Nozzle plate, liquid droplet discharge head, liquid droplet discharge apparatus, and method for manufacturing nozzle plate
By using {110} plane mask layer and non-wet etching technology on a single crystal silicon substrate, the nozzle flow path formed by {111} plane is solved, and the problem of insufficient density and injection characteristics of the nozzle plate is achieved, and the density is achieved and Stable droplets eject.
Patent Information
- Application Number
- CN202280093735.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-17
- Publication Date
- 2024-11-08
AI Technical Summary
The conventional nozzle plate is formed by anisotropic wet etching on a single crystal silicon substrate, resulting in a square shape, resulting in a decrease in the number of nozzle flow paths, and the high density cannot be achieved.
The mask layer formation and anisotropic wet etching are used to use the {110} surface of a single crystal silicon substrate. In combination with the use of a non-wet etching layer, the nozzle linear portion and the nozzle conical portion are designed to form a nozzle flow with the {111} surface. and a linear communication path is formed by dry etching to optimize the shape of the nozzle flow path to improve density and injection characteristics.
The high density of the nozzle plate and stable droplet ejection are achieved, the injection characteristics of the nozzle are improved, and the problems of vibration and insufficient ejection of the meniscus are avoided.
Smart Images

Figure CN118922919A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a nozzle plate, a liquid droplet discharging head, a liquid droplet discharging device, and a method for manufacturing the nozzle plate. Background Art
[0002] Conventionally, as a method for manufacturing a nozzle plate of a droplet discharging head of a droplet discharging device, there is known a method of forming nozzle flow paths by anisotropic wet etching a single crystal silicon substrate (for example, see Patent Document 1).
[0003] Patent Document 1: Japanese Patent No. 5519263
[0004] However, when anisotropic wet etching is performed on a single crystal silicon substrate whose surface crystal orientation is {100}, since the etching action advances in a fixed direction, only a nozzle flow path having a square opening on the surface opposite to the droplet discharge surface can be formed. Therefore, when a plurality of nozzle flow paths are arranged on the single crystal silicon substrate, the number of nozzle flow paths having a square opening is less than that of nozzle flow paths having a long hole opening. Summary of the invention
[0005] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a nozzle plate, a liquid droplet ejection head, a liquid droplet ejection device, and a method for manufacturing a nozzle plate that can increase the density of nozzles.
[0006] In order to solve the above-mentioned problems, the invention described in claim 1 provides a nozzle plate including a plurality of nozzle flow paths penetrating therethrough for discharging droplets from nozzles on a single crystal silicon substrate, wherein:
[0007] The first surface and the second surface of the single crystal silicon substrate are {110} planes, and the second surface is a surface facing the first surface and is a surface on which the nozzle is formed.
[0008] The invention described in claim 2 is the nozzle plate according to claim 1, wherein:
[0009] The nozzle flow path includes a surface composed of a {111} surface.
[0010] The invention described in claim 3 is the nozzle plate described in claim 1 or 2, wherein:
[0011] The nozzle flow path includes a nozzle tapered portion, in which a cross-sectional area orthogonal to a discharge direction of liquid droplets, that is, a flow path area, gradually narrows as it moves from the first surface toward the second surface.
[0012] The nozzle tapered portion includes a {111} surface.
[0013] The invention described in claim 4 is the nozzle plate described in claim 3, wherein:
[0014] The nozzle tapered portion is formed of a {111} surface.
[0015] The invention described in claim 5 is a nozzle plate according to claim 3 or 4, wherein:
[0016] The nozzle flow path includes a nozzle straight portion on the second surface side of the nozzle tapered portion.
[0017] The flow path area of the nozzle straight portion is smaller than the flow path area of the nozzle tapered portion.
[0018] The invention described in claim 6 is the nozzle plate described in claim 5, wherein:
[0019] A non-wet etching layer formed by masking, thermal oxidation or high-concentration doping,
[0020] The nozzle straight portion has the non-wet etching layer at an end portion on the first surface side.
[0021] The invention described in claim 7 is a nozzle plate according to claim 5 or 6, wherein:
[0022] The nozzle straight portion is continuous with an end portion of the nozzle tapered portion on the second surface side.
[0023] The invention described in claim 8 is a nozzle plate according to any one of claims 5 to 7, wherein:
[0024] When viewed from the first surface side, at least a portion of the ridgelines constituting the nozzle straight portion on the first surface side is substantially in contact with a surface constituting the nozzle tapered portion that is substantially perpendicular to the first surface.
[0025] The invention described in claim 9 is a nozzle plate according to claim 1 or 2, wherein:
[0026] The nozzle flow path has:
[0027] The nozzle tapered portion has a cross-sectional area orthogonal to the discharge direction of the droplets, that is, a flow path area that gradually narrows as it moves from the first surface toward the second surface; and
[0028] The straight communication passage portion is continuous with the first surface side of the nozzle tapered portion, and a pair of opposing surfaces of the straight communication passage portion are substantially parallel.
[0029] The nozzle tapered portion and the linear communication path portion include {111} surfaces.
[0030] The invention described in claim 10 is the nozzle plate described in claim 9, wherein:
[0031] The nozzle tapered portion and the linear communication path portion are formed of {111} surfaces.
[0032] The invention described in claim 11 is a nozzle plate according to claim 9 or 10, wherein:
[0033] The nozzle flow path includes a nozzle straight portion on the second surface side of the nozzle tapered portion.
[0034] The flow path area of the nozzle straight portion is smaller than the flow path area of the nozzle tapered portion.
[0035] The invention described in claim 12 is the nozzle plate described in claim 11, wherein:
[0036] A non-wet etching layer formed by masking, thermal oxidation or high-concentration doping,
[0037] The nozzle straight portion has the non-wet etching layer at an end portion on the first surface side.
[0038] The invention described in claim 13 is a nozzle plate according to claim 11 or 12, wherein:
[0039] The nozzle straight portion is continuous with an end portion of the nozzle tapered portion on the second surface side.
[0040] The invention described in claim 14 is a nozzle plate according to any one of claims 11 to 13, wherein:
[0041] When viewed from the first surface side, at least a portion of ridgelines constituting the nozzle straight portion on the first surface side substantially contacts a surface constituting the straight communication path portion that is substantially perpendicular to the first surface.
[0042] The invention described in claim 15 is a nozzle plate according to any one of claims 5 to 8 and claims 11 to 14, wherein:
[0043] When observed from the side of the above-mentioned first surface, the absolute value of the difference in distance between the intersection line of the two conical surfaces constituting the above-mentioned nozzle conical portion when they are imaginarily extended and the two points or lines farthest away in the direction parallel to the above-mentioned first surface or the above-mentioned second surface in the <100> direction on the ridge line where the surface constituting the above-mentioned nozzle straight portion and the conical surface constituting the above-mentioned nozzle conical portion intersect is within 0.5μm.
[0044] The invention described in claim 16 provides a liquid droplet ejection head, wherein:
[0045] A nozzle plate according to any one of claims 1 to 15 is provided.
[0046] The invention described in claim 17 provides a liquid droplet discharge device, wherein:
[0047] A liquid droplet ejection head as described in claim 16 is provided.
[0048] The invention described in claim 18 provides a method for manufacturing a nozzle plate of a droplet ejection head, comprising:
[0049] In a first step, a surface mask layer is formed on a first surface of a single crystal silicon substrate whose surface crystal orientation is a {110} plane;
[0050] In a second step, an opening pattern that becomes an opening of a nozzle flow path is formed on the surface mask layer; and
[0051] In the third step, anisotropic wet etching is performed on the single crystal silicon substrate located below the opening pattern from the surface.
[0052] The invention described in claim 19 is a method for manufacturing a nozzle plate according to claim 18, wherein:
[0053] In the third step, a nozzle tapered portion is formed in which a cross-sectional area orthogonal to a discharge direction of liquid droplets, that is, a flow path area gradually narrows from the first surface toward a second surface facing the first surface.
[0054] The invention described in claim 20 is a method for manufacturing a nozzle plate according to claim 19, wherein:
[0055] The first step includes forming a back mask layer on the second surface of the single crystal silicon substrate.
[0056] After the third step above:
[0057] In a fourth step, a nozzle pattern serving as a nozzle is formed on the back mask layer; and
[0058] In the fifth step, a nozzle straight portion is formed by penetrating the single crystal silicon substrate under the nozzle pattern from the surface by dry etching.
[0059] The invention described in claim 21 provides a method for manufacturing a nozzle plate of a liquid droplet ejection head, comprising:
[0060] In the first step, a front mask layer is formed on a first surface of a single crystal silicon substrate whose surface crystal orientation is a {110} plane, and a back mask layer is formed on a second surface opposite to the first surface.
[0061] A second step is to form a nozzle pattern to become a nozzle on the back mask layer;
[0062] The third step is to form a deep hole that becomes a straight part of the nozzle by deep-digging the single crystal silicon substrate located under the nozzle pattern from the back side by dry etching until halfway;
[0063] The fourth step is to form a nozzle mask layer on the side wall of the deep hole;
[0064] The fifth step is to perform deep digging processing on the single crystal silicon substrate located under the deep hole from the back side by dry etching;
[0065] A sixth step is to form an opening pattern to become an opening portion on the surface mask layer;
[0066] In a seventh step, the single crystal silicon substrate located in the opening pattern is deep-dug by dry etching from the surface; and
[0067] In the eighth step, the single crystal silicon substrate is subjected to through-processing from the front and back sides by anisotropic wet etching to form a nozzle flow path having a nozzle straight portion, a nozzle tapered portion, and a straight connecting path portion.
[0068] When the thickness of the above-mentioned single crystal silicon substrate is set to T, the diameter of the above-mentioned nozzle straight portion is set to D, the depth of the above-mentioned nozzle straight portion is set to h, the width of the above-mentioned opening portion in the <110> direction is set to L, and the angle formed by the above-mentioned first surface and the above-mentioned second surface of the above-mentioned single crystal silicon substrate and the {111} plane of the conical surface of the two surfaces constituting the above-mentioned nozzle conical portion is set to θ (θ=Acοоs(2 / √6)≈35.26°), the depth H of the above-mentioned deep hole formed in the above-mentioned seventh step satisfies the following (1).
[0069] (1) T-(H+(L / 2)tanθ)≥h-(D / 2)tanθ
[0070] The invention described in claim 22 is a method for manufacturing a nozzle plate according to claim 21, wherein:
[0071] When the above-mentioned first surface is set to a (1 1 0) surface, the width of the nozzle pattern formed in the above-mentioned second step in the [-1 11] direction and the width in the [1-1-1] direction are wider than the width of the opening pattern formed in the above-mentioned sixth step in the [-1 1 1] direction and the width in the [1-1-1] direction.
[0072] According to the nozzle plate, the liquid droplet ejection head, the liquid droplet ejection device, and the method for manufacturing the nozzle plate of the present invention, both high density of the nozzles and appropriate ejection characteristics can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0073] Figure 1 It is a schematic perspective view of the liquid droplet discharge device according to this embodiment.
[0074] Figure 2 It is a schematic side cross-sectional view of the liquid droplet ejection head according to this embodiment.
[0075] Figure 3A It is an enlarged plan view of a nozzle plate showing the nozzle flow path according to the present embodiment.
[0076] Figure 3B is along Figure 3A Side cross-sectional view of the nozzle plate along line IIIB-IIIB.
[0077] Figure 3C It is a perspective cross-sectional view of a nozzle plate showing a nozzle flow path according to the present embodiment.
[0078] Figure 4 It is an enlarged plan view of a nozzle plate showing a nozzle flow path according to another embodiment.
[0079] Figure 5 It is a cross-sectional view of the nozzle plate showing main steps of the method for manufacturing the nozzle plate according to the first embodiment.
[0080] Figure 6 It is a cross-sectional view of the nozzle plate showing main steps of a method for manufacturing the nozzle plate according to a modification of the first embodiment.
[0081] Figure 7 It is a cross-sectional view of the nozzle plate showing main steps of the method for manufacturing the nozzle plate according to the second embodiment.
[0082] Figure 8 It is a cross-sectional view of the nozzle plate showing main steps of the method for manufacturing the nozzle plate according to the third embodiment.
[0083] Fig. 9 This is a cross-sectional view of the nozzle plate showing the relationship of the deep holes formed in the eighth step of the method for manufacturing the nozzle plate according to the third embodiment. DETAILED DESCRIPTION
[0084] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. However, the scope of the invention is not limited to the illustrated examples. In addition, in the following description, the same reference numerals are used for parts having the same functions and structures, and their descriptions are omitted.
[0085] In addition, the Miller index describing the crystal plane and direction is generally defined as follows, and this specification is also based on this.
[0086] (hkl): specific surface
[0087] {hkl}: equivalent surface
[0088] [hkl]: Specific direction
[0089] <h k l> : Equivalent direction
[0090] In addition, unless otherwise specified, in the examples in the specification, it is described as follows:
[0091] Wafer bonding side: (1 1 0) surface
[0092] Wafer discharge side surface: (-1-1 0) surface,
[0093] Among the four surfaces constituting the nozzle tapered portion, two tapered surfaces are (-1-1 1) surface and (-1-1-1) surface.
[0094] The vertical surface of the four surfaces constituting the nozzle tapered portion and the two opposing surfaces having long sides of the four surfaces constituting the side surfaces of the linear communication path portion: the (-1 1 1) surface and the (1-1-1) surface
[0095] Among the four surfaces constituting the side surfaces of the linear communication path portion, two opposing surfaces having short sides are the (1-11) surface and the (-11-1) surface.
[0096] However, of course, as long as the surface and direction are equivalent to the described content, they are not limited to the description.
[0097] [Inkjet recording device]
[0098] First, as a liquid droplet ejection device according to the present embodiment, a configuration example of an inkjet recording device 1 including an inkjet head 10 as a liquid droplet ejection head is disclosed.
[0099] In the following description, as shown in the respective figures, the conveying direction of the recording medium PD in the inkjet recording device 1 is set as the front-back direction, the direction perpendicular to the conveying direction in the conveying surface of the recording medium PD is set as the left-right direction, and the direction perpendicular to the front-back direction and the left-right direction (the direction of ejection of ink) is set as the up-down direction. In addition, the inkjet head 10 is also described in the direction based on the state of being installed in the inkjet recording device 1.
[0100] In addition, unless otherwise specified, the above wafer surface orientation is followed and recorded as follows: top: [1 1 0] direction
[0101] Down: [-1-1 0] direction
[0102] Left: [-1 1 1] direction
[0103] Right: [1-1-1] direction
[0104] Front: [1-1 2] direction
[0105] After: [-1 1-2] direction.
[0106] However, of course, as long as the surface and direction are equivalent to the described content, they are not limited to the description.
[0107] Figure 1 1 is a schematic perspective view showing an inkjet recording device 1 according to the present embodiment. The inkjet recording device 1, for example, uses a conveyor unit T including a conveyor belt T1 and a conveyor roller T2 to convey a recording medium PD such as paper in a front-rear direction through a plurality of units U. A plurality of inkjet heads 10 are disposed in each unit U, and each inkjet head 10 ejects ink of various colors to print on the recording medium PD.
[0108] [Inkjet head]
[0109] Figure 2 This is a schematic side cross-sectional view of an inkjet head 10 viewed from the side. The inkjet head 10 is composed of a head chip 11, a common ink chamber 12, a support substrate 13, a wiring component 14, a drive unit 15, etc. Figure 2 A cross section of the inkjet head 10 on a plane including four nozzles N is shown.
[0110] [Head chip]
[0111] The head chip 11 is a structure for discharging ink from the nozzles N, and is formed by stacking a plurality of ( Figure 2 The bottom plate in the head chip 11 is the nozzle plate 110.
[0112] On the bonding surface (first surface) Ba of the nozzle plate 110 (see Figure 3B ), for example, a piezoelectric plate 120, a vibration plate 130, a spacer substrate 140, and a wiring substrate 150 are adhered and stacked in sequence upward.
[0113] The nozzle plate 110 is provided with a plurality of nozzle channels 111 having the structure of the present invention, and the nozzles N, which are the openings of the nozzle channels 111, can be connected to the discharge surface (second surface) Bb (see Figure 3B ) discharges ink approximately vertically, and the discharge surface (second surface) Bb is an exposed surface of the nozzle plate 110 and is a surface opposite to the bonding surface Ba.
[0114] The piezoelectric plate 120, the vibration plate 130, the spacer substrate 140, and the wiring substrate 150 are provided with ink flow paths connected to the nozzles N, and the surface of the wiring substrate 150 on the exposed side (upper side) is opened. The common ink chamber 12 is provided on the exposed surface of the wiring substrate 150 so as to cover all the openings.
[0115] The ink stored in the ink chamber forming member (not shown) of the common ink chamber 12 is supplied to each nozzle N through the ink flow path from the opening of the wiring substrate 150. In addition, the pressure chamber provided to penetrate the piezoelectric body plate 120 deforms together with the vibration plate 130 by the displacement (deformation) of the piezoelectric element in the storage portion adjacent to the pressure chamber, thereby imparting pressure changes to the ink. As a result, the ink is discharged downward from the nozzle N as droplets.
[0116] In addition, in the head chip 11 , it is preferable that the openings of the ink flow paths on the bonding surfaces of the respective plates have shapes similar to each other, and more preferably have the same shape.
[0117] In addition, the nozzle plate 110 is not limited to the structure of being bonded to the piezoelectric body plate 120. In other words, another plate may be provided between the nozzle plate 110 and the piezoelectric body plate 120. In addition, the method of bonding the nozzle plate 110 to the other plate may be bonding or joining, and is not limited.
[0118] [Nozzle plate]
[0119] Figure 3A This is an enlarged top view showing one nozzle flow path 111 of the nozzle plate 110 as viewed from the bonding surface Ba side. Figure 3B It means along Figure 3A A cross-sectional view of a nozzle flow path 111 taken along line IIIB-IIIB. Figure 3C It is a perspective cross-sectional view showing one nozzle flow channel 111 .
[0120] The nozzle plate 110 is provided with a plurality of nozzle channels 111 on the single crystal silicon substrate B. The nozzle channels 111 have FIG. 3A to FIG. 3C Nozzle N shown.
[0121] (Single crystal silicon substrate)
[0122] The single crystal silicon substrate B is a plate-shaped member made of single crystal silicon (Si) with a thickness of, for example, about 50 μm to 725 μm, and the crystal orientations of the front and back surfaces of the substrate are {110} planes.
[0123] By using the single crystal silicon substrate B as the base material of the nozzle plate 110 , the nozzle N can be processed with high precision in the manufacturing process, and the nozzle N with less positional error and shape deviation can be formed.
[0124] (Nozzle flow path)
[0125] The nozzle flow path 111 is a through hole that passes from the first surface, that is, the bonding surface Ba, to the second surface, that is, the discharge surface Bb, of the single crystal silicon substrate B. In particular, Figure 3B as well as Figure 3CAs shown, from the discharge surface Bb toward the bonding surface Ba, for example, a nozzle N, a nozzle straight portion 1111, a nozzle tapered portion 1112, and a straight communication path portion 1113 are provided.
[0126] <Nozzle>
[0127] The nozzles N are cylindrical holes with a circular or polygonal cross section in the left-right direction. The nozzles N are arranged in a matrix on the discharge surface Bb side of the single crystal silicon substrate B, and the bonding surface Ba side is connected to the nozzle straight portion 1111 .
[0128] For example, when the cross-sectional shape of the nozzle N in the direction perpendicular to the discharge direction is a perfect circle, the diameter of the opening can be set to about 10 μm to 45 μm.
[0129] <Nozzle straight section>
[0130] like Figure 3B As shown, the nozzle straight portion 1111 is formed to communicate with the nozzle tapered portion 1112 and is perpendicular to the discharge surface Bb of the single crystal silicon substrate B.
[0131] The cross-sectional area of the nozzle straight portion 1111 relative to the ink discharge direction, i.e., the flow path area, is formed to be smaller than the flow path area of the end portion on the discharge surface Bb side of the nozzle tapered portion 1112. As a result, the resistance applied when the ink is ejected from the nozzle N becomes larger, and the vibration of the meniscus can be suppressed, making the shape of the meniscus more stable.
[0132] In addition, when the single crystal silicon substrate B includes a non-wet etching layer, the non-wet etching layer may be provided as an end portion of the nozzle straight portion 1111 on the bonding surface Ba side.
[0133] The non-wet etching layer can be formed by, for example, performing masking, thermal oxidation processing, or high-concentration doping on the single crystal silicon substrate B, and the progress of anisotropic wet etching can be suppressed in the manufacturing process of the nozzle plate 110 described later. Therefore, by providing the non-wet etching layer in advance on the single crystal silicon substrate B, the length of the discharge direction of the nozzle straight portion 1111 can be predetermined in advance. Therefore, the nozzle straight portion 1111 having the non-wet etching layer as the end portion on the bonding surface Ba side can be said to be a nozzle straight portion 1111 with high precision.
[0134] Alternatively, as the single crystal silicon substrate B having a non-wet etching layer, an SOI (Silicon On Insulator) in which an oxide film is provided inside a silicon wafer and a thin silicon layer is formed thereon may be used.
[0135] In addition, Figure 3B as well as Figure 3CIn the example, the nozzle straight portion 1111 is formed continuously with the end of the nozzle tapered portion 1112 on the discharge surface Bb side, but the invention is not limited thereto. However, when the nozzle straight portion 1111 is not continuous with the nozzle tapered portion 1112, and a surface (platform plane) substantially perpendicular to the surface constituting the nozzle straight portion 1111 exists at the connection between the two, there is a concern that the ink discharged from the nozzle N will be drawn into the bubbles retained on the platform plane, resulting in insufficient ejection. Therefore, it is preferred that the nozzle straight portion 1111 is formed to be continuous with the end of the nozzle tapered portion 1112 on the discharge surface Bb side.
[0136] In addition, even when the nozzle straight portion 1111 is continuous with the nozzle tapered portion 1112, if the entire surface of the end portion on the discharge surface Bb side of the nozzle tapered portion 1112 is not substantially continuous with the end portion on the bonding surface Ba side of the nozzle straight portion 1111, there is a concern that a straight line (platform ridge) portion perpendicular to the nozzle straight portion 1111 is generated at the portion where the nozzle tapered portions 1112 and 1112 intersect each other, and bubbles may be retained on the platform ridge. Therefore, it is also preferable that the nozzle straight portion 1111 is formed to be continuous with the entire surface of the end portion on the discharge surface Bb side of the nozzle tapered portion 1112.
[0137] <Nozzle taper>
[0138] The nozzle tapered portion 1112 is composed of two surfaces ((-1-1-1) surface and (-1-1 1) surface) whose crystal planes are {111} planes, and has a substantially constant angle taper such that the flow path area gradually narrows from the bonding surface Ba toward the discharge surface Bb. By providing the nozzle tapered portion 1112 in the nozzle flow path 111, even when the meniscus of the ink retreats to the depth of the nozzle flow path 111 due to high-speed driving, the shape of the meniscus and the ink ejection can be stabilized.
[0139] In addition, if Figure 3B As shown, it is preferred that the absolute value of the difference in distance α and β between the farthest points or lines in the direction parallel to the bonding surface Ba or the discharge surface Bb (the [0 0 1] direction and the [00-1] direction when the bonding surface Ba is set to the (1 1 0) plane) in the <110> direction of the ridgeline where the outer diameter of the nozzle N and the nozzle tapered portions 1112, 1112 constituting the two surfaces are intersected by an imaginary intersection line P when the surfaces constituting the two surfaces of the nozzle tapered portions 1112, 1112 are imaginarily extended is formed to be within 0.5 μm, so that the eccentricity in the nozzle straight portion 1111 and the nozzle tapered portion 1112 is reduced.
[0140] <Straight connecting passage>
[0141] The linear connecting path portion 1113 is composed of four planes ((-1 1 1) plane, (1-1-1) plane, (1-1-1) plane, (-1 1-1) plane) whose crystal planes are {111} planes, and is set from the end of the nozzle tapered portion 1112 on the bonding surface Ba side to the bonding surface Ba.
[0142] like Figure 3A As shown, the straight connecting path portion 1113 is constructed with two groups of opposing surfaces that are approximately parallel, and the length of the sides where the surfaces constituting the straight connecting path portion 1113 intersect with the bonding surface Ba is longer than the sides of other surfaces, and the sides where the bonding surface Ba intersects with the surfaces constituting the straight connecting path portion 1113 can be an elongated, approximately parallelogram shape.
[0143] As described above, if the openings in the bonding surface Ba of the nozzle flow path 111 are substantially parallelogram-shaped, that is, elongated, the density of the nozzles N in the nozzle plate 110 can be increased compared to a case of a square shape.
[0144] In addition, if Figure 4 As shown, it is preferably configured such that, when viewed from the top from the bonding surface Ba side, at least a portion of the ridgeline on the bonding surface Ba side of the ridgeline constituting the nozzle straight portion 1111 is approximately in contact with a surface of the surface constituting the straight connecting path portion 1113 that is approximately perpendicular to the bonding surface Ba.
[0145] With such a nozzle flow path 111 , the eccentricity is contained in a very small range, and therefore the injection stability is excellent.
[0146] In addition, FIG. 3A to FIG. 3C , the two surfaces constituting the nozzle tapered portion 1112 and the four surfaces constituting the linear connecting passage portion 1113 are all constituted by {111} surfaces, but the present invention is not limited thereto. That is, in the manufacturing process described later, the nozzle flow path 111 including {111} surfaces and surfaces in other directions may be formed by stopping the anisotropic wet etching midway.
[0147] In addition, FIG. 3A to FIG. 3C 2 shows an example of a nozzle flow path 111 including a nozzle straight portion 1111, a nozzle tapered portion 1112, and a straight communication path portion 1113, but these are not essential structures. The nozzle flow path 111 may be a through hole including at least the nozzle N.
[0148] In addition, in the above, the nozzle plate 110 that is attached to the inkjet head 10 and discharges ink is exemplified, but the liquid discharged from the nozzle plate 110 is not limited to ink.
[0149] [Effects of the Invention]
[0150] As shown above, the nozzle plate 110 of the present embodiment has a plurality of through nozzle flow paths 111 for discharging droplets on the single crystal silicon substrate B, the bonding surface Ba and the discharge surface Bb of the single crystal silicon substrate B are {110} surfaces, the discharge surface Bb is a surface opposite to the bonding surface Ba, and is a surface on which the nozzle N is formed.
[0151] According to this structure, the cross-section of the nozzle channel 111 on the bonding surface Ba side can be substantially parallelogram-shaped, that is, elongated. Therefore, compared with a case where the cross-section is square, the nozzles N can be densely packed in the nozzle plate 110 .
[0152] In addition, the nozzle flow path 111 includes a surface composed of a {111} surface.
[0153] According to this structure, the nozzle flow path 111 has a stable shape.
[0154] The nozzle flow path 111 includes a nozzle tapered portion 1112 in which a cross-sectional area orthogonal to the discharge direction of the droplets, that is, a flow path area, gradually narrows from the bonding surface Ba toward the discharge surface Bb.
[0155] According to this configuration, even when the meniscus of ink retreats to the deep part of the nozzle channel 111 due to high-speed driving, the shape of the meniscus and the ink ejection can be stabilized.
[0156] The nozzle flow path 111 includes a nozzle straight portion 1111 which is provided on the discharge surface Bb side of the nozzle tapered portion 1112 and has a flow path area that is smaller than the flow path area of the nozzle tapered portion 1112 .
[0157] According to this structure, the resistance during droplet discharge becomes larger, the vibration of the meniscus can be suppressed, the shape of the meniscus can be made more stable, and the ejection stability can be improved.
[0158] Furthermore, the nozzle plate 110 includes a non-wet etching layer formed by masking, thermal oxidation or high-concentration doping, and the nozzle straight portion 1111 can have the non-wet etching layer as an end portion on the bonding surface Ba side.
[0159] According to this structure, the formation position of the nozzle straight portion 1111 is defined by the non-wet etching layer, and therefore the accuracy of the nozzle straight portion 1111 is high.
[0160] In addition, the nozzle straight portion 1111 can be provided continuously to the end portion of the nozzle tapered portion 1112 on the second surface side.
[0161] According to this configuration, since the nozzle flow path 111 does not have a land surface, it is possible to prevent the ink discharged from the nozzle N from being drawn into the bubbles accumulated on the land surface and causing insufficient ejection.
[0162] In addition, when viewed from the top side of the bonding surface Ba, at least a portion of the ridgeline on the bonding surface Ba side of the ridgeline constituting the nozzle straight portion 1111 is in substantial contact with a surface substantially perpendicular to the bonding surface Ba among the surfaces constituting the nozzle tapered portion 1112 or the straight connecting path portion 1113 (the (-1 1 1) surface and the (1-1-1) surface when the bonding surface Ba is set to the (1 1 0) surface).
[0163] According to this structure, Figure 4 A nozzle flow path 111 having less eccentricity in the front-to-back direction.
[0164] [Method for manufacturing nozzle plate]
[0165] [First embodiment]
[0166] Next, based on Figure 5 A method for manufacturing the above-mentioned nozzle plate 110 according to the first embodiment will be described.
[0167] The method for manufacturing a nozzle plate according to the first embodiment is a method for manufacturing a nozzle plate 110 of a liquid droplet ejection head 10, comprising: Figure 5 The steps A-1 to A-3 shown are a method for manufacturing the nozzle plate 110 in which the nozzle flow path 111 including at least the nozzles N is formed.
[0168] (A-1 process)
[0169] First, as the A-1 process (first process), a surface mask layer 112 and a back mask layer 113 are uniformly formed on the bonding surface (first surface: (1 1 0) surface) Ba and the discharge surface (second surface: (-1-1 0) surface) Bb of a single crystal silicon substrate B whose surface crystal orientation is the {110} plane.
[0170] In addition, hereinafter, when there is no particular distinction between the front mask layer 112 and the back mask layer 113 , they are collectively referred to as a “mask layer”.
[0171] <Mask layer>
[0172] The material for forming the mask layer may be, for example, an oxide such as SiO2 (silicon oxide), a metal plating based on Al (aluminum), Cr (chromium), or a resin, but there is no particular limitation as long as the material can stop the progress of etching during the anisotropic wet etching described later and is not removed by etching.
[0173] The thickness of the mask layer (length in the vertical direction) is not particularly limited, but is preferably 0.1 to 50 μm, and particularly preferably 0.5 to 20 μm. This is because a thickness of 0.5 μm or more improves the etching stop effect, and a thickness of 20 μm or less facilitates the formation of the mask layer.
[0174] However, when the mask layer is formed by the above-mentioned thermal oxidation method, the thickness is preferably 1 to 5 μm.
[0175] Alternatively, the mask layer may be Figure 5 The single-layer structure shown may also be a multi-layer structure.
[0176] (A-2 process)
[0177] Next, as step A-2 (second step), an opening pattern 114 to be the opening of the nozzle flow path 111 is formed on the surface mask layer 112 .
[0178] Specifically, first, a resist pattern is formed on the surface mask layer 112 by a known photolithography technique.
[0179] <Resist pattern>
[0180] In the formation of the resist pattern, a positive photoresist or a negative photoresist can be used. As the positive photoresist and the negative photoresist, known materials can be used. For example, as the negative photoresist, ZPN-1150-90 manufactured by Zeon Corporation of Japan can be used. In addition, as the positive photoresist, OFPR-800LB and OEBR-CAP112PM manufactured by Tokyo Ohka Kogyo Co., Ltd. can be used.
[0181] The resist layer is formed by coating using a spin coater or the like to have a predetermined thickness, and then a pre-baking treatment is performed under conditions such as 110° C. and 90 seconds.
[0182] In order to improve adhesion, HMDS treatment may be performed before resist coating. HMDS treatment can use an organic material called hexamethyldisilazane, for example, OAP (hexamethyldisilazane, manufactured by Tokyo Ohka Industry Co., Ltd.). Similar to resist coating, it may be applied using a spin coater, and even if exposed to hexamethyldisilazane vapor, the effect of improving adhesion can be expected.
[0183] After the resist layer is formed, the resist layer is exposed using a predetermined mask and an aligner. For example, in the case of a contact aligner, the resist layer is exposed at about 50 mJ / cm 2 Then, by immersing in a developer (for example, NMD-3 manufactured by Tokyo Ohka Kogyo Co., Ltd. for 60 to 90 seconds), the photosensitive portion of the resist layer is removed, and a resist pattern is formed on the surface mask layer 112.
[0184] After the resist pattern is formed, the surface mask layer 112 is dry-etched (DE1) using the resist pattern as a mask to form an opening pattern 114. After the opening pattern 114 is formed, the resist pattern is removed.
[0185] <Dry Etching>
[0186] As dry etching (DE1), a dry etching device such as an RIE (Reactive Ion Etching) device, an ICP (Inductively Coupled Plasma)-RIE etching device, which is a dry etching device that uses an inductively coupled discharge method, can be used. In addition, as a process gas, CHF3 (trifluoromethane), CF4 (tetrafluoromethane), etc. can be used.
[0187] As an example, using a dry etching apparatus RIE-100C manufactured by SUMCO Corporation, etching is performed for a predetermined time under the conditions of a CHF 3 gas flow rate of 80 sccm, a pressure of 3 Pa, and an RF power of 90 W, thereby forming the opening pattern 114 .
[0188] The shape of the opening pattern 114 is not particularly limited. However, when the anisotropic wet etching (WE) is performed to the end in the A-3 step described later, the opening formed by the edges where the four surfaces ((-1-1-1) surface, (-1-1 1) surface, (-1 1 1) surface, and (1-1-1) surface) constituting the nozzle tapered portion 1112 intersect with the bonding surface Ba ((1 1 0) surface) is in the shape of a roughly parallelogram circumscribing the opening pattern 114. Therefore, from the viewpoint of improving the quality and production efficiency of the nozzle plate 110, it is preferred that the shape of the opening pattern 114 is also a roughly parallelogram shape that follows the orientation of these surfaces.
[0189] <Removal of resist pattern>
[0190] The resist pattern can be removed by, for example, a wet process using acetone or an acid solution or a dry process using oxygen plasma.
[0191] (A-3 process)
[0192] Finally, as step A-3 (third step), the opening pattern 114 is anisotropically wet-etched (WE) from at least the bonding surface Ba side of the single crystal silicon substrate B, thereby forming the nozzle channel 111 having the nozzle tapered portion 1112 .
[0193] <Anisotropic wet etching>
[0194] In anisotropic wet etching, an alkaline aqueous solution such as KOH (potassium hydroxide), TMAH (tetramethylammonium hydroxide), or EDP (ethylenediaminecatechol) is used.
[0195] [Effects of the Invention]
[0196] According to the method for manufacturing the nozzle plate 110 according to the first embodiment of the present invention described above, it is possible to form the nozzle flow path 111 including the nozzle tapered portion 1112 having a very stable shape composed of {111} surfaces.
[0197] In addition, in the case of a single crystal silicon substrate B whose surface crystal orientation is a {110} plane, the plane formed when the anisotropic wet etching is performed to the end from the surface has an extremely slow etching rate compared to other planes, and thus becomes a {111} plane involved in the so-called "etching stop". Therefore, in the condition management of anisotropic wet etching, which is generally prone to production deviation, it is possible to perform production management with a margin that can absorb the production deviation.
[0198] In addition, when the through hole, i.e., the nozzle flow path 111, is formed by anisotropic wet etching on the single crystal silicon substrate B whose surface crystal orientation is the {110} plane from the bonding surface Ba, the opening of the nozzle flow path 111 on the bonding surface Ba side can be an elongated substantially parallelogram shape, i.e., an elongated shape. Therefore, in the nozzle plate 110, the nozzles N can be densely arranged.
[0199] In addition, in the A-1 process, mask layers are formed on both surfaces of the single crystal silicon substrate B, but the present invention is not limited thereto. Specifically, for example, when anisotropic wet etching is performed by immersing the single crystal silicon substrate B in an etching solution, it is necessary to form a back mask layer 113 on the discharge surface Bb. However, when anisotropic wet etching is performed only on the bonding surface Ba, the back mask layer 113 may not be provided.
[0200] In addition, when the back mask layer 113 is formed on the discharge surface Bb, it is necessary to remove at least the back mask layer 113 covering the nozzle N after the A-3 step, but it is optional to remove the other back mask layers 113 and the surface mask layer 112. In addition, when the mask layer is formed of SiO2, for example, it can be removed by fluoric acid.
[0201] In addition, in the A-3 process, the nozzle tapered portion 1112 is formed by anisotropic wet etching (WE), but the present invention is not limited thereto.
[0202] It can also be, for example, Figure 6As shown, after the A-2 process, the single crystal silicon substrate B under the opening pattern 114 is dry etched (DE2) to form a straight connecting path portion 1113, and as the A-3a process (the third process), after time control is performed so that the anisotropic wet etching (WE) stops halfway, the discharge surface Bb is dry etched (DE1) to form a nozzle pattern 115 that becomes the nozzle N, and the single crystal silicon substrate B under the nozzle pattern 115 is dry etched (DE2) to provide a through hole, thereby forming the nozzle flow path 111.
[0203] At this time, the dry etching (DE2) can be performed using an ICP-RIE etching device that adopts an inductively coupled plasma as a discharge form.
[0204] In addition, after the opening pattern 114 is formed in the A-2 process, a deep hole is formed by dry etching (DE2) using a Si deep digging device, and the deep hole is anisotropically wet etched (WE) in the A-3 process, thereby providing a nozzle flow path 111 having a nozzle tapered portion 1112 and a straight connecting path portion 1113.
[0205] [Second embodiment]
[0206] Next, based on Figure 7 A method for manufacturing the nozzle plate 110 according to the second embodiment will be described.
[0207] The method for manufacturing the nozzle plate 110 of the second embodiment performs steps A-3b to A-5 after step A-2 of the method for manufacturing the nozzle plate 110 of the first embodiment. Therefore, detailed descriptions of steps A-1 and A-2 are omitted.
[0208] (A-4 process)
[0209] After anisotropic wet etching (WE) is performed to form deep holes in step A-3b (third step), a nozzle pattern 115 serving as the nozzle N is formed on the back mask layer 113 in step A-4 (fourth step).
[0210] Specifically, in step A-3b of the second embodiment, anisotropic wet etching (WE) is performed until an etching stop is applied to the {111} plane formed by the anisotropic wet etching (WE) on all the surfaces constituting the nozzle tapered portion 1112 .
[0211] The method for forming the nozzle pattern 115 in the A-4 step is the same as the method for forming the opening pattern 114 in the A-2 step.
[0212] (A-5 process)
[0213] Next, as the A-5 step (fifth step), the nozzle pattern 115 provided in the A-4 step is dry-etched (DE2). Then, the nozzle flow path 111 including the nozzle straight portion 1111 and the nozzle tapered portion 1112 provided in the A-3b step is formed by connecting the hole that becomes the nozzle straight portion 1111 to the nozzle tapered portion 1112.
[0214] [Effects of the Invention]
[0215] According to the method for manufacturing the nozzle plate 110 according to the second embodiment of the present invention described above, it is possible to form the nozzle flow path 111 including the nozzle straight portion 1111 and the nozzle tapered portion 1112 having a very stable shape formed of a {111} surface.
[0216] Alternatively, etching may be stopped in step A-3b by subjecting the single crystal silicon substrate B to masking, thermal oxidation processing, or high-concentration doping, or by using SOI as the single crystal silicon substrate B to obtain a single crystal silicon substrate B having a non-wet etching layer.
[0217] In this way, since the height of the nozzle straight portion 1111 formed in the A-5 step is uniquely determined, the nozzle straight portion 1111 can be formed with higher precision.
[0218] Alternatively, when the single crystal silicon substrate B having a non-wet etching layer is used as the nozzle plate 110, after the A-2 step, the A-4 step and the A-5 step are performed after deep digging by dry etching (DE2), and after the A-5 step, anisotropic wet etching (WE) is performed from both sides of the bonding surface Ba and the discharge surface Bb as the A-3b step. In this way, the nozzle flow path 111 having the nozzle straight portion 1111 in the non-wet etching layer, and having the straight communication path portion 1113 and the nozzle tapered portion 1112 can be formed.
[0219] [Third Embodiment]
[0220] Next, based on Figure 8 A method for manufacturing a nozzle plate according to a third embodiment of the present invention and a nozzle plate manufactured thereby will be described.
[0221] The method for manufacturing the nozzle plate 110 according to the third embodiment includes: Figure 8 In the following description, detailed descriptions of the contents of the manufacturing process of the nozzle plate that overlap with those of the first embodiment and the second embodiment are omitted.
[0222] (B-1 process, B-2 process)
[0223] First, in the B-1 step (first step), a surface mask layer 112 and a back mask layer 113 are uniformly formed on the bonding surface Ba ((1 1 0) surface) and the discharge surface Bb ((-1-1 0) surface) of the single crystal silicon substrate B whose surface crystal orientation is the {110} plane. Then, as the B-2 step (second step), a nozzle pattern 115 serving as the nozzle N is formed on the back mask layer 113.
[0224] (B-3 process)
[0225] Next, as step B-3 (third step), the nozzle straight portion 1111 is formed by dry etching (DE2) the single crystal silicon substrate B under the nozzle pattern 115 in accordance with the predetermined length of the nozzle straight portion 1111.
[0226] (B-4 process)
[0227] Next, as step B-4 (fourth step), a nozzle mask layer 116 is formed along the inner surface of the nozzle straight portion 1111. The material and formation method of the nozzle mask layer 116 are the same as those of the mask layer in step A-1.
[0228] Then, the nozzle mask layer 116 formed at the bottom of the nozzle straight portion 1111 is removed. The nozzle mask layer 116 at the bottom of the nozzle straight portion 1111 can be removed by dry etching using an RIE device or the like, but due to the verticality of the etchant used in the dry etching of the RIE device, the nozzle mask layer 116 formed on the side portion is more difficult to remove by dry etching than the bottom portion. Therefore, the nozzle mask layer 116 at the bottom is etched first, and the nozzle mask layer 116 remains on the side portion.
[0229] In addition, by setting the dry etching conditions in the B-4 step to low pressure or high bias, the nozzle mask layer 116 on the side surface may be more difficult to be etched.
[0230] (B-5 process)
[0231] Next, as step B-5 (fifth step), the nozzle straight portion 1111 is further deepened by dry etching (DE2).
[0232] (B-6 process, B-7 process)
[0233] Next, as a B-6 step (sixth step), an opening pattern 114 is formed on the surface mask layer 112 to become the opening portion of the nozzle flow path 111. Then, as a B-7 step (seventh step), the single crystal silicon substrate B under the opening pattern 114 is dry-etched (DE2) to provide a hole that becomes the linear communication path portion 1113.
[0234] In addition, in the B-7 step, preferably in all the nozzle flow paths 111, Figure 8 As shown, dry etching (DE2) is performed until the hole provided in the B-5 step is connected, and the single crystal silicon substrate B is penetrated. When the through hole is provided in the B-7 step, the hydrogen gas generated when the anisotropic wet etching (WE) is performed in the B-8 step (eighth step) described later is uniformly and efficiently discharged, so that the etching progress is uniform. As a result, shape deviation is not likely to occur in each nozzle flow path 111.
[0235] However, penetration is not essential in step B-7. If penetration is not achieved in step B-7, if excavation is advanced until just before penetration, the time until penetration by wet etching can be shortened in the wet etching step of step B-8.
[0236] (B-8 process)
[0237] Next, as step B-8, anisotropic wet etching (WE) is performed from both sides of the bonding surface Ba and the discharge surface Bb to enlarge the hole provided in step B-5 and the hole provided in step B-7, thereby forming the nozzle tapered portion 1112. In addition, at this time, the nozzle straight portion 1111 is protected by the nozzle mask layer 116, so that the progress of etching is suppressed and remains.
[0238] In addition, if Fig. 9 As shown, regarding the depth H of the hole formed in the B-7 step of the manufacturing method of the nozzle plate 110 of the third embodiment, when the bonding surface Ba is set to the (1 1 0) surface and the discharge surface Bb is set to the (-1-1 0) surface, the thickness of the single crystal silicon substrate B is set to T, the width of the nozzle straight portion 1111 in the [0 0 1] direction and the [0 0-1] direction is set to D, the depth of the nozzle straight portion 1111 (the length in the discharge direction) is set to h, the width of the opening pattern 114 in the [0 0 1] direction and the [0 0-1] direction is set to L, and the angle between the (-1-1 0) surface and the (-1-1-1) surface of the single crystal silicon substrate B is set to θ (θ=Cos -1 (2 / √6)≈35.26 degrees), T-(H+(L / 2)tanθ)≥h-(D / 2)tanθ is satisfied.
[0239] In addition, Fig. 9 In the diagram, the left side "T-(H+(L / 2)tanθ)" is illustrated as LA, and the right side "h-(D / 2)tanθ" is illustrated as LB.
[0240] [Effects of the Invention]
[0241] According to the method for manufacturing the nozzle plate 110 of the third embodiment described above, the nozzle mask layer 116 formed on the nozzle channel 111 suppresses the progress of etching during anisotropic wet etching (WE), thereby forming a nozzle straight portion 1111 of a desired length in the nozzle channel 111 .
[0242] In addition, in the B-8 process, etching proceeds from both the end of the nozzle straight portion 1111 on the bonding surface Ba side and the end of the hole provided in the B-7 process on the discharge surface Bb side. However, by making the depth H of the hole formed in the B-7 process satisfy the above-mentioned relationship, the two conical surfaces of the nozzle tapered portion 1112 finally formed must be formed continuously from the bonding surface Ba side of the nozzle straight portion 1111. Therefore, the nozzle straight portion 1111 and the nozzle tapered portion 1112 can be made without positional offset, the eccentricity can be reduced, the symmetry of the flow of ink can be maintained, and the nozzle flow path 111 with a stable ejection angle can be obtained.
[0243] In addition, in the final nozzle flow path 111, an etching stop is applied to the {111} surface circumscribed with the ridgeline on the bonding surface Ba side of the hole opened in the B-7 step and the nozzle straight portion 1111. Therefore, there is no positional deviation or step difference between the nozzle tapered portion 1112 and the straight connecting path portion 1113, and a stable nozzle flow path 111 can be obtained.
[0244] In addition, in the dry etching process, precise control is difficult due to dry etching conditions such as the concentration distribution of the etchant and the distribution of the voltage, and manufacturing errors are likely to occur. However, as long as the above relationship is satisfied, the surface constituting the nozzle tapered portion 1112 formed in the B-8 process is formed continuously from the end of the bonding surface Ba side of the surface constituting the nozzle straight portion 1111. Therefore, the depth H of the hole formed in the B-7 process can be set to be slightly reduced from the depth of the final desired straight connecting path portion 1113 with a margin, and the manufacturing error caused by this process can be reduced. As a result, a nozzle plate 110 with stable injection characteristics can be manufactured.
[0245] In addition, it is preferable to configure the nozzle pattern 115 formed in the B-2 step so that its width in the [-1 1 1] direction and the [1-1-1] direction is wider than the opening pattern 114 formed in the B-6 step so that its width in the [-1 1 1] direction and the [1-1-1] direction is wider.
[0246] When the above-mentioned structure is satisfied, when the anisotropic wet etching is carried out to the end in the B-8 process, the four surfaces constituting the straight connecting path portion 1113 reach the {111} surface ((-1 1 1) surface·(1-1-1) surface·(1-1 1) surface·(-1 1-1) surface) which is circumscribed to the outermost diameter of the opening pattern 114 or the nozzle pattern 115. As a result, at least a portion of the ridgeline on the bonding surface Ba side of the surface constituting the nozzle straight portion 1111 is roughly in contact with the (-1 1 1) surface and the (1-1-1) surface of the surface constituting the straight connecting path portion 1113, so that the nozzle flow path 111 can be less eccentric in the [-1 1 1] direction and the [1-1-1] direction.
[0247] In the above, after the steps B-3 to B-5 of providing the nozzle straight portion 1111 from the discharge surface Bb, the steps B-6 and B-7 of providing the hole that becomes the straight communication path portion 1113 from the bonding surface Ba are performed, but the present invention is not limited thereto. That is, the hole that becomes the straight communication path portion 1113 may be provided before the nozzle straight portion 1111.
[0248] In addition, after step B-8, the bonding surface Ba of the single crystal silicon substrate B may be removed by etching, grinding or polishing to adjust the thickness of the nozzle plate 110 and the depth of the linear communication path portion 1113 to a desired size. In addition, a step of removing the mask layer including the nozzle mask layer 116 may be performed.
[0249] Furthermore, in the manufacturing method of each embodiment, in order to use the nozzle plate 110 for a long period of time, at least one protective film may be formed.
[0250] In this case, a step of forming a protective film that covers at least a portion of the surface including the inside of the nozzle flow path 111 is performed after the final step of each embodiment.
[0251] As the protective film, a material that does not dissolve due to contact with ink can be selected and used, such as a metal oxide film (tantalum pentoxide, hafnium oxide, niobium oxide, titanium oxide, zirconium oxide, etc.), a metal silicate film containing silicon in the metal oxide film (tantalum silicate, hafnium silicate, niobium silicate, titanium silicate, zirconium silicate, etc.), SiC (silicon carbide) film, DLC (diamond carbon) film, and a material used for forming a mask layer. In addition, an organic film such as polyimide, polyamide, and polyparaxylene can also be used as the protective film.
[0252] The thickness of the protective film is not particularly limited, and can be, for example, 0.05 μm to 20 μm.
[0253] Example
[0254] Next, the results of evaluating the preferred configurations of the examples and comparative examples of the present invention will be described. The present invention will be specifically described below using the examples, but the present invention is not limited thereto.
[0255] [Sample production]
[0256] A nozzle plate 110 having 1280 nozzle channels 111 formed as in the following embodiments and comparative examples was manufactured. Then, a piezoelectric plate 120 having the same cross-sectional shape in the left-right direction of the ink channel as the cross-sectional shape in the left-right direction at the bonding surface Ba of the nozzle plate 110 was bonded to each nozzle plate 110 to form an inkjet head 10, and the inkjet head 10 was mounted on an inkjet recording device 1.
[0257] (Example 1)
[0258] The nozzle flow path 111 is formed through the following steps A-1 to A-3.
[0259] Step A-1: On a 50 μm thick single crystal silicon substrate B whose surface crystal orientations are (1 1 0) and (-1-1 0), a 1 μm thick surface mask layer 112 and a back surface mask layer 113 are formed by thermal oxidation.
[0260] A-2 step: A pattern having a substantially parallelogram shape with a base of 130 μm and a height of 50 μm and with each side angle matching the angle between the (-1 1 1) plane, (1-1-1) plane, (1-1 1) plane, and (-11-1) plane is formed on the surface mask layer 112 by using a positive photoresist. Then, an opening pattern 114 is formed by performing dry etching (DE1) using an RIE device.
[0261] In addition, CHF3 gas was used as etching gas. In addition, after dry etching, the photoresist was removed by immersion in acetone.
[0262] Step A-3: The sample was immersed in a 40 wt % 80° C. KOH solution for 35 minutes to perform anisotropic wet etching (WE), thereby forming a nozzle tapered portion 1112 composed of a {111} plane.
[0263] In addition, after the A-3 step, the mask layer is removed by fluoric acid.
[0264] (Example 2)
[0265] The nozzle flow path 111 is formed through the following steps A-1 to A-5.
[0266] Step A-1: On a single crystal silicon substrate B having a thickness of 83 μm and a surface crystal orientation of (1 1 0) and (-1-1 0), a surface mask layer 112 and a back mask layer 113 having a thickness of 1 μm are formed by thermal oxidation.
[0267] A-2 step: A pattern having a substantially parallelogram shape with a base of 130 μm and a height of 50 μm and with each side angle matching the angle between the (-1 1 1) plane, (1-1-1) plane, (1-1 1) plane, and (-11-1) plane is formed on the surface mask layer 112 by using a positive photoresist. Then, an opening pattern 114 is formed by performing dry etching (DE1) using an RIE device.
[0268] Step A-3: Anisotropic wet etching (WE) was performed for 35 minutes under the same conditions as in Example 1 to form a nozzle tapered portion 1112 composed of {111} planes.
[0269] Step A-4: The pattern formed on the back mask layer 113 is dry-etched (DE1) using an RIE apparatus to form a perfect circular nozzle pattern 115 with a diameter of φ30 μm.
[0270] In addition, CHF3 gas was used as the etching gas.
[0271] Process A-5: Using a Si deep digging device, the single crystal silicon substrate B under the nozzle pattern 115 is subjected to dry etching (DE2) based on the Bosch process to connect it with the nozzle tapered portion 1112 set in the A-3 process to form a nozzle straight portion 1111 with a depth of 40.6 μm.
[0272] In addition, SF6 and C4F8 gases are used as etching gases.
[0273] In addition, after the A-5 step, the mask layer is removed by fluoric acid.
[0274] (Example 3)
[0275] The nozzle flow path 111 is formed through the following steps A-1 to A-5.
[0276] A-1 step: On the discharge surface Bb of the single crystal silicon substrate B whose surface crystal orientation is (1 1 0) and (-1-1 0), a thick SiO2 film with a thickness of 10 μm is formed as a non-wet etching layer by thermal oxidation, and the overall thickness is set to 50 μm. In addition, a surface mask layer 112 with a thickness of 1 μm is formed on the bonding surface Ba by thermal oxidation. In addition, a back mask layer 113 is formed on the discharge surface Bb by a positive photoresist on the non-wet etching layer.
[0277] A-2 step: A pattern having a substantially parallelogram shape with a base of 130 μm and a height of 50 μm and with each side angle matching the angle between the (-1 1 1) plane, (1-1-1) plane, (1-1 1) plane, and (-11-1) plane is formed on the surface mask layer 112 by using a positive photoresist. Then, an opening pattern 114 is formed by performing dry etching (DE1) using an RIE device.
[0278] Step A-3: Anisotropic wet etching (WE) was performed for 35 minutes under the same conditions as in Example 1 to form a nozzle tapered portion 1112 composed of {111} planes.
[0279] Step A-4: The pattern formed on the back mask layer 113 is dry-etched (DE1) using an RIE apparatus to form a perfect circular nozzle pattern 115 with a diameter of φ30 μm.
[0280] Step A-5: Dry etching (DE2) is performed using an RIE apparatus to form a nozzle straight portion 1111 having a depth of 10 μm.
[0281] (Example 4)
[0282] The nozzle flow path 111 is formed through the following steps A-1 to A-5.
[0283] A-1 step: On the discharge surface Bb of the single crystal silicon substrate B whose surface crystal orientation is (1 1 0) and (-1-1 0), a thick SiO2 film with a thickness of 10 μm is formed as a non-wet etching layer by thermal oxidation, and the overall thickness is set to 50 μm. In addition, a surface mask layer 112 with a thickness of 1 μm is formed on the bonding surface Ba by thermal oxidation. In addition, a back mask layer 113 is formed on the discharge surface Bb by a positive photoresist on the non-wet etching layer.
[0284] A-2 step: A pattern having a substantially parallelogram shape with a base of 130 μm and a height of 15 μm, which is narrower than the diameter φ30 μm of the nozzle pattern 115 opened in the subsequent step A-4, and with the angles of each side matching the angles between the (-11 1) plane, (1-1-1) plane, (1-1 1) plane, and (-1 1-1) plane, is formed on the surface mask layer 112 by a positive photoresist. Then, the A-4 step and the A-5 step are performed to form a through hole.
[0285] A-3 process: By performing anisotropic wet etching (WE) for 35 minutes on the through hole set in the A-2 process, a nozzle flow path 111 is formed in which the ridge line on the bonding surface Ba side of the nozzle straight portion 1111 is roughly in contact with the end of the discharge surface Bb side of the tapered two surfaces of the nozzle tapered portion 1112 composed of {111} surfaces, and the two surfaces of the nozzle tapered portion 1112 composed of {111} surfaces that are perpendicular to the bonding surface Ba.
[0286] (Example 5)
[0287] The single crystal silicon substrate B is set to SOI.
[0288] In addition, after the single crystal silicon substrate B is deep-dug in the A-5 step, the SiO2 layer (Box layer) is dug using an RIE device to form a through hole. The other conditions are the same as those in Example 2.
[0289] (Example 6)
[0290] The nozzle flow path 111 is formed through the following steps A-1 to A-3.
[0291] Step A-1: On a 100 μm thick single crystal silicon substrate B whose surface crystal orientations are (1 1 0) and (-1-1 0), a 1 μm thick front mask layer 112 and a 1 μm back mask layer 113 are formed by thermal oxidation.
[0292] A-2 step: A pattern having a substantially parallelogram shape with a base of 130 μm and a height of 50 μm and with each side angle matching the angle between the (-1 1 1) plane, (1-1-1) plane, (1-1 1) plane, and (-11-1) plane is formed on the surface mask layer 112 by using a positive photoresist. Then, an opening pattern 114 is formed by performing dry etching (DE1) using an RIE device.
[0293] Then, using a Si deep etching device, the single crystal silicon substrate B below the opening pattern 114 is subjected to dry etching (DE2) based on the Bosch process to form a hole with a depth of 51 μm.
[0294] Step A-3: The holes formed after step A-2 are subjected to anisotropic wet etching (WE) for 35 minutes, and then the mask layer is removed by fluoric acid to form a nozzle channel 111 having a linear communication channel portion 1113 and a nozzle tapered portion 1112 .
[0295] (Example 7)
[0296] The nozzle flow path 111 is formed through the following steps B-1 to B-8.
[0297] Step B-1: On a 200 μm thick single crystal silicon substrate B whose surface crystal orientation is {110} plane, a 3 μm thick front mask layer 112 and a back mask layer 113 are formed by thermal oxidation.
[0298] Step B-2: The pattern formed on the back mask layer 113 is dry-etched (DE1) using an RIE apparatus to form a perfect circular nozzle pattern 115 with a diameter of φ30 μm.
[0299] In addition, CHF3 was used as the etching gas.
[0300] Step B-3: Using a Si deep etching device, the single crystal silicon substrate B under the nozzle pattern 115 is subjected to dry etching (DE2) based on the Bosch process to form a nozzle straight portion 1111 with a depth of 40.6 μm.
[0301] In addition, SF6 and C4F8 gases are used as etching gases.
[0302] Step B-4: A mask layer with a thickness of 1 μm is formed on the nozzle straight portion 1111 by a thermal oxidation method, and then only the mask layer at the bottom is removed by an RIE device to form a nozzle mask layer 116 .
[0303] Step B-5: Dry etching (DE2) based on the Bosch process is performed using a Si deep etching device to form a deep hole with a depth of 120 μm in the nozzle straight portion 1111 .
[0304] Step B-6: A pattern of a substantially parallelogram shape of 130 μm×50 μm with each side angle matching the angle between the (-1 1 1) plane·(1-1-1) plane·(1-1 1) plane·(-1 1-1) plane is formed on the surface mask layer 112 by using a positive photoresist. Then, dry etching (DE1) is performed using an RIE device to form an opening pattern 114.
[0305] Furthermore, the photoresist was removed by immersion in acetone after dry etching (DE1).
[0306] Step B-7: By using a Si deep etching device, the single crystal silicon substrate B under the opening pattern 114 is dry-etched (DE2) to form a hole with a depth of 100 μm to communicate with the deep hole provided in step B-5.
[0307] In addition, at this time, the thickness (T) of the single crystal silicon substrate B = 200 μm, the diameter (D) of the nozzle straight portion 1111 = 30 μm, the depth (h) of the nozzle straight portion 1111 = 40.6 μm, the width (L) of the opening pattern 114 in the {110} direction = 149.45 μm, and the depth (H) of the hole formed in the B-7 process = 100 μm, so the following is satisfied,
[0308] According to T-(H+(L / 2)tanθ)≈47.17
[0309] and h-(D / 2)tanθ≈29.99,
[0310] And T-(H+(L / 2)tanθ)≥h-(D / 2)tanθ.
[0311] Step B-8: Anisotropic wet etching (WE) was performed by immersing in a 40 wt · 80° C. KOH solution for 80 minutes to form a nozzle channel 111 including a nozzle straight portion 1111 , a nozzle tapered portion 1112 , and a straight communication channel portion 1113 .
[0312] Furthermore, after step B-8, the mask layer is removed by fluoric acid.
[0313] (Example 8)
[0314] In the B-1 step, a thick SiO 2 film having a thickness of 10 μm is formed as a non-wet etching layer on the discharge surface Bb by a thermal oxidation method, and then a back mask layer 113 is formed.
[0315] The other conditions are the same as those in Example 7.
[0316] (Example 9)
[0317] The nozzle pattern 115 provided in the B-2 step was formed into an elliptical shape having a major axis of 60.3 μm and a minor axis of 14.9 μm.
[0318] The other conditions are the same as those in Example 8.
[0319] (Example 10)
[0320] As the single crystal silicon substrate B, SOI is used.
[0321] The other conditions are the same as those in Example 7.
[0322] (Example 11)
[0323] The nozzle pattern 115 provided in the B-2 step was formed into an elliptical shape with a major axis of 60.3 μm and a minor axis of 14.9 μm, and the opening pattern 114 provided in the B-6 step was set to 130 μm×35 μm.
[0324] The other conditions are the same as those in Example 7.
[0325] In addition, at this time, the thickness (T) of the single crystal silicon substrate B = 200 μm, the width (D) of the nozzle straight portion 1111 = 14.9 μm, the depth (h) of the nozzle straight portion 1111 = 35.3 μm, the width (L) of the opening pattern 114 in the {110} direction = 149.45 μm, and the depth (H) of the hole formed in the B-7 process = 100 μm, so the following is satisfied,
[0326] According to T-(H+(L / 2)tanθ)≈47.12
[0327] and h-(D / 2)tanθ≈30.03,
[0328] And T-(H+(L / 2)tanθ)≥h-(D / 2)tanθ.
[0329] (Comparative Example 1)
[0330] Anisotropic wet etching (WE) was performed on a single crystal silicon substrate B having a surface crystal orientation of {100} and a thickness of 200 μm to form a nozzle channel 111 having a square shape of 130 μm×130 μm in cross section in the left-right direction on the bonding surface Ba.
[0331] (Comparative Example 2)
[0332] Anisotropic wet etching (WE) was performed on a single crystal silicon substrate B having a surface crystal orientation of {100} and a thickness of 200 μm to form a nozzle channel 111 having a square shape of 50 μm×50 μm in cross section in the left-right direction on the bonding surface Ba.
[0333] The following Tests 1 and 2 were performed using the inkjet recording apparatus 1 equipped with the inkjet head 10 including the nozzle plates 110 of Examples 1 to 13 and Comparative Examples 1 and 2 described above.
[0334] [Test 1. Emission angle test]
[0335] When UV ink heated to a viscosity of 8 cP was ejected at a driving voltage with an average droplet velocity of about 6 m / s, the ejection angles of 1,280 nozzles were evaluated to be within ±several degrees.
[0336] [Test 2. Upper speed limit test]
[0337] At a drive frequency of 40kHz, the ejection speed of the UV ink heated to a viscosity of 8cP was increased from 5m / s, and the ejection speed at which the number of nozzles N that produced insufficient ejection was 5 or more out of 100 nozzles was measured. In addition, when the ejection speed was 9m / s or more, it was not easy to produce insufficient ejection even if the ejection speed became higher, that is, the meniscus stability was excellent, and the evaluation was "0". In addition, when the ejection speed was 11m / s or more, the meniscus stability was particularly excellent, and the evaluation was "◎".
[0338] Table I shows the results of Tests 1-2.
[0339] [Table 1]
[0340]
[0341] In Comparative Example 2, the hole size was too small, 50 μm×50 μm, so that even if the driving voltage was increased to 30 V, ink could not be ejected.
[0342] [evaluate]
[0343] When Example 1-11 is compared with Comparative Example 1-2, when the nozzle flow path 111 is formed on a single crystal silicon substrate B whose surface crystal orientation is {100} plane, the opening on the bonding surface Ba side can only be made square, and only one of a nozzle plate with excellent injection characteristics but low nozzle density and a nozzle plate with excellent nozzle density but low injection characteristics can be manufactured. In contrast, it can be seen that when the nozzle flow path 111 is formed on a single crystal silicon substrate B whose surface crystal orientation is {110} plane, the opening on the bonding surface Ba side can be made into a slender shape of 50μm×130μm, so that both high density of nozzles N and improved injection characteristics can be achieved.
[0344] In particular, when Examples 1 and 6 are compared with other Examples, it can be seen that the ejection angle is increased and the ejection characteristics are improved by forming the nozzle straight portion 1111 in the nozzle flow path 111 .
[0345] In addition, if Examples 1, 4, 6, 9 and 11 are compared with other Examples, it can be seen that by not providing a platform plane and a platform ridge line in the nozzle flow path 111, or by making the platform plane and the platform ridge line extremely small, the stability of the curved liquid surface is improved, thereby becoming a nozzle plate 110 that is less likely to cause insufficient injection.
[0346] Industrial Applicability
[0347] The present invention can be used for a nozzle plate, a liquid droplet ejection head, a liquid droplet ejection device, and a method for manufacturing a nozzle plate that can achieve both high nozzle density and appropriate ejection characteristics.
[0348] Explanation of the reference numerals: B…single crystal silicon substrate; Ba…bonding surface (first surface); Bb…discharge surface (second surface); 1…inkjet recording device (liquid droplet discharge device); 10…inkjet head (liquid droplet discharge head); 110…nozzle plate; 111…nozzle flow path; 1111…nozzle straight portion; 1112…nozzle conical portion; 1113…straight connecting path portion; 112…surface mask layer; 113…back mask layer; 114…opening pattern; 115…nozzle pattern; 116…nozzle mask layer; N…nozzle.
Claims
1. A nozzle plate, comprising a plurality of nozzle flow paths extending through a single crystal silicon substrate and configured to discharge droplets from nozzles, in, The first surface and the second surface of the single crystal silicon substrate are {110} planes, and the second surface is a surface opposite to the first surface and is a surface on which the nozzle is formed.
2. The nozzle plate according to claim 1, in, The nozzle flow path includes a surface composed of a {111} surface.
3. The nozzle plate according to claim 1 or 2, in, The nozzle flow path includes a nozzle tapered portion, in which a cross-sectional area orthogonal to a discharge direction of liquid droplets, that is, a flow path area, gradually narrows as it moves from the first surface toward the second surface. The nozzle tapered portion includes a {111} surface.
4. The nozzle plate according to claim 3, in, The nozzle tapered portion is composed of a {111} surface.
5. The nozzle plate according to claim 3 or 4, in, The nozzle flow path includes a nozzle straight portion on the second surface side of the nozzle tapered portion, The flow path area of the straight portion of the nozzle is smaller than the flow path area of the tapered portion of the nozzle.
6. The nozzle plate according to claim 5, in, A non-wet etching layer formed by masking, thermal oxidation or high-concentration doping, The nozzle straight portion has the non-wet etching layer at an end portion on the first surface side.
7. The nozzle plate according to claim 5 or 6, in, The nozzle straight portion is continuous with an end portion of the nozzle tapered portion on the second surface side.
8. The nozzle plate according to any one of claims 5 to 7, in, When viewed from the first surface side, at least a portion of the ridgelines constituting the nozzle straight portion on the first surface side is substantially in contact with a surface constituting the nozzle tapered portion that is substantially perpendicular to the first surface.
9. The nozzle plate according to claim 1 or 2, in, The nozzle flow path comprises: The nozzle tapered portion has a cross-sectional area orthogonal to the discharge direction of the liquid droplets, that is, a flow path area that gradually narrows as it moves from the first surface toward the second surface; and A straight communication passage portion is continuous with the first surface side of the nozzle tapered portion, and a pair of opposing surfaces of the straight communication passage portion are substantially parallel. The nozzle tapered portion and the linear communication path portion include {111} surfaces.
10. The nozzle plate according to claim 9, in, The nozzle tapered portion and the linear communication path portion are formed of {111} surfaces.
11. The nozzle plate according to claim 9 or 10, in, The nozzle flow path includes a nozzle straight portion on the second surface side of the nozzle tapered portion, The flow path area of the straight portion of the nozzle is smaller than the flow path area of the tapered portion of the nozzle.
12. The nozzle plate according to claim 11, in, A non-wet etching layer formed by masking, thermal oxidation or high-concentration doping, The nozzle straight portion has the non-wet etching layer at an end portion on the first surface side.
13. The nozzle plate according to claim 11 or 12, in, The nozzle straight portion is continuous with an end portion of the nozzle tapered portion on the second surface side.
14. The nozzle plate according to any one of claims 11 to 13, in, When viewed from the first surface side, at least a portion of ridgelines constituting the nozzle straight portion on the first surface side substantially contacts a surface constituting the straight communication path portion that is substantially perpendicular to the first surface.
15. The nozzle plate according to any one of claims 5 to 8 and claims 11 to 14, in, When observed from the first surface side, the absolute value of the difference in distance between the two points or lines farthest from each other in the direction parallel to the first surface or the second surface in the <100> direction on the ridge line where the surface constituting the nozzle straight portion and the conical surface constituting the nozzle conical portion intersect is within 0.5 μm.
16. A liquid droplet discharge head, in, A nozzle plate according to any one of claims 1 to 15 is provided.
17. A liquid droplet discharge device, in, A liquid droplet ejection head according to claim 16 is provided.
18. A method for manufacturing a nozzle plate of a liquid droplet ejection head, in, have: In a first step, a surface mask layer is formed on a first surface of a single crystal silicon substrate whose surface crystal orientation is a {110} plane; a second step of forming an opening pattern that becomes an opening of a nozzle flow path on the surface mask layer; as well as In a third step, anisotropic wet etching is performed on the single crystal silicon substrate located below the opening pattern from the surface.
19. The method for manufacturing a nozzle plate according to claim 18, in, In the third step, a nozzle tapered portion is formed in which a cross-sectional area orthogonal to a discharge direction of liquid droplets, that is, a flow path area gradually narrows from the first surface toward a second surface facing the first surface.
20. The method for manufacturing a nozzle plate according to claim 19, in, The first step includes forming a back mask layer on the second surface of the single crystal silicon substrate. After the third step: A fourth step is to form a nozzle pattern to become a nozzle on the back mask layer; as well as In the fifth step, a nozzle straight portion is formed by penetrating the single crystal silicon substrate under the nozzle pattern from the surface by dry etching.
21. A method for manufacturing a nozzle plate of a liquid droplet ejection head, in, have: In a first step, a surface mask layer is formed on a first surface of a single crystal silicon substrate whose surface crystal orientation is a {110} plane, and a back mask layer is formed on a second surface opposite to the first surface; A second step of forming a nozzle pattern to become a nozzle on the back mask layer; A third step is to form a deep hole that becomes a straight part of the nozzle by deep-digging the single crystal silicon substrate located under the nozzle pattern from the back side by dry etching until halfway; The fourth step is to form a nozzle mask layer on the side wall of the deep hole; The fifth step is to perform deep digging processing on the single crystal silicon substrate located under the deep hole from the back side by dry etching; A sixth step is to form an opening pattern serving as an opening portion on the surface mask layer; The seventh step is to perform deep digging processing on the single crystal silicon substrate located in the opening pattern by dry etching from the surface; as well as In the eighth step, the single crystal silicon substrate is subjected to through-processing from the front and back sides by anisotropic wet etching to form a nozzle flow path having a nozzle straight portion, a nozzle tapered portion, and a straight connecting path portion. When the thickness of the single crystal silicon substrate is set to T, the diameter of the nozzle straight portion is set to D, the depth of the nozzle straight portion is set to h, the width of the opening in the <110> direction is set to L, and the angle formed by the first surface and the second surface of the single crystal silicon substrate and the {111} plane of the tapered surface constituting the two surfaces of the nozzle tapered portion is set to θ, the depth H of the deep hole formed in the seventh step satisfies the following (1), wherein θ=Acοоs(2 / √6)≈35.26°, (1)T-(H+(L / 2)tanθ)≥h-(D / 2)tanθ.
22. The method for manufacturing a nozzle plate according to claim 21, in, When the first surface is set to a (1 1 0) surface, the width of the nozzle pattern formed in the second step in the [-1 1 1] direction and the width in the [1-1-1] direction are wider than the width of the opening pattern formed in the sixth step in the [-1 1 1] direction and the width in the [1-1-1] direction.