of resin composition more, improve more with the adhesion of the surface-covered titanium oxide (A), can further relax the aggregation of the surface-covered titanium oxide (A) in the resin composition, improve more dispersibility, can obtain the cured product with excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent hygroscopic heat resistance.
[0166] As the cyanate compound, any known cyanate compound can be used as long as it is a compound having two or more cyanato groups (also called "cyanate groups") directly bonded to an aromatic ring in one molecule. The cyanate compound can be used alone or in combination of two or more.
[0167] Examples of such cyanate compounds include phenol novolac type cyanate compounds, cresol novolac type cyanate compounds, naphthalene ring-containing novolac type cyanate compounds, allyl group-containing novolac type cyanate compounds, naphthol aralkyl type cyanate compounds, naphthylene ether type cyanate compounds, xylene resin type cyanate compounds, bisphenol M type cyanate compounds, bisphenol A type cyanate compounds, diallyl bisphenol A type cyanate compounds, bisphenol E type cyanate compounds, bisphenol F type cyanate compounds, biphenyl aralkyl type cyanate compounds, Cyanate compounds, bis(3,3-dimethyl-4-cyanatophenyl)methane, 1,3-dicyanatobenzene, 1,4-dicyanatobenzene, 1,3,5-tricyanatobenzene, 1,3-dicyanatonaphthalene, 1,4-dicyanatonaphthalene, 1,6-dicyanatonaphthalene, 1,8-dicyanatonaphthalene, 2,6-dicyanatonaphthalene, 2,7-dicyanatonaphthalene, 1,3,6-tricyanatonaphthalene, 4,4'-dicyanatobiphenyl, bis(4-cyanatophenyl)ether, bis(4-cyanatophenyl)sulfide and bis(4-cyanatophenyl)sulfone. In addition, these cyanate compounds may be prepolymers or polymers of cyanate compounds.
[0168] Among them, the cyanate compound preferably contains one or more selected from the group consisting of phenol novolac type cyanate compounds, naphthol aralkyl type cyanate compounds, naphthylene ether type cyanate compounds, xylene resin type cyanate compounds, bisphenol M type cyanate compounds, bisphenol A type cyanate compounds, diallyl bisphenol A type cyanate compounds, bisphenol E type cyanate compounds, bisphenol F type cyanate compounds, and biphenyl aralkyl type cyanate compounds, and prepolymers or polymers of these cyanate compounds, and more preferably naphthol aralkyl type cyanate compounds, from the viewpoint that the surface-coated titanium oxide (A) is more well dispersed, a resin composition having more excellent moisture absorption heat resistance, low thermal expansion coefficient, and high glass transition temperature when cured, and more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained, and further, an insulating layer having a more suitable surface hardness can be obtained. Furthermore, when the resin composition contains these cyanate compounds, the water absorption of the resin composition can be further suppressed, the adhesion with the surface-coated titanium oxide (A) can be further improved, the aggregation of the surface-coated titanium oxide (A) in the resin composition can be further alleviated, the dispersibility can be further improved, and there is a tendency that a cured product having excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent moisture absorption heat resistance can be obtained.
[0169] As such a naphthol aralkyl type cyanate ester compound, a compound represented by formula (13) is more preferable.
[0170]
[0171] In formula (13), R 3 Each independently represents a hydrogen atom or a methyl group, and a hydrogen atom is preferred. In formula (13), n3 is an integer greater than or equal to 1, preferably an integer of 1 to 20, and more preferably an integer of 1 to 10.
[0172] As the bisphenol A type cyanate ester compound, one or more selected from the group consisting of 2,2-bis(4-cyanatophenyl)propane and a prepolymer of 2,2-bis(4-cyanatophenyl)propane may be used.
[0173] As such bisphenol A type cyanate compounds, commercially available products can be used, for example, Primaset (registered trademark) BADCy (trade name, Lonza Corporation, 2,2-bis(4-cyanatophenyl)propane, cyanate group equivalent: 139 g / eq.) and CA210 (trade name, Mitsubishi Gas Chemical Co., Ltd., a prepolymer of 2,2-bis(4-cyanatophenyl)propane, cyanate group equivalent: 139 g / eq.).
[0174] These cyanate compounds can also be produced according to known methods. As a specific production method, for example, the method described in Japanese Patent Application Laid-Open No. 2017-195334 (particularly paragraphs 0052 to 0057) can be cited.
[0175] The content of the cyanate compound is preferably 1 to 65 parts by mass, more preferably 2 to 60 parts by mass, further preferably 3 to 55 parts by mass, further preferably 4 to 50 parts by mass, further preferably 5 to 45 parts by mass, and particularly preferably 6 to 40 parts by mass relative to a total of 100 parts by mass of the resin solid component in the resin composition. By making the content of the cyanate compound within the above range, there is a tendency that the surface-coated titanium oxide (A) is further well dispersed, a resin composition having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature, and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) can be obtained when curing, and an insulating layer having further suitable surface hardness can be obtained. Furthermore, by setting the content of the cyanate compound within the above range, the water absorption of the resin composition can be further suppressed, the adhesion with the surface-coated titanium oxide (A) can be further improved, the aggregation of the surface-coated titanium oxide (A) in the resin composition can be further alleviated, the dispersibility can be further improved, and there is a tendency that a cured product having excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and excellent moisture absorption heat resistance can be obtained.
[0176] (Phenol compounds)
[0177] The resin composition of the present embodiment may contain a phenol compound. As long as the phenol compound has two or more phenolic hydroxyl groups in one molecule, any known phenol compound may be used appropriately, and the type thereof is not particularly limited. The phenol compound may be used alone or in combination of two or more.
[0178] Examples of the phenolic compound include cresol novolac type phenolic resins, biphenyl aralkyl type phenolic resins represented by formula (14), naphthol aralkyl type phenolic resins represented by formula (15), aminotriazine novolac type phenolic resins, naphthalene type phenolic resins, phenol novolac resins, alkylphenol novolac resins, bisphenol A type novolac resins, dicyclopentadiene type phenolic resins, Xylok type phenolic resins, terpene-modified phenolic resins, and polyvinylphenols.
[0179] Among them, from the viewpoint of obtaining excellent moldability and surface hardness, the phenol compound preferably contains one or more selected from the group consisting of cresol novolac type phenolic resin, biphenyl aralkyl type phenolic resin represented by formula (14), naphthol aralkyl type phenolic resin represented by formula (15), aminotriazine novolac type phenolic resin and naphthalene type phenolic resin, and more preferably contains one or more selected from the group consisting of biphenyl aralkyl type phenolic resin represented by formula (14) and naphthol aralkyl type phenolic resin represented by formula (15).
[0180]
[0181] In formula (14), R 4 Each independently represents a hydrogen atom or a methyl group, n 4 It is an integer from 1 to 10.
[0182]
[0183] In formula (15), R 5 Each independently represents a hydrogen atom or a methyl group, n 5 It is an integer from 1 to 10.
[0184] The content of the phenolic compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and still more preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When the content of the phenolic compound is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.
[0185] (Alkenyl-substituted nadic imide compound)
[0186] The resin composition of the present embodiment may also contain an alkenyl-substituted nadic imide compound. The alkenyl-substituted nadic imide compound is not particularly limited as long as it is a compound having one or more alkenyl-substituted nadic imide groups in one molecule. The alkenyl-substituted nadic imide compound may be used alone or in combination of two or more.
[0187] Examples of the alkenyl-substituted nadic acid imide compound include compounds represented by the following formula (2d).
[0188]
[0189] In formula (2d), R 1 Each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms (such as a methyl group or an ethyl group), and R 2 It represents an alkylene group having 1 to 6 carbon atoms, a phenylene group, a biphenylene group, a naphthylene group, or a group represented by the formula (16) or (17).
[0190]
[0191] In formula (16), R 3 represents methylene, isopropylidene, CO, O, S or SO 2 .
[0192]
[0193] In formula (17), R 4 Each independently represents an alkylene group having 1 to 4 carbon atoms or a cycloalkylene group having 5 to 8 carbon atoms.
[0194] The alkenyl-substituted nadic acid imide compound represented by formula (2d) may be a commercially available product or a product produced by a known method. Examples of commercially available products include BANI-M and BANI-X (these are trade names, Maruzen Petrochemical Co., Ltd.).
[0195] The content of the alkenyl-substituted nadic acid imide compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and even more preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When the content of the alkenyl-substituted nadic acid imide compound is within the above range, there is a tendency for the adhesiveness, heat resistance, etc. to be more excellent.
[0196] (Oxetane resin)
[0197] The resin composition of the present embodiment may contain an oxetane resin. The oxetane resin is not particularly limited, and a generally known oxetane resin may be used. The oxetane resin may be used alone or in combination of two or more.
[0198] Examples of the oxetane resin include oxetane, 2-methyloxetane, 2,2-dimethyloxetane, 3-methyloxetane, alkyloxetanes such as 3,3-dimethyloxetane, 3-methyl-3-methoxymethyloxetane, 3,3-bis(trifluoromethyl)perfluorooxetane, 2-chloromethyloxetane, 3,3-bis(chloromethyl)oxetane, biphenyl-type oxetane, OXT-101 (trade name, Toagosei Co., Ltd.), and OXT-121 (trade name, Toagosei Co., Ltd.).
[0199] The content of the oxetane resin is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and still more preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When the content of the oxetane resin is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.
[0200] (Benzoxazine compounds)
[0201] The resin composition of the present embodiment may also contain a benzoxazine compound. As the benzoxazine compound, there is no particular limitation as long as it is a compound having two or more dihydrobenzoxazine rings in one molecule, and commonly known benzoxazine compounds can be used. The benzoxazine compound can be used alone or in combination of two or more.
[0202] Examples of the benzoxazine compound include bisphenol A-type benzoxazine BA-BXZ, bisphenol F-type benzoxazine BF-BXZ, and bisphenol S-type benzoxazine BS-BXZ (these are trade names, Konishi Chemical Industries, Ltd.).
[0203] The content of the benzoxazine compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and even more preferably 10 to 30 parts by mass relative to 100 parts by mass of the total resin solid content in the resin composition. When the content of the benzoxazine compound is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.
[0204] (Compound having a polymerizable unsaturated group)
[0205] The resin composition of the present embodiment may also contain a compound having an unsaturated group capable of polymerization. The compound having an unsaturated group capable of polymerization is not particularly limited, and generally known compounds may be used. The compound having an unsaturated group capable of polymerization may be used alone or in combination of two or more.
[0206] Examples of the compound having a polymerizable unsaturated group include vinyl compounds such as ethylene, propylene, styrene, divinylbenzene, and divinylbiphenyl; (meth)acrylates of monohydric or polyhydric alcohols such as methyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; epoxy (meth)acrylates such as bisphenol A epoxy (meth)acrylate and bisphenol F epoxy (meth)acrylate; and benzocyclobutene resins.
[0207] The content of the compound having a polymerizable unsaturated group is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and further preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. By making the content of the compound having a polymerizable unsaturated group within the above range, there is a tendency for better adhesion, flexibility, etc.
[0208] <Packing (C)>
[0209] From the viewpoint of obtaining a resin composition containing surface-covered titanium oxide (A) and a thermosetting compound (B) with further good dispersibility with surface-covered titanium oxide (A), obtaining a resin composition having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature and further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) when solidified, the resin composition of the present embodiment preferably further includes a filler (C) different from the surface-covered titanium oxide (A). If the filler (C) is different from the surface-covered titanium oxide (A), there is no particular restriction. One filler (C) can be used alone, or two or more can be used in combination.
[0210] The average particle size (D50) of the filler (C) is preferably 0.10 to 10.0 μm, more preferably 0.30 to 5.0 μm. If the average particle size (D50) is within the above range, there is a tendency to obtain a resin composition having further good dispersibility with the surface-covered titanium oxide (A) in the resin composition containing the surface-covered titanium oxide (A) and the thermosetting compound (B), and having further excellent hygroscopic heat resistance, low thermal expansion coefficient, and high glass transition temperature when cured, as well as further excellent dielectric properties (high dielectric constant and low dielectric loss tangent). The average particle size (D50) of the filler (C) can be calculated in the same manner as the average particle size (D50) of the surface-covered titanium oxide (A).
[0211] Examples of the filler (C) include silicon dioxide, silicon compounds (such as white carbon), metal oxides (such as aluminum oxide, titanium dioxide, strontium titanate (SrTiO 3 ), calcium titanate (CaTiO 3 ), titanium oxide (TiO 2 ),MgSiO 4 MgTiO 3 、ZnTiO 3 、ZnTiO 4 、CaTiO 3 、SrTiO 3 、SrZrO 3 , BaTi 2 O 5 , BaTi 4 O 9 , Ba 2 Ti 9 O 20 、Ba(Ti,Sn) 9 O 20 、ZrTiO 4 、(Zr,Sn)TiO 4 、BaNd2 Ti 5 O 14 、BaSmTiO 14 、Bi 2 O 3 -BaO-Nd 2 O 3 -TiO 2 ,La 2 Ti 2 O 7 、Barium titanate (BaTiO 3 )、Ba(Ti,Zr)O 3 、(Ba,Sr)TiO 3 , molybdenum compounds (e.g. molybdic acid, ZnMoO 4 and Zn 3 Mo 2 O 9 Such as zinc molybdate, ammonium molybdate, sodium molybdate, potassium molybdate, calcium molybdate, molybdenum disulfide, molybdenum trioxide, molybdic acid hydrate, (NH 4 )Zn 2 Mo 2 O 9 ·(H 3 (e.g., zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (such as zinc ammonium molybdate hydrate (( ... Glass, M-glass G20, glass staple (including glass powders such as E glass, T glass, D glass, S glass and Q glass), hollow glass, spherical glass, and inorganic fillers such as metal particles that have been insulated with gold, silver, palladium, copper, nickel, iron, cobalt, zinc, Mn-Mg-Zn series, Ni-Zn series, Mn-Zn series, carbonyl iron, Fe-Si series, Fe-Al-Si series and Fe-Ni series; rubber powders such as styrene type, butadiene type and acrylic type; core-shell type rubber powder; silicone resin powder; silicone rubber powder; organic fillers such as silicone composite powder.
[0212] Among them, from the viewpoint of obtaining a resin composition having further good dispersibility with the surface-covered titanium oxide (A) in the resin composition containing the surface-covered titanium oxide (A) and the thermosetting compound (B), and having further excellent moisture absorption heat resistance, low thermal expansion coefficient, and high glass transition temperature when cured, as well as further excellent dielectric properties (high dielectric constant and low dielectric loss tangent), the filler (C) preferably contains one or more selected from the group consisting of silica, alumina, barium titanate, strontium titanate, calcium titanate, aluminum nitride, boron nitride, boehmite, aluminum hydroxide, zinc molybdate, silicone rubber powder, and silicone composite powder, more preferably contains one or more selected from the group consisting of silica, talc, and zinc molybdate, and further preferably contains silica.
[0213] As silicon dioxide, for example, natural silicon dioxide, fused silica, synthetic silica, fumed silica and hollow silica etc. can be listed. If resin combination includes silicon dioxide, then there is a tendency that processability is more excellent. These silicon dioxides can be used alone as one, or two or more can be used in combination. Among them, from the viewpoint of having low thermal expansion coefficient and excellent dispersibility in resin combination, it is preferably selected from more than one of the group consisting of fused silica and hollow silica.
[0214] As silica, commercially available products can be used, and examples thereof include SC2050-MB, SC5050-MOB, SC2500-SQ, SC4500-SQ, SC4053-SQ, and SC5050-MOB (these are trade names, manufactured by Admatechs Corporation); and SFP-130MC (trade name, manufactured by Denka Corporation).
[0215] The filler (C) may also be a surface-treated filler having an inorganic oxide formed on at least a portion of the surface of the filler core particle. Examples of such fillers include surface-treated molybdenum compound particles (supported type) having an inorganic oxide formed on at least a portion of the surface of a core particle composed of a molybdenum compound.
[0216] The inorganic oxide can be applied to at least a portion of the surface of the filler core particles. The inorganic oxide can be applied locally to the surface of the filler core particles or applied in a manner that covers the entire surface of the filler core particles. From the viewpoint of appropriately suppressing the water absorption of the resin composition, the inorganic oxide is preferably applied uniformly in a manner that covers the entire surface of the filler core particles, i.e., a film of the inorganic oxide is preferably uniformly formed on the surface of the filler core particles.
[0217] As the inorganic oxide, one having excellent heat resistance is preferred, and the type thereof is not particularly limited, but metal oxides are more preferred. Examples of the metal oxide include SiO 2 、Al2 O 3 、TiO 2 、ZnO、In 2 O 3 SnO 2 、NiO、CoO、V 2 O 5 , CuO, MgO and ZrO 2 These can be used alone or in combination of two or more. Among these, from the viewpoints of heat resistance, insulation properties, and cost, it is preferred to select silicon dioxide (SiO 2 ), titanium dioxide (TiO 2 ), aluminum oxide (Al 2 O 3 ) and zirconium dioxide (ZrO 2 ), more preferably silicon dioxide.
[0218] The thickness of the inorganic oxide on the surface can be appropriately set according to the desired performance and is not particularly limited. From the perspective of forming a uniform inorganic oxide coating, having better adhesion to the filler core particles, and being able to further suppress the water absorption of the resin composition, the thickness is preferably 3 to 500 nm, more preferably 5 to 200 nm, and further preferably 10 to 100 nm.
[0219] Examples of the surface-treated molybdenum compound particles (supported type) include particles obtained by surface-treating molybdenum compound particles using a silane coupling agent, or particles obtained by surface-treating the particles with an inorganic oxide by a sol-gel method or a liquid phase deposition method.
[0220] As the surface-treated molybdenum compound particles, it is preferred that the inorganic oxide is imparted to at least a portion of the surface or the entire surface of the core particle composed of the molybdenum compound, that is, it is imparted to at least a portion of the periphery or the entire periphery of the core particle. In such surface-treated molybdenum compound particles, it is more preferred that silicon dioxide is imparted as an inorganic oxide to at least a portion of the surface or the entire surface of the core particle composed of the molybdenum compound, that is, it is imparted to at least a portion of the periphery or the entire periphery of the core particle. As the core particle composed of the molybdenum compound, it is more preferred to be at least one selected from the group consisting of molybdic acid, zinc molybdate, and zinc ammonium molybdate hydrate, and zinc molybdate is further preferred.
[0221] From the viewpoint of dispersibility in the resin composition, the average particle size (D50) of the surface-treated molybdenum compound particles is preferably 0.1 to 10 μm, more preferably 0.5 to 8 μm, further preferably 1 to 4 μm, and further preferably 1 to 3 μm. The average particle size (D50) of the surface-treated molybdenum compound particles can be calculated in the same manner as the average particle size (D50) of the surface-coated titanium oxide (A).
[0222] The core particles composed of a molybdenum compound can be produced by various known methods such as a pulverization method and a granulation method, and the production method is not particularly limited. In addition, commercially available products can also be used.
[0223] The method for producing the surface-treated molybdenum compound particles is not particularly limited, and the surface-treated molybdenum compound particles are obtained by appropriately using various known methods such as sol-gel method, liquid phase deposition method, dip coating method, spray coating method, printing method, chemical plating method, sputtering method, evaporation method, ion plating method, and CVD method. The inorganic oxide or its precursor is imparted to the surface of the core particle composed of the molybdenum compound, thereby obtaining the surface-treated molybdenum compound particles. The method for imparting the inorganic oxide or its precursor to the surface of the core particle composed of the molybdenum compound can be any of a wet method and a dry method.
[0224] As a preferred method for producing surface-treated molybdenum compound particles, for example, the following method can be cited: a molybdenum compound (core particle) is dispersed in an alcohol solution in which metal alkoxides such as silicon alkoxides (alkoxysilanes) and aluminum alkoxides are dissolved, and a mixed solution of water, alcohol and a catalyst is added dropwise while stirring to hydrolyze the alkoxide, thereby forming a film of silicon oxide or aluminum oxide on the surface of the compound as a low-refractive index film, and then the obtained powder is separated from the solid and liquid, and heat-treated after vacuum drying. As other preferred production methods, for example, the following method can be cited: a molybdenum compound (core particle) is dispersed in an alcohol solution in which metal alkoxides such as silicon alkoxides and aluminum alkoxides are dissolved, and a mixing treatment is performed at high temperature and low pressure to form a film of silicon oxide or aluminum oxide on the surface of the compound, and then the obtained powder is vacuum dried and pulverized. By these methods, surface-treated molybdenum compound particles having a film of metal oxides such as silicon dioxide and aluminum oxide on the surface of the molybdenum compound can be obtained.
[0225] From the viewpoint of obtaining a resin composition having further good dispersibility with the surface-covered titanium oxide (A) in a resin composition containing the surface-covered titanium oxide (A) and the thermosetting compound (B), and having further excellent moisture absorption heat resistance, low thermal expansion coefficient, high glass transition temperature, and dielectric properties (low dielectric loss tangent) when cured, the content of the filler (C) is preferably 50 to 300 parts by mass, more preferably 70 to 200 parts by mass, and further preferably 100 to 150 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When two or more fillers (C) are contained, the total amount may be within the above range.
[0226] In terms of volume ratio (surface-coated titanium oxide (A): filler (C)), the surface-coated titanium oxide (A) and filler (C) are preferably included in the range of 15:85 to 85:15, more preferably in the range of 20:80 to 80:20, and further preferably in the range of 25:75 to 75:25. If the volume ratio is in the above range, there is a tendency for the surface-coated titanium oxide (A) and filler (C) to be more well dispersed in the thermosetting compound (B). Therefore, in a resin composition such as a resin varnish, the surface-coated titanium oxide (A) and filler (C) are not unevenly distributed, so the water absorption caused by the titanium oxide is further suppressed, and an insulating layer with further excellent moisture absorption heat resistance can be obtained. In addition, a molded product with excellent coating properties and good appearance can also be obtained. In addition, in the resin composition, since the surface-coated titanium oxide (A) and filler (C) are well dispersed, the thermal expansion coefficient of the insulating layer can be appropriately controlled, and a dielectric path can be efficiently formed. Therefore, there is a tendency to favorably obtain an insulating layer having excellent moisture absorption heat resistance and a low thermal expansion coefficient, and having a high dielectric constant and a low dielectric loss tangent.
[0227] In addition, in the resin composition of the present embodiment, from the viewpoint of miniaturization of the circuit and high capacitance of the capacitor, which contributes to miniaturization of high-frequency electrical components, filler (C) can be used with a filler having a high dielectric constant. Examples of such fillers include titanium oxide (TiO 2 ),MgSiO 4 MgTiO 3 、ZnTiO 3 、ZnTiO 4 、CaTiO 3 、SrTiO 3 、SrZrO 3 , BaTi 2 O 5 , Ba 2 Ti 9 O 20 、Ba(Ti,Sn) 9 O 20 、ZrTiO 4 、(Zr,Sn)TiO 4 、BaNd 2 Ti 5 O 14 、BaSmTiO 14 、Bi 2 O 3 -BaO-Nd 2 O 3 -TiO 2 ,La 2 Ti2 O 7 、BaTiO 3 、Ba(Ti,Zr)O 3 and (Ba,Sr)TiO 3 , and metal particles obtained by insulating gold, silver, palladium, copper, nickel, iron, cobalt, zinc, Mn-Mg-Zn, Ni-Zn, Mn-Zn, carbonyl iron, Fe-Si, Fe-Al-Si, Fe-Ni, etc. These fillers may be used alone or in combination of two or more.
[0228] <Silane coupling agent>
[0229] The resin composition of the present embodiment may further contain a silane coupling agent. By containing a silane coupling agent, the resin composition has a tendency to further improve the dispersibility of the surface-covered titanium oxide (A) in the resin composition and the filler (C) compounded as needed, and to further improve the bonding strength between each component contained in the resin composition and the substrate described later. The silane coupling agent can be used alone or in combination of two or more.
[0230] The silane coupling agent is not particularly limited, and the silane coupling agent commonly used for the surface treatment of inorganic substances can be used. For example, aminosilane compounds (for example, 3-aminopropyl triethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane, etc.), epoxy silane compounds (for example, 3-glycidoxypropyl trimethoxysilane, etc.), acrylic silane compounds (for example, γ-acryloxypropyl trimethoxysilane, etc.), cationic silane compounds (for example, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyl trimethoxysilane hydrochloride, etc.), styryl silane compounds, phenyl silane compounds, etc. The silane coupling agent can be used alone or in combination of two or more. Among these, the silane coupling agent is preferably selected from one or more of the group consisting of epoxy silane compounds and styryl silane compounds. Examples of the epoxysilane compound include KBM-403, KBM-303, KBM-402, and KBE-403 (trade names, Shin-Etsu Chemical Co., Ltd.) Examples of the styrylsilane compound include KBM-1403 (trade name, Shin-Etsu Chemical Co., Ltd.).
[0231] The content of the silane coupling agent is not particularly limited, and may be 0.1 to 5.0 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.
[0232] <Wetting and dispersing agent>
[0233] The resin composition of the present embodiment may further contain a wetting dispersant. The resin composition contains a wetting dispersant, which tends to further improve the dispersibility of the filler (C). The wetting dispersant may be used alone or in combination of two or more.
[0234] The wetting dispersant may be a known dispersant (dispersion stabilizer) for dispersing the filler (C), and examples thereof include DISPER BYK (registered trademark)-110, 111, 118, 180, 161, 2009, 2152, 2155, W996, W9010, and W903 (these are trade names, BYK Japan Co., Ltd.).
[0235] The content of the wetting and dispersing agent is not particularly limited, but is preferably 0.5 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the total resin solid content in the resin composition.
[0236] <Curing accelerator>
[0237] The resin composition of the present embodiment may further contain a curing accelerator. The curing accelerator may be used alone or in combination of two or more.
[0238] Examples of curing accelerators include imidazoles such as triphenylimidazole (e.g., 2,4,5-triphenylimidazole); organic peroxides such as benzoyl peroxide, lauroyl peroxide, acetyl peroxide, p-chlorobenzoyl peroxide, and di-tert-butyl peroxyphthalate; azo compounds such as azobisnitrile; N,N-dimethylbenzylamine, N,N-dimethylaniline, N,N-dimethyltoluidine, 2-N-ethylphenylaminoethanol, tri-n-butylamine, pyridine, quinoline, N-methylmorpholine, triethanolamine, triethylenediamine, tetramethylbutylenediamine, N-methylpiperidine, Tertiary amines such as pyridine; phenols such as phenol, xylenol, cresol, resorcinol, and catechol; organic metal salts such as lead naphthenate, lead stearate, zinc naphthenate, zinc octoate, manganese octoate, tin oleate, dibutyltin maleate, manganese naphthenate, cobalt naphthenate, and iron acetylacetonate; substances obtained by dissolving these organic metal salts in hydroxyl-containing compounds such as phenol and bisphenol; inorganic metal salts such as tin chloride, zinc chloride, and aluminum chloride; organic tin compounds such as dioctyltin oxide, other alkyl tins, and alkyl tin oxides; phosphorus compounds such as triphenylphosphine and phosphonium borate compounds, etc. Among these, triphenylimidazoles such as 2,4,5-triphenylimidazole and manganese octoate have a tendency to promote the curing reaction and make the glass transition temperature higher, so they are preferred.
[0239] The content of the curing accelerator is not particularly limited, but may be 0.001 parts by mass or more and 1.0 parts by mass or less relative to 100 parts by mass of the total resin solid content in the resin composition.
[0240] <Solvent>
[0241] The resin composition of the present embodiment may further contain a solvent. By containing a solvent, the resin composition has a tendency to further improve the viscosity of the resin composition during preparation, further improve the handling property (operability), and further improve the impregnation property of the substrate. The solvent may be used alone or in combination of two or more.
[0242] The solvent is not particularly limited as long as it can dissolve part or all of the components in the resin composition, and examples thereof include ketones (acetone, methyl ethyl ketone, etc.), aromatic hydrocarbons (e.g., toluene, xylene, etc.), amides (e.g., dimethylformamide, etc.), propylene glycol monomethyl ether and its acetate, etc.
[0243] <Other ingredients>
[0244] The resin composition of the present embodiment may contain ingredients other than the above within the range that does not impair the desired properties. For example, flame retardant compounds include bromine compounds such as 4,4'-dibromobiphenyl, nitrogen-containing compounds such as phosphate esters, melamine phosphate, melamine, benzoguanamine, and silicon compounds. In addition, various additives include ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, lubricants, defoamers, dispersants, leveling agents (surface adjusters), gloss agents, inhibitors, and the like.
[0245] The content of other components is not particularly limited, but is usually 0.01 parts by mass or more and 10 parts by mass or less, respectively, relative to 100 parts by mass of the total resin solid content in the resin composition.
[0246] [Method for producing resin composition]
[0247] The method for manufacturing the resin composition of the present embodiment is not particularly limited, and for example, the following method can be cited: surface-coated titanium oxide (A), thermosetting compound (B) and the above-mentioned optional components as required are mixed and fully stirred. At this time, in order to uniformly dissolve or disperse each component, known treatments such as stirring, mixing, and kneading treatment can be performed. Specifically, by using a stirring tank equipped with a stirrer with appropriate stirring capacity for stirring and dispersing treatment, the dispersibility of the surface-coated titanium oxide (A) and the filler (C) mixed as required in the resin composition can be improved. The above-mentioned stirring, mixing, and kneading treatment can be appropriately performed using, for example, a device for mixing such as a ball mill, a bead mill, or a known device such as a mixing device of a revolution or autogenous type.
[0248] In addition, when preparing the resin composition, a solvent can be used as needed to prepare a resin varnish. There is no particular limitation on the type of solvent as long as it can dissolve the resin in the resin composition. Specific examples thereof are as described above. The resin varnish can be obtained by adding 10 to 900 parts by mass of a solvent, usually relative to 100 parts by mass of the components in the resin composition from which the solvent has been removed, and performing the aforementioned known treatments (stirring, mixing, and kneading treatments, etc.). The type of solvent is not particularly limited as long as it is a type of solvent that can dissolve the resin in the resin composition. Specific examples thereof are as described above.
[0249] In addition, in the resin composition of the present embodiment, the water absorption calculated by the above formula (i) is 0.40% or less. Such a resin composition can be obtained, for example, by controlling the functional group density of the thermosetting compound (B). That is, by controlling the functional group density of the thermosetting compound (B) to be relatively low, the crosslinking points in the resin composition can be reduced. As a result, the hygroscopicity caused by the hydrophilic groups of the crosslinking points can be reduced, and the water absorption of the resin composition can be controlled to be less than 0.40%.
[0250] [use]
[0251] The resin composition of the present embodiment can be suitably used as a raw material for a cured product, a prepreg, a film-like underfill, a resin sheet, a laminate, a build-up material, a non-conductive film, a metal foil-clad laminate, a printed circuit board, and a fiber-reinforced composite material, or can be suitably used in the manufacture of a semiconductor device. These are described below.
[0252] [cured material]
[0253] The cured product is obtained by curing the resin composition of the present embodiment. As a method for manufacturing a cured product, for example, the resin composition of the present embodiment can be melted or dissolved in a solvent (solvent), flowed into a mold, and cured under normal conditions using heat, light, etc. to obtain it. During thermal curing, from the viewpoint of efficiently curing and preventing the degradation of the obtained cured product, the curing temperature is preferably within the range of 120 to 300°C.
[0254] [Prepreg]
[0255] The prepreg of the present embodiment contains a substrate, and a resin composition of the present embodiment impregnated or coated on the substrate. For example, the resin composition of the present embodiment (for example, uncured state (A stage)) can be impregnated or coated on the substrate, and then dried at 120 to 220 ° C for about 2 to 15 minutes to semi-cured (B stage), thereby obtaining the prepreg of the present embodiment. At this time, the amount of the resin composition (also including the cured product of the resin composition) attached to the substrate, that is, the amount of the resin composition relative to the total amount of the semi-cured prepreg (including the surface-covered titanium oxide (A), and the filler (C) compounded as needed) is preferably in the range of 20 to 99% by mass. It should be noted that the semi-cured state (B stage) refers to the fact that the components contained in the resin composition do not actively start to react (curing), but the resin composition is in a dry state, that is, the state where the solvent is volatilized to the extent of no adhesion by heating, and also includes a state where it will not cure even if it is not heated and only the solvent evaporates. In the present embodiment, the minimum melt viscosity in the semi-cured state (B stage) is generally less than 20,000 Pa·s. The lower limit of the minimum melt viscosity is, for example, more than 10 Pa·s. It should be noted that, in the present embodiment, the minimum melt viscosity is measured by the following method. That is, using 1 g of resin powder collected from the resin composition as a sample, the minimum melt viscosity is measured using a rheometer (ARES-G2 (trade name), TA Instruments). Here, a disposable plate with a plate diameter of 25 mm is used to measure the minimum melt viscosity of the resin powder in the range of more than 40°C and less than 180°C, at a heating rate of 2°C / min, a frequency of 10.0 rad / sec, and a strain of 0.1%.
[0256] As a substrate, as long as it is a substrate for various printed circuit board materials, there is no particular limitation. As the material of the substrate, for example, glass fiber (for example, E-glass, D-glass, L-glass, S-glass, T-glass, Q-glass, UN-glass and NE-glass, etc.), inorganic fibers other than glass fiber (for example, quartz, etc.), organic fibers (for example, polyimide, polyamide, polyester, liquid crystal polyester and polytetrafluoroethylene, etc.) can be cited. As the form of the substrate, there is no particular limitation, and it can be cited: woven fabric, non-woven fabric, roving, short glass fiber mat and surface mat, etc. These substrates can be used alone or in combination with more than two kinds. Among these substrates, from the viewpoint of dimensional stability, it is preferred to implement a woven fabric with super fiber opening treatment and filling treatment, and from the viewpoint of moisture absorption and heat resistance, it is preferably a glass fabric after surface treatment using a silane coupling agent, etc., which has been treated with epoxy silane and amino silane. From the viewpoint of having excellent dielectric properties, glass fibers such as E-glass, L-glass, NE-glass and Q-glass are preferred.
[0257] [Resin sheet]
[0258] The resin sheet of the present embodiment contains the resin composition of the present embodiment. The resin sheet can be a resin sheet with a support body containing a support body and a layer formed by the resin composition of the present embodiment disposed on the surface of the support body. The resin sheet can be used as a laminated film or a dry film solder resist. There is no particular limitation on the manufacturing method of the resin sheet, for example, the following method can be cited: a solution obtained by dissolving the resin composition of the present embodiment in a solvent is applied (coated) to the support body and dried to obtain a resin sheet.
[0259] Examples of the support include polyethylene film, polypropylene film, polycarbonate film, polyethylene terephthalate film, ethylene tetrafluoroethylene copolymer film, release film having a release agent coated on the surface of these films, organic film substrates such as polyimide film, conductor foils such as copper foil and aluminum foil, glass plates, SUS plates, and plate-like materials such as FRP, but are not particularly limited.
[0260] As a coating method (coating method), for example, the following method can be cited: a solution obtained by dissolving the resin composition of the present embodiment in a solvent is applied to a support using a rod coater, a die coater, a scraper, a Baker applicator, etc. In addition, after drying, the support can be peeled off or etched from a resin sheet with a support laminated with a support and a resin composition, thereby making a single-layer sheet (resin sheet). In addition, the solution obtained by dissolving the resin composition of the present embodiment in a solvent can be supplied to a mold having a sheet-shaped film cavity and dried, etc., so that a single-layer sheet (resin sheet) can be obtained without using a support.
[0261] It should be noted that in the preparation of the single-layer sheet or the resin sheet with a support of the present embodiment, the drying conditions when removing the solvent are not particularly limited. From the viewpoint of easily removing the solvent in the resin composition and inhibiting the progress of curing during drying, it is preferably carried out at a temperature of 20 to 200°C for 1 to 90 minutes. In addition, in the single-layer sheet or the resin sheet with a support, the resin composition can be used in an uncured state after only the solvent is dried, and can also be used in a semi-cured (B-stage) state as needed. In addition, the thickness of the resin layer of the single-layer sheet or the resin sheet with a support of the present embodiment can be adjusted according to the concentration of the solution of the resin composition of the present embodiment and the coating thickness, and is not particularly limited. From the viewpoint of easily removing the solvent during drying, it is preferably 0.1 to 500 μm.
[0262] [Laminated board]
[0263] The laminate of the present embodiment contains one or more of the group consisting of the prepreg and resin sheet of the present embodiment. For prepreg and resin sheet, when stacking more than 2 kinds, the resin composition used in each prepreg and resin sheet can be the same or different. In addition, when using both prepreg and resin sheet, the resin composition used in them can be the same or different. In the laminate of the present embodiment, one or more of the group consisting of prepreg and resin sheet can be semi-cured state (B stage), or can be fully cured state (C stage).
[0264] [Metal foil-clad laminate]
[0265] The metal foil-clad laminate of the present embodiment includes the laminate of the present embodiment and a metal foil disposed on one surface or both surfaces of the laminate.
[0266] Furthermore, the metal foil-clad laminate may include at least one prepreg according to the present embodiment and a metal foil laminated on one or both surfaces of the prepreg.
[0267] Furthermore, the metal foil-clad laminate may include at least one resin sheet of the present embodiment and a metal foil laminated on one surface or both surfaces of the resin sheet.
[0268] In the metal foil clad laminate of the present embodiment, the resin compositions used in the prepregs and the resin sheets may be the same or different, and when both prepregs and resin sheets are used, the resin compositions used in these may be the same or different. In the metal foil clad laminate of the present embodiment, one or more selected from the group consisting of prepregs and resin sheets may be in a semi-cured state or in a fully cured state.
[0269] In the metal foil clad laminate of the present embodiment, the metal foil is laminated on one or more selected from the group consisting of the prepreg of the present embodiment and the resin sheet of the present embodiment, wherein the metal foil is preferably laminated in a manner that contacts the surface of one or more selected from the group consisting of the prepreg of the present embodiment and the resin sheet of the present embodiment. "The metal foil is laminated in a manner that contacts the surface of one or more selected from the group consisting of the prepreg and the resin sheet" means that there is no layer such as an adhesive layer between the prepreg or the resin sheet and the metal foil, and the prepreg or the resin sheet is in direct contact with the metal foil. As a result, there is a tendency that the metal foil peel strength of the metal foil clad laminate is improved and the insulation reliability of the printed circuit board is improved.
[0270] The metal foil clad laminate of the present embodiment may have one or more prepregs and / or resin sheets of the present embodiment overlapped, and metal foil disposed on one or both sides of the prepregs and / or resin sheets. As a method for manufacturing the metal foil clad laminate of the present embodiment, for example, the following method can be cited: overlap one or more prepregs and / or resin sheets of the present embodiment, dispose metal foil on one or both sides thereof and perform laminate molding. As a molding method, the method commonly used when molding laminates and multilayer boards for printed circuit boards can be cited. More specifically, the following method can be cited: using a multi-stage punching machine, a multi-stage vacuum punching machine, a continuous molding machine, an autoclave molding machine, etc., at a temperature of about 180 to 350°C, a heating time of about 100 to 300 minutes, and a surface pressure of 20 to 100 kgf / cm 2 The laminate molding is performed under the conditions of about 1:1.
[0271] In addition, by combining the prepreg and / or resin sheet of the present embodiment with a circuit board for the inner layer obtained separately and performing stacking molding, a multilayer board can also be made. As a manufacturing method for a multilayer board, for example, by configuring a copper foil with a thickness of about 35 μm on both sides of the prepreg and / or resin sheet of the present embodiment overlapping more than one sheet, after stacking and forming a copper foil-clad laminate using the above-mentioned molding method, an inner layer circuit is formed, and the circuit is subjected to blackening treatment to form an inner layer circuit board, and then, the inner layer circuit board and the prepreg and / or resin sheet of the present embodiment are alternately configured piece by piece, and copper foil is further configured in the outermost layer, and stacking molding is preferably performed under vacuum under the above-mentioned conditions to obtain a multilayer board. The metal foil-clad laminate of the present embodiment can be suitably used as a printed circuit board.
[0272] (metal foil)
[0273] The metal foil is not particularly limited, and examples thereof include gold foil, silver foil, copper foil, tin foil, nickel foil, and aluminum foil. Among them, copper foil is preferred. As the copper foil, there is no particular limitation as long as it is a copper foil commonly used for printed circuit board materials, and examples thereof include rolled copper foil and electrolytic copper foil. Among them, electrolytic copper foil is preferred from the viewpoint of copper foil peel strength and fine wiring formation. The thickness of the copper foil is not particularly limited, and may be about 1.5 to 70 μm.
[0274] [Printed Circuit Board]
[0275] The printed circuit board of the present embodiment has an insulating layer and a conductor layer disposed on one or both sides of the insulating layer, and the insulating layer contains a cured product of the resin composition of the present embodiment. The insulating layer preferably contains at least one of a layer (a layer containing a cured product) formed by the resin composition of the present embodiment and a layer (a layer containing a cured product) formed by a prepreg. Such a printed circuit board can be manufactured according to a conventional method, and its manufacturing method is not particularly limited, for example, the above-mentioned metal foil-clad laminate can be used to manufacture. An example of a method for manufacturing a printed circuit board is shown below.
[0276] First, prepare the above-mentioned metal foil-clad laminate. Then, the surface of the metal foil-clad laminate is subjected to etching treatment and the inner layer circuit is formed to make an inner substrate. On the inner layer circuit surface of the inner substrate, a surface treatment for improving bonding strength is performed as needed, and then the required number of prepregs are overlapped on the inner layer circuit surface, and then the metal foil for the outer layer circuit is stacked on its outside, and heated and pressed to form an integral body. In this way, a multilayer laminate having an insulating layer formed between the metal foil for the inner layer circuit and the outer layer circuit and consisting of a cured product of the resin composition of the present embodiment can be manufactured. Then, after the opening processing for through holes and vias is performed for the multilayer laminate, a plated metal coating that conducts the metal foil for the inner layer circuit and the outer layer circuit is formed on the wall surface of the hole, and then the metal foil for the outer layer circuit is subjected to etching treatment to form an outer layer circuit, thereby manufacturing a printed circuit board.
[0277] The printed wiring board obtained in the above manufacturing example has the following structure: it has an insulating layer and a conductor layer formed on the surface of the insulating layer, and the insulating layer contains the cured product of the resin composition of this embodiment. That is, the prepreg of this embodiment (containing a substrate and the cured product of the resin composition of this embodiment impregnated or coated on the substrate) and the layer of the resin composition of the metal foil-clad laminate of this embodiment (the layer containing the cured product of the resin composition of this embodiment) are composed of the insulating layer containing the cured product of the resin composition of this embodiment.
[0278] [Semiconductor devices]
[0279] The semiconductor device can be manufactured by mounting a semiconductor chip on the conductive part of the printed circuit board of this embodiment. Here, the conductive part refers to the part of the multilayer printed circuit board that transmits electrical signals, and its position can be the surface or the embedded part. In addition, the semiconductor chip is not particularly limited as long as it is a circuit element using semiconductor as a material.
[0280] The method for mounting semiconductor chips when manufacturing semiconductor devices is not particularly limited as long as the semiconductor chips can function effectively. Specifically, the following methods are mentioned: wire bonding mounting method, flip chip mounting method, mounting method using solderless build-up layer (BBUL), mounting method using anisotropic conductive film (ACF), mounting method using non-conductive film (NCF), etc.
[0281] [Example]
[0282] The present embodiment will be described in more detail below using examples and comparative examples. The present embodiment is not limited in any way by the following examples.
[0283] [Method for measuring average particle size]
[0284] The average particle diameter (D50) of the surface-coating titanium oxide and the filler (fused spherical silica) was calculated by measuring the particle size distribution by a laser diffraction-scattering method using a laser diffraction-scattering particle size distribution measuring apparatus (Microtrac MT3300EXII (trade name), Microtrac BEL Co., Ltd.) under the following measurement conditions.
[0285] (Measurement conditions of laser diffraction-scattering particle size distribution measuring device)
[0286] (Surface covered with titanium oxide)
[0287] Solvent: methyl ethyl ketone, solvent refractive index: 1.33, particle refractive index: 2.72, transmittance: 85±5%.
[0288] (filler)
[0289] Solvent: methyl ethyl ketone, solvent refractive index: 1.33, particle refractive index: 1.45 (fused spherical silica), transmittance: 85±5%.
[0290] [Synthesis Example 1] Synthesis of Naphthol Arylalkyl Cyanate Compound (SN495V-CN)
[0291] 300 g (1.28 mol in terms of OH group) of naphthol aralkyl type phenol resin (SN495V (trade name), OH group (hydroxyl) equivalent: 236 g / eq., Nippon Steel Chemical Co., Ltd.) and 194.6 g (1.92 mol) of triethylamine (1.5 mol per 1 mol of hydroxyl group) were dissolved in 1800 g of dichloromethane to prepare solution 1. 125.9 g (2.05 mol) of cyanogen chloride (1.6 mol per 1 mol of hydroxyl group), 293.8 g of dichloromethane, 194.5 g (1.92 mol) of 36% hydrochloric acid (1.5 mol per 1 mol of hydroxyl group) and 1205.9 g of water were added to solution 1 over 30 minutes while stirring and maintaining the liquid temperature at -2 to -0.5°C. After the injection of solution 1 is completed, the mixture is stirred at the same temperature for 30 minutes, and then a solution (solution 2) obtained by dissolving 65 g (0.64 mol) of triethylamine (0.5 mol relative to 1 mol of hydroxyl group) in 65 g of dichloromethane is injected over 10 minutes. After the injection of solution 2 is completed, the mixture is stirred at the same temperature for 30 minutes to terminate the reaction. Then, the reaction solution is allowed to stand to separate the organic phase from the aqueous phase, and the obtained organic phase is washed 5 times with 1300 g of water. The conductivity of the wastewater after the fifth washing was 5 μS / cm, confirming that the ionic compounds that can be removed by water-based washing were fully removed. The organic phase after washing was concentrated under reduced pressure, and finally concentrated to dryness at 90°C for 1 hour to obtain the target naphthol aralkyl type cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq., R in the above formula (13) 3 All of them are hydrogen atoms, and n3 is an integer of 1 to 10) (orange viscous material) 331g. The infrared absorption spectrum of the obtained SN495V-CN shows 2250cm -1 The absorption of the cyanate group was not shown, and the absorption of the hydroxyl group was not shown.
[0292] [Example 1]
[0293] 80 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), 20 parts by mass of a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation), 80 parts by mass of a surface-coated titanium oxide (crystal structure: rutile type, titanium dioxide surface-treated with silicon dioxide, aluminum oxide, and dimethyl silicone (total content of silicon dioxide, aluminum oxide, and dimethyl silicone: 3% by mass), titanium oxide content: 97% by mass, average particle size (D50): 0.21 μm, CR-63 (trade name), Ishihara Sangyo Co., Ltd.), 80 parts by mass of fused spherical silica (SC4500-SQ (trade name), flat Average particle size (D50): 1.1 μm, Admatechs Co., Ltd.) 120 parts by mass, silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.) 4 parts by mass, wetting and dispersing agent (DISPERBYK (registered trademark) -161 (trade name), BYK Co., Ltd.) 2 parts by mass, wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK Co., Ltd.) 2 parts by mass, 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.) 0.1 parts by mass, and methyl ethyl ketone 100 parts by mass were mixed to obtain a resin varnish. The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 in volume ratio (surface-covering titanium oxide: filler).
[0294] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg, and the surface pressure was 30 kgf / cm 2 The laminate was then vacuum pressed at 220°C for 120 minutes to obtain a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.
[0295] [Example 2]
[0296] 8 parts by mass of the naphthol aralkyl cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name), K.I. Chemical Industry Co., Ltd.), 28 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), and a naphthalene-based epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica, alumina and dimethyl silicone (total content of silica, alumina and dimethyl silicone: 3% by mass), titanium oxide content: 97% by mass , average particle size (D50): 0.21 μm, CR-63 (trade name), Ishihara Sangyo Co., Ltd.), 80 parts by mass, fused spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, Admatechs Co., Ltd.), 120 parts by mass, a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass, a wetting and dispersing agent (DISPERBYK (registered trademark) -161 (trade name), BYK Corporation), 2 parts by mass, a wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK Corporation), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish. The blending ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.
[0297] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg, and the surface pressure was 30 kgf / cm 2The laminate was formed by vacuum pressing at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The measurement results are shown in Table 1.
[0298] [Example 3]
[0299] 8 parts by mass of the naphthol aralkyl cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name), K.I. Chemical Industry Co., Ltd.), 28 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), and a naphthalene-based epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with alumina and organosilane (total content of alumina and organosilane: 2% by mass), titanium oxide content: 98% by mass, average particle size (D 50): 0.40 μm, R-22L (trade name, Sakai Chemical Industry Co., Ltd.), 80 parts by mass of fused spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, Admatechs Co., Ltd.), 120 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark)-161 (trade name), BYK Corporation), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), BYK Corporation), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.) and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish. The blending ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.
[0300] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg, and the surface pressure was 30 kgf / cm 2 The laminate was formed by vacuum pressing at 220°C for 120 minutes to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The measurement results are shown in Table 1.
[0301] [Example 4]
[0302] 8 parts by mass of the naphthol aralkyl cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name), K.I. Chemicals Co., Ltd.), 28 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), and a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, a surface-covered titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with alumina and silicone oil (total content of alumina and silicone oil: 2% by mass), titanium oxide content: 98% by mass, average particle size (D50 ): 0.20 μm, R-11P (trade name), Sakai Chemical Industry Co., Ltd.), 80 parts by mass of fused spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, Admatechs Co., Ltd.), 120 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark)-161 (trade name), BYK Corporation), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), BYK Corporation), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish. The blending ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.
[0303] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg, and the surface pressure was 30 kgf / cm 2The laminate was then vacuum pressed at 220°C for 120 minutes to obtain a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.
[0304] [Example 5]
[0305] 8 parts by mass of the naphthol aralkyl cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name), K.I. Chemicals Co., Ltd.), 28 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), and a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Corporation, a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are obtained by polymerizing structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, and a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with alumina, organosilane and silicone oil (total content of alumina, organosilane and silicone oil: 5% by mass), titanium oxide content: 95% by mass, average A resin varnish was obtained by mixing 80 parts by mass of R-39 (trade name), particle size (D50): 0.23 μm, Sakai Chemical Industry Co., Ltd.), 120 parts by mass of fused spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, Admatechs Co., Ltd.), 4 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 2 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark)-161 (trade name), BYK Corporation), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), BYK Corporation), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone. The blending ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.
[0306] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg, and the surface pressure was 30 kgf / cm 2 The laminate was then vacuum pressed at 220°C for 120 minutes to obtain a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.
[0307] [Comparative Example 1]
[0308] 80 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), 20 parts by mass of a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation), 80 parts by mass of a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silicon dioxide and aluminum oxide (total content of silicon dioxide and aluminum oxide: 15% by mass), titanium oxide content: 85% by mass, average particle size (D50): 0.25 μm, PFC-211 (trade name), Ishihara Sangyo Co., Ltd.), 80 parts by mass of fused spherical silica (SC4500-SQ (trade name), average particle size (D5 0): 1.1 μm, Admatechs Co., Ltd.), 120 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark)-161 (trade name), BYK Co., Ltd.), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), BYK Co., Ltd.), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish. The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide: filler) in terms of volume ratio.
[0309] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg, and the surface pressure was 30 kgf / cm 2 The laminate was then vacuum pressed at 220°C for 120 minutes to obtain a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.
[0310] [Comparative Example 2]
[0311] 8 parts by mass of the naphthol aralkyl cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq.) obtained in Synthesis Example 1, 28 parts by mass of 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane (BMI-80 (trade name), K.I. Chemicals Co., Ltd.), 28 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), and a naphthalene-type epoxy resin (EPICLON EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., DIC Corporation) 12 parts by mass, a modified polyphenylene ether compound (OPE-2St1200 (trade name), Mitsubishi Gas Chemical Co., Ltd., a compound represented by formula (7) (in formula (7), X is formula (8), and -(YO)- and -(OY)- are polymerized from structural units of formula (11)), number average molecular weight 1187, vinyl equivalent: 590 g / eq., minimum melt viscosity: 1000 Pa·s) 24 parts by mass, a surface-coated titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica and alumina (total content of silica and alumina: 15% by mass), titanium oxide content: 85% by mass, average particle size (D 50): 0.25 μm, PFC-211 (trade name, Ishihara Sangyo Co., Ltd.), 80 parts by mass of fused spherical silica (SC4500-SQ (trade name), average particle size (D50): 1.1 μm, Admatechs Co., Ltd.), 120 parts by mass of a silane coupling agent (KBM-1403 (trade name), Shin-Etsu Chemical Co., Ltd.), 4 parts by mass of a wetting and dispersing agent (DISPERBYK (registered trademark)-161 (trade name), BYK Corporation), 2 parts by mass of a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), BYK Corporation), 0.1 parts by mass of 2,4,5-triphenylimidazole (Tokyo Chemical Industry Co., Ltd.) and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish. The blending ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) in terms of volume ratio.
[0312] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) with a thickness of 0.094 mm, and heated and dried at 130°C for 3 minutes to obtain a prepreg with a thickness of 0.1 mm. Then, electrolytic copper foil (3EC-M3-VLP (trade name), Mitsui Mining and Smelting Co., Ltd.) with a thickness of 12 μm was placed on the upper and lower surfaces of the obtained prepreg, and the surface pressure was 30 kgf / cm 2The laminate was then vacuum pressed at 220°C for 120 minutes to obtain a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.
[0313] [Comparative Example 3]
[0314] A prepreg was prepared in the same manner as in Example 1 except that 80 parts by mass of surface-covered titanium oxide (crystal structure: rutile type, obtained by surface-treating titanium dioxide with silica, alumina and dimethyl silicone (total content of silica, alumina and dimethyl silicone: 3% by mass), titanium oxide content: 97% by mass, average particle size (D50): 0.21 μm, CR-63 (trade name), Ishihara Sangyo Co., Ltd.) was used instead of 80 parts by mass of surface-covered titanium oxide (titanium oxide particles 41% by mass, silica 57% by mass, alkyl silane 2% by mass, inorganic particles containing multiple titanium oxide particles, average particle size (D50): 4.5 μm, SUNSIL-Tin50AS (trade name), Linden Co., Ltd.). The mixing ratio (content ratio) of the surface-covering titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covering titanium oxide:filler) by volume ratio.
[0315] An attempt was made to produce a metal foil-clad laminate using the obtained prepreg, but voids were generated on the entire surface of the metal foil-clad laminate, and the metal foil-clad laminate could not be produced.
[0316] [Comparative Example 4]
[0317] A prepreg was prepared in the same manner as in Example 1 except that 80 parts by mass of surface-covered titanium oxide (crystal structure: rutile type, titanium dioxide surface-treated with silica, alumina and dimethyl silicone (total content of silica, alumina and dimethyl silicone: 3% by mass), titanium oxide content: 97% by mass, average particle size (D50): 0.21 μm, CR-63 (trade name), Ishihara Sangyo Co., Ltd.) was used instead of 80 parts by mass of surface-covered titanium oxide (titanium dioxide surface-treated with silica and alumina, titanium oxide content: 91% by mass, average particle size (D50): 0.20 μm, R-21 (trade name), Sakai Chemical Industry Co., Ltd.). The blending ratio (content ratio) of the surface-covered titanium oxide and the filler (SC4500-SQ (trade name)) in the resin varnish was 26:74 (surface-covered titanium oxide: filler) in terms of volume ratio.
[0318] An attempt was made to produce a metal foil-clad laminate using the obtained prepreg, but voids were generated on the entire surface of the metal foil-clad laminate, and the metal foil-clad laminate could not be produced.
[0319] [Evaluation method]
[0320] (1) Water absorption
[0321] Two sheets of the prepreg obtained in the examples and comparative examples were stacked, and electrolytic copper foils (3EC-M3-VLP (trade name), Mitsui Mining & Smelting Co., Ltd.) with a thickness of 12 μm were placed on the upper and lower surfaces. 2 The sample was vacuum pressed at 220°C for 120 minutes and laminated to produce a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.2 mm. The copper foil on both sides of the metal foil-clad laminate was completely etched to obtain an unclad plate with a thickness of 0.2 mm in which the copper foil on both sides was completely removed. The unclad plate was cut into a size of 50 mm × 50 mm (miniaturized) to obtain a sample for measurement. The sample for measurement was dried in a dryer at 150°C for 1 hour. Then, the dry mass M1 (g) of the sample for measurement was measured. Next, the dried sample for measurement was subjected to a 168-hour moisture absorption treatment in a constant temperature and humidity chamber (FX-222P (trade name), Kusumoto Chemicals Co., Ltd.) at 85°C and 85% RH (relative humidity). After 168 hours of moisture absorption treatment, the sample for measurement was taken out of the constant temperature and humidity chamber and weighed, and the mass after the weighing value became constant was defined as M2 (g). The water absorption (%) was calculated using the obtained masses M1 and M2 according to the following formula (i).
[0322] Water absorption (%) = [(M2-M1) / M1] × 100… (i)
[0323] (2) Glass transition temperature (Tg)
[0324] The copper foils on both sides of the metal foil-clad laminate obtained in the examples and comparative examples were completely etched to obtain an unclad plate with a thickness of 0.1 mm in which the copper foils on both sides were completely removed. The unclad plate was cut into a size of 40 mm × 4.5 mm (miniaturized) to obtain a sample for measurement. The sample for measurement was used to measure the glass transition temperature (Tg, ° C) by the DMA method in accordance with JIS C6481 using a dynamic viscoelasticity analyzer (Q800 (trade name), TA instruments).
[0325] (3) Coefficient of thermal expansion (CTE)
[0326] The copper foils on both sides of the metal foil-clad laminate obtained in the examples and comparative examples were completely etched to obtain a bare board with a thickness of 0.1 mm in which the copper foils on both sides were completely removed. The bare board was cut into a size of 40 mm × 4.5 mm (miniaturized) to obtain a sample for measurement. Using the sample for measurement, the thermal expansion coefficient (CTE, ppm / °C) in the direction below 60°C to 120°C was measured using a thermomechanical analyzer (Q400 (trade name), TA instruments) at a temperature of 10°C per minute from 40°C to 340°C in accordance with JIS C6481. The measurement direction was the longitudinal direction (Warp) of the glass cloth of the laminate.
[0327] (4) Relative dielectric constant (Dk) and dielectric loss tangent (Df)
[0328] The copper foils on both sides of the metal foil-clad laminates obtained in Examples and Comparative Examples were completely etched to obtain bare boards with a thickness of 0.1 mm from which the copper foils on both sides were completely removed. The bare boards were cut into a size of 1 mm×65 mm (miniaturized) to obtain measurement samples.
[0329] The relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz were measured using a network analyzer (Agilent 8722ES (trade name), Agilent Technologies Co., Ltd.) using the sample for measurement. It should be noted that the relative dielectric constant (Dk) and dielectric loss tangent (Df) were measured under a temperature of 23°C ± 1°C and a humidity of 50% RH (relative humidity) ± 5% RH.
[0330] Then, the measurement sample was dried in a dryer at 120°C for 1 hour. The dried measurement sample was subjected to a 168-hour moisture absorption treatment in a thermostatic hygrostat (FX-222P (trade name), Kusumoto Chemicals Co., Ltd.) at a temperature of 85°C ± 1°C and a humidity of 85% RH ± 5% RH. The relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz were measured using a network analyzer (Agilent 8722ES (trade name), Agilent Technologies Co., Ltd.) for the measurement sample after the 168-hour moisture absorption treatment.
[0331] (5) Hygroscopic heat resistance evaluation
[0332] Ultra-thin copper foil with a carrier (MT18FL (trade name), Mitsui Mining & Smelting Co., Ltd., thickness: 1.5 μm) was placed on the upper and lower surfaces of the prepregs obtained in the examples and comparative examples, and the surface pressure was 30 kgf / cm 2The laminated plate was subjected to vacuum pressing for 120 minutes at a temperature of 220°C, thereby producing a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.1 mm. Then, the copper foil on both sides was completely etched to obtain an unclad plate with all the copper foil on both sides removed. A prepreg with a thickness of 0.06 mm (GHPL-970LF (LD) (trade name), Mitsubishi Gas Chemical Co., Ltd.) was arranged on the upper and lower surfaces of the unclad plate, and an electrolytic copper foil with a thickness of 12 μm (3EC-M3-VLP (trade name), Mitsui Mining & Smelting Co., Ltd.) was arranged on the upper and lower surfaces thereof, and the surface pressure was 30 kgf / cm 2 The obtained laminate was cut into a size of 50 mm × 50 mm (miniaturized), and the copper foil on one side was completely removed by etching, and on the other side, half of the copper foil on the surface was removed by etching, thereby preparing a sample for measurement. The obtained sample for measurement was treated for 2 hours at 121°C and 2 atmospheres of saturated water vapor using a pressure cooker tester (PC-3 type (trade name), Hirayama Manufacturing Co., Ltd.), and then immersed in a solder bath at 260°C or 280°C for 60 seconds, and visually observed whether there was any abnormality in the appearance change. Each measurement was performed on 5 sheets respectively, and from these 5 sheets, when the appearance abnormality was observed to be 0 to 1 sheet, it was evaluated as "AA", and when the appearance abnormality was observed to be 2 to 5 sheets, it was evaluated as "CC", and the results are shown in Table 1. It should be noted that, in the sample after immersion, if swelling is observed at the interface between the metal foil and the insulating layer, for example, it is judged that the appearance is abnormal. In the table, "PCT2.0h" indicates the result after 2 hours of treatment using a pressure cooker tester.
[0333] Table 1
[0334]
[0335] This application is based on the Japanese patent application (Japanese Patent Application No. 2022-46305) filed on March 23, 2022, the contents of which are incorporated herein by reference.
[0336] Industrial Applicability
[0337] The resin composition of this embodiment can be used as a raw material for a cured product, a prepreg, a film-like underfill, a resin sheet, a laminate, a buildup material, a non-conductive film, a metal foil-clad laminate, a printed wiring board, and a fiber-reinforced composite material, or can be suitably used in the manufacture of a semiconductor device.
Claims
1. A resin composition comprising a surface-covered titanium oxide (A) and a thermosetting compound (B), The water absorption calculated by the following formula (i) is 0.40% or less; Water absorption (%) = [(M2-M1) / M1] × 100… (i) In formula (i), M1 represents: a prepreg having a thickness of 0.1 mm obtained by laminating two sheets of E glass cloth having a thickness of 0.094 mm by impregnation and coating the resin composition, and then heating and drying at 130°C for 3 minutes, and applying a surface pressure of 30 kgf / cm 2 and temperature of 220°C for 120 minutes to perform vacuum pressing for lamination molding, and the obtained laminated board is dried at 150°C for 1 hour, and the mass (g) of the dried laminated board (a); M2 represents: the mass (g) of the dried laminated board (a) after moisture absorption treatment at 85°C and 85% RH for 168 hours.
2. The resin composition according to claim 1, wherein The surface-covering titanium oxide (A) has an organic layer and / or an inorganic oxide layer on the surface of titanium oxide particles.
3. The resin composition according to claim 2, wherein The surface-covering titanium oxide (A) further has the organic layer on the surface of the inorganic oxide layer.
4. The resin composition according to claim 2, wherein The total amount of the organic layer and the inorganic oxide layer is 0.1 to 10% by mass based on 100% by mass of the surface-covering titanium oxide (A).
5. The resin composition according to claim 2, wherein The inorganic oxide layer is one or more selected from the group consisting of a layer containing silicon dioxide, a layer containing zirconium oxide, and a layer containing aluminum oxide.
6. The resin composition according to claim 2, wherein The organic layer is a layer surface-treated with an organic silicon compound.
7. The resin composition according to claim 6, wherein The organosilicon compound includes one or more selected from the group consisting of a silane coupling agent, an organosilane, and an organopolysiloxane.
8. The resin composition according to claim 2, wherein The content of the titanium oxide in the surface-covering titanium oxide (A) is 90 to 99.9% by mass based on 100% by mass of the surface-covering titanium oxide (A).
9. The resin composition according to claim 1, wherein The content of the surface-covering titanium oxide (A) is 50 to 500 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.
10. The resin composition according to claim 1, wherein The thermosetting compound (B) includes one or more selected from the group consisting of maleimide compounds, epoxy compounds, modified polyphenylene ether compounds, cyanate compounds, phenol compounds, alkenyl-substituted nadic imide compounds, oxetane resins, benzoxazine compounds, and compounds having a polymerizable unsaturated group.
11. The resin composition according to claim 10, wherein The maleimide compound comprises one or more selected from the group consisting of bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)phenyl)propane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, a maleimide compound represented by the following formula (1), and a maleimide compound represented by the following formula (2); In formula (1), R 1 Each independently represents a hydrogen atom or a methyl group, and n1 is an integer from 1 to 10; In formula (2), R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, and n2 is an average value and represents 1<n2≤5.
12. The resin composition according to claim 10, wherein The epoxy compound includes one or more selected from the group consisting of biphenyl aralkyl epoxy resins, naphthalene epoxy resins, and naphthylene ether epoxy resins.
13. The resin composition according to claim 10, wherein The modified polyphenylene ether compound comprises a compound represented by the following formula (3); In formula (3), X represents an aromatic group, -(YO) m - represents a polyphenylene ether portion; R1, R2 and R3 each independently represent a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group; m represents an integer of 1 to 100, n represents an integer of 1 to 6, and q represents an integer of 1 to 4.
14. The resin composition according to claim 10, wherein The cyanate compound includes one or more selected from the group consisting of phenol novolac type cyanate compound, naphthol aralkyl type cyanate compound, naphthylene ether type cyanate compound, xylene resin type cyanate compound, bisphenol M type cyanate compound, bisphenol A type cyanate compound, diallyl bisphenol A type cyanate compound, bisphenol E type cyanate compound, bisphenol F type cyanate compound, biphenyl aralkyl type cyanate compound, and prepolymers or polymers of these cyanate compounds. 15 . The resin composition according to claim 1 , further comprising a filler (C) different from the surface-covering titanium oxide (A).
16. The resin composition according to claim 15, wherein The filler (C) includes one or more selected from the group consisting of silica, alumina, barium titanate, strontium titanate, calcium titanate, aluminum nitride, boron nitride, boehmite, aluminum hydroxide, zinc molybdate, silicone rubber powder, and organic silicon composite powder.
17. The resin composition according to claim 15, wherein The content of the filler (C) is 50 to 300 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.
18. The resin composition according to claim 1, which is used for a printed circuit board. 19 . A prepreg comprising a substrate and the resin composition according to claim 1 impregnated or coated on the substrate. 20 . A resin sheet comprising the resin composition according to claim 1 .
21. A laminate comprising the prepreg according to claim 19.
22. A laminate comprising the resin sheet according to claim 20. 23 . A metal foil-clad laminate comprising the laminate according to claim 21 and a metal foil disposed on one or both surfaces of the laminate. 24 . A metal foil-clad laminate comprising the laminate according to claim 22 and a metal foil disposed on one or both surfaces of the laminate. 25 . A printed wiring board comprising an insulating layer and a conductor layer disposed on one or both surfaces of the insulating layer, wherein the insulating layer contains a cured product of the resin composition according to claim 1 .