High molecular weight GPAM containing anionic polysaccharide promoters

By combining high molecular weight cationic GPAM with anionic polysaccharide accelerators, the problem of GPAM's sensitivity to environmental conditions during papermaking is solved, resulting in a significant improvement in the dry strength and tear resistance of paper products.

CN118922600APending Publication Date: 2024-11-08KEMIRA OY

Patent Information

Application Number
CN202380021321.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2023-02-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing glyoxylated polyacrylamide (GPAM) is sensitive to environmental conditions during the papermaking process, resulting in unstable dry strength properties, especially performance loss under high pH and high alkalinity conditions, and the use of precipitated calcium carbonate further affects its performance.

Method used

A composition is formed by combining high molecular weight cationic glyoxal polyacrylamide (GPAM) with anionic polysaccharide accelerators (such as carboxymethyl cellulose, CMC) to enhance the dry strength of paper or paperboard. By adding this composition to cellulose fiber raw materials, the tensile strength, bursting resistance and compression resistance of paper products can be improved.

Benefits of technology

It significantly improves the dry tensile strength, burst resistance and compression resistance of paper products, and outperforms the effects of using low molecular weight GPAM and anionic polyacrylamide (APAM) accelerators alone at lower doses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The present invention provides a composition and method for strengthening a paper product. The compositions of the present invention comprise a combination of at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer and at least one anionic polysaccharide promoter ("APP"). The method of the present invention for manufacturing a paper product having enhanced dry strength properties comprises adding to a fibrous feedstock comprising cellulosic fibers at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer, and at least one anionic polysaccharide promoter ("APP").
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Applications

[0002] This application claims priority to U.S. Provisional Application No. 63 / 309,749 filed on February 14, 2022 and Finnish Application No. FI20225307 filed on April 7, 2022, the contents of both applications being incorporated by reference in their entirety. Technical Field

[0003] The present invention generally relates to a combination of at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer and at least one anionic polysaccharide accelerator ("APP") for strengthening paper and paperboard, and methods of using the combination. More specifically, the present invention relates to adding a cationic GPAM comprising a high molecular weight base polymer and an APP to a cellulosic fiber feedstock to form a strengthened paper product having improved tensile strength. Background Art

[0004] In papermaking applications, strengthening agents are often used to provide the desired properties required in the final paper product. These properties include dry and wet tensile strength. Tensile strength is a measure of the resistance of a finished paper or paperboard product to break or tear under a force load.

[0005] Glyoxylated polyacrylamide (GPAM) products are widely used in the papermaking industry and are commonly used to improve the wet strength and dry strength of paper. GPAM is usually prepared by the reaction between glyoxal and a cationic polyacrylamide base polymer, which usually contains acrylamide monomers and cationic monomers, such as DADMAC (for example, as described in U.S. Patents 3,556,932, 4,605,702 and 7,828,934). Original GPAM has been reported in U.S. Patent 3,556,932. The molecular weight of the cationic polyacrylamide base polymer is less than 25,000Da, and the molar ratio of acrylamide to diallyldimethylammonium chloride is 99:1 to 75:1. U.S. Patent No. 9328462 and U.S. Patent No. 9506195 claim the combination of GPAM and anionic polyacrylamide (APAM) to improve the dehydration rate of papermaking and enhance the strength properties of paper.

[0006] GPAM is a common temporary wet strength resin. For example, glyoxylated polyacrylamide can improve the initial wet strength of many household toilet papers, a useful property because household toilet papers are often in contact with water during use. Glyoxylated polyacrylamide applied to paper products can also improve the compressive strength and dimensional stability of many paperboard products. GPAM is typically added to the pulp suspension before the paper is formed. After the treated paper is dried, GPAM is thought to form covalent bonds with the paper cellulose, thereby improving the dry strength of the paper.

[0007] However, reactive strength resins (such as GPAM) have certain limitations and are not suitable for certain types of paper. First, reactive strength resins increase the wet strength of paper because the covalent bonds remain intact in water. High wet strength can cause difficulties in repulping and dispersion. To break down high wet strength paper, excessive mechanical force, harsh chemicals, or both are required. If wet strength is not desired, care must be taken. The formation of covalent bonds is sensitive to environmental conditions (such as pH, alkalinity, inorganic ions, and temperature). Paper machine white water is a rather complex system that may hinder the performance of reactive strength resins. This may be an important reason why many conflicting results have been reported on the performance of reactive dry strength resins (such as GPAM).

[0008] High pH and high alkalinity levels can adversely affect GPAM dry strength properties. It is generally believed that hydroxide ions interact with aldehyde groups during the thermal drying process, deactivating GPAM as a strength resin. Therefore, GPAM is generally not recommended for use when the wet-end pH is above 8.0, the alkalinity level is above 200 ppm, or both. Precipitated calcium carbonate (PCC) is one of the most popular inorganic fillers in modern papermaking, especially for printing and writing papers. PCC significantly increases the wet-end alkalinity level, resulting in a loss of GPAM performance. In addition, since PCC is introduced through recycled printing and writing paper, GPAM is not effective on some recycled pulp furnishes.

[0009] It is therefore an object of the present invention to provide a composition for increasing the dry strength of paper or paperboard which composition provides an increase in dry strength compared to the use of GPAM alone.

[0010] Another object of the present application is to provide a papermaking method for making paper having enhanced dry strength properties over that of GPAM alone.

[0011] The present application discloses compositions and methods for enhancing the dry strength of paper products using high molecular weight cationic GPAM as a strengthening agent in combination with an anionic polysaccharide accelerator ("APP"). The new system exhibits improved strength properties of paper compared to GPAM / APAM systems where the molecular weight of the GPAM base polymer is less than 50 kDa. The method of the present invention meets the paper industry's need for a cost-effective and efficient strengthening agent. Summary of the invention

[0012] The present disclosure generally encompasses compositions or combinations of materials for strengthening paper or paperboard. The composition or combination may include at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer; and at least one anionic polysaccharide accelerator ("APP").

[0013] The present disclosure also generally encompasses a method for making one or more paper products having enhanced strength properties. The method may include adding to a fiber feedstock comprising cellulosic fibers at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer; and at least one anionic polysaccharide accelerator ("APP").

[0014] In particular, the results disclosed herein demonstrate that a combination of high molecular weight cationic GPAM and APP can be used to enhance the strength parameters and repulpability of one or more paper products, optionally absorbent paper products.

[0015] The methods of making one or more paper products of the present invention have one or more of the following advantages: (i) improved dry tensile strength; (ii) improved resistance to rupture (as measured by bursting strength); (iii) improved resistance to compression (as measured by the STFI compression test); and (iv) improved resistance to tearing compared to paper products made in an equivalent manner using cationic GPAM and anionic polyacrylamide (APAM) promoters comprising lower molecular weight base polymers (e.g., less than 50 kDa).

[0016] The present disclosure provides a composition for strengthening paper or paperboard, optionally an aqueous composition. In some embodiments, the composition comprises at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer; and at least one anionic polysaccharide promoter ("APP"), optionally carboxymethyl cellulose (CMC). In some embodiments, the high molecular weight base polymer has a weight average molecular weight selected from at least 50 kDa, at least 80 kDa, at least 100 kDa, at least 250 kDa, and 100 kDa-5000 kDa.

[0017] The present disclosure also provides a material combination. In some embodiments, the combination comprises at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer, optionally an aqueous composition; and at least one anionic polysaccharide promoter ("APP"), optionally carboxymethyl cellulose (CMC).

[0018] In some embodiments, the high molecular weight base polymer (a) has a weight average molecular weight selected from at least 50 kDa, at least 80 kDa, at least 100 kDa, at least 250 kDa, and 100 kDa-5000 kDa. In some embodiments, when the combination of materials (a) and (b) is added separately, simultaneously, or as a premixed combination to a papermaking system or a furnish composition comprising a furnish composition, the furnish composition comprises cellulose fibers for making paper or paperboard, wherein (a) and (b) may be added in any order, and a paper or paperboard material having enhanced strength is produced compared to when the combination of materials (a) and (b) is not added to the papermaking system or the furnish composition.

[0019] In some embodiments, at least one cationic GPAM comprising a high molecular weight base polymer comprises one or more of the following properties:

[0020] a) comprising a weight ratio range of glyoxal:base polymer selected from 1:99 to 50:50 and 5:95 to 20:80; b) obtained by reacting glyoxal with said high molecular weight base polymer, wherein the high molecular weight base polymer comprises an acrylamide-based copolymer comprising a neutral monomer, a cationic monomer and optionally an anionic monomer, further wherein

[0021] i) the neutral monomer is selected from monomers containing primary amides, which monomers include acrylamide, methacrylamide, ethyl acrylamide, crotonamide, N-methyl acrylamide, N-butyl acrylamide, N-ethyl methacrylamide and any combination thereof;

[0022] ii) the cationic monomer is selected from acryloyloxyethyl trimethyl ammonium chloride ("AETAC"), methacryloyloxyethyl trimethyl ammonium chloride ("MAETAC"), methacrylamidopropyl trimethyl ammonium chloride ("MAPTAC"), acrylamidopropyl trimethyl ammonium chloride ("APTAC"), methacryloyloxyethyl dimethyl ammonium sulfate, diallyl dimethyl ammonium chloride ("DADMAC"); dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, including but not limited to dimethylaminoethyl acrylate ("DMAEA"), dimethylaminoethyl methacrylate ("DMAEA"), dimethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl acrylate methyl sulfate quaternary salt, dimethylaminoethyl acrylate benzyl chloride quaternary salt, dimethylaminoethyl acrylate sulfate, dimethylaminoethyl acrylate hydrochloride, diethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate ester methyl sulfate quaternary salt, dimethylaminoethyl methacrylate benzyl chloride quaternary salt, dimethylaminoethyl methacrylate sulfate, dimethylaminoethyl methacrylate hydrochloride, dimethylaminoethyl methacrylate hydrochloride; dialkylaminoalkyl acrylamides and methacrylamides and their quaternary or acid salts, including but not limited to acrylamidopropyl trimethylammonium chloride, dimethylaminopropyl acrylamide, dimethylaminopropyl acrylamide methyl sulfate quaternary salt, dimethylaminopropyl acrylamide sulfate, dimethylaminopropyl acrylamide hydrochloride, methacrylamidopropyl trimethylammonium chloride, dimethylaminopropyl methacrylamide, dimethylaminopropyl methacrylamide methyl sulfate quaternary salt, dimethylaminopropyl methacrylamide sulfate, dimethylaminopropyl methacrylamide hydrochloride, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; and diallyl dialkyl ammonium halides, including but not limited to diallyl diethyl ammonium chloride and diallyl dimethyl ammonium chloride ("DADMAC") and any combination thereof; and

[0023] iii) the optional anionic monomer contains a functional group selected from carboxylic acid, sulfonic acid, phosphonic acid, their corresponding water-soluble salts, their corresponding water-dispersible salts and any combination thereof, including but not limited to acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinyl sulfonic acid, 2-acrylamide-2-methylpropanesulfonic acid (AMPS), acrylamidomethylsulfonic acid, acrylamidoethanesulfonic acid, 2-hydroxy-3-acrylamidopropanesulfonic acid, styrenesulfonic acid, vinylphosphonic acid and their corresponding alkali metal, alkaline earth metal and ammonium salts and any combination thereof;

[0024] c) obtainable by reacting glyoxal with a cationic base copolymer consisting of acrylamide and DADMAC, and optionally in aqueous form;

[0025] d) having a cationic monomer content percentage in the range of 5 wt% to 60 wt%, an anionic monomer content percentage in the range of 0 wt% to 50 wt%, and the remaining monomer content is nonionic;

[0026] e) having a cationic charge density range selected from the ranges of 0.02 meq / g to 5 meq / g, 1 meq / g to 4 meq / g, and 1.4 meq / g to 2 meq / g at pH 8.0;

[0027] f) formulated in a manner selected from the group consisting of: (i) a dry powder and (ii) an aqueous solution comprising a GPAM solids weight percentage range selected from the group consisting of 1%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to the paper machine; and

[0028] g) when added to a papermaking system or composition comprising cellulosic fibers for making paper or paperboard, at a dosage selected from the ranges of 0.2 lb / ton to 25 lb / ton, 4 lb / ton to 12 lb / ton, and 1 lb / ton to 10 lb / ton of dry fiber.

[0029] In some embodiments, the at least one anionic polysaccharide promoter comprises one or more of the following properties:

[0030] a) having a weight average molecular weight selected from 10 kDa-5000 kDa, 20 kDa-2000 kDa and 40 kDa-1000 kDa;

[0031] b) comprising an anionic polysaccharide selected from the group consisting of anionic starch-based polysaccharides, anionic alginate-based polysaccharides, anionic guar-based polysaccharides, anionic cellulose-based polysaccharides, the anionic cellulose-based polysaccharides including but not limited to carboxymethylcellulose (CMC), oxidized cellulose, anionic cellulose ethers and any combination thereof;

[0032] c) comprising carboxymethyl cellulose (CMC), optionally in aqueous form or in dry powder form;

[0033] d) having a net anionic charge;

[0034] e) has a value selected from the group consisting of 0.1 meq / g to 10 meq / g, as measured by Mütek charge titration at pH 8.5,

[0035] anionic charge density ranges from 0.5 meq / g to 7.5 meq / g and from 1 meq / g to 5 meq / g;

[0036] f) having a degree of substitution (DS) of anionic charge on the polysaccharide selected from the group consisting of 0.02-2.5, 0.3-2.0, and 0.5-1.8;

[0037] g) a degree of polymerization (DP) of an anionic polysaccharide having residues selected from the ranges of 500-25,000, 100-10,000, and 200-5,000;

[0038] h) formulated in a manner selected from the group consisting of: (i) as a dry powder and (ii) as an aqueous solution comprising a weight percent range of APP solids selected from the group consisting of 0.5%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to the paper machine;

[0039] i) when formulated into an aqueous solution comprising said anionic polysaccharide promoter, optionally 2 wt% CMC, said solution has a viscosity selected from at least 5 cps, at least 10 cps, at least 20 cps and 5 cps-10 cps at pH=7 and 23°C; and

[0040] .j) when added to a papermaking system or composition comprising cellulosic fibers for making paper or paperboard, at a dosage selected from the ranges of 0.1 lb / ton to 15 lb / ton, 0.2 lb / ton to 8 lb / ton, and 0.5 lb / ton to 6 lb / ton of dry fiber.

[0041] In certain embodiments, the composition or combination of (a) and (b) comprises one or more of the following properties: a) when combined, formulated in a manner selected from the group consisting of: (i) at least one dry powder (ii) at least one aqueous solution; b) when combined, having a weight ratio of GPAM:APP (dry:dry) selected from the range of 1:20 to 20:1, 1:15 to 15:1, 1:10 to 10:1, 10:1 to 1:2 and 5:1 to 3:1; and / or

[0042] c) when combined, have a net charge selected from the range of -5 meq / g to +5 meq / g, 0 meq / g to +5 meq / g, and +1 meq / g to +3.5 meq / g.

[0044] In an exemplary embodiment, the at least one cationic GPAM comprises a high molecular weight base polymer comprising a copolymer of: (i) a cationic monomer selected from DADMAC, AETAC, and combinations thereof; (ii) a nonionic monomer selected from acrylamide, methacrylamide, and combinations thereof; and (iii) an anionic monomer optionally selected from acrylic acid, its corresponding water-soluble salts, water-dispersible alkali metal salts, alkaline earth metal salts, ammonium salts, and combinations thereof, or comprising a cationic monomer selected from acrylamide and DADMAC, and optionally the at least one cationic GPAM is in aqueous form.

[0045] In an exemplary embodiment, the at least one anionic polysaccharide promoter comprises an anionic cellulose-based polysaccharide, including but not limited to carboxymethyl cellulose (CMC), oxidized cellulose, anionic cellulose ethers, and any combination thereof, or the at least one anionic polysaccharide promoter comprises carboxymethyl cellulose (CMC).

[0046] In some exemplary embodiments, the composition and / or combination optionally comprises at least one anionic acrylamide-based (APAM) accelerator comprising a copolymer of acrylamide and acrylic acid, a water-soluble salt corresponding to the acrylic acid, a water-dispersible alkali metal salt, an alkaline earth metal salt, an ammonium salt, and combinations thereof.

[0047] In an exemplary embodiment, when the composition or combination is added to a papermaking system or composition comprising cellulosic fibers for making paper or paperboard, a paper product is produced comprising one or more of the following properties:

[0048] a) a GPAM solids percentage selected from the range of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product;

[0049] b) an anionic polysaccharide promoter solids percentage selected from the ranges of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product; and

[0050] c) (i) improved dry tensile strength; (ii) improved resistance to rupture (as measured by bursting strength); (iii) improved resistance to compression (as measured by the STFI compression test); and (iv) improved tear resistance compared to paper products prepared in an equivalent manner using cationic GPAM and anionic polyacrylamide (APAM) promoters comprising lower molecular weight base polymers (e.g., less than 50 kDa).

[0051] The present invention also provides a furnish composition for making paper or paperboard, which has been treated with at least one strengthening system selected from the group consisting of compositions and material combinations for strengthening paper or paperboard. In some embodiments, the furnish composition comprises an aqueous slurry of a fiber raw material containing cellulosic fibers, and further comprises one or more of the following:

[0052] a) an aqueous slurry of cellulosic fibers, optionally obtained from a source selected from the group consisting of softwood fibers, hardwood fibers, recycled fibers, refined fibers, mill broke fibers, non-wood fibers including but not limited to wheat straw pulp, and mixtures of any of the foregoing;

[0053] b) pulp selected from kraft pulp, bleached pulp, unbleached pulp, process water from pulp, paper and / or board production, neutral sulfite semi-chemical (NSSC) pulp, mechanical pulp and mixtures of any of the foregoing;

[0055] c) a raw material selected from thick stock, thick stock diluted with chemical water, synthetic water, white water and / or process water, and thin stock, and any mixture of the foregoing;

[0056] In some embodiments, when at least one strengthening system is added to a papermaking system and / or a furnish composition comprising the furnish composition, the amount of the at least one strengthening system is sufficient to improve the strength properties of paper or paperboard produced from the furnish composition as compared to when the strengthening system is not added to the papermaking system or the furnish composition comprising the furnish composition.

[0057] The present disclosure also generally encompasses a papermaking method for making one or more paper products (optionally one or more absorbent paper products) from a fiber raw material comprising cellulose fibers. In some embodiments, the method comprises adding:

[0058] a) at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer, wherein the high molecular weight base polymer has a weight average molecular weight selected from the group consisting of at least 50 kDa, at least 80 kDa, at least 100 kDa, at least 250 kDa, and 100 kDa to 5000 kDa; and

[0059] b) at least one anionic polysaccharide accelerator ("APP"), optionally carboxymethylcellulose (CMC).

[0060] In some embodiments, during the papermaking process, (a) and (b) are added separately, simultaneously, or as a premixed combination at one or more points during the papermaking process selected from any time before, during, and after the formation of the paper product; and / or (a) and (b) are added separately, simultaneously, or as a premixed combination at one or more locations in the papermaking system; and / or (a) and (b) may be added as separate compositions in any order, or as a premixed composition comprising (a) and (b), optionally an aqueous composition, further optionally, wherein when (a) and (b) are added separately, the addition of (a) and (b) is simultaneous or close in time, for example, (a) and (b) are added within two hours, one hour, 30 minutes, 10 minutes, 1 minute, or less than 1 minute apart.

[0061] In some embodiments, at least one cationic GPAM and at least one anionic polysaccharide promoter:

[0062] a) formulated as a dry polymer or an aqueous solution, each solution having a solid weight percent range selected from the ranges of 1%-25%, 1%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before addition to the paper machine;

[0063] b) adding during the process to obtain a weight ratio of GPAM:APP (dry:dry) selected from the ranges of 1:20 to 20:1, 1:15 to 15:1, 1:10 to 10:1, 10:1 to 1:2 and 5:1 to 3:1;

[0064] c) when combined, have a net charge selected from the range of -5 meq / g to +5 meq / g, 0 meq / g to +5 meq / g, and +1 meq / g to +3.5 meq / g;

[0066] d) adding during the process in a manner selected from the following additions of cationic GPAM and aqueous APP solutions:

[0067] (i) added simultaneously; (ii) added sequentially in any order; (iii) added together as a premixed solution; and (iv) any combination thereof;

[0068] e) adding said cationic GPAM and APP aqueous solution during said process in a manner selected from the group consisting of: (i) adding said cationic GPAM and APP aqueous solution to said aqueous fibrous stock comprising cellulosic fibers at the wet end of a paper machine prior to forming said paper product; (ii) adding said cationic GPAM and APP aqueous solution to a formed cellulosic fiber web during forming said paper product; (iii) adding said cationic GPAM and APP aqueous solution to one or more surfaces of said paper product after said paper product is formed; and (iv) any combination thereof;

[0069] f) when added to the aqueous fiber feedstock comprising cellulosic fibers, adding a dosage of the at least one cationic GPAM selected from the range of 0.2 lb / ton to 25 lb / ton, 4 lb / ton to 12 lb / ton, and 1 lb / ton to 10 lb / ton of dry fiber and a dosage selected from the range of 0.1 lb / ton to 15 lb / ton, 0.2 lb / ton to 8 lb / ton, and

[0070] A dosage of said at least one anionic polysaccharide promoter in the range of 0.5 lb / ton to 6 lb / ton of dry fiber; and / or

[0071] g) added during the process, wherein the addition points include but are not limited to in the hydrapulper, before refining the pulp, after refining the pulp, at the fan pump, before the headbox, at the headbox, by spraying, printing, coating and impregnation onto the paper web, onto preformed paper (e.g. by slot sizing), and on dry paper (e.g. by spraying), and any combination thereof.

[0072] In some embodiments, at least one cationic GPAM comprising a high molecular weight base polymer comprises one or more of the following properties:

[0073] a) comprising a weight ratio range of glyoxal:base polymer selected from 1:99 to 50:50 and 5:95 to 20:80; b) obtained by reacting glyoxal with the high molecular weight base polymer, wherein the high molecular weight base polymer comprises an acrylamide-based copolymer comprising a neutral monomer, a cationic monomer and optionally an anionic monomer, further wherein

[0074] i) the neutral monomer is selected from monomers containing primary amides, which monomers include acrylamide, methacrylamide, ethyl acrylamide, crotonamide, N-methyl acrylamide, N-butyl acrylamide, N-ethyl methacrylamide and any combination thereof;

[0075] ii) the cationic monomer is selected from acryloyloxyethyl trimethyl ammonium chloride ("AETAC"), methacryloyloxyethyl trimethyl ammonium chloride ("MAETAC"), methacrylamidopropyl trimethyl ammonium chloride ("MAPTAC"), acrylamidopropyl trimethyl ammonium chloride ("APTAC"), methacryloyloxyethyl dimethyl ammonium sulfate, diallyl dimethyl ammonium chloride ("DADMAC"); dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, including but not limited to dimethylaminoethyl acrylate ("DMAEA"), dimethylaminoethyl methacrylate ("DMAEA"), dimethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl acrylate methyl sulfate quaternary salt, dimethylaminoethyl acrylate benzyl chloride quaternary salt, dimethylaminoethyl acrylate sulfate, dimethylaminoethyl acrylate hydrochloride, diethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate ester methyl sulfate quaternary salt, methacrylate dimethylaminoethyl benzyl chloride quaternary salt, methacrylate dimethylaminoethyl sulfate, methacrylate dimethylaminoethyl hydrochloride, methacryloyl dimethylaminoethyl hydrochloride; dialkylaminoalkyl acrylamides and methacrylamides and their quaternary or acid salts, including but not limited to acrylamidopropyl trimethyl ammonium chloride, dimethylaminopropyl acrylamide, dimethylaminopropyl acrylamide methyl sulfate quaternary salt, dimethylaminopropyl acrylamide sulfate, dimethylaminopropyl acrylamide hydrochloride, methacrylamidopropyl trimethyl ammonium chloride, dimethylaminopropyl methacrylamide, dimethylaminopropyl methacrylamide methyl sulfate quaternary salt, dimethylaminopropyl methacrylamide sulfate, dimethylaminopropyl methacrylamide hydrochloride, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; and diallyl dialkyl ammonium halides, including but not limited to diallyl diethyl ammonium chloride and diallyl dimethyl ammonium chloride ("DADMAC") and any combination thereof; and

[0077] iii) the optional anionic monomer contains a functional group selected from carboxylic acid, sulfonic acid, phosphonic acid, their corresponding water-soluble salts, their corresponding water-dispersible salts and any combination thereof, including but not limited to acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinyl sulfonic acid, 2-acrylamide-2-methylpropanesulfonic acid (AMPS), acrylamidomethylsulfonic acid, acrylamidoethanesulfonic acid, 2-hydroxy-3-acrylamidopropanesulfonic acid, styrenesulfonic acid, vinylphosphonic acid and their corresponding alkali metal, alkaline earth metal and ammonium salts and any combination thereof;

[0078] c) obtainable by reacting glyoxal with a cationic base copolymer consisting of acrylamide and DADMAC, and optionally in aqueous form;

[0079] d) having a cationic monomer content percentage in the range of 5 wt%-60 wt%, an anionic monomer content percentage in the range of 0 wt%-50 wt%, and the remaining monomer content is non-ionic; and / or e) having a cationic charge density range selected from the range of 0.02meq / g-5meq / g, 1meq / g-4meq / g and 1.4meq / g-2meq / g at pH 8.0.

[0080] In some embodiments, the at least one anionic polysaccharide promoter comprises one or more of the following properties:

[0081] a) having a weight average molecular weight selected from 10 kDa-5000 kDa, 20 kDa-2000 kDa and 40 kDa-1000 kDa;

[0082] b) comprising an anionic polysaccharide selected from the group consisting of anionic starch-based polysaccharides, anionic alginate-based polysaccharides, anionic guar-based polysaccharides, anionic cellulose-based polysaccharides, the anionic cellulose-based polysaccharides including but not limited to carboxymethylcellulose (CMC), oxidized cellulose, anionic cellulose ethers and any combination thereof; or comprising carboxymethylcellulose (CMC);

[0083] c) having a net anionic charge;

[0084] d) having an anionic charge density range selected from the ranges of 0.1 meq / g to 10 meq / g, 0.5 meq / g to 7.5 meq / g, and 1 meq / g to 5 meq / g as measured by Mütek charge titration at pH 8.5;

[0085] e) having a degree of substitution (DS) of anionic charge on the polysaccharide selected from the group consisting of 0.02-2.5, 0.3-2.0, and 0.5-1.8;

[0086] f) having a degree of polymerization (DP) of anionic polysaccharides selected from the ranges of 500-25,000, 100-10,000 and 200-5,000;

[0087] g) formulated in a manner selected from the group consisting of: (i) as a dry powder and (ii) as an aqueous solution comprising a weight percent range of APP solids selected from the group consisting of 0.5%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to the paper machine; and

[0088] h) when formulated into an aqueous solution comprising 2 wt% CMC, the solution has a viscosity selected from the group consisting of at least 5 cps, at least 10 cps, at least 20 cps, and 5 cps-20 cps at pH=7 and 23°C.

[0089] In some embodiments, the fiber feedstock comprising cellulosic fibers comprises one or more of the following: a) an aqueous slurry comprising cellulosic fibers obtained from a source selected from the group consisting of softwood fibers, hardwood fibers, recycled fibers, refined fibers, mill broke fibers, non-wood fibers including but not limited to wheat straw pulp, and mixtures of any of the foregoing;

[0090] b) optionally comprising pulp selected from kraft pulp, bleached pulp, unbleached pulp, process water from pulp, paper and / or paperboard production, neutral sulfite semi-chemical (NSSC) pulp, mechanical pulp and mixtures of any of the foregoing;

[0091] c) optionally comprising a feedstock selected from thick stock, thick stock diluted with chemical water, synthetic water, white water and / or process water and thin stock, and mixtures of any of the foregoing; and / or

[0092] d) having a pH selected from the ranges of 3.0-9.0, 4.0-8.0, and 4.5-7.5.

[0093] In an exemplary embodiment,

[0094] a) at least one cationic GPAM comprising a high molecular weight base polymer comprising a copolymer of: (i) a cationic monomer selected from DADMAC, AETAC and combinations thereof; (ii) a nonionic monomer selected from acrylamide, methacrylamide and combinations thereof; and (iii) an anionic monomer optionally selected from acrylic acid, its corresponding water-soluble salts, water-dispersible alkali metal salts, alkaline earth metal salts, ammonium salts and combinations thereof, or the at least one cationic GPAM comprising a high molecular weight base polymer is obtainable by reacting glyoxal with a cationic base copolymer consisting of acrylamide and DADMAC, and is optionally in aqueous form;

[0096] b) at least one anionic polysaccharide promoter comprises anionic cellulose-based polysaccharides, including but not limited to carboxymethyl cellulose (CMC), oxidized cellulose, anionic cellulose ethers, and any combination thereof, or the at least one anionic polysaccharide promoter comprises carboxymethyl cellulose (CMC); and / or

[0098] c) wherein the method optionally comprises adding at least one anionic acrylamide-based (APAM) accelerator comprising a copolymer of acrylamide and acrylic acid, the corresponding water-soluble salts of acrylic acid, water-dispersible alkali metal salts, alkaline earth metal salts, ammonium salts and combinations thereof.

[0099] In some embodiments, the method results in the formation of a paper product. In some embodiments, the paper product comprises one or more of the following properties:

[0100] a) comprising a weight percentage of said at least one cationic GPAM comprising a high molecular weight base polymer selected from the range of 0.02%-10% and 0.05%-5% by weight of dry paper;

[0101] b) comprising a weight percentage of said at least one anionic polysaccharide promoter selected from the range of 0.02%-10% and 0.05%-5% by weight of dry paper;

[0102] c) exhibit (i) increased dry tensile strength; (ii) increased resistance to rupture, as measured by bursting strength; (iii) increased resistance to compression, as measured by the STFI compression test; and (iv) increased resistance to tearing compared to paper products prepared in an equivalent manner using cationic GPAM and / or anionic polyacrylamide (APAM) accelerators comprising lower molecular weight base polymers (e.g., less than 50 kDa); and / or

[0103] d) selected from the following paper products comprising a cellulosic paperboard web, which paper products optionally mainly include cellulosic fibers and fiber-based products, including but not limited to hand sheets, paperboard-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging board types, toilet tissue and towel types, paper materials, paper towels, diapers, sanitary napkins, training pants, panty liners, incontinence briefs, tampons, urine pads, cat litter box liners, coffee filters, air filters, dryer pads, floor cleaning pads, absorbent facial tissue, absorbent bathroom tissue, napkins, wrapping paper, paperboard boxes, bag paper and other paper products, etc.

[0104] The present invention also provides a paper product comprising one or more compositions or a combination of (a) and (b) for strengthening paper or paperboard obtainable by the method disclosed herein. In some embodiments, the paper product comprises one or more of the following properties:

[0105] a) comprising a percentage of said at least one cationic GPAM comprising a high molecular weight base polymer selected from the range of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product;

[0106] b) comprising a percentage of said at least one anionic polysaccharide promoter selected from the range of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product;

[0107] c) exhibit (i) increased dry tensile strength; (ii) increased resistance to rupture, as measured by bursting strength; (iii) increased resistance to compression, as measured by the STFI compression test; and (iv) increased resistance to tearing compared to paper products prepared in an equivalent manner using cationic GPAM and / or anionic polyacrylamide (APAM) accelerators comprising lower molecular weight base polymers (e.g., less than 50 kDa); and / or

[0108] d) selected from the following paper products comprising a cellulosic paperboard web, which paper products optionally mainly include cellulosic fibers and fiber-based products, including but not limited to hand sheets, paperboard-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging board types, toilet tissue and towel types, paper materials, paper towels, diapers, sanitary napkins, training pants, panty liners, incontinence briefs, tampons, urine pads, cat litter box liners, coffee filters, air filters, dryer pads, floor cleaning pads, absorbent facial tissue, absorbent bathroom tissue, napkins, wrapping paper, paperboard boxes, bag paper and other paper products, etc. DETAILED DESCRIPTION

[0109] Before describing the present invention, the following definitions are provided. Unless otherwise indicated, all terms should be interpreted as understood by those skilled in the art.

[0110] definition

[0111] As used herein, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Unless otherwise specifically stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs.

[0112] As used herein, the terms "papermaking process" and "papermaking application" generally refer to any process that can produce any form of paper and / or paperboard products. For example, these processes include making paper products from pulp, such as processes that include forming an aqueous cellulosic papermaking furnish, draining the furnish to form paper, and drying the paper. The steps of forming the papermaking furnish, draining, and drying can be performed in any conventional manner generally known in the art. In some cases, papermaking processes and applications can include the use of one or more polymer solutions, wherein the polymer solution can include one or more cationic starches, one or more DPAMs, one or more CPAMs, one or more GPAMs, one or more anionic dry polyacrylamides (ADPAMs), and / or one or more polyaminoamide-epichlorohydrin (PAE) resins, for example, as paper strengthening agents and / or wet strength agents.

[0113] As used herein, the term "fiber" refers to the basic structural unit of paper or paperboard.

[0114] As used herein, the terms "recycled fiber" and "recovered fiber" refer to paper, paperboard, and fiber waste from retail stores, office buildings, residences, manufacturing plants, and the like, after they have passed through their end use as consumer products. Manufacturing waste includes: dry paper and paperboard waste generated after the papermaking process is completed, including, for example: envelope cuttings, bookbinding trimmings, and other paper and paperboard waste generated by printing, cutting, forming, and other processing operations; bag, box, and carton manufacturing waste; factory wrapping paper and discarded stock; and finished paper and paperboard that is repulped from obsolete inventory of paper and paperboard manufacturers, merchants, wholesalers, distributors, printers, converters, or others. Specifically, the term "recycled fiber" includes recycled fiber obtained by processing paper and other consumer cellulosic materials such as paper, old corrugated containerboard (OCC), mixed office waste (MOW), old magazines (OMG), unbleached kraft pulp, neutral sulfite semi-chemical (NCCS) pulp, and / or mechanical pulp. The raw material of recycled fiber can be selected from old corrugated boxboard, mixed office waste, old newsprint, old magazines, double-lined kraft paper and any mixture thereof. Mixed waste (MXW) means a recycled mixture of recycled cardboard (such as OCC, linerboard and / or folding boxboard) and recycled paper (such as old newsprint, old magazines and / or office waste paper). Mixed office waste means recycled fiber materials mainly containing copy paper, printing paper and offset paper. Double-lined kraft paper means recycled fiber materials containing clean, sorted, unprinted corrugated cardboard cartons, boxes, papers or scraps (such as kraft paper or jute liner). Linerboard (WLC) means a multi-layer paperboard, one or more of which contains deinked fiber materials and / or non-deinked recycled fiber materials, which are derived from, for example, OCC, mixed office waste or old newspaper (ONP). The presence of any of these recycled fiber materials in the fiber suspension generally reduces drainage and paper strength and provides a large amount of starch, hydrophobic and colloidal substances to the process.

[0115] As used herein, the term "OCC" refers to old corrugated cardboard and / or containerboard. Corrugated boxes are those boxes made of three layers of individual paper, two layers of liner paper, and a corrugated or corrugated layer sandwiched between them. Brown paper bags are usually accepted for recycling with OCC. The term OCC means recycled fiber material with a liner paper such as test liner paper, jute or kraft paper, and may also include double sorted old corrugated containerboard (DS OCC).

[0116] As used herein, the term "brokes" or "mill broke" refers to paper that becomes only suitable for repulping during the papermaking process, such as scraps or off-spec paper. Broke is reusable material that never leaves the mill and is not considered recycled or recovered. Broke is a valuable source of fiber that can be recycled within the mill.

[0117] As used herein, the term "coated broke" refers to broke that contains coatings that are applied to the base paper during the paper manufacturing process. When the broken paper contains these coatings, special problems arise in recycling to recover fiber value because these coatings introduce materials that are not normally present in the original fiber raw material used to make the base paper. Coated broke may also contain dyes and / or other additives. In this application, coated broke includes surface-sized, dyed and / or creped broke.

[0118] As used herein, the term "recycled fiber composition" generally refers to a composition comprising recycled cellulosic fibers, typically a composition where most or all of the fibers are recycled fibers, such as at least 40%, 50%, 60%, 70%, 80%, 90% or 100%.

[0119] As used herein, the term "fiber suspension" is understood to mean an aqueous suspension comprising fibers, preferably recycled fibers, and optionally fillers. For example, the fiber suspension may contain at least 5%, preferably 10%-30%, more preferably 11%-19% of mineral fillers. The mineral filler may be any filler conventionally used in paper and board manufacturing, such as ground calcium carbonate, precipitated calcium carbonate, clay, talc, gypsum, titanium dioxide, synthetic silicates, aluminum trihydrate, barium sulfate, magnesium oxide or any mixture thereof.

[0120] As used herein, the term "slurry" generally refers to a mixture of water, dissolved pulp, and optionally other soluble or insoluble components produced or added during the stock preparation stage of papermaking.

[0121] As used herein, the term "furnish" or "papermaking furnish" generally refers to a mixture of cellulose fibers, pulp, optional fillers, dyes, and water used to make paper or paperboard.

[0122] As used herein, the term "thick stock" generally refers to a mixture of papermaking pulp and other materials having a consistency of about 1% to 5%.

[0123] As used herein, the term "thin stock" generally refers to a mixture of papermaking pulp and other materials that has been diluted with white water or other process water in a fan pump to a consistency of less than 1%.

[0124] As used herein, the term "white water" generally refers to process water within a paper machine system, and in particular to water that is removed from the paper during the paper forming process.

[0125] As used herein, the term "fixed" means that a substance is at least temporarily or permanently bound or attached to fibers.

[0126] As used herein, the term "flocculation" generally refers to the tendency of fibers to aggregate into bundles under flow, especially in the presence of retention aids; the term also refers to the behavior of high mass polymers to form bridges between suspended colloidal particles, causing strong, relatively irreversible aggregation.

[0127] The term "flocculant" generally refers to an agent that can bridge, neutralize, or promote the coagulation of particles into larger aggregates, generally resulting in more efficient settling. Flocculation methods generally involve the addition of a flocculant followed by mixing to promote collisions between particles, thereby causing unstable particles to aggregate into larger particles that can be removed by gravity settling or by other means (e.g., centrifugation, filtration).

[0128] As used herein, the term "polymer" or "polymer additive" and their similar terms are used in the ordinary sense understood by those skilled in the art, and therefore can be used herein to refer to or describe a macromolecule (or a group of such molecules) that may contain repeating units. Polymers can be formed in a variety of ways, including by polymerizing monomers and / or by chemically modifying one or more repeating units of a precursor polymer. Unless otherwise specified, polymers can include "homopolymers", which can contain substantially identical repeating units, which can be formed, for example, by polymerizing specific monomers. Unless otherwise specified, polymers can also include "copolymers", which can contain two or more different repeating units, which can be formed, for example, by copolymerizing two or more different monomers and / or by chemically modifying one or more repeating units of a precursor polymer. Unless otherwise specified, polymers or copolymers can also include "terpolymers", which generally refer to polymers containing three or more different repeating units. Any of the one or more polymers discussed herein can be used in any applicable method, such as as a reinforcing agent or promoter.

[0129] As used herein, the term "monomer" generally refers to nonionic monomers, anionic monomers, cationic monomers, zwitterionic monomers, betaine monomers, and zwitterion pair monomers.

[0130] As used herein, the term "anionic monomer" may refer to anionic monomers that are substantially all or partly (in equilibrium) anionic in the pH range of about 4.0 to about 9.0. An "anionic monomer" may be neutral at low pH (pH of about 2 to about 6), or anionic at low pH.

[0131] As used herein, the term "cationic monomer" generally refers to a monomer having a positive charge or a monomer that is positively charged at a pH within the normal operating range of a paper machine process.

[0132] As used herein, the term "nonionic monomer" generally refers to a monomer having a neutral charge.

[0133] As used herein, the term "glyoxalation percentage" refers to the percentage of glyoxalated acrylamide-based monomers in the polymers (eg, the first base polymer and / or the second base polymer) of the cationic GPAM composition.

[0134] As used herein, the term "GPAM content" refers to the sum of the glyoxalated base polymer plus free glyoxal in the cationic GPAM composition.

[0135] As used herein, the term "water-soluble" generally refers to a polymer preparation that is completely miscible with water. When mixed with excess water, the cationic emulsion polymer in the polymer preparation preferably completely dissolves, and the resulting polymer solution preferably contains no discrete polymer particles or particles.

[0136] As used herein, the term "aqueous solution" or "solution" generally refers to a mixture of water and one or more completely dissolved water-soluble solutes. The solution may be homogeneous. When mixed with excess water, the cationic emulsion polymer in the polymer article is preferably completely dissolved, and the resulting polymer solution is preferably free of discrete polymer particles or particles.

[0137] As used herein, the terms "aqueous suspension", "aqueous slurry" or "slurry" generally refer to a heterogeneous mixture of a fluid containing insoluble or sparingly soluble solid particles that are large enough to settle. The suspensions and slurries of the present invention may also contain a certain amount of solid particles, generally referred to as colloidal particles, which cannot settle completely or require a long time to settle completely.

[0138] As used herein, the term "polyacrylamide" or "PAM" generally refers to polymers and copolymers comprising an acrylamide moiety, and the term encompasses any polymer or copolymer comprising an acrylamide moiety, such as one or more acrylamide (co)polymers. In some cases, the PAM may comprise anionic PAM (APAM), cationic PAM (CPAM) and / or sulfonated PAM (SPAM).

[0139] As used herein, the term "glyoxalated polyacrylamide" ("GPAM") generally refers to a polymer obtained by reacting glyoxal with a polyacrylamide base polymer. Methods for producing glyoxalated polyacrylamide are known in the art. (See, e.g., U.S. Pat. No. 3,556,932, which first disclosed the synthesis of GPAM compositions prepared by reacting glyoxal with cationic polyacrylamide). In some cases, the polyacrylamide backbone of the GPAM can incorporate a small amount of cationic monomers, allowing the polymer to be self-retained on the fiber. Generally, the GPAM comprises a reactive polymer that can covalently bind to cellulose when dehydrated.

[0140] As used herein, the term "GPAM" generally refers to cationic wet strength and / or dry strength resins, including PAM resins used to make moisture-resistant papers such as liquid packaging, napkins, and tissues. The positively charged resin electrostatically adsorbs to negatively charged fines and fibers, thereby increasing the overall efficiency of the production process. The term DPAM refers to polyacrylamide in dry form (e.g., powder form); CPAM refers to cationic polyacrylamide; GPAM refers to glyoxalated polyacrylamide

[0141] As used herein, the term "poly-DADMAC" refers to polydiallylmethylammonium chloride, which is a fully charged cationic polymer commonly used as a standard for cationic demand titrations.

[0142] As used herein, the terms "accelerator", "anionic polysaccharide accelerator" and "APP" generally refer to any anionic polysaccharide additive that can enhance the ability of a reinforcing sizing agent (e.g., a cationic GPAM) to strengthen a finished paper product. Accelerators can also impart desirable physical properties to paper products, such as enhanced wet strength, dry strength, and wet attenuation. Accelerators of the present disclosure include anionic PACs, "APAMs," and the like.

[0143] As used herein, the terms "CMC" and "carboxymethyl cellulose" refer to cellulose derivatives in which carboxymethyl groups (-CH2-COOH) are bound to some of the hydroxyl groups of the glucopyranose monomers constituting the cellulose backbone.

[0144] As used herein, the term "zeta potential" refers to the average electrical potential on the hydrodynamic slip plane adjacent to a solid surface when the solid surface is exposed to a liquid. Zeta potential data provide a method for papermakers to predict how a furnish will respond to the addition of cationic or anionic additives. Zeta potential is a good predictor of the magnitude of the electrical repulsion between particles of known size and shape as a function of distance. Fiber slurries with high absolute Zeta potentials (greater than plus or minus 20 mV) are likely to remain in a stable dispersion during storage.

[0145] As used herein, the terms "charge demand", "polymer charge demand" and "PCD" generally refer to the amount of polymer (cation or anion) consumed at the equivalence point of a polyelectrolyte titration. It is based on the principle that oppositely charged polymers tend to neutralize each other in a 1:1 stoichiometry.

[0146] As used herein, the term "paper machine wet end" or "wet end" generally refers to the portion of the papermaking process between pulping (or bleaching) and wet pressing of the paper.

[0147] As used herein, the term "consistency" generally refers to the oven dry mass percentage (ie, 100%* oven dry mass / total mass) in a feedstock, slurry, or furnish.

[0148] The terms "total solids" or "total suspended solids" are used interchangeably herein and generally refer to the total amount or weight of suspended solids contained in oil sands or other sands containing dispersions. "Total solids" or "total suspended solids" generally do not include dissolved solids.

[0149] As used herein, the term "ppm" refers to parts per million based on milligrams of solute per liter of aqueous solution or slurry (eg, mg / L).

[0150] As used herein, the term "lbs / ton" or "# / T" means the dry mass pounds of added material (eg, additives, solutes, and / or particulates) per ton of suspended solids (eg, AKD weight per total dry ton of suspended solids).

[0151] As used herein, the term "kg / t" or "kg / ton" means kilograms of dry mass (additives, solutes and / or particles) per ton of slurry, feedstock and / or furnish.

[0152] As used herein, the phrase "weight %" means the number of pounds of dry mass of additive per dry mass of solids in a formulation, solution or slurry multiplied by 100%.

[0153] Detailed description of the invention

[0154] Glyoxylated polyacrylamide (GPAM) is commonly used in various paper products to enhance dry strength and temporary wet strength. For example, it can be used to increase the initial wet strength of many household toilet papers that come into contact with water during use. Glyoxylated polyacrylamide is also used to increase the compressive strength and dimensional stability of many paperboard products.

[0155] Cationic glyoxalated polyacrylamide is a well-known strength resin and is often considered a benchmark for dry strength. The polyacrylamide backbone typically contains a small amount of a cationic monomer, such as diallyldimethylammonium chloride (DADMAC), which enables the polymer to self-retain on the fiber. GPAM is a reactive polymer that can covalently bind to cellulose when dehydrated. However, the addition of water can quickly reverse this reaction, resulting in a rapid decay in wet strength.

[0156] Carboxymethyl cellulose is produced from cellulose and monochloroacetic acid in the presence of sodium hydroxide. The role of the sodium hydroxide is to convert the cellulose into alkali cellulose, which can come into contact with the monochloroacetic acid and react. This reaction introduces carboxymethyl groups on the cellulose chain and makes hydration of the molecule possible. Since each anhydroglucose unit has three hydroxyl groups, the maximum DS of CMC is 3. The common DS range for commercial CMC products is between 0.5 and 1.5.

[0157] CMC has long been known to be an effective dry strength resin for paper. CMC contains both hydroxyl and carboxyl groups, which can form hydrogen bonds with cellulose and help improve the dry strength of paper. However, CMC is anionic and therefore requires a cationic fixative to remain on the surface of anionic cellulose fibers when added at the wet end.

[0158] The present disclosure generally encompasses compositions or combinations of materials for enhancing the dry strength and / or wet strength of paper or paperboard. The composition or combination may include at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer; and at least one anionic polysaccharide accelerator ("APP").

[0159] The present disclosure also generally encompasses a method for making one or more paper products having enhanced dry strength properties. The method may include adding to a fiber feedstock comprising cellulosic fibers at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer; and at least one anionic polysaccharide accelerator ("APP").

[0160] Surprisingly, it was found that the combination of high molecular weight (MW) cationic GPAM and APP containing carboxymethyl cellulose (CMC) provides synergistically improved handsheet dry strength compared to GPAM alone and GPAM in combination with an anionic polyacrylamide (APAM) accelerator.

[0161] Without being bound by theory, it can be speculated that the synergistic improvement in dry strength may be due to the higher degree of polymerization and higher cationic charge provided by GPAM1 combined with the use of anionic CMC, which acts to maintain the anionic zeta potential of the system. These results are surprising because the lower dose levels of CMC outperformed the higher dose levels of APAM in all strength tests.

[0162] Specifically, the results disclosed herein also demonstrate that the combination of high molecular weight cationic GPAM and APP can be used to enhance the dry strength parameters of one or more paper products, optionally absorbent paper products.

[0163] The methods of making one or more paper products of the present invention have one or more of the following advantages: (i) improved dry tensile strength; (ii) improved resistance to rupture (as measured by bursting strength); (iii) improved resistance to compression (as measured by the STFI compression test); and (iv) improved resistance to tearing compared to paper products made in an equivalent manner using cationic GPAM and anionic polyacrylamide (APAM) promoters comprising lower molecular weight base polymers (e.g., less than 50 kDa).

[0164] The present disclosure provides a composition for strengthening paper or paperboard, optionally an aqueous composition. In some embodiments, the composition comprises at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer; and at least one anionic polysaccharide promoter ("APP"), optionally carboxymethyl cellulose (CMC). In some embodiments, the high molecular weight base polymer has a weight average molecular weight selected from at least 50 kDa, at least 80 kDa, at least 100 kDa, at least 250 kDa, and 100 kDa-5000 kDa.

[0165] The present disclosure also provides a material combination. In some embodiments, the combination comprises at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer, optionally an aqueous composition; and at least one anionic polysaccharide promoter ("APP"), optionally carboxymethyl cellulose (CMC).

[0166] In some embodiments, the high molecular weight base polymer (a) has a weight average molecular weight selected from at least 50 kDa, at least 80 kDa, at least 100 kDa, at least 250 kDa, and 100 kDa-5000 kDa. In some embodiments, when the combination of materials (a) and (b) is added separately, simultaneously, or as a premixed combination to a papermaking system or a furnish composition comprising a furnish composition, the furnish composition comprises cellulose fibers for making paper or paperboard, wherein (a) and (b) may be added in any order, and a paper or paperboard material having enhanced strength is produced compared to when the combination of materials (a) and (b) is not added to the papermaking system or the furnish composition.

[0167] In some embodiments, at least one cationic GPAM comprising a high molecular weight base polymer comprises one or more of the following properties:

[0168] a) comprising a weight ratio range of glyoxal:base polymer selected from 1:99 to 50:50 and 5:95 to 20:80; b) obtained by reacting glyoxal with said high molecular weight base polymer, wherein the high molecular weight base polymer comprises an acrylamide-based copolymer comprising a neutral monomer, a cationic monomer and optionally an anionic monomer, further wherein

[0169] i) the neutral monomer is selected from monomers containing primary amides, which monomers include acrylamide, methacrylamide, ethyl acrylamide, crotonamide, N-methyl acrylamide, N-butyl acrylamide, N-ethyl methacrylamide and any combination thereof;

[0170] ii) the cationic monomer is selected from acryloyloxyethyl trimethyl ammonium chloride ("AETAC"), methacryloyloxyethyl trimethyl ammonium chloride ("MAETAC"), methacrylamidopropyl trimethyl ammonium chloride ("MAPTAC',), acrylamidopropyl trimethyl ammonium chloride ("APTAC"), methacryloyloxyethyl dimethyl ammonium sulfate, diallyl dimethyl ammonium chloride ("DADMAC"); dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, including but not limited to dimethylaminoethyl acrylate ("DMAEA"), dimethylaminoethyl methacrylate ("DMAEA"), dimethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl acrylate methyl sulfate quaternary salt, dimethylaminoethyl acrylate benzyl chloride quaternary salt, dimethylaminoethyl acrylate sulfate, dimethylaminoethyl acrylate hydrochloride, diethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate ester methyl sulfate quaternary salt, dimethylaminoethyl methacrylate benzyl chloride quaternary salt, dimethylaminoethyl methacrylate sulfate, dimethylaminoethyl methacrylate hydrochloride, dimethylaminoethyl methacrylate hydrochloride; dialkylaminoalkyl acrylamides and methacrylamides and their quaternary or acid salts, including but not limited to acrylamidopropyl trimethylammonium chloride, dimethylaminopropyl acrylamide, dimethylaminopropyl acrylamide methyl sulfate quaternary salt, dimethylaminopropyl acrylamide sulfate, dimethylaminopropyl acrylamide hydrochloride, methacrylamidopropyl trimethylammonium chloride, dimethylaminopropyl methacrylamide, dimethylaminopropyl methacrylamide methyl sulfate quaternary salt, dimethylaminopropyl methacrylamide sulfate, dimethylaminopropyl methacrylamide hydrochloride, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; and diallyl dialkyl ammonium halides, including but not limited to diallyl diethyl ammonium chloride and diallyl dimethyl ammonium chloride ("DADMAC") and any combination thereof; and

[0171] iii) the optional anionic monomer contains a functional group selected from carboxylic acid, sulfonic acid, phosphonic acid, their corresponding water-soluble salts, their corresponding water-dispersible salts and any combination thereof, including but not limited to acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinyl sulfonic acid, 2-acrylamide-2-methylpropanesulfonic acid (AMPS), acrylamidomethylsulfonic acid, acrylamidoethanesulfonic acid, 2-hydroxy-3-acrylamidopropanesulfonic acid, styrenesulfonic acid, vinylphosphonic acid and their corresponding alkali metal, alkaline earth metal and ammonium salts and any combination thereof;

[0172] c) obtainable by reacting glyoxal with a cationic base copolymer consisting of acrylamide and DADMAC, and optionally in aqueous form;

[0173] d) having a cationic monomer content percentage in the range of 5 wt% to 60 wt%, an anionic monomer content percentage in the range of 0 wt% to 50 wt%, and the remaining monomer content is nonionic;

[0174] e) having a cationic charge density range selected from the ranges of 0.02 meq / g to 5 meq / g, 1 meq / g to 4 meq / g, and 1.4 meq / g to 2 meq / g at pH 8.0;

[0175] f) formulated in a manner selected from the group consisting of: (i) a dry powder and (ii) an aqueous solution comprising a GPAM solids weight percentage range selected from the group consisting of 1%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to the paper machine; and

[0176] g) when added to a papermaking system or composition comprising cellulosic fibers for making paper or paperboard, at a dosage selected from the ranges of 0.2 lb / ton to 25 lb / ton, 4 lb / ton to 12 lb / ton, and 1 lb / ton to 10 lb / ton of dry fiber.

[0177] In some embodiments, the at least one anionic polysaccharide promoter comprises one or more of the following properties:

[0178] a) having a weight average molecular weight selected from 10 kDa-5000 kDa, 20 kDa-2000 kDa and 40 kDa-1000 kDa;

[0179] b) comprising anionic polysaccharides selected from the group consisting of anionic starch-based polysaccharides, anionic alginate-based polysaccharides, anionic guar-based polysaccharides, anionic cellulose-based polysaccharides, including but not limited to carboxymethylcellulose (CMC), oxidized cellulose, anionic cellulose ethers, and any combination thereof;

[0180] c) comprising carboxymethyl cellulose (CMC), optionally in aqueous form or in dry powder form;

[0181] d) having a net anionic charge;

[0182] e) has a value selected from the group consisting of 0.1 meq / g to 10 meq / g, as measured by Mütek charge titration at pH 8.5,

[0183] anionic charge density ranges from 0.5 meq / g to 7.5 meq / g and from 1 meq / g to 5 meq / g;

[0184] f) having a degree of substitution (DS) of anionic charge on the polysaccharide selected from the group consisting of 0.02-2.5, 0.3-2.0, and 0.5-1.8;

[0185] g) a degree of polymerization (DP) of an anionic polysaccharide having residues selected from the ranges of 500-25,000, 100-10,000, and 200-5,000;

[0186] h) formulated in a manner selected from the group consisting of: (i) as a dry powder and (ii) as an aqueous solution comprising a weight percent range of APP solids selected from the group consisting of 0.5%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to the paper machine;

[0187] i) when formulated into an aqueous solution comprising said anionic polysaccharide promoter, optionally 2 wt% CMC, said solution has a viscosity selected from at least 5 cps, at least 10 cps, at least 20 cps and 5 cps-10 cps at pH=7 and 23°C; and

[0188] .j) when added to a papermaking system or composition comprising cellulosic fibers for making paper or paperboard, at a dosage selected from the ranges of 0.1 lb / ton to 15 lb / ton, 0.2 lb / ton to 8 lb / ton, and 0.5 lb / ton to 6 lb / ton of dry fiber.

[0189] In certain embodiments, the composition or combination of (a) and (b) comprises one or more of the following properties: a) when combined, formulated in a manner selected from: (i) at least one dry powder (ii) at least one aqueous solution;

[0190] b) when combined, has a weight ratio of GPAM:APP (dry:dry) selected from the ranges of 1:20 to 20:1, 1:15 to 15:1, 1:10 to 10:1, 10:1 to 1:2, and 5:1 to 3:1; and / or

[0191] c) when combined, has a value selected from -5 meq / g to +5 meq / g, 0 meq / g to +5 meq / g, and +1 meq / g to

[0192] Net charge in the range of +3.5 meq / g.

[0193] In an exemplary embodiment, the at least one cationic GPAM comprises a high molecular weight base polymer comprising a copolymer of: (i) a cationic monomer selected from DADMAC, AETAC, and combinations thereof; (ii) a nonionic monomer selected from acrylamide, methacrylamide, and combinations thereof; and (iii) an anionic monomer optionally selected from acrylic acid, its corresponding water-soluble salts, water-dispersible alkali metal salts, alkaline earth metal salts, ammonium salts, and combinations thereof, or comprising a cationic monomer selected from acrylamide and DADMAC, and optionally the at least one cationic GPAM is in aqueous form.

[0194] In an exemplary embodiment, the at least one anionic polysaccharide promoter comprises an anionic cellulose-based polysaccharide, including but not limited to carboxymethyl cellulose (CMC), oxidized cellulose, anionic cellulose ethers, and any combination thereof, or the at least one anionic polysaccharide promoter comprises carboxymethyl cellulose (CMC).

[0195] In some embodiments, the composition and / or combination optionally comprises at least one anionic acrylamide-based (APAM) accelerator comprising a copolymer of acrylamide and acrylic acid, a water-soluble salt corresponding to acrylic acid, a water-dispersible alkali metal salt, an alkaline earth metal salt, an ammonium salt, and combinations thereof.

[0196] In an exemplary embodiment, when the composition or combination is added to a papermaking system or composition comprising cellulosic fibers for making paper or paperboard, a paper product is produced comprising one or more of the following properties:

[0197] a) a GPAM solids percentage selected from the range of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product;

[0198] b) an anionic polysaccharide promoter solids percentage selected from the ranges of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product; and

[0199] c) (i) improved dry tensile strength; (ii) improved resistance to rupture (as measured by bursting strength); (iii) improved resistance to compression (as measured by the STFI compression test); and (iv) improved tear resistance compared to paper products prepared in an equivalent manner using cationic GPAM and anionic polyacrylamide (APAM) promoters comprising lower molecular weight base polymers (e.g., less than 50 kDa).

[0200] The present invention also provides a furnish composition for making paper or paperboard, which has been treated with at least one strengthening system selected from the group consisting of compositions and material combinations for strengthening paper or paperboard. In some embodiments, the furnish composition comprises an aqueous slurry of a fiber raw material containing cellulosic fibers, and further comprises one or more of the following:

[0201] a) an aqueous slurry of cellulosic fibers, optionally obtained from a source selected from the group consisting of softwood fibers, hardwood fibers, recycled fibers, refined fibers, mill broke fibers, non-wood fibers including but not limited to wheat straw pulp, and mixtures of any of the foregoing;

[0202] b) selected from kraft pulp, bleached pulp, unbleached pulp, process water from pulp, paper and / or paperboard production, neutral sulfite semi-chemical (NSSC) pulp, mechanical pulp and mixtures of any of the foregoing

[0203] Pulp of composite materials;

[0204] c) a raw material selected from thick stock, thick stock diluted with chemical water, synthetic water, white water and / or process water, and thin stock, and any mixture of the foregoing;

[0205] In some embodiments, when at least one strengthening system is added to a papermaking system and / or a furnish composition comprising the furnish composition, the amount of the at least one strengthening system is sufficient to improve the strength properties of paper or paperboard produced from the furnish composition as compared to when the strengthening system is not added to the papermaking system or the furnish composition comprising the furnish composition.

[0206] The present disclosure also generally encompasses a papermaking method for making one or more paper products (optionally one or more absorbent paper products) from a fiber raw material comprising cellulose fibers. In some embodiments, the method comprises adding:

[0207] a) at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer, wherein the high molecular weight base polymer has a weight average molecular weight selected from the group consisting of at least 50 kDa, at least 80 kDa, at least 100 kDa, at least 250 kDa, and 100 kDa to 5000 kDa; and

[0208] b) at least one anionic polysaccharide accelerator ("APP"), optionally carboxymethylcellulose (CMC).

[0209] In some embodiments, during the papermaking process, (a) and (b) are added separately, simultaneously, or as a premixed combination at one or more points during the papermaking process selected from any time before, during, and after the formation of the paper product; and / or (a) and (b) are added separately, simultaneously, or as a premixed combination at one or more locations in the papermaking system; and / or (a) and (b) may be added as separate compositions in any order, or as a premixed composition comprising (a) and (b), optionally an aqueous composition, further optionally, wherein when (a) and (b) are added separately, the addition of (a) and (b) is simultaneous or close in time, for example, (a) and (b) are added within two hours, one hour, 30 minutes, 10 minutes, 1 minute, or less than 1 minute apart.

[0210] In some embodiments, at least one cationic GPAM comprising a high molecular weight base polymer and at least one anionic polysaccharide promoter:

[0211] a) formulated as a dry polymer or an aqueous solution, each solution having a solid weight percent range selected from the ranges of 1%-25%, 1%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before addition to the paper machine;

[0212] b) adding during the process to obtain a weight ratio of GPAM:APP (dry:dry) selected from the ranges of 1:20 to 20:1, 1:15 to 15:1, 1:10 to 10:1, 10:1 to 1:2 and 5:1 to 3:1;

[0213] c) when combined, have a net charge selected from the range of -5 meq / g to +5 meq / g, 0 meq / g to +5 meq / g, and +1 meq / g to 3.5 meq / g;

[0215] d) adding during the process in a manner selected from the following additions of cationic GPAM and aqueous APP solutions:

[0216] (i) added simultaneously; (ii) added sequentially in any order; (iii) added together as a premixed solution; and (iv) any combination thereof;

[0217] e) adding said cationic GPAM and APP aqueous solution during said process in a manner selected from the group consisting of: (i) adding said cationic GPAM and APP aqueous solution to said aqueous fibrous stock comprising cellulosic fibers at the wet end of a paper machine prior to forming said paper product; (ii) adding said cationic GPAM and APP aqueous solution to a formed cellulosic fiber web during forming said paper product; (iii) adding said cationic GPAM and APP aqueous solution to one or more surfaces of said paper product after said paper product is formed; and (iv) any combination thereof;

[0218] f) adding a dosage of said at least one cationic GPAM selected from the ranges of 0.2 lb / ton-25 lb / ton, 4 lb / ton-12 lb / ton, and 1 lb / ton-10 lb / ton of dry fiber and a dosage of said at least one anionic polysaccharide promoter selected from the ranges of 0.1 lb / ton-15 lb / ton, 0.2 lb / ton-8 lb / ton, and 0.5 lb / ton-6 lb / ton of dry fiber when added to said aqueous fiber feedstock comprising cellulosic fibers; and / or

[0219] g) added during the process, wherein the addition points include but are not limited to in the hydrapulper, before refining the pulp, after refining the pulp, at the fan pump, before the headbox, at the headbox, by spraying, printing, coating and impregnation onto the paper web, onto preformed paper (e.g. by slot sizing), and on dry paper (e.g. by spraying), and any combination thereof.

[0220] In some embodiments, at least one cationic GPAM comprising a high molecular weight base polymer comprises one or more of the following properties:

[0221] a) comprising a weight ratio range of glyoxal:base polymer selected from 1:99 to 50:50 and 5:95 to 20:80; b) obtained by reacting glyoxal with the high molecular weight base polymer, wherein the high molecular weight base polymer comprises an acrylamide-based copolymer comprising a neutral monomer, a cationic monomer and optionally an anionic monomer, further wherein

[0222] i) the neutral monomer is selected from monomers containing primary amides, which monomers include acrylamide, methacrylamide, ethyl acrylamide, crotonamide, N-methyl acrylamide, N-butyl acrylamide, N-ethyl methacrylamide and any combination thereof;

[0223] ii) the cationic monomer is selected from acryloyloxyethyl trimethyl ammonium chloride ("AETAC"), methacryloyloxyethyl trimethyl ammonium chloride ("MAETAC"), methacrylamidopropyl trimethyl ammonium chloride ("MAPTAC"), acrylamidopropyl trimethyl ammonium chloride ("APTAC"), methacryloyloxyethyl dimethyl ammonium sulfate, diallyl dimethyl ammonium chloride ("DADMAC"); dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, including but not limited to dimethylaminoethyl acrylate ("DMAEA"), dimethylaminoethyl methacrylate ("DMAEA"), dimethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl acrylate methyl sulfate quaternary salt, dimethylaminoethyl acrylate benzyl chloride quaternary salt, dimethylaminoethyl acrylate sulfate, dimethylaminoethyl acrylate hydrochloride, diethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate ester methyl sulfate quaternary salt, dimethylaminoethyl methacrylate benzyl chloride quaternary salt, dimethylaminoethyl methacrylate sulfate, dimethylaminoethyl methacrylate hydrochloride, dimethylaminoethyl methacrylate hydrochloride; dialkylaminoalkyl acrylamides and methacrylamides and their quaternary salts or acid salts, including but not limited to acrylamidopropyl trimethylammonium chloride, dimethylaminopropyl acrylamide, dimethylaminopropyl acrylamide methyl sulfate quaternary salt, dimethylaminopropyl acrylamide sulfate, dimethylaminopropyl acrylamide hydrochloride, methacrylamidopropyl trimethylammonium chloride, dimethylaminopropyl methacrylamide, dimethylaminopropyl methacrylamide methyl sulfate quaternary salt, dimethylaminopropyl methacrylamide sulfate, dimethylaminopropyl methacrylamide hydrochloride, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; and diallyl dialkyl ammonium halides, including but not limited to diallyl diethyl ammonium chloride and diallyl dimethyl ammonium chloride ("DADMAC") and any combination thereof; and

[0224] iii) the optional anionic monomer contains a functional group selected from carboxylic acid, sulfonic acid, phosphonic acid, their corresponding water-soluble salts, their corresponding water-dispersible salts and any combination thereof, including but not limited to acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinyl sulfonic acid, 2-acrylamide-2-methylpropanesulfonic acid (AMPS), acrylamide methanesulfonic acid, acrylamide ethanesulfonic acid, 2-hydroxy-

[0225] 3-Acrylamide propanesulfonic acid, styrenesulfonic acid, vinylphosphonic acid and their corresponding alkali metal, alkaline earth metal and ammonium salts and any combination thereof;

[0226] c) obtainable by reacting glyoxal with a cationic base copolymer consisting of acrylamide and DADMAC, and optionally in aqueous form;

[0227] d) having a cationic monomer content percentage in the range of 5 wt% to 60 wt%, an anionic monomer content percentage in the range of 0 wt% to 50 wt%, and the remaining monomer content is nonionic; and / or

[0228] e) having a cationic charge density range selected from the ranges of 0.02 meq / g to 5 meq / g, 1 meq / g to 4 meq / g, and 1.4 meq / g to 2 meq / g at pH 8.0.

[0229] In some embodiments, the at least one anionic polysaccharide promoter comprises one or more of the following properties:

[0230] a) having a weight average molecular weight selected from 10 kDa-5000 kDa, 20 kDa-2000 kDa and 40 kDa-1000 kDa;

[0231] b) comprising an anionic polysaccharide selected from the group consisting of anionic starch-based polysaccharides, anionic alginate-based polysaccharides, anionic guar-based polysaccharides, anionic cellulose-based polysaccharides, the anionic cellulose-based polysaccharides including but not limited to carboxymethylcellulose (CMC), oxidized cellulose, anionic cellulose ethers and any combination thereof; or comprising carboxymethylcellulose (CMC);

[0232] c) having a net anionic charge;

[0233] d) having an anionic charge density range selected from the ranges of 0.1 meq / g to 10 meq / g, 0.5 meq / g to 7.5 meq / g, and 1 meq / g to 5 meq / g as measured by Mütek charge titration at pH 8.5;

[0234] e) having a degree of substitution (DS) of anionic charge on the polysaccharide selected from the group consisting of 0.02-2.5, 0.3-2.0, and 0.5-1.8;

[0235] f) having a degree of polymerization (DP) of anionic polysaccharides selected from the ranges of 500-25,000, 100-10,000 and 200-5,000;

[0236] g) formulated in a manner selected from the group consisting of: (i) as a dry powder and (ii) as an aqueous solution comprising a weight percent range of APP solids selected from the group consisting of 0.5%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to the paper machine; and

[0237] h) when formulated into an aqueous solution comprising 2 wt% CMC, the solution has a viscosity selected from the group consisting of at least 5 cps, at least 10 cps, at least 20 cps, and 5 cps-20 cps at pH=7 and 23°C.

[0238] In some embodiments, the fiber feedstock comprising cellulosic fibers comprises one or more of the following: a) an aqueous slurry comprising cellulosic fibers obtained from a source selected from the group consisting of softwood fibers, hardwood fibers, recycled fibers, refined fibers, mill broke fibers, non-wood fibers including but not limited to wheat straw pulp, and mixtures of any of the foregoing;

[0239] b) optionally comprising pulp selected from kraft pulp, bleached pulp, unbleached pulp, process water from pulp, paper and / or paperboard production, neutral sulfite semi-chemical (NSSC) pulp, mechanical pulp and mixtures of any of the foregoing;

[0240] c) optionally comprising a feedstock selected from thick stock, thick stock diluted with chemical water, synthetic water, white water and / or process water and thin stock, and mixtures of any of the foregoing; and / or

[0241] d) having a pH selected from the ranges of 3.0-9.0, 4.0-8.0, and 4.5-7.5.

[0242] In an exemplary embodiment,

[0243] a) at least one cationic GPAM comprising a high molecular weight base polymer comprising a copolymer of: (i) a cationic monomer selected from DADMAC, AETAC and combinations thereof; (ii) a nonionic monomer selected from acrylamide, methacrylamide and combinations thereof; and (iii) an anionic monomer optionally selected from acrylic acid, its corresponding water-soluble salts, water-dispersible alkali metal salts, alkaline earth metal salts, ammonium salts and combinations thereof, or the at least one cationic GPAM comprising a high molecular weight base polymer is obtainable by reacting glyoxal with a cationic base copolymer consisting of acrylamide and DADMAC, and is optionally in aqueous form;

[0245] b) at least one anionic polysaccharide promoter comprises anionic cellulose-based polysaccharides, including but not limited to carboxymethyl cellulose (CMC), oxidized cellulose, anionic cellulose ethers, and any combination thereof, or the at least one anionic polysaccharide promoter comprises carboxymethyl cellulose (CMC); and / or

[0247] c) wherein the method optionally comprises adding at least one anionic acrylamide-based (APAM) accelerator comprising a copolymer of acrylamide and acrylic acid, the corresponding water-soluble salts of acrylic acid, water-dispersible alkali metal salts, alkaline earth metal salts, ammonium salts and combinations thereof.

[0248] In some embodiments, the method results in the formation of a paper product. In some embodiments, the paper product comprises one or more of the following properties:

[0249] a) comprising a weight percentage of said at least one cationic GPAM comprising a high molecular weight base polymer selected from the range of 0.02%-10% and 0.05%-5% by weight of dry paper;

[0250] b) comprising a weight percentage of said at least one anionic polysaccharide promoter selected from the range of 0.02%-10% and 0.05%-5% by weight of dry paper;

[0251] c) exhibit (i) increased dry tensile strength; (ii) increased resistance to rupture, as measured by bursting strength; (iii) increased resistance to compression, as measured by the STFI compression test; and (iv) increased resistance to tearing compared to paper products prepared in an equivalent manner using cationic GPAM and / or anionic polyacrylamide (APAM) accelerators comprising lower molecular weight base polymers (e.g., less than 50 kDa); and / or

[0252] d) selected from the following paper products comprising a cellulosic paperboard web, which paper products optionally mainly include cellulosic fibers and fiber-based products, including but not limited to hand sheets, paperboard-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging board types, toilet tissue and towel types, paper materials, paper towels, diapers, sanitary napkins, training pants, panty liners, incontinence briefs, tampons, urine pads, cat litter box liners, coffee filters, air filters, dryer pads, floor cleaning pads, absorbent facial tissue, absorbent bathroom tissue, napkins, wrapping paper, paperboard boxes, bag paper and other paper products, etc.

[0253] The present invention also provides a paper product comprising one or more compositions or a combination of (a) and (b) for strengthening paper or paperboard obtainable by the method disclosed herein. In some embodiments, the paper product comprises one or more of the following properties:

[0254] a) comprising a percentage of said at least one cationic GPAM comprising a high molecular weight base polymer selected from the range of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product;

[0255] b) comprising a percentage of said at least one anionic polysaccharide promoter selected from the range of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product;

[0256] c) exhibit (i) increased dry tensile strength; (ii) increased resistance to rupture, as measured by bursting strength; (iii) increased resistance to compression, as measured by the STFI compression test; and (iv) increased resistance to tearing compared to paper products prepared in an equivalent manner using cationic GPAM and / or anionic polyacrylamide (APAM) accelerators comprising lower molecular weight base polymers (e.g., less than 50 kDa); and / or

[0257] d) selected from the following paper products comprising a cellulosic paperboard web, which paper products optionally mainly include cellulosic fibers and fiber-based products, including but not limited to hand sheets, paperboard-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging board types, toilet tissue and towel types, paper materials, paper towels, diapers, sanitary napkins, training pants, panty liners, incontinence briefs, tampons, urine pads, cat litter box liners, coffee filters, air filters, dryer pads, floor cleaning pads, absorbent facial tissue, absorbent bathroom tissue, napkins, wrapping paper, paperboard boxes, bag paper and other paper products, etc.

[0258] Having described the present invention in detail, the invention is further described in the following examples.

[0259] Example

[0260] The following examples are presented for illustrative purposes only and are not intended to be limiting.

[0261] Example 1: Strengthening Handsheets Using High Molecular Weight Cationic GPAM and APP

[0262] To determine the effectiveness of cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight (MW) base polymer and an anionic polysaccharide accelerator ("APP") for strengthening paper or paperboard products, two GPAM samples and one APP, carboxymethyl cellulose (CMC), were prepared and used to strengthen handsheets.

[0263] Preparation of Cationic GPAM and CMC

[0264] GPAM1 and GPAM2 are prepared by reacting glyoxal with a cationic base copolymer of acrylamide and DADMAC to achieve a weight ratio of glyoxal to base polymer ranging from 5:95 to 10:90. GPAM1 and GPAM2 have the same monomer composition. Polymer molecular weights were measured using gel permeation chromatography. Molecular weight calculations were performed using calibration based on polyethylene oxide standards.

[0265] The weight average molecular weight (MW) of the GPAM1 base polymer is 250 kDa, while the weight average molecular weight of the GPAM2 base polymer is 10 kDa. GPAM1 has a higher charge density (+1.7 meq / g) and molecular weight (250 kDa). GPAM2 has a lower charge density (+0.35 meq / g) and molecular weight (10 kDa).

[0266] The anionic polysaccharide promoter CMC has a negative charge density of about -2.8 meq / g. CMC was formulated into a 2% CMC aqueous solution with a viscosity of 60 cps measured by an LVT Brookfield viscometer using a #2 spindle at 60 rpm at 23°C.

[0267] For comparison, anionic polyacrylamide (APAM) composed of a copolymer of acrylamide and acrylic acid was prepared. APAM contained about 10% by weight of acrylic acid and had a weight average molecular weight of about 300 kDa as determined by gel permeation chromatography. The samples are listed in Table 1.

[0268] GPAM1, GPAM2 and APAM samples were formulated as aqueous solutions containing approximately 8 wt% solids content.

[0269] The GPAM, CMC and APAM solutions were then combined to form a reinforcement system for handsheet preparation.

[0270] Table 1: GPAM, CMC and APAM

[0271]

[0272] Handsheet preparation

[0273] An unbleached kraft pulp furnish is obtained and the strengthening system of the present invention is prepared by treating a portion of the furnish with cationic GPAM1 (MW 250 kDa) or cationic GPAM2 (MW 10 kDa) at a dosage level of 0, 4, 8 or 12 lb / ton, where lb / ton represents the number of pounds of dry polymer per ton of solids in the furnish. The resulting slurry is then treated with CMC at a dosage level of 0, 1, 2, 3.75 or 5 lb / ton or APAM at a dosage level of 0, 2, 4 and 8 lb / ton. During the addition of the polymer, all of the slurry is thoroughly mixed. After mixing, the weight ratio of GPAM:CMC (dry:dry) is about 4:1, and the combined net charge is +1 meq / g to +3.5 meq / g.

[0274] A portion of the batch was also treated with 6 lb / ton of alum in the following order of addition. The remainder of the batch was treated with 6 lb / ton of alum and 4 lb / ton of rosin size in the following order of addition.

[0275] For the alum treated batch, the chemical addition sequence and mixing times are summarized below:

[0276] - At 60 seconds, add alum.

[0277] - At 45 seconds, add GPAM1 or GPAM2 (if used).

[0278] - At 30 seconds, add CMC or APAM (if used).

[0279] At 0 seconds, the agitator was stopped and a hand sheet was made.

[0280] For the alum and rosin size treated furnishes, the chemical addition sequence and mixing times are summarized below:

[0281] - At 60 seconds, add GPAM1 or GPAM2 (if used).

[0282] - At 50 seconds, add CMC or APAM (if used).

[0283] - At 35 seconds, add alum.

[0284] - At 25 seconds, add rosin glue.

[0285] At 0 seconds, the agitator was stopped and a hand sheet was made.

[0286] Handsheets (about 175.8 g / m 2 ). After chemical treatment of the furnish, a 50 mL aliquot was removed to measure the solution charge, and the remaining furnish was used to make 36 gram sheets of paper. The sheets were pressed using an air roller press (set at 15 psi) and then drum dried (set at 240°F, total drying time 200 seconds). The sheets were also cured in a forced air oven set at 105°C for 5 minutes.

[0287] Prior to testing, the handsheet samples were conditioned at least overnight at 23°C and 50% relative humidity. This follows the method of "TAPPI T 402om-93: Standard Conditioning and Testing Conditions for Paper, Paperboard, Pulp, Handsheets, and Related Products".

[0288] Example 2: Comparison of GPAM 1 and GPAM 2 in strengthening handsheets

[0289] To determine the effect of cationic GPAM molecular weight on handsheet strength, handsheets prepared according to Example 1 using cationic GPAM1 (high MW, high charge) or GPAM2 (low MW, low charge) in combination with anionic polysaccharide promoters of the present invention, CMC or APAM were tested and used as a basis for comparison. The basic function of CMC is to keep the Zeta potential of the system anionic. Zeta potential is the parameter that determines the electrical interaction between particles, and higher values ​​(positive or negative) prevent flocculation. The pH of the pulp was adjusted to about 4.9 before adding 6 lb / ton alum and to about 4.7 after the addition of alum. The conductivity was about 1000 μS / cm.

[0290] The handsheets were tested to determine their compressive strength (as measured by cross direction (CD) and machine direction (MD) STFI compression tests (CD STFI and MD STFI)), burst strength (burst resistance), cross direction dry tensile strength (CD DT), cross direction and machine direction tear strength (CD Tear and MD Tear), as described below.

[0291] STFI compression (CD STFI, MD STFI)

[0292] The STFI compression test is used to determine the compressive strength of handsheets. The specimen is placed in two clamps that are pressed against each other until compression failure occurs. The maximum force that causes failure is measured and reported in pounds-force per inch (lb / in). The higher the value, the higher the compressive strength of the paper or paperboard. This test follows TAPPI Test Method 826pm-92: Short Span Compressive Strength of Containerboard. Sixteen measurements are made for CD and twelve for MD under each condition using a Lorentzen & Wettre (L&W) Compression Strength Tester STFI, and the average is reported. The results are based on 175.8 g / m 2 The basis weight is normalized.

[0293] Bursting strength (bursting resistance)

[0294] The burst strength test is widely used as a measure of the resistance of many types of paper to rupture. The test is designed to measure the bursting strength of paper and paper products from 4 psi to 200 psi (30 kPa to 1400 kPa). Burst strength is defined as the hydrostatic pressure required to cause the material to rupture when the pressure is increased at a controlled constant rate through a rubber diaphragm to a circular area of ​​1.20 inches (30.5 mm) in diameter, in pounds per square inch (psi) or kilopascals (kPa). The test follows TAPPI Test Method T 403om-10: Bursting Strength of Paper. Sixteen measurements were made at each condition using a TMI Burst Tester Model 13-60-00-0001, and the average value is reported. The data is recorded in psi (pounds per square inch). The higher the bursting strength measurement, the stronger the paper. The results are based on 175.8 g / m 2 The basis weight is normalized.

[0295] Dry tensile strength (CD DT)

[0296] Tensile strength is measured by applying a constant rate of elongation to a sample and recording three tensile break properties of paper and paperboard. These three properties are: (i) the force per unit width required to break the specimen (tensile strength), (ii) the elongation at break (stretch), and (iii) the energy absorbed per unit area of ​​the specimen before breaking (tensile energy absorption). Only dry tensile strength measurements are reported herein. This method is applicable to all types of paper, but not corrugated paperboard. The procedure refers to TAPPI Test Method T494. Twelve measurements are made in the cross direction under each condition, and the average is reported. Results are based on 175.8 g / m 2 The basis weight was normalized. A Thwing-Albert QC3A tensile testing machine was used in this study.

[0297] Tear test (CD tear and MD tear)

[0298] Tear testing measures the force perpendicular to the plane of the paper required to tear a sheet of paper a specified distance after tearing has started using an Elmendorf-type tear tester. One or more sheets of sample material are torn together a fixed distance using the pendulum of an Elmendorf-type tear tester. The work done during tearing is measured by the loss of potential energy of the pendulum. The instrument scale is calibrated to indicate the average force applied when a certain number of paper layers are torn together (the work done divided by the total distance torn). For a single sheet of paper, tear resistance is measured directly in grams. This test follows TAPPI method T 414om-88: Internal Tear Resistance of Paper (Elmendorf-Type Tester). Use the Thwing-Albert The tester made eight measurements in the machine direction MD and four measurements in the cross direction CD under each condition, and the average value was reported.

[0299] Polymer Charge Demand (PCD)

[0300] The charge demand is the amount of polymer (cation or anion) consumed at the equivalence point of a polyelectrolyte titration. It is based on the principle that oppositely charged polymers tend to neutralize each other in a 1:1 stoichiometry.

[0301] The charge demand of the solution phase is measured using an AFG CAS contact charge analyzer. The aqueous solution is filtered from the chemically treated pulp sample using a 100 mesh screen. A 10.0 ml aliquot of the filtered sample is placed in the measuring cell and the probe is inserted. The piston of the measuring cell oscillates and a high flow rate is generated. Any charged material adsorbed on the surface of the measuring cell and the piston is separated from its counter ion by the flow, thus generating a streaming current. The two electrodes in the measuring cell receive this current. A polyelectrolyte of opposite charge (polyDADMAC for anionic samples and PVSK for cationic samples) is added until the potential zero point is reached. The amount of titrant used is recorded. The results are usually expressed in μEq / L of sample.

[0302] The results are shown in Table 2.

[0303] Table 2: Comparison of GPAM1 (high MW, high charge) and GPAM2 (low MW, low charge) Papermaking strength test results

[0304]

[0305] Results showed that GPAM1 and GPAM2 improved the strength properties of the handsheets compared to the control condition (6 lb / ton alum only). GPAM1, which has a higher charge density and higher molecular weight, showed an average 4.2% improvement in strength over GPAM2 in all test modes, with a maximum improvement of 11% in specific strength tests.

[0306] It was surprisingly found that the combination of GPAM1 with low doses of CMC (1 lb / ton or 2 lb / ton) provided synergistic strength enhancement in all tests compared to the combination of GPAM1 with higher doses of APAM (2 lb / ton or 4 lb / ton).

[0307] For example, adding 2 lb / ton of liquid CMC provides an average 8.1% strength increase over adding 8 lb / ton of GPAM1 alone. In contrast, adding 4 lb / ton of improved APAM provides an average 3.2% strength increase over adding 8 lb / ton of GPAM1 alone.

[0308] These results strongly suggest that high MW, high charge GPAMs provide better dry strength enhancement than low MW, low charge GPAMs. In addition, these results provide preliminary proof of concept that the combination of APPs (such as CMC) with high MW, high charge GPAMs provides unexpected synergistic enhancement of dry strength in multiple test modes.

[0309] Without being bound by theory, it can be speculated that the synergistic improvement in dry strength may be due to the higher degree of polymerization and higher cationic charge provided by GPAM1 combined with the use of anionic CMC, which acts to maintain the zeta potential of the anions in the system.

[0310] Unexpected results were also observed in the PCD results, which showed that high dosages of GPAM1 (8 lb / ton) alone provided the smallest negative PCD values. The addition of CMC (2 lb / ton) provided a greater change in PCD values ​​(closer to the PCD values ​​of untreated pulp, e.g., -76 μEq / L) than the addition of higher dosages of APAM (4 lb / ton). These results were surprising because lower dosage levels of CMC outperformed higher dosage levels of APAM in all strength tests while providing PCD values ​​closer to untreated pulp (-38 μEq / L).

[0311] These results also strongly suggest that the combination of higher molecular weight GPAM1 with CMC accelerator is more suitable for producing paper or paperboard with enhanced strength properties.

[0312] Example 3: Effect of addition order and rosin size on high-dose GPAM1 and CMC reinforced handsheets

[0313] To determine the effect of addition order and rosin size on the reinforcing effect of the high MW cationic GPAM and APP combinations of the present invention, handsheets prepared according to Example 1 were tested using high dosages of GPAM1 (high MW, high charge, 12 lb / ton) in combination with CMC and alum alone (added before GPAM1 and CMC) or with alum and rosin size (added after GPAM1 and CMC). APAM was used as a basis for comparison.

[0314] The pH of the pulp was adjusted to about 4.7 before adding 6 lb / ton of alum and about 4.57 after adding alum. The conductivity was about 1000 μS / cm

[0315] The handsheets were analyzed for CD STFI, MD STFI, Burst, CD DT, and MD Tear as tested in Example 2. The results are shown in Tables 3 and 4.

[0316] Table 3: Handsheet strength test results with alum added before GPAM1 and CMC

[0317]

[0318] Table 4: Handsheet strength test results after adding alum and rosin size after GPAM1 and CMC

[0319]

[0320] The results showed that the combination of GPAM1 and CMC was effective in improving the dry strength properties of handsheets using alum alone as well as alum and rosin size, regardless of the order of addition.

[0321] It was surprisingly found that the addition of APAM (4 lb / ton) with alum alone resulted in a decrease in CD tear strength compared to GPAM 1 alone. In contrast, the anionic polysaccharide accelerator CMC provided equivalent or improved handsheet strength in all tested modes compared to GPAM 1 alone.

[0322] These results provide proof of concept that the inventive system for improving paper strength comprising high molecular weight GPAM and APP can be used in a variety of papermaking applications under a variety of conditions.

Claims

1. A composition for strengthening paper or paperboard, optionally an aqueous composition, comprising: (a) at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer; and (b) at least one anionic polysaccharide accelerator ("APP"), optionally carboxymethylcellulose (CMC); The high molecular weight base polymer has a weight average molecular weight selected from at least 50 kDa, at least 80 kDa, at least 100 kDa, at least 250 kDa, or 100 kDa-5000 kDa, inclusive.

2. A material combination, the combination comprising: (a) at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer, optionally an aqueous composition; and (b) at least one anionic polysaccharide accelerator ("APP"), optionally carboxymethylcellulose (CMC); wherein the high molecular weight base polymer (a) has a weight average molecular weight selected from at least 50 kDa, at least 80 kDa, at least 100 kDa, at least 250 kDa, and 100 kDa-5000 kDa; and Further, wherein when the combination of materials (a) and (b) is added separately, simultaneously or as a premixed combination to a papermaking system or a furnish composition comprising a furnish composition, the furnish composition comprises cellulose fibers for making paper or paperboard, wherein (a) and (b) may be added in any order, and a paper or paperboard material having enhanced strength is produced compared to when the combination of materials (a) and (b) is not added to the papermaking system or the furnish composition.

3. The composition or combination according to claim 1 or 2, wherein the at least one cationic GPAM comprising a high molecular weight base polymer comprises one or more of the following properties: (a) comprising a weight ratio range of glyoxal:base polymer selected from 1:99 to 50:50 and 5:95 to 20:80; (b) obtained by reacting glyoxal with the high molecular weight base polymer, wherein the high molecular weight base polymer comprises an acrylamide-based copolymer, the copolymer comprises a neutral monomer, a cationic monomer and optionally an anionic monomer, further wherein (i) the neutral monomer is selected from monomers containing primary amides, and the monomers include acrylamide, methacrylamide, ethyl acrylamide, crotonamide, N-methyl acrylamide, N-butyl acrylamide, N-ethyl methacrylamide and any combination thereof; (ii) the cationic monomer is selected from acryloyloxyethyl trimethyl ammonium chloride ("AETAC"), methacryloyloxyethyl trimethyl ammonium chloride ("MAETAC"), methacrylamidopropyl trimethyl ammonium chloride ("MAPTAC"), acrylamidopropyl trimethyl ammonium chloride ("APTAC"), methacryloyloxyethyl dimethyl ammonium sulfate, diallyl dimethyl ammonium chloride ("DADMAC"); dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, including but not limited to dimethylaminoethyl acrylate ("DMAEA"), dimethylaminoethyl methacrylate ("DMAEA"), dimethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl acrylate methyl sulfate quaternary salt, dimethylaminoethyl acrylate benzyl chloride quaternary salt, dimethylaminoethyl acrylate sulfate, dimethylaminoethyl acrylate hydrochloride, diethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate quaternary salts of ethyl ester methyl sulfate, quaternary salts of dimethylaminoethyl methacrylate benzyl chloride, quaternary salts of dimethylaminoethyl methacrylate sulfate, dimethylaminoethyl methacrylate hydrochloride, dimethylaminoethyl methacrylate hydrochloride; dialkylaminoalkyl acrylamides and methacrylamides and their quaternary salts or acid salts, including but not limited to acrylamidopropyl trimethyl ammonium chloride, dimethylaminopropyl acrylamide, dimethylaminopropyl acrylamide methyl sulfate quaternary salt, dimethylaminopropyl acrylamide sulfate, dimethylaminopropyl acrylamide hydrochloride, methacrylamidopropyl trimethyl ammonium chloride, dimethylaminopropyl methacrylamide, dimethylaminopropyl methacrylamide methyl sulfate quaternary salt, dimethylaminopropyl methacrylamide sulfate, dimethylaminopropyl methacrylamide hydrochloride, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; and diallyl dialkyl ammonium halides, including but not limited to diallyl diethyl ammonium chloride and diallyl dimethyl ammonium chloride ("DADMAC") and any combination thereof; and (iii) the optional anionic monomer contains a functional group selected from carboxylic acid, sulfonic acid, phosphonic acid, their corresponding water-soluble salts, their corresponding water-dispersible salts and any combination thereof, including but not limited to acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinyl sulfonic acid, 2-acrylamide-2-methylpropanesulfonic acid (AMPS), acrylamide methanesulfonic acid, acrylamide ethanesulfonic acid, 2-hydroxy-3-acrylamide propanesulfonic acid, styrene sulfonic acid, vinyl phosphonic acid and their corresponding alkali metal, alkaline earth metal and ammonium salts and any combination thereof; (c) obtainable by reacting glyoxal with a cationic base copolymer consisting of acrylamide and DADMAC, and optionally in aqueous form; (d) having a cationic monomer content percentage in the range of 5 wt% to 60 wt%, an anionic monomer content percentage in the range of 0 wt% to 50 wt%, and the remaining monomer content is nonionic; (e) having a cationic charge density at pH 8.0 selected from the range of 0.02 meq / g to 5 meq / g, 1 meq / g to 4 meq / g, and 1.4 meq / g to 2 meq / g; (f) formulated in a manner selected from the group consisting of: (i) a dry powder and (ii) an aqueous solution comprising a GPAM solids weight percentage range selected from the group consisting of 1%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to a paper machine; and (g) when added to a papermaking system or composition comprising cellulosic fibers for making paper or paperboard, at a dosage selected from the ranges of 0.2 lb / ton-25 lb / ton, 4 lb / ton-12 lb / ton, and 1 lb / ton-10 lb / ton of dry fibers.

4. The composition or combination according to claim 1, 2 or 3, wherein the at least one anionic polysaccharide promoter comprises one or more of the following properties: (a) having a weight average molecular weight selected from 10 kDa-5000 kDa, 20 kDa-2000 kDa and 40 kDa-1000 kDa; (b) comprising an anionic polysaccharide selected from the group consisting of anionic starch-based polysaccharides, anionic alginate-based polysaccharides, anionic guar-based polysaccharides, anionic cellulose-based polysaccharides, including but not limited to carboxymethylcellulose (CMC), oxidized cellulose, anionic cellulose ethers, and any combination thereof; (c) comprising carboxymethyl cellulose (CMC), optionally in aqueous form or in dry powder form; (d) having a net anionic charge; (e) having an anionic charge density range selected from the ranges of 0.1 meq / g to 10 meq / g, 0.5 meq / g to 7.5 meq / g, and 1 meq / g to 5 meq / g as measured by Mütek charge titration at pH 8.5; (f) having a degree of substitution (DS) of anionic charge on the polysaccharide selected from the group consisting of 0.02-2.5, 0.3-2.0, and 0.5-1.8; (g) a degree of polymerization (DP) of an anionic polysaccharide having residues selected from the ranges of 500-25,000, 100-10,000, and 200-5,000; (h) formulated in a manner selected from the group consisting of: (i) as a dry powder and (ii) as an aqueous solution, the aqueous solution comprising a weight percent range of APP solids selected from the group consisting of 0.5%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to the paper machine; (i) when formulated into an aqueous solution comprising the anionic polysaccharide promoter, optionally 2 wt% CMC, the solution has a viscosity selected from at least 5 cps, at least 10 cps, at least 20 cps and 5 cps-10 cps at pH=7 and 23°C; and (j) when added to a papermaking system or composition comprising cellulose fibers for making paper or paperboard, at a dosage selected from the ranges of 0.1 lb / ton-15 lb / ton, 0.2 lb / ton-8 lb / ton, and 0.5 lb / ton-6 lb / ton of dry fibers.

5. A composition or combination according to any one of the preceding claims, wherein: (a) the composition or the combination of (a) and (b), when combined, is formulated in a manner selected from the group consisting of: (i) at least one dry powder (ii) at least one aqueous solution; (b) the composition or the combination of (a) and (b), when combined, having a weight ratio of GPAM:APP (dry:dry) selected from the ranges of 1:10 to 10:1, 10:1 to 1:2, and 5:1 to 3:1; and (c) the composition or the combination of (a) and (b), when combined, has a net charge selected from the range of -5 meq / g to +5 meq / g, 0 meq / g to +5 meq / g, and +1 meq / g to +3.5 meq / g.

6. A composition or combination according to any one of the preceding claims, wherein: (a) the at least one cationic GPAM comprising a high molecular weight base polymer comprises a high molecular weight base polymer comprising a copolymer of: (i) a cationic monomer selected from DADMAC, AETAC and combinations thereof; (ii) a nonionic monomer selected from acrylamide, methacrylamide and combinations thereof; and (iii) an anionic monomer optionally selected from acrylic acid, a water-soluble salt corresponding to said acrylic acid, a water-dispersible alkali metal salt, an alkaline earth metal salt, an ammonium salt and combinations thereof, or comprising a cationic monomer selected from acrylamide and DADMAC, and optionally the at least one cationic GPAM is in aqueous form; (b) the at least one anionic polysaccharide promoter comprises an anionic cellulose-based polysaccharide, including but not limited to carboxymethyl cellulose (CMC), oxidized cellulose, anionic cellulose ethers, and any combination thereof, or the at least one anionic polysaccharide promoter comprises carboxymethyl cellulose (CMC); and (c) wherein the composition and / or the combination optionally comprises at least one anionic acrylamide-based (APAM) accelerator comprising a copolymer of acrylamide and acrylic acid, a water-soluble salt corresponding to the acrylic acid, a water-dispersible alkali metal salt, an alkaline earth metal salt, an ammonium salt, and combinations thereof.

7. A composition or combination according to any one of the preceding claims, wherein when said composition or combination is added to a papermaking system or composition comprising cellulosic fibers for making paper or paperboard, a paper product is produced comprising one or more of the following properties: (a) a GPAM solids percentage selected from the range of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product; (b) an anionic polysaccharide promoter solids percentage selected from the ranges of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of the dry paper product; and (c) (i) improved dry tensile strength; (ii) improved resistance to rupture (as measured by bursting strength); (iii) improved resistance to compression (as measured by the STFI compression test); and (iv) improved tear resistance compared to paper products prepared in an equivalent manner using cationic GPAM and anionic polyacrylamide (APAM) promoters comprising lower molecular weight base polymers (e.g., less than 50 kDa).

8. A furnish composition for making paper or paperboard, said furnish composition having been treated with at least one strengthening system selected from the composition for strengthening paper or paperboard and the material combination according to any one of the preceding claims, wherein said furnish composition comprises an aqueous slurry of a fiber raw material comprising cellulosic fibers, and further comprises one or more of the following: (a) an aqueous slurry of cellulosic fibers, optionally obtained from a source selected from the group consisting of softwood fibers, hardwood fibers, recycled fibers, refined fibers, mill broke fibers, non-wood fibers including but not limited to wheat straw pulp, and mixtures of any of the foregoing; (b) a pulp selected from the group consisting of kraft pulp, bleached pulp, unbleached pulp, process water from pulp, paper and / or paperboard production, neutral sulfite semi-chemical (NSSC) pulp, mechanical pulp and mixtures of any of the foregoing; and (c) a raw material selected from thick stock, thick stock diluted with chemical water, synthetic water, white water and / or process water, and thin stock, and any mixture of the foregoing; Further, wherein when the at least one strengthening system is added to a papermaking system comprising the furnish composition and / or to the furnish composition, the amount of the at least one strengthening system is sufficient to improve the strength properties of paper or paperboard produced from the furnish composition, compared to when the strengthening system is not added to the papermaking system comprising the furnish composition or to the furnish composition.

9. A papermaking process for making one or more paper products, optionally one or more absorbent paper products, from a fibrous raw material comprising cellulose fibers, wherein the process comprises adding: (a) at least one cationic glyoxalated polyacrylamide ("GPAM") comprising a high molecular weight base polymer, wherein the high molecular weight base polymer has a weight average molecular weight selected from the group consisting of at least 50 kDa, at least 80 kDa, at least 100 kDa, at least 250 kDa, and 100 kDa to 5000 kDa; and (b) at least one anionic polysaccharide accelerator ("APP"), optionally carboxymethylcellulose (CMC); in During the papermaking process, (a) and (b) are added separately, simultaneously or as a premixed combination at one or more points during the papermaking process selected from any time before, during and after the paper product is formed; and / or (a) and (b) are added separately, simultaneously or as a premixed combination at one or more locations in the papermaking system; and / or (a) and (b) may be added as separate compositions in any order, or as a premixed composition comprising (a) and (b), optionally an aqueous composition, further optionally wherein when (a) and (b) are added separately, the addition of (a) and (b) is simultaneous or close in time, for example, (a) and (b) are added within two hours, one hour, 30 minutes, 10 minutes, 1 minute or less than 1 minute of each other.

10. The method of claim 9, wherein the at least one cationic GPAM comprising a high molecular weight base polymer and the at least one anionic polysaccharide promoter: (a) formulated as a dry polymer or an aqueous solution, each solution having a solid weight percentage selected from the range of 1%-25%, 1%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to the paper machine; (b) adding during the process to obtain a weight ratio of GPAM:APP (dry:dry) selected from the ranges of 1:10 to 10:1, 10:1 to 1:2, and 5:1 to 3:1; (c) when combined, have a net charge selected from the range of -5 meq / g to +5 meq / g, 0 meq / g to +5 meq / g, and +1 meq / g to +3.5 meq / g; (d) adding during the method in a manner selected from the following additions of the cationic GPAM and APP aqueous solutions: (i) simultaneously; (ii) sequentially in any order; (iii) together as a premixed solution; and (iv) any combination thereof; (e) adding said cationic GPAM and APP aqueous solution during said process in a manner selected from the group consisting of: (i) adding said cationic GPAM and APP aqueous solution to said aqueous fibrous stock comprising cellulosic fibers at the wet end of a paper machine prior to forming said paper product; (ii) adding said cationic GPAM and APP aqueous solution to a formed cellulosic fiber web during formation of said paper product; (iii) adding the cationic GPAM and APP aqueous solution to one or more surfaces of the paper product after the paper product is formed; and (iv) any combination thereof; (f) adding a dosage of said at least one cationic GPAM selected from the ranges of 0.2 lb / ton-25 lb / ton, 0.5 lb / ton-12 lb / ton, and 1 lb / ton-10 lb / ton of dry fiber and a dosage of said at least one anionic polysaccharide promoter selected from the ranges of 0.1 lb / ton-15 lb / ton, 0.2 lb / ton-8 lb / ton, and 0.5 lb / ton-6 lb / ton of dry fiber when added to said aqueous fiber feedstock comprising cellulosic fibers; and (g) added during the process, wherein the addition points include but are not limited to in the hydrapulper, before refining the pulp, after refining the pulp, at the fan pump, before the headbox, at the headbox, by spraying, printing, coating and impregnation onto the paper web, onto preformed paper (e.g. by slot sizing), and onto dry paper (e.g. by spraying), and any combination thereof.

11. The method according to claim 9 or 10, wherein the at least one cationic GPAM comprising a high molecular weight base polymer comprises one or more of the following properties: (a) comprising a weight ratio range of glyoxal:base polymer selected from 1:99 to 50:50 and 5:95 to 20:80; (b) obtained by reacting glyoxal with the high molecular weight base polymer, wherein the high molecular weight base polymer comprises an acrylamide-based copolymer, the copolymer comprises a neutral monomer, a cationic monomer and optionally an anionic monomer, further wherein (i) the neutral monomer is selected from monomers containing primary amides, and the monomers include acrylamide, methacrylamide, ethyl acrylamide, crotonamide, N-methyl acrylamide, N-butyl acrylamide, N-ethyl methacrylamide and any combination thereof; (ii) the cationic monomer is selected from acryloyloxyethyl trimethyl ammonium chloride ("AETAC"), methacryloyloxyethyl trimethyl ammonium chloride ("MAETAC"), methacrylamidopropyl trimethyl ammonium chloride ("MAPTAC"), acrylamidopropyl trimethyl ammonium chloride ("APTAC"), methacryloyloxyethyl dimethyl ammonium sulfate, diallyl dimethyl ammonium chloride ("DADMAC"); dialkylaminoalkyl acrylates and dialkylaminoalkyl methacrylates and their quaternary salts or acid salts, including but not limited to dimethylaminoethyl acrylate ("DMAEA"), dimethylaminoethyl methacrylate ("DMAEA"), dimethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl acrylate methyl sulfate quaternary salt, dimethylaminoethyl acrylate benzyl chloride quaternary salt, dimethylaminoethyl acrylate sulfate, dimethylaminoethyl acrylate hydrochloride, diethylaminoethyl acrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate methyl chloride quaternary salt, dimethylaminoethyl methacrylate quaternary salts of ethyl ester methyl sulfate, quaternary salts of dimethylaminoethyl methacrylate benzyl chloride, quaternary salts of dimethylaminoethyl methacrylate sulfate, dimethylaminoethyl methacrylate hydrochloride, dimethylaminoethyl methacrylate hydrochloride; dialkylaminoalkyl acrylamides and methacrylamides and their quaternary or acid salts, including but not limited to acrylamidopropyl trimethylammonium chloride, dimethylaminopropyl acrylamide, dimethylaminopropyl acrylamide methyl sulfate quaternary salt, dimethylaminopropyl acrylamide sulfate, dimethylaminopropyl acrylamide hydrochloride, methacrylamidopropyl trimethylammonium chloride, dimethylaminopropyl methacrylamide, dimethylaminopropyl methacrylamide methyl sulfate quaternary salt, dimethylaminopropyl methacrylamide sulfate, dimethylaminopropyl methacrylamide hydrochloride, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; and diallyl dialkyl ammonium halides, including but not limited to diallyl diethyl ammonium chloride and diallyl dimethyl ammonium chloride ("DADMAC") and any combination thereof; and (iii) the optional anionic monomer contains a functional group selected from carboxylic acid, sulfonic acid, phosphonic acid, their corresponding water-soluble salts, their corresponding water-dispersible salts and any combination thereof, including but not limited to acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinyl sulfonic acid, 2-acrylamide-2-methylpropanesulfonic acid (AMPS), acrylamide methanesulfonic acid, acrylamide ethanesulfonic acid, 2-hydroxy-3-acrylamide propanesulfonic acid, styrene sulfonic acid, vinyl phosphonic acid and their corresponding alkali metal, alkaline earth metal and ammonium salts and any combination thereof; (c) obtainable by reacting glyoxal with a cationic base copolymer consisting of acrylamide and DADMAC, and optionally in aqueous form; (d) having a cationic monomer content percentage in the range of 5 wt% to 60 wt%, an anionic monomer content percentage in the range of 0 wt% to 50 wt%, and the remaining monomer content is nonionic; (e) having a cationic charge density range selected from the ranges of 0.02 meq / g to 5 meq / g, 1 meq / g to 4 meq / g, and 1.4 meq / g to 2 meq / g at pH 8.

0.

12. The method of claim 9, 10 or 11, wherein the at least one anionic polysaccharide promoter comprises one or more of the following properties: (a) having a weight average molecular weight selected from 10 kDa-5000 kDa, 20 kDa-2000 kDa and 40 kDa-1000 kDa; (b) comprising an anionic polysaccharide selected from the group consisting of anionic starch-based polysaccharides, anionic alginate-based polysaccharides, anionic guar-based polysaccharides, anionic cellulose-based polysaccharides, the anionic cellulose-based polysaccharides including but not limited to carboxymethyl cellulose (CMC), oxidized cellulose, anionic cellulose ethers and any combination thereof; or comprising carboxymethyl cellulose (CMC); (c) having a net anionic charge; (d) having an anionic charge density range selected from the ranges of 0.1 meq / g to 10 meq / g, 0.5 meq / g to 7.5 meq / g, and 1 meq / g to 5 meq / g as measured by Mütek charge titration at pH 8.5; (e) having a degree of substitution (DS) of anionic charge on the polysaccharide selected from the group consisting of 0.02-2.5, 0.3-2.0, and 0.5-1.8; (f) having a degree of polymerization (DP) of anionic polysaccharide selected from the ranges of 500-25,000, 100-10,000 and 200-5,000; (g) formulated in a manner selected from the group consisting of: (i) as a dry powder and (ii) as an aqueous solution comprising a weight percent range of APP solids selected from the group consisting of 0.5%-15%, 2%-10% and 4%-8%, wherein the aqueous solution is optionally further diluted before being added to a paper machine; and (h) when formulated into an aqueous solution comprising 2 wt% CMC, the solution has a viscosity selected from the group consisting of at least 5 cps, at least 10 cps, at least 20 cps, and 5 cps-20 cps at pH = 7 and 23°C.

13. The method according to claim 9, 10, 11 or 12, wherein the fiber raw material comprising cellulose fibers: (a) an aqueous slurry comprising cellulosic fibers obtained from a source selected from the group consisting of softwood fibers, hardwood fibers, recycled fibers, refined fibers, mill broke fibers, non-wood fibers including but not limited to wheat straw pulp, and mixtures of any of the foregoing; (b) optionally comprising pulp selected from kraft pulp, bleached pulp, unbleached pulp, process water from pulp, paper and / or paperboard production, neutral sulfite semi-chemical (NSSC) pulp, mechanical pulp and mixtures of any of the foregoing; (c) optionally comprising a feedstock selected from the group consisting of a thick stock, a thick stock diluted with chemical water, synthetic water, white water and / or process water, a thin stock and a mixture of any of the foregoing; and (d) having a pH selected from the ranges of 3.0-9.0, 4.0-8.0, and 4.5-7.

5.

14. The method according to any one of claims 9 to 13, wherein: (a) the at least one cationic GPAM comprising a high molecular weight base polymer comprises a high molecular weight base polymer comprising a copolymer of: (i) a cationic monomer selected from DADMAC, AETAC and combinations thereof; (ii) a nonionic monomer selected from acrylamide, methacrylamide and combinations thereof; and (iii) an anionic monomer optionally selected from acrylic acid, a water-soluble salt corresponding to the acrylic acid, a water-dispersible alkali metal salt, an alkaline earth metal salt, an ammonium salt and combinations thereof, or the at least one cationic GPAM comprising a high molecular weight base polymer is obtainable by reacting glyoxal with a cationic base copolymer consisting of acrylamide and DADMAC, and is optionally in aqueous form; (b) the at least one anionic polysaccharide promoter comprises anionic cellulose-based polysaccharides, including but not limited to carboxymethyl cellulose (CMC), oxidized cellulose, anionic cellulose ethers and any combination thereof, or the at least one anionic polysaccharide promoter comprises carboxymethyl cellulose (CMC); and / or (c) wherein the method optionally comprises adding at least one anionic acrylamide-based (APAM) accelerator comprising a copolymer of acrylamide and acrylic acid, a water-soluble salt corresponding to the acrylic acid, a water-dispersible alkali metal salt, an alkaline earth metal salt, an ammonium salt, and combinations thereof.

15. The method of any one of claims 9-14, wherein the method results in the formation of a paper product, wherein the paper product: (a) comprising a weight percentage of said at least one cationic GPAM comprising a high molecular weight base polymer selected from the range of 0.02%-10% and 0.05%-5% by weight of said dry paper; (b) comprising a weight percentage of said at least one anionic polysaccharide promoter selected from the range of 0.02%-10% and 0.05%-5% of said dry paper weight; (c) exhibit (i) increased dry tensile strength; (ii) increased resistance to rupture, as measured by bursting strength; (iii) increased resistance to compression, as measured by the STFI compression test; and (iv) increased resistance to tearing compared to paper products prepared in an equivalent manner using cationic GPAM and / or anionic polyacrylamide (APAM) accelerators comprising lower molecular weight base polymers (e.g., less than 50 kDa); and (d) paper products selected from the group consisting of cellulosic paperboard webs, optionally predominantly comprising cellulosic fibers and fiber-based products, including but not limited to hand sheets, paperboard-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging paperboards, toilet tissues and towels, paper materials, paper towels, diapers, sanitary napkins, training pants, panty liners, incontinence briefs, tampons, urine pads, litter box liners, coffee filters, air filters, dryer pads, floor cleaning pads, absorbent facial tissue, absorbent bathroom tissue, napkins, wrapping paper, paperboard boxes, bag paper, and other paper products, and the like.

16. A paper product comprising one or more compositions for strengthening paper or paperboard according to any one of claims 1 to 8 or a combination of (a) and (b), obtainable by a method according to any one of claims 9 to 15, wherein the paper product: (a) comprising a percentage of said at least one cationic GPAM comprising a high molecular weight base polymer selected from the range of 0.02 wt% to 10 wt% and 0.05 wt% to 5 wt% of said dry paper product; (b) comprising a percentage of said at least one anionic polysaccharide promoter selected from the range of 0.02 wt. % to 10 wt. % and 0.05 wt. % to 5 wt. % of said dry paper product; (c) exhibit (i) increased dry tensile strength; (ii) increased resistance to rupture, as measured by bursting strength; (iii) increased resistance to compression, as measured by the STFI compression test; and (iv) increased resistance to tearing compared to paper products prepared in an equivalent manner using cationic GPAM and / or anionic polyacrylamide (APAM) accelerators comprising lower molecular weight base polymers (e.g., less than 50 kDa); and (d) paper products selected from the group consisting of cellulosic paperboard webs, optionally predominantly comprising cellulosic fibers and fiber-based products, including but not limited to hand sheets, paperboard-based products, beverage carriers, towels, milk and juice cartons, food trays, paper bags, liners for corrugated boxes, packaging paperboards, toilet tissues and towels, paper materials, paper towels, diapers, sanitary napkins, training pants, panty liners, incontinence briefs, tampons, urine pads, litter box liners, coffee filters, air filters, dryer pads, floor cleaning pads, absorbent facial tissue, absorbent bathroom tissue, napkins, wrapping paper, paperboard boxes, bag paper, and other paper products, and the like.

Citation Information

Patent Citations

  • Method for increasing paper strength

    CN105899729A

  • Glyoxalated inter-copolymers with high and adjustable charge density

    US20060270801A1

  • Paper product and method for increasing the strength thereof

    US20190177492A1

  • Compositions and methods for increased wet and dry strength

    WO2021188705A1

Cited By

  • Polycarboxyl copolymer water-based composition for internal addition of packaging paper board pulp, internal synergy of packaging paper short retention pulp and synergy of bamboo pulp paper wet end fibers as well as preparation and application methods of polycarboxyl copolymer water-based composition

    CN122257292A