Method for manufacturing fiber and apparatus for manufacturing fiber

By stretching at high speed torsion and rotation before curing during the fiber manufacturing process, combined with the torsion force provided by the cyclone flow and the rotating roller, the problem of insufficient cyclone flow velocity and difficulty in spiral flow expansion is solved, and the fiber is realized Efficient diameter-finement.

CN118922592APending Publication Date: 2024-11-08TORAY INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380027258.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-02-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing fiber manufacturing methods, the fiber cyclone flow velocity is insufficient or the spiral flow is difficult to expand, resulting in the fiber being unable to fully fine the diameter and the polymer solution cannot be further stretched after cooling and curing.

Method used

By stretching the fibrous polymer discharged from the spinneret die before curing, at high speed torsion and rotation, the torsional force is provided by cyclone flow and rotating rollers to ensure that the fibers are fully pulled in a deformable state stretch.

Benefits of technology

The diameter of the fiber is minimized, the fiber is fine-grained, and the fiber is fine-grained, ensuring that the fiber can be fully deformed and stretched before curing, solving the problem of poor fiber fine-grained effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922592A_ABST
    Figure CN118922592A_ABST
Patent Text Reader

Abstract

The invention provides a fiber manufacturing method and a fiber manufacturing device, which can effectively obtain fibers with very small fiber diameters by twisting and stretching a fibrous polymer discharged from a discharge hole at a high speed in a state that the polymer before curing is easy to deform. In this method for producing fibers, a torsional force in the rotational direction is applied to a single discharged fibrous polymer on a plane perpendicular to the discharge direction of the polymer about the fibrous polymer, thereby causing the fibrous polymer to rotate about the center of the cross-section of the fibrous polymer. The drawing is performed such that the discharge speed (Vmm / sec) of the polymer discharged from the spinning die and the rotational speed (W times / sec) of the fibrous polymer satisfy W / V > = 0.1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to methods and apparatus suitable for manufacturing fibers. Background Technology

[0002] In recent years, there has been a demand for finer fibers in many fields. Various studies and developments have been conducted on methods for expelling thermoplastic polymers from a spinning spinneret in a fibrous form and then stretching them, and these methods have been implemented using several stretching devices. Common stretching methods include: rotating a roller in contact with the expelled fiber to create a speed difference; injecting a high-speed airflow into the traveling fiber and applying tension to the fiber using the friction generated between the fiber and the airflow; and so on.

[0003] Patent Document 1 discloses a method for stretching traveling filaments. Patent Document 1 discloses a method in which a gas jet is ejected from three or more nozzles arranged around the outlet of a spinneret to form a swirling flow around the fiber, thereby stretching the fiber by spraying the gas jet onto the fiber. This stretching method, which involves causing the discharged fiber to swirl, enables the fiberization of difficult-to-fiber materials.

[0004] In addition, as another method of stretching using swirling flow, Patent Document 2 discloses a method in which compressed air is supplied to the interior of a pipe with spiral-shaped protrusions on its inner wall and a cross-sectional area decreasing towards the downstream, causing a traveling fiber to pass through the pipe, thereby stretching it. In this method, the fiber is given a stretching force by utilizing the velocity difference in the fiber's direction of travel within the pipe, and the fiber is twisted by utilizing the spiral airflow, thereby enabling the fiber diameter to be reduced.

[0005] In addition, as another method for stretching traveling filaments, in Patent Document 3, a tubular fiber spinning needle has an inlet for introducing a polymer solution and an outlet that is a non-fixed end for discharging the polymer solution. When the outlet side is vibrated or rotated by the jet of compressed gas at the inlet, the polymer is discharged from the outlet, thereby generating a stretching force acting on the polymer solution, dividing the polymer solution at the outlet into droplets, and the droplets are stretched by the jet of compressed gas, thereby enabling the production of fibers at a high polymer injection speed.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: Japanese Patent Application Publication No. 60-119212

[0009] Patent Document 2: Japanese Patent Application Publication No. 2002-266154

[0010] Patent Document 3: Japanese Patent Application Publication No. 2022-32977 Summary of the Invention

[0011] The problem that the invention aims to solve

[0012] In the fiber manufacturing method disclosed in Patent Document 1, a configuration is disclosed in which a gas jet is supplied by multiple inclined nozzles to form a swirling flow near the discharge section. However, in the nozzle configuration of Patent Document 1, a straight airflow formed by compressed gas is directly injected into an open space. Therefore, the gas expands before forming the swirling flow, and the airflow speed decreases before colliding with the fiber, thus making it impossible to increase the swirling speed of the fiber. As a result, the swirling speed of the fiber is small, and sometimes the effect of reducing the fiber diameter cannot be fully obtained.

[0013] Furthermore, in the fiber manufacturing method disclosed in Patent Document 2, a spiral airflow is formed inside a pipe, and the fiber is twisted and stretched using this spiral airflow. However, in this method, while a spiral airflow is formed on the wall of the pipe, it is difficult for the spiral airflow to expand in the central part, and the airflow expands in a straight line along the length of the pipe. Therefore, it is difficult to apply the rotational force generated by the spiral airflow to the fiber, and the stretching effect brought about by twisting the fiber cannot be obtained, resulting in a situation where the fiber diameter cannot be reduced. In particular, even if the discharge pipe is positioned away from the discharge hole of the spinneret, the fiber is already in a cooled and solidified state inside the pipe, so the fiber cannot be stretched sufficiently.

[0014] In the fiber manufacturing method disclosed in Patent Document 3, a polymer solution is discharged while the fiber spinning needles are vibrating or rotating, thereby stretching the fiber. In this method, since a force is applied to the polymer from the wall of the outlet, a force to twist the discharged polymer cannot be directly applied from the compressed gas jet, thus failing to achieve the stretching effect resulting from the twisting of the fiber. Furthermore, since the area from the compressed gas jet injection point to the outlet where the polymer is discharged is not sealed, the compressed gas jet decelerates near the outlet, resulting in insufficient fiber stretching.

[0015] Therefore, the object of the present invention is to provide a method and apparatus for manufacturing fibers, which can obtain fibers with very small diameters by stretching the fibrous polymer discharged from the discharge hole while the polymer is in a deformable state before curing, by twisting it at high speed.

[0016] Methods for solving problems

[0017] The fiber manufacturing method of the present invention, which solves the above-mentioned problems, is a method of manufacturing fibers by stretching a fibrous polymer discharged from a spinneret having discharge holes. The fibrous polymer discharged from the spinneret is given a torsional force that rotates the fibrous polymer about the center of a cross section perpendicular to the polymer discharge direction in a manner that satisfies the following formula, thereby causing the fibrous polymer to be stretched while rotating.

[0018] W / V≥0.1[times / mm]

[0019] V: Ejection velocity of the fibrous polymer [mm / second]

[0020] W: Rotation speed of the fibrous polymer [times / second]

[0021] The fiber manufacturing method of the present invention preferably has any one or more of the following features (1) to (4).

[0022] (1) At one or more points in the range where the temperature of the fibrous polymer discharged from the above-mentioned spinneret is above (melting point of the fibrous polymer - 50°C), the fibrous polymer is rotated in a manner that satisfies the following formula.

[0023] W / V≥0.1[times / mm]

[0024] V: Ejection velocity of the fibrous polymer [mm / second]

[0025] W: Rotation speed of the fibrous polymer [times / second]

[0026] (2) By exposing the fibrous polymer to a swirling flow that rotates in the direction of rotation, a torsional force is imparted to the direction of rotation.

[0027] (3) The above-mentioned fibrous polymers are rotated around a straight line extending from the above-mentioned discharge hole in the direction of polymer discharge, so that the above-mentioned fibrous polymers are stretched while rotating.

[0028] (4) By bringing a roller that rotates in the opposite direction to the above-mentioned rotation direction into contact with the above-mentioned fibrous polymer, a torsional force in the above-mentioned rotation direction is imparted.

[0029] The fiber manufacturing apparatus of the present invention, which solves the above-mentioned problems, is an apparatus for producing fibers by stretching a fibrous polymer, comprising: a spinneret having a discharge orifice for discharging the fibrous polymer; an airflow nozzle disposed around the fibrous polymer discharged from the discharge orifice and used for spraying airflow; and an airflow sealing member disposed below the polymer discharge direction of the discharge orifice, having a space through which the fibrous polymer passes and a wall surrounding the space, wherein a swirling flow is formed by the jet stream sprayed from the airflow nozzle into the space, thereby imparting a torsional force in the rotational direction to the fibrous polymer, so that the fibrous polymer rotates about the center of a cross section perpendicular to the polymer discharge direction.

[0030] In the fiber manufacturing apparatus of the present invention, it is preferable that the fibrous polymer revolves around a straight line extending from the discharge hole in the polymer discharge direction by forming a swirling flow from the jet stream ejected from the airflow nozzle into the space.

[0031] Another aspect of the present invention for solving the above-mentioned problems is a fiber manufacturing apparatus that stretches a fibrous polymer to manufacture fibers, comprising: a spinneret having a discharge orifice for discharging the fibrous polymer; and a rotating roller configured to contact the fibrous polymer discharged from the discharge orifice.

[0032] By rotating the aforementioned rotating roller, a torsional force in the direction of rotation is applied to the aforementioned fibrous polymer, causing the aforementioned fibrous polymer to rotate about the center of a cross section perpendicular to the discharge direction.

[0033] In this invention, "polymer discharge direction" refers to the direction in which the fibrous polymer is discharged from the discharge hole.

[0034] In this invention, "torsional force" refers to the force that acts on the fiber surface in a direction of rotation, with the center of the fiber cross-section as the axis, in a plane perpendicular to the length direction of the fiber.

[0035] In this invention, "polymer discharge rate" refers to the length of polymer discharged from the discharge hole in the discharge direction per unit time, which is calculated by dividing the volume of polymer discharged from the discharge hole per unit time by the cross-sectional area of ​​the discharge hole.

[0036] In this invention, "rotation speed" refers to the rotational speed at which the fiber rotates 360 degrees per unit time in a plane perpendicular to the length direction of the fiber, with the center of the fiber cross-section as the axis.

[0037] In this invention, "swirling airflow" refers to an airflow that continuously rotates in a circular direction around a point 1 in a plane perpendicular to the length direction of the fiber.

[0038] The effects of the invention

[0039] According to the present invention, fibers with very small diameters can be manufactured by stretching the fibrous polymer discharged from the discharge hole while it is in a deformable state before curing, by twisting it at high speed. Attached Figure Description

[0040] [ Figure 1 ] Figure 1 A schematic cross-sectional view illustrating one embodiment of the fiber manufacturing apparatus of the present invention.

[0041] [ Figure 2 ] Figure 2 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention.

[0042] [ Figure 3 ] Figure 3 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention.

[0043] [ Figure 4 ] Figure 4 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention.

[0044] [ Figure 5 ] Figure 5 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention.

[0045] [ Figure 6 ] Figure 6 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention.

[0046] [ Figure 7 ] Figure 7 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention.

[0047] [ Figure 8 ] Figure 8 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention.

[0048] [ Figure 9 ] Figure 9 This is a schematic cross-sectional view showing an embodiment of a conventional fiber manufacturing apparatus.

[0049] [ Figure 10 ] Figure 10 This is a schematic cross-sectional view showing an embodiment of a conventional fiber manufacturing apparatus.

[0050] [ Figure 11 ] Figure 11This is a schematic cross-sectional view showing an embodiment of a conventional fiber manufacturing apparatus.

[0051] [ Figure 12 ] Figure 12 A schematic diagram illustrating the shape of the airflow sealing member in the fiber manufacturing apparatus of the present invention.

[0052] [ Figure 13 ] Figure 13 This is a schematic diagram illustrating the formation pattern of the swirling flow in the space of the airflow enclosure member in the fiber manufacturing apparatus of the present invention.

[0053] [ Figure 14 ] Figure 14 A schematic diagram illustrating an example of the shape of an airflow sealing member in a fiber manufacturing apparatus according to the present invention.

[0054] [ Figure 15 ] Figure 15 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention.

[0055] [ Figure 16 ] Figure 16 A schematic diagram illustrating the setting angle of the air nozzle.

[0056] [ Figure 17 ] Figure 17 A schematic diagram illustrating the jet direction of the jet stream from the air nozzle.

[0057] [ Figure 18 ] Figure 18 A schematic cross-sectional view illustrating a method for measuring the rotational speed of a single fibrous polymer.

[0058] [ Figure 19 ] Figure 19 A schematic cross-sectional view illustrating a method for measuring the tensile force of a single fibrous polymer.

[0059] [ Figure 20 ] Figure 20 A schematic diagram illustrating the setting angle of the air nozzle.

[0060] [ Figure 21 ] Figure 21 This is a schematic diagram of the molecular arrangement in the discharge section.

[0061] [ Figure 22 ] Figure 22 This is a schematic cross-sectional view showing an embodiment of a conventional fiber manufacturing apparatus. Detailed Implementation

[0062] Hereinafter, with reference to the accompanying drawings, various embodiments of the fiber manufacturing apparatus of the present invention and the fiber manufacturing method using the manufacturing apparatus will be described in detail. Figure 1 A schematic cross-sectional view illustrating one embodiment of the fiber manufacturing apparatus of the present invention. Figures 2-8 This is a schematic cross-sectional view of another embodiment of the fiber manufacturing apparatus of the present invention. Figures 9-11 These are schematic cross-sectional views of embodiments of conventional fiber manufacturing apparatus. In each figure, Figures A and B, shown on the right side of the figures, are cross-sectional views at lines A and B in the embodiments shown on the left side of the figures. These figures are schematic diagrams used to accurately convey the key points of the invention. The figures are simplified; the spinning apparatus of the present invention is not particularly limited, and the size ratios, etc., can be changed according to the embodiments. Furthermore, to facilitate understanding of the torsional force, the polymer 3 discharged from the discharge port 2 is depicted in enlarged dimensions in each figure.

[0063] First, the stretching phenomenon of fiber 4 in the fiber manufacturing method of the present invention will be explained. See [link to documentation]. Figure 9 Typically, in conventional fiber manufacturing methods known as meltblown fiber manufacturing, a single fiber 4 formed from polymer 3 discharged from a discharge port 2 is subjected to a tensile force 16 by directly spraying a jet stream 11 through two opposing nozzles. The polymer 3 is discharged from the discharge port 2 in a low-viscosity state, and the fiber 4 is stretched in the polymer discharge direction by the applied tensile force 16. At this time, the molecular orientation of the polymer 3 within the fiber 4 is aligned along the length of the fiber. On the other hand, by promoting molecular orientation within the fiber 4, the polymer 3 is difficult to deform in the orientation direction, i.e., difficult to stretch. Therefore, conventional manufacturing methods have limitations in reducing the diameter of the fiber 4.

[0064] In order to solve the above-mentioned problems, the inventors of this application conducted repeated and in-depth research, and as a result, focused on the direction of molecular orientation of fiber 4. As mentioned above, in conventional stretching methods, the stretching direction of fiber 4 is the same as the orientation of molecular orientation. Therefore, it is believed that by making this direction different, the stretching resistance caused by molecular orientation can be suppressed.

[0065] Reference Figure 21The relationship between the molecular orientation of polymer 3 and stretching is explained. Polymer 3 contains molecular chains 22. When polymer 3 is discharged from the discharge hole 2 during spinning, it is aligned along the length direction of the fiber 4. It is further aligned by stretching with a stretching force 16, and the molecular chains 22 are oriented as shown in Figure (a). Due to the orientation of the molecular chains 22 within polymer 3, there is no room for deformation in the orientation direction, and stretching of polymer 3 in the orientation direction is suppressed. That is, in conventional stretching methods, since the stretching force 16 is applied only in the length direction to stretch polymer 3, after the molecular chains 22 are oriented in the length direction by stretching polymer 3, further stretching in the length direction is suppressed. Therefore, it is considered that disturbing the orientation of the molecular chains 22 during stretching is effective in preventing stretching suppression. It was investigated that by applying a force that causes polymer 3 to move in a direction perpendicular to the length direction in addition to the stretching force 16 along the length direction during stretching, the orientation of the molecular chains 22 within polymer 3 is disturbed. As a means, the method focuses on rotating the fiber 4 about the center of the cross-section perpendicular to the discharge direction, i.e., applying a torsional force in the direction of rotation. Through the rotation of the fiber 4, the polymer 3 moves within the cross-section of the fiber 4, disrupting the orientation of the molecular chains 22 as shown in Figure (b). Especially in the molten state of the polymer 3, the molecular chains 22 are easily movable; therefore, by rotating the fiber 4, the effect of disrupting the molecular chains 22 can be more effectively achieved.

[0066] Thus, in the discharge portion of polymer 3 where the molecules within polymer 3 are oriented, and in the stretching portion of fiber 4, a torsional force is continuously applied in a direction perpendicular to the length direction of fiber 4, which is the stretching direction, causing fiber 4 to rotate at high speed, thereby disrupting the molecular orientation in the length direction and stretching fiber 4.

[0067] In addition, such as Figure 1 As shown, in the method of imparting torsional force to fiber 4 using the swirling flow 12, fiber 4, in addition to its own rotation, also revolves around the center of the swirling flow 12 with the discharge section as a fixed point. This promotes the disruption of molecular orientation along the length direction, enabling more effective stretching of fiber 4. In the configuration of imparting torsional force using the swirling flow 12, fiber 4 rotates at high speed around a straight line from the discharge hole 2 along the polymer discharge direction as its central axis. Through this swirling motion, centrifugal force acts on fiber 4, thereby promoting the stretching of fiber 4. The high-speed rotation of the discharged fiber 4 enables the fiber 4 to be reduced in diameter. The revolution speed of fiber 4 is preferably 100 times / second or more, more preferably 500 times / second or more.

[0068] In this context, the inventors of this application discovered during their research that, in order to achieve a smaller fiber diameter, fiber 4 needs to rotate at a high speed. In such cases... Figure 9In conventional manufacturing methods as shown, only a tensile force 16 in the longitudinal direction is applied to the fiber 4, and it is impossible to apply a torsional force to the fiber 4 to promote stretching. Furthermore, in... Figure 10 In conventional manufacturing methods, although the jet stream 11 is ejected from an angled airflow nozzle 5 arranged in a swirling manner, it is ejected into the atmosphere, causing the jet stream 11 to diffuse and fail to form a swirling flow, thus failing to impart a torsional force sufficient to rotate the fiber 4 at a sufficient speed. By stretching the fiber 4 using the manufacturing method of the present invention, the fiber 4 can be stretched while maintaining its easily deformable state relative to the stretching direction, thereby enabling the fiber 4 to be made thinner. Thus, it has been found that by applying a stretching force 16 acting on the fiber 4 in the length direction while causing the fiber 4 to rotate about the center of a section perpendicular to the length direction, the stretching efficiency of the fiber 4 is increased, thereby enabling the fiber 4 to be made thinner.

[0069] To achieve a smaller fiber diameter, the rotation speed of fiber 4 relative to the discharge speed of polymer 3 is crucial. During the spinning of fiber 4, stretching easily occurs near the discharge portion of discharge hole 2. When the rotation speed is slow relative to the discharge speed, the number of rotations relative to the length of the discharged fiber 4 is small, meaning the torsional force acting on the molecules in fiber 4 is weak, and the effect of disrupting molecular arrangement by the torsional force cannot be fully obtained, thus failing to promote stretching. Therefore, the fiber 4 needs to be rotated such that the discharge speed V (mm / s) and rotation speed W (times / s) satisfy W / V ≥ 0.1 (times / mm). Preferably, W / V ≥ 0.2 (times / mm). Furthermore, when the rotation speed is fast relative to the discharge linear speed, the number of rotations relative to the length of the discharged fiber 4 is large, meaning the torsional force acting on fiber 4 is large, which may cause fiber 4 to break due to shear stress generated in fiber 4. Therefore, it is preferable to adjust the discharge linear speed and the number of rotations so that W / V ≤ 5000 (times / mm).

[0070] It should be noted that, since it is difficult to measure the spin speed of the fiber during spinning, the spin speed in this invention, as described in “(1) Spin speed of the fiber (times / second)” of the embodiment described later, is the value obtained by measuring the spin speed of the fiber during rest.

[0071] Furthermore, the closer the torsional force that causes the fiber 4 to rotate is to the discharge section where the stretching phenomenon actively occurs, the more easily it is affected by the torsional force, and the easier it is to obtain a torsional stretching effect. Therefore, as the position where the torsional force is applied, a distance of 100 mm or less from the discharge direction of the discharge hole 2 of the spinneret 1 is preferred, and 50 mm or less is more preferred. In addition, by causing the fiber 4 to rotate within the stretching-promoting range, the effects of the present invention can be obtained. Therefore, when the polymer 3 in the fiber 4 is a crystalline polymer, it is preferable that the W / V ratio is ≥0.1 (times / mm) at at least one location in the temperature range above -50°C where the melting point is.

[0072] Next, the apparatus configuration for implementing such a manufacturing method is shown. To make the fiber 4 rotate, there are the following methods: a method of generating a torsional force in the fiber 4 by using a swirling flow; and a method of making the fiber 4 directly contact a rotating roller, thereby causing the torsional force to act on the fiber 4.

[0073] Reference Figure 1 The apparatus for manufacturing the fibers of the present invention will now be described. Figure 1 This is one embodiment of a fiber manufacturing apparatus that uses a swirling flow to generate torsional force in fiber 4. Figure 1 The fiber manufacturing apparatus 100 shown comprises the following components: a spinneret 1 having an outlet 2 for discharging polymer 3, which serves as the raw material for fiber 4; an air nozzle 5 disposed around the polymer 3 discharged from the outlet 2 and spraying a jet stream 11; an airflow sealing member 6 disposed below the polymer discharge direction of the outlet 2 and having a space 7 through which the polymer 3 and fiber 4 pass, and a wall 8 surrounding the space 7; and a winding roller 14 for winding the fiber 4. In this apparatus, the jet stream 11 is sprayed from the air nozzle 5 toward the wall 8 of the airflow sealing member 6, forming a swirling flow 12 within the space 7. Then, the fiber 4 obtained from the polymer 3 discharged from the spinneret 1 passes through this swirling flow 12 and is subsequently wound by the winding roller 14.

[0074] Reference Figure 12 The specific structure of the airflow sealing member 6 will be described below. The airflow sealing member 6 is composed of a cylindrical wall 8, and the space 7 surrounded by the wall 8 becomes the airflow passage. The space 7 is a through hole that extends from one end face of the airflow sealing member 6 to the other end face. The space 7 does not need to be completely surrounded by the wall 8 along its entire length; it is sufficient that the space 7 is completely surrounded by the wall 8 at a portion of its length.

[0075] Reference Figure 13 , 17 The flow of air based on the airflow sealing member 6 will be explained. Figure 13 This is a schematic diagram illustrating the formation pattern of the swirling flow in the space of the airflow enclosure member in the fiber manufacturing apparatus of the present invention. Figure 17A schematic diagram illustrating the jet direction of the jet stream from the air nozzle. (See diagram for example.) Figure 13 As shown, the jet stream 11, which has a velocity component in the circumferential direction of the fiber 4, is ejected toward the space 7 by colliding with the wall 8 of the airflow sealing member 6 from the air nozzle 5, thereby forming a high-speed swirling flow 12. Here, as... Figure 17 As shown, regarding the jet direction of the jet stream 11, the direction from the front end of the air nozzle 5 toward the center of the fiber 4 is defined as the radial direction, and the direction inclined at 90° from the radial direction is defined as the circumferential direction.

[0076] Refer again Figure 1 As shown in the cross-sectional view along line A, a jet stream 11 with a velocity component in the circumferential direction of the fiber 4 is ejected by colliding with the wall 8 of the airflow sealing member 6 from the air nozzle 5. In this way, as shown in the cross-sectional view along line B, a swirling flow 12 is formed around the fiber 4. By passing the fiber 4 through the swirling flow 12, a torsional force 17 is applied to the fiber 4, causing the fiber 4 to rotate at high speed. As a result, a tensile force 16 acting in the longitudinal direction of the fiber 4 and a torsional force 17 acting in the direction perpendicular to the longitudinal direction of the fiber 4 are imparted to the fiber 4, thereby stretching the fiber 4. Using this stretching method, it is possible to promote the reduction of the diameter of the fiber 4, and thus it is possible to stably obtain a small-diameter fiber 4.

[0077] Figure 10 This is a schematic cross-sectional view illustrating an embodiment of a conventional fiber manufacturing apparatus. Figure 10 In the fiber manufacturing apparatus 100I shown, the jet stream 11 is directly injected from the air nozzle 5 into an open space without surrounding walls 8. Because the jet stream 11 expands and diffuses immediately after injection, it is difficult to form a swirling flow 12, and thus impossible to generate the torsional force required to rotate the fiber 4 at a sufficient rotational speed. To generate a swirling flow that allows the fiber 4 to rotate sufficiently, it is necessary to prevent the diffusion of the jet stream 11. By providing an airflow sealing member 6 in the fiber manufacturing apparatus 100 of the present invention, the diffusion of the jet stream 11 can be prevented, enabling the fiber 4 to be made thinner.

[0078] Reference Figure 16 The air jet angle of the air nozzle 5 relative to the travel direction of the fiber 4 will be explained. Figure 16 This is a schematic diagram illustrating the setting angle of the air nozzle. If the angle α is small relative to the travel direction of the fiber 4, the rotational speed component of the swirling flow 12 tends to weaken. Conversely, if the angle α is greater than 90°, the airflow is injected in the opposite direction to the travel direction of the fiber 4, thus generating an airflow in the opposite direction to the stretching direction of the fiber 4, which easily hinders the stretching of the fiber 4. Therefore, the angle α between the air injection direction and the travel direction of the fiber 4 is preferably 5 to 90°.

[0079] Reference Figure 20 The jet angle of the jet stream 11 from the air nozzle 5 in a cross section perpendicular to the direction of travel of the fiber 4 will be explained. Figure 20 This is a schematic diagram illustrating the setting angle of the air nozzle in a cross-section perpendicular to the fiber's travel direction. If the angle β between the straight line connecting the center of the air nozzle 5's discharge portion and the center of the fiber 4 (the shortest straight line connecting the air nozzle 5 and the fiber 4) and the jet direction of the jet stream 11 is small, the jet stream 11 will directly collide with the fiber 4, making it difficult to form a swirling flow 12. Conversely, if the angle β is large, the jet will be sprayed in the opposite direction to the fiber 4, easily resulting in energy loss. Therefore, the angle β between the straight line connecting the center of the air nozzle 5's discharge portion and the center of the fiber 4 and the air jet direction is preferably 5 to 90°.

[0080] Figure 2 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention. Figure 1 In the fiber manufacturing apparatus 100, an air jet 11 is supplied by an air nozzle 5, forming a swirling flow 12 inside the airflow sealing member 6. On the other hand, as... Figure 2 The fiber manufacturing apparatus 100A shown thus allows for the dispersed supply of the jet stream 11 by providing multiple air nozzles 5, thereby enabling a more stable swirling flow 12. Therefore, it is preferable to use two or more air nozzles 5 for jetting, and more preferably three or more.

[0081] When using two or more air nozzles 5, by supplying the jet stream 11 evenly, a swirling flow 12 with less turbulence can be formed, enabling the fiber 4 to rotate continuously. Therefore, when using two or more air nozzles 5, it is preferable to... Figure 2 Air nozzles 5 are evenly arranged on the circle shown by the dashed line in A, and jet streams 11 are sprayed in the circumferential direction of the circle.

[0082] In order to form a swirling flow 12 in the space 7 of the airflow enclosure 6, the cross-sectional area of ​​the airflow path of the air nozzle is preferably smaller than the cross-sectional area of ​​the space 7. The cross-sectional shape of the airflow path of the air nozzle 5 is not limited to circular or rectangular, and can be any cross-sectional shape.

[0083] Figure 3 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention. Figure 1In the fiber manufacturing apparatus 100, the horizontal cross-sectional area of ​​the space of the airflow sealing member 6 is constant from the upper opening 9 to the lower opening 10. However, in order to draw the jet stream 11 from the air nozzle 5 into the space 7 of the airflow sealing member 6, the larger the cross-sectional area of ​​the space 7 at the upper opening 9 of the airflow sealing member 6, the easier it is to draw in the jet stream 11; conversely, the smaller the cross-sectional area of ​​the space 7 at the lower opening 10, the faster the airflow within the airflow sealing member 6 becomes, and the easier it is for the swirling flow 12 to accelerate. Therefore, as... Figure 3 In the fiber manufacturing apparatus 100B shown, the space 7 is preferably a structure in which the cross-sectional area at the lower opening 10 is reduced compared to the upper opening 9.

[0084] Since the fiber 4 rotates due to the swirling flow 12 formed by the airflow sealing member 6, and the center of the swirling flow 12 is aligned with the discharge direction of the fiber 4, the fiber 4 can be effectively rotated. Therefore, the central axis of the spiral of the swirling flow at the lower opening 10 of the airflow sealing member 6 is preferably aligned with the travel direction of the fiber 4.

[0085] The airflow sealing component 6 is a component that forms a swirling flow 12 from the jet flow 11. It can be as follows: Figure 1 The fiber manufacturing apparatus 100 shown in the diagram allows the swirling flow 12, formed by approximately half of the inner wall of the airflow sealing member 6, to collide with the fiber 4, which can also be achieved as shown in the diagram. Figure 3 The fiber manufacturing apparatus 100B shown in this way causes the swirling flow 12 to collide with the fiber 4 only from near the lower opening 10 of the airflow sealing member 6.

[0086] Figure 14 This is a schematic diagram illustrating an example of the shape of an airflow sealing member in a fiber manufacturing apparatus according to the present invention. Figure 14 As shown in the example, the airflow sealing member 6 can take various forms. The shape of the airflow sealing member 6 can be a circular and constant cross-section in the horizontal direction of space 7, as in (a), or a circular and conical cross-section in the horizontal direction of space 7, as in (b). Alternatively, it can be a rectangular and constant cross-section in the horizontal direction of space 7, as in (c), or a circular cross-section in the horizontal direction of space 7 with a passageway formed in the wall, as in (d). Furthermore, the airflow sealing member 6 can have forms other than those shown in (a) to (d).

[0087] Figure 15 This is a schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention. It should be noted that... Figure 15 The diagram of winding roller 14 is omitted. Figure 1 In the fiber manufacturing apparatus 100, the supply of the swirling flow 12 sometimes becomes unstable due to the influence of gas other than the jet flow 11 at the upper opening 9 of the airflow sealing member 6. Therefore, as Figure 15 In the fiber manufacturing apparatus 100K and 100L shown, the upper opening 9 of the airflow sealing member 6 can block the portion of the air nozzle 5 other than the air injection port.

[0088] If the cross-sectional area of ​​the space 7 of the airflow sealing member 6 is too small, the fiber 4 will adhere to the wall of the airflow sealing member 6 when it passes through, thereby easily deteriorating its spinnability. On the other hand, if the cross-sectional area is too large, the swirling flow 12 will slow down, and the torsional force used to make the fiber 4 rotate will easily weaken. Therefore, the cross-sectional area of ​​the surface with the smallest cross-sectional area of ​​the space 7 is preferably 1 mm. 2 Above and 100mm 2 the following.

[0089] Figure 7 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention. Figure 7 In the fiber manufacturing apparatus 100F, the spinneret 1 has multiple discharge holes 2, from which polymer 3 is discharged, stretching multiple fibers 4. Additionally, the fiber manufacturing apparatus 100F has one more air nozzle 5 than the number of discharge holes 2. Jet streams 11 are ejected from the air nozzle 5, which is arranged in a serrated pattern sandwiching one discharge hole 2, forming swirling flows 12 around each fiber 4. For a closed airflow member 6, using the spinneret 1 with multiple discharge holes 2, jet streams 11 are ejected from the multiple air nozzles 5 in such a way that each fiber 4 discharged from each discharge hole 2 generates a swirling flow 12. In the fiber manufacturing apparatus 100F, the production capacity of fine-diameter fibers 4 can be improved.

[0090] Figure 5 The schematic cross-sectional view shown is for another embodiment of the fiber manufacturing apparatus of the present invention, in which the fiber is in direct contact with a rotating roller, and a torsional force is applied to the fiber.

[0091] Figure 5 The fiber manufacturing apparatus 100D shown comprises the following components: a spinneret 1 having a discharge orifice 2 for discharging polymer 3; a rotating roller 13 arranged in contact with a fiber 4, wherein the fiber 4 is obtained by stretching the polymer 3 discharged from the discharge orifice 2; and a winding roller 14 for winding the fiber 4. In this apparatus, with the fiber 4 obtained from the polymer 3 discharged from the spinneret 1 in contact with the rotating roller 13, the rotating roller 13 is rotated, a torsional force 17 is applied to the fiber 4, and the fiber 4 is wound using the winding roller 14. In the fiber manufacturing apparatus 100D, the fiber 4 is stretched while being subjected to a tensile force 16 acting in the length direction and a torsional force 17 acting in the direction perpendicular to the length direction. This facilitates the reduction of the fiber diameter, thus enabling the stable production of fine-diameter fibers 4.

[0092] In the fiber manufacturing apparatus 100D, the rotating roller 13 rotates at a high speed, resulting in the following situation: the traveling fiber 4 collides with the corner of the side of the rotating roller 13 and is cut off. Therefore, the corner of the side of the rotating roller 13 is preferably curved.

[0093] The rotating roller 13 comes into contact with the traveling fiber 4, so if it operates continuously, the side portion of the rotating roller 13 in contact with the fiber 4 will wear. Therefore, the side portion of the rotating roller 13 is preferably made of ceramic.

[0094] Regarding the setting angle of the shaft of the rotating roller 13, in Figure 5 In the middle, it is set parallel to the direction of travel of fiber 4, but as long as the torsional force 17 can be applied to fiber 4, it can be tilted in the range of 0 to 85 degrees from the direction parallel to the direction of travel of fiber 4.

[0095] Figure 8 A schematic cross-sectional view illustrating another embodiment of the fiber manufacturing apparatus of the present invention. Figure 8 In the fiber manufacturing apparatus 100G shown, in order to effectively apply the torsional force 17 to the fiber 4, a plurality of spinnerets 1 are arranged around a rotating roller 13, so that multiple fibers 4 discharged from each spinneret 1 come into contact with the rotating roller 13, and are subjected to torsional force for spinning. In the fiber manufacturing apparatus 100G, the production capacity of fine-diameter fibers 4 can be improved.

[0096] Next, the common preferred embodiments of the present invention will be described.

[0097] See Figure 1 , 7 The recycling methods for fiber 4 are not limited to... Figure 1 The winding roller 10 shown can also be used Figure 7 The fiber rollers and other components shown are used for recycling. By using the conveyor 12 and fiber rollers, the fiber 4 can be moved without restricting its position at the recycling location, thus allowing it to twist freely without constraining its position and improving the stretching effect.

[0098] This invention is highly versatile and can be applied to the manufacture of all known fibers. Therefore, it is not particularly limited by the polymers constituting the fibers. For example, examples of polymers constituting fiber 4 include polyester, polyamide, polyphenylene sulfide, polyolefin, polyethylene, and polypropylene. Furthermore, these polymers may contain various functional particles and organic compounds, such as matting agents like titanium dioxide, silica, kaolin, anti-coloring agents, stabilizers, antioxidants, deodorizers, flame retardants, silk friction reducers, coloring pigments, and surface modifiers, without impairing spinning stability, and may also include copolymers.

[0099] The polymer constituting fiber 4 can be composed of a single component or multiple components. In the case of multiple components, for example, a core-sheath or a combination thereof can be used.

[0100] The cross-sectional shape of the fiber 4 can be circular, triangular, flat, polygonal, star-shaped, or hollow. By making the cross-sectional shape different from a perfect circle, the surface area per unit volume increases, making it easier to withstand the torsional force 17 from the swirling flow 12 and the rotating mill 13, thus increasing the rotational speed and resulting in finer fibers 4. Therefore, it is preferable to form a flat cross-sectional shape from a perfect circle, and more preferably a cross-sectional shape with uneven surfaces.

[0101] Furthermore, although the purpose of this invention is to manufacture fine-diameter fibers 4, the fineness of the monofilaments is not particularly limited.

[0102] Example

[0103] The present invention will be described in more detail below with examples. It should be noted that the methods for measuring characteristic values ​​in the examples are as follows.

[0104] (1) Fiber rotation speed (times / second)

[0105] Figure 18 A schematic diagram illustrating the method for measuring the rotational speed of a fiber is shown. A single 32-dtex PET filament, 19, is fixed from the top of a spinneret 1, and a high-speed camera 18 is installed. A mark is made of black ink on the fiber surface at a distance of 10 mm from the outlet surface of the discharge hole 2 of the spinneret 1. The behavior of the fiber at the marked mark is observed for 0.1 seconds using the high-speed camera 18. In the captured dynamic image, the number of rotations of the measuring fiber 19 is counted based on the movement of the mark, thereby measuring the number of fiber rotations per second, which is used as the fiber's rotational speed. Regarding the measurement of the number of rotations in the apparatus of the embodiments and comparative examples described later, the measuring fiber 19 and the high-speed camera 18 are installed in the apparatus of the embodiments and comparative examples, and the measurement is performed with the air nozzle 5 and the rotary mill 14 in operation.

[0106] (2) Average fiber diameter (μm)

[0107] Ten samples were randomly collected from the spun fibers, and their surfaces were photographed at 1000x magnification using a microscope. The fiber width was determined based on the photographs, and their average value was used as the average fiber diameter.

[0108] (3) Discharge speed (mm / second)

[0109] Based on the polymer discharge rate (mm) from the discharge orifice of the spinning spinneret set under various conditions. 3 / second) and the cross-sectional area of ​​the discharge hole at the spinneret exit (mm²) 3 Based on the following formula, the discharge rate is calculated.

[0110] • Discharge rate = Polymer discharge rate / Discharge orifice cross-sectional area

[0111] (4) Tensile force (mN)

[0112] Figure 19 A schematic diagram illustrating the method for measuring traction force is shown. First, a single 32-dtex PET measuring fiber 19 is fixed to a tension meter 20 (AIKOH ENGINEERING MODEL-RX-1) at a length 1000 mm from the lower surface of the spinneret. An airflow ejected from the air nozzle 5 collides with the measuring fiber 19, and the resulting tension (mN) is measured using the tension meter 16. This measurement is repeated 5 times, and the average value (mN) is taken as the tensile force. Regarding the measurement of tensile force in the apparatus of the embodiments and comparative examples described later, the measuring fiber 19 is fixed to the apparatus of the embodiments and comparative examples, and the measurement is performed with the air nozzle 5 in operation.

[0113] (5) Temperature of the fiber discharge section (°C)

[0114] A thermocouple measuring section is installed at a distance of 10 mm from the outlet surface of the spinneret discharge hole in the discharge direction to measure the ambient temperature of the spinneret discharge section during spinning. This measurement is repeated 3 times and recorded as the fiber discharge section temperature (°C).

[0115] (Examples 1-8, Comparative Examples 1-5)

[0116] use Figures 1-11 The manufacturing apparatus shown is used for fiber production. The raw material resin is selected according to ASTM-D1238, with a melt flow rate of 1100 g / 10 min and a density of 0.9 g / cm³ under the conditions of a weight of 2.16 kg and a temperature of 230 °C. 3Polypropylene resin with a melting point of 180℃ was used. The polymer, with a molten resin temperature of 280℃, was discharged from the spinneret outlet through a nozzle with an orifice diameter of 0.25 mm and a single-orifice discharge rate of 2 g / min. Fibers were manufactured under the conditions shown in Tables 1-3, where hot air at 280℃ was supplied through an air nozzle with an orifice diameter of 2 mm, an angle of 10° between the air jet direction and the fiber travel direction, and a tensile force of 15 mN. The polymer discharge velocity at this time was 755 mm / s. The experimental results are shown in Tables 1-3.

[0117] [Example 1]

[0118] Evaluate the effect of utilizing the torsion of the swirling flow. (Using...) Figure 1 The fiber manufacturing apparatus 100 shown discharges polymer 3 from one discharge port 2 of the spinneret 1. An air nozzle 5 is configured such that the angle β between the straight line connecting the air nozzle discharge section and the fiber center and the jet direction is 80°. A jet stream is supplied from one air nozzle 5 into the space 7 of an airflow-sealing member 6 with an inner diameter of Φ5 mm and a height of 5 mm. The fiber 4 is stretched by a torsional force applied by a swirling flow 12 from a position directly below the discharge port 2, and then wound by a winding roller 14. The fiber discharge section temperature during spinning is 215°C, the fiber rotation frequency W / discharge velocity V is 0.79 times / mm, and the average fiber diameter of the collected fibers is 2.60 μm.

[0119] It should be noted that during spinning, the temperature of the fibrous polymer reaches its maximum at the discharge orifice 2. As the distance from the discharge orifice 2 increases, the temperature of the fibrous polymer decreases. Therefore, by measuring the temperature and rotation speed of the fibrous polymer at approximately the same location near the discharge orifice, if its temperature is above (the melting point of the fibrous polymer - 50°C) and the W / V at that location is above 0.1 times / mm, it can be considered that the fibrous polymer rotates at at least one location where its temperature is above (the melting point of the fibrous polymer - 50°C) and satisfies W / V ≥ 0.1 times / mm. The same principle applies to the following examples and comparative examples.

[0120] [Example 2]

[0121] Evaluate the impact of the number of air nozzles. (Use...) Figure 2The fiber manufacturing apparatus 100A shown discharges polymer 3 from one discharge port 2 of the spinneret 1. Air nozzles 5 are configured such that the angle β = 80° between the line connecting the air nozzle discharge section and the fiber center and the air jet direction. Jet flow is supplied from the three air nozzles 5 into the space 7 of the airflow sealing member 6, and the fiber 4 is stretched under torsional force from a position directly below the discharge port 2. The fiber 4 is then wound using a winding roller 14. During spinning, the fiber discharge section temperature is 209°C, the fiber rotation frequency W / discharge velocity V is 0.83 times / mm, and the average fiber diameter of the collected fibers is 2.59 μm.

[0122] [Example 3]

[0123] Evaluate the effect of swirling flow generated by airflow enclosures of different shapes. Using Figure 3 The fiber manufacturing apparatus 100B shown discharges polymer 3 from one discharge hole 2 of the spinneret 1. Air nozzles 5 are configured such that the angle β = 80° between the straight line connecting the air nozzle discharge section and the fiber center and the air jet direction. Jet flow is supplied from the three air nozzles 5 into the space 7 of the airflow sealing member 6 (inner diameter Φ 5 mm, height 5 mm, cone angle 60°, distance between the air discharge surface and the polymer discharge surface 5 mm). Fiber 4 is stretched under torsional force from a position directly below the discharge hole 2 outlet, and wound using a winding roller 14. The fiber discharge section temperature during spinning is 195°C, the fiber rotation frequency W / discharge speed V is 0.92 times / mm, and the average fiber diameter of the collected fibers is 2.56 μm.

[0124] [Example 4]

[0125] The effect of temperature reduction is evaluated when utilizing the torsion of swirling flow. (Using...) Figure 4 The fiber manufacturing apparatus 100C shown discharges polymer 3 from one discharge port 2 of the spinneret 1. Air nozzles are arranged such that the angle β between the line connecting the air nozzle discharge section and the fiber center and the air jet direction is 80°. Jet flow is supplied from three air nozzles into the space 7 of the airflow sealing member 6, and fiber 4 is stretched under torsional force from a position 200 mm from the outlet of discharge port 2. Fiber 4 is then wound using a winding roller 14. The fiber discharge section temperature during spinning is 124°C, the fiber rotation frequency W / discharge velocity V is 0.75 times / mm, and the average fiber diameter of the collected fibers is 3.16 μm.

[0126] [Example 5]

[0127] Evaluate the effect of the torsion of the rotating roller. (Using...) Figure 5The fiber manufacturing apparatus 100D shown discharges polymer 3 from one discharge hole 2 of the spinneret 1. A torsional force is applied to the fiber 4 by bringing it into contact with a rotating roller 13 (speed: 30 rpm) positioned 200 mm from the outlet of the discharge hole 2, and then winding the fiber 4 using a winding roller 14. The fiber discharge temperature during spinning is 120°C, the fiber rotation frequency W / discharge velocity V is 0.22 times / mm, and the average fiber diameter of the collected fibers is 3.37 μm.

[0128] [Example 6]

[0129] The impact of changing fiber collection to a conveyor system was evaluated. (Using...) Figure 6 The fiber manufacturing apparatus 100E shown discharges polymer 3 from one discharge port 2 of the spinneret 1. Air nozzles are arranged such that the angle β between the line connecting the air nozzle discharge section and the fiber center and the air jet direction is 80°. Jet flow is supplied from three air nozzles 5 into the space 7 of the airflow sealing member 6, and the fiber 4 is stretched under torsional force from a position directly below the outlet of the discharge port 2. The fiber 4 is collected by a conveyor 15. The fiber discharge section temperature during spinning is 209°C, the fiber rotation frequency W / discharge velocity V is 0.87 times / mm, and the average fiber diameter of the collected fibers is 2.58 μm.

[0130] [Example 7]

[0131] Evaluate the impact of increasing the number of discharge orifices in the spinneret. (Using...) Figure 7 The fiber manufacturing apparatus 100F shown discharges polymer 3 from 10 discharge holes 2 of the spinneret 1. Eleven air nozzles are arranged in a sawtooth pattern, with the angle β = 80° between the line connecting the air nozzle discharge section and the fiber center and the air jet direction, and each nozzle is positioned opposite one discharge hole 2. A jet stream is supplied from the air nozzles 5 into the space of the airflow sealing member 7, forming swirling flows 12 around each polymer. The fiber 4 is stretched under torsional force from a position directly below the discharge hole 2 outlet, and collected by a conveyor 15. The fiber discharge section temperature during spinning is 190°C, the fiber rotation frequency W / discharge velocity V is 0.59 times / mm, and the average fiber diameter of the collected fibers is 2.66 μm.

[0132] [Example 8]

[0133] Evaluate the effect of increasing the number of discharge holes relative to the rotating roller. Using... Figure 8The fiber manufacturing apparatus 100G shown discharges polymer 3 from each of the discharge holes 2 of 10 spinnerets 1. Ten fibers 4 are brought into contact with a rotating roller 13 positioned 200 mm from the outlet of the discharge hole 2, thereby applying a torsional force to the fibers 4, which are then wound around by a winding roller 14. The fiber discharge temperature during spinning is 120°C, the fiber rotation frequency W / discharge speed V is 0.20 times / mm, and the average fiber diameter of the collected fibers is 3.40 μm.

[0134] [Comparative Example 1]

[0135] A conventional spinning method using an airflow without swirling components is evaluated. Using... Figure 9 The fiber manufacturing apparatus 100H shown discharges polymer 3 from one discharge port 2 of the spinneret 1. The air nozzles are configured such that the angle β between the straight line connecting the air nozzle discharge section and the fiber center and the air jet direction is 0°. Jet streams are ejected from two air nozzles 5 to the discharged polymer 3, thereby stretching the fiber 4, which is then wound around the fiber 4 using a winding roller 14. During spinning, the fiber discharge section temperature is 184°C, the fiber does not rotate, and the average fiber diameter of the collected fibers is 4.77 μm.

[0136] [Comparative Example 2]

[0137] A review of conventional spinning methods that involve injecting a jet stream along the circumferential direction of the fiber in the atmosphere is conducted. Using... Figure 10 The fiber manufacturing apparatus 100I shown is as follows: Polymer 3 is discharged from one discharge hole 2 of the spinneret 1. The air nozzles are arranged such that the angle β between the straight line connecting the air nozzle discharge section and the fiber center and the air jet direction is 80°. Jet streams are ejected from three air nozzles 5 to the discharged polymer 3, thereby stretching the fiber 4, which is then wound by a winding roller 14. During spinning, the fiber discharge section temperature is 175°C, the fiber does not rotate, and the average fiber diameter of the collected fibers is 4.65 μm.

[0138] [Comparative Example 3]

[0139] A conventional spinning method using a jet of air without swirling components and with multiple discharge holes was evaluated. Figure 11 The fiber manufacturing apparatus 100J shown discharges polymer from 10 discharge holes 2 of a spinneret 1. Twenty air nozzles 5 are arranged such that the angle β between the line connecting the air nozzle discharge section and the fiber center and the air jet direction is 0°, with one discharge hole 2 sandwiched between them. For the polymer 3 discharged from each discharge hole 2, jet streams are ejected from two opposing air nozzles, thereby stretching the fiber 4, which is then collected by a conveyor 15. During spinning, the fiber discharge section temperature is 185°C, the fiber does not rotate, and the average fiber diameter of the collected fibers is 4.95 μm.

[0140] [Comparative Example 4]

[0141] By reducing the angle β between the straight line connecting the air nozzle discharge section and the fiber center and the air injection direction, the swirling flow of the injected air is suppressed, thereby evaluating the effect on the fiber rotation frequency. Figure 22 The fiber manufacturing apparatus 100M shown discharges polymer 3 from one discharge port 2 of the spinneret 1. An air nozzle is configured such that the angle β = 3° between the line connecting the air nozzle discharge section and the fiber center and the air jet direction. A jet stream is supplied from one air nozzle 5 into the space 7 of the airflow sealing member 6. The fiber 4 is stretched under torsional force from a position directly below the discharge port outlet, and wound using a winding roller 14. The fiber rotation frequency W / discharge velocity V is less than 0.1 times / m. The fiber discharge section temperature during spinning is 210°C, the fiber rotation frequency W / discharge velocity V is 0.05 times / mm, and the average fiber diameter of the collected fibers is 4.58 μm.

[0142] [Comparative Example 5]

[0143] The effect of reducing the rotational speed of a rotating roller during its torsion process was evaluated. Figure 5 The fiber manufacturing apparatus 100D shown discharges polymer 3 from one discharge hole 2 of the spinneret 1, bringing fiber 4 into contact with a rotating roller 13 (rotation speed: 5 rpm) positioned 200 mm from the discharge hole outlet. This causes a torsional force to act on the fiber 4, which is then wound around by the winding roller 13. The fiber rotation frequency W / discharge velocity V is less than 0.1 times / mm. The fiber discharge temperature during spinning is 120°C, the fiber rotation frequency W / discharge velocity V is 0.03 times / mm, and the average fiber diameter of the collected fibers is 4.67 μm.

[0144] The evaluation conditions and results for each embodiment and comparative example are summarized in Tables 1-3. In Examples 1, 2, 3, 4, 6, and 7, the fibers were twisted using a swirling flow; in Examples 5 and 8, the fibers were twisted using a rotating roller. This improved the fiber diameter reduction compared to Comparative Examples 1-5. Furthermore, in Example 1, the temperature at the twisted portion was high, which further improved the fiber diameter reduction compared to Example 4.

[0145] [Table 1]

[0146]

[0147] [Table 2]

[0148]

[0149] [Table 3]

[0150] (Table 3)

[0151]

[0152] Industrial availability

[0153] The manufacturing method and apparatus of the present invention are not limited to filaments, but can also be applied to the spinning of fibers for other purposes such as nonwoven fabrics.

[0154] Explanation of reference numerals in the attached figures

[0155] 1. Spinneret

[0156] 2 Discharge holes

[0157] 3 polymers

[0158] 4 fibers

[0159] 5 air nozzles

[0160] 6 airflow sealing components

[0161] 7 spaces

[0162] 8 walls

[0163] 9. Upper opening

[0164] 10. Lower opening

[0165] 11 Jet Stream

[0166] 12 Swirling Flow

[0167] 13 Rotating rollers

[0168] 14 winding rollers

[0169] 15 Conveyors

[0170] 16 Tensile force

[0171] 17 Torsional force

[0172] 18 High-speed cameras

[0173] 19. Determination of fiber properties

[0174] 20 Tension gauge

[0175] 21 Rotation Measurement Points

[0176] 22 molecular chains

Claims

1. A method for producing fibers, the method comprising: stretching a fibrous polymer discharged from a spinneret having a discharge hole to produce fibers, The fibrous polymer discharged from the spinneret is subjected to a torsional force that rotates the fibrous polymer about the center of a cross section perpendicular to the polymer discharge direction as an axis in a manner satisfying the following formula, thereby stretching the fibrous polymer while rotating. W / V≥0.1[times / mm] V: Discharge velocity of fibrous polymer [mm / sec] W: Rotation speed of fibrous polymer [times / second].

2. The method for producing the fiber according to claim 1, in, The fibrous polymer is rotated at one or more locations in a range where the temperature of the fibrous polymer discharged from the spinneret is equal to or higher than (melting point of the fibrous polymer - 50°C), so as to satisfy the following formula: W / V≥0.1[times / mm] V: Discharge velocity of fibrous polymer [mm / sec] W: Rotation speed of fibrous polymer [times / second].

3. The method for producing the fiber according to claim 1 or 2, in, The fibrous polymer is exposed to a swirling flow swirling in the rotation direction, thereby imparting a torsional force in the rotation direction.

4. The method for producing a fiber according to any one of claims 1 to 3, in, The fibrous polymer is caused to revolve around a straight line extending from the discharge hole in the polymer discharge direction as a central axis, and the fibrous polymer is stretched while rotating.

5. The method for producing the fiber according to claim 1 or 2, in, A torsional force in the rotation direction is imparted by bringing a roller rotating in a direction opposite to the rotation direction into contact with the fibrous polymer.

6. A fiber manufacturing device, which is a device for manufacturing fibers by stretching a fibrous polymer, comprising: a spinneret having a discharge hole for discharging the fibrous polymer; an air flow nozzle disposed around the fibrous polymer discharged from the discharge hole and configured to spray an air flow; and an airflow sealing member disposed below the discharge hole in the polymer discharge direction and having a space through which the fiber polymer passes and a wall surrounding the space, The jet jetted from the air flow nozzle into the space forms a swirling flow, thereby applying a twisting force in a rotational direction to the fibrous polymer, so that the fibrous polymer rotates about the center of a cross section perpendicular to the polymer discharge direction.

7. The fiber manufacturing device according to claim 6, in, The jet flow ejected from the air flow nozzle into the space forms a swirling flow, so that the fibrous polymer revolves around a straight line extending from the discharge hole in the polymer discharge direction as a central axis.

8. A fiber manufacturing device, which is a device for manufacturing fibers by stretching a fibrous polymer, comprising: a spinneret having discharge holes for discharging a fibrous polymer; and a rotating roller arranged so as to contact the fibrous polymer discharged from the discharge hole, By rotating the rotating roller, a torsional force in the rotation direction is applied to the fibrous polymer, so that the fibrous polymer rotates about the center of the cross section perpendicular to the discharge direction as an axis.

Citation Information

Patent Citations

  • Spinning assembly for piezoelectric material-containing polymeric fiber and melt spinning method using the same

    JP2002266154A

  • Device and method for manufacturing polymer fiber and use of polymer fiber

    JP2022032977A

  • Melt-blown nozzle component for preparing nanofibers and nozzle device

    CN103510164A

  • Tornado cyclone type device for preparing nano twisting electrostatic spinning nozzle

    CN104726943A

  • Stretching device as well as manufacturing device and manufacturing method for fiber and fiber web

    CN111868312A