Positive electrode active material for nonaqueous electrolyte secondary battery
By using composite oxides and non-aqueous electrolytes with Fm-3m crystal structure, the discharge capacity of the non-aqueous electrolyte secondary battery is improved, the problem of insufficient capacity of the positive electrode active material in the prior art is solved, and high output and high energy are achieved Density of battery performance.
Patent Information
- Application Number
- CN202280093699.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2022-12-13
- Publication Date
- 2024-11-08
AI Technical Summary
The cathode active substances of existing nonaqueous electrolyte secondary batteries are insufficient during the discharge process, making it difficult to meet the needs of high output and high energy density.
Using composite oxides with a spatial group Fm-3m crystal structure as the positive electrode active material, through specific composition and preparation methods, including mixing LixTMtmMyO2-fFf composite oxides with acetylene black and polyvinylidene fluoride, using N-methyl -2-pyrrolidone is dispersed and a composite material layer is formed on aluminum foil, combining non-aqueous electrolytes of fluoroethylene carbonate and methyl propionate to prepare a half-cell.
The dV/dq-SOC curve with more than 1 peak in the range of SOC of more than 10% and less than 40% is significantly improved, and the performance of nonaqueous electrolyte secondary battery with high output and high energy density is achieved.
Smart Images

Figure CN118922960A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a technology of a positive electrode active material for a non-aqueous electrolyte secondary battery. Background Art
[0002] As a high-output, high-energy-density secondary battery, for example, a nonaqueous electrolyte secondary battery is widely used, which includes a positive electrode, a negative electrode, and a nonaqueous electrolyte and performs charge and discharge by transferring lithium ions etc. between the positive electrode and the negative electrode.
[0003] For example, Patent Document 1 discloses, as a positive electrode active material used in a non-aqueous electrolyte secondary battery, a composite oxide having a crystal structure belonging to the space group Fm-3m, containing lithium and molybdenum and containing substantially no chromium.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-202954 Summary of the invention
[0007] An object of the present disclosure is to provide a positive electrode active material for a non-aqueous electrolyte secondary battery having a high discharge capacity.
[0008] The positive electrode active material for a non-aqueous electrolyte secondary battery as one embodiment of the present disclosure has a crystal structure belonging to the space group Fm-3m and is represented by the general formula: Li x TM tm M y O 2-f F f The composite oxide shown in the above general formula, TM is a transition metal, M is a non-transition metal, and Q is set to be 2×tm×{1-(1-f / 2) 5}, Q<1 is satisfied, and when the aforementioned composite oxide is made into a half-cell by the following method, the half-cell is charged at 25°C with a charging current of 0.1C to a termination voltage in the range of 4.7 to 4.95V, the ratio dV / dq of the change dV in the voltage V of the aforementioned half-cell to the change dq in the battery capacity q of the aforementioned half-cell and the relationship between the charging rate SOC of the aforementioned half-cell, that is, the dV / dq-SOC curve, has one or more peaks in the range of SOC above 10% and below 40%, and is a positive electrode active material for a non-aqueous electrolyte secondary battery. (Method: The composite oxide, acetylene black and polyvinylidene fluoride are mixed in a mass ratio of 7:2:1, and N-methyl-2-pyrrolidone is used to disperse them to prepare a slurry for a positive electrode composite material layer. The slurry for the positive electrode composite material layer is applied on an aluminum foil, dried, and then rolled in a manner such that the film thickness is in the range of 20 to 50 μm. Then, the mold is demolded into 20 mm×20 mm to obtain a positive electrode. The electrode body obtained by sandwiching a separator between the positive electrode and a metal lithium foil (thickness 0.3 mm) as a negative electrode is housed in an outer shell of an aluminum laminate film, and a non-aqueous electrolyte in which LiPF6 is dissolved in a mixed solvent of fluoroethylene carbonate and methyl propionate (volume ratio 1:3) in a concentration of 1 mol / L is injected into the aforementioned outer shell, which is sealed to produce a half-cell.)
[0009] According to one aspect of the present disclosure, a positive electrode active material for a non-aqueous electrolyte secondary battery having a high discharge capacity can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of an embodiment.
[0011] Figure 2 This is a diagram showing the X-ray diffraction results of Example 1.
[0012] Figure 3 This is a diagram showing the X-ray diffraction results of Example 3.
[0013] Figure 4 3 is a diagram showing the X-ray diffraction result of Comparative Example 1.
[0014] Figure 5 3 is a diagram showing the X-ray diffraction result of Comparative Example 3.
[0015] Figure 6 dV / dq-SOC curves of the half cells of Examples 1-2 and Comparative Examples 1-2.
[0016] Figure 7 dV / dq-SOC curves of the half cells of Examples 3, 5, 6 and Comparative Example 4. DETAILED DESCRIPTION
[0017] An example of a nonaqueous electrolyte secondary battery using the positive electrode active material for a nonaqueous electrolyte secondary battery disclosed in the present invention will be described below.
[0018] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of an embodiment. Figure 1 The non-aqueous electrolyte secondary battery 10 shown in the figure comprises: a wound electrode body 14 in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween, a non-aqueous electrolyte, insulating plates 18 and 19 respectively arranged above and below the electrode body 14, and a battery case 15 for accommodating the above components. The battery case 15 is composed of a shell body 16 and a sealing body 17 for blocking the opening of the shell body 16. It should be noted that, instead of the wound electrode body 14, an electrode body of other forms such as a laminated electrode body in which a positive electrode and a negative electrode are alternately laminated with a separator interposed therebetween may be applied. In addition, as the battery case 15, examples include a cylindrical, square, coin-shaped, button-shaped, etc., a resin case (laminated battery) formed by laminating metal cases and resin sheets.
[0019] The non-aqueous electrolyte includes, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Examples of the non-aqueous solvent include esters, ethers, nitriles, amides, and mixed solvents of two or more thereof. The non-aqueous solvent may also be a halogen-substituted product obtained by replacing at least a portion of the hydrogen in these solvents with a halogen atom such as fluorine. Examples of the electrolyte salt include lithium salts such as LiPF6. It should be noted that the non-aqueous electrolyte is not limited to a liquid electrolyte, and may also be a solid electrolyte using a gel-like polymer or the like.
[0020] The shell body 16 is, for example, a metal container in a cylindrical shape with a bottom. A gasket 28 is provided between the shell body 16 and the sealing body 17 to ensure the airtightness inside the battery. The shell body 16 has, for example, a bulging portion 22 in which a part of the side surface bulges inwardly and supports the sealing body 17. The bulging portion 22 is preferably formed in an annular shape along the circumferential direction of the shell body 16, and the sealing body 17 is supported by its upper surface.
[0021] The sealing body 17 has a structure in which a partially opened metal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cover 27 are stacked in sequence from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective central portions, and the insulating member 25 is sandwiched between their respective peripheral portions. When the internal pressure of the non-aqueous electrolyte secondary battery 10 rises due to heat caused by an internal short circuit, for example, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 up to the cover 27 side, and the current path between the lower valve body 24 and the upper valve body 26 is cut off. When the internal pressure rises further, the upper valve body 26 breaks, and the gas is discharged from the opening of the cover 27.
[0022] Figure 1 In the non-aqueous electrolyte secondary battery 10 shown, the positive electrode lead 20 attached to the positive electrode 11 extends to the sealing body 17 side through the through hole of the insulating plate 18, and the negative electrode lead 21 attached to the negative electrode 12 extends to the bottom side of the case body 16 through the outside of the insulating plate 19. The positive electrode lead 20 is connected to the lower surface of the partially opened metal plate 23 as the bottom plate of the sealing body 17 by welding or the like, and the cover 27 as the top plate of the sealing body 17 electrically connected to the partially opened metal plate 23 becomes the positive terminal. The negative electrode lead 21 is connected to the bottom inner surface of the case body 16 by welding or the like, and the case body 16 becomes the negative terminal.
[0023] The positive electrode 11 , the negative electrode 12 , and the separator 13 are described in detail below.
[0024] <Positive electrode>
[0025] The positive electrode 11 includes a positive electrode current collector and a positive electrode composite material layer disposed on the positive electrode current collector. The positive electrode current collector may be made of a foil of a metal such as aluminum that is stable within the potential range of the positive electrode, or a thin film having the metal disposed on the surface. The thickness of the positive electrode current collector is preferably in the range of 1 μm or more and 20 μm or less, for example.
[0026] The positive electrode composite material layer preferably contains a positive electrode active material, and further contains a binder, a conductive material, etc. The thickness of the positive electrode composite material layer is preferably in the range of, for example, 10 μm or more and 300 μm or less.
[0027] The positive electrode 11 is obtained, for example, by applying a positive electrode composite material slurry containing a positive electrode active material, a binder, a conductive material, etc., on a positive electrode current collector and drying the slurry to form a positive electrode composite material layer on the positive electrode current collector, and rolling the positive electrode composite material layer.
[0028] The positive electrode active material includes a composite oxide having a crystal structure belonging to the space group Fm-3m.
[0029] The crystal structure belonging to the space group Fm-3m means that in the diffraction pattern obtained by X-ray diffraction (XRD) measurement, there is a peak that can be attributed to the space group Fm-3m. It should be noted that the "-3" in the space group "Fm-3m" represents the object element of the 3-fold regression axis, and should be marked with "-" above the original "3". The X-ray diffraction pattern of the composite oxide can be measured by powder X-ray diffraction using an X-ray diffraction device (Rigaku's "MiniFlexII") and the line source is set to CuKα rays, the tube voltage is set to 40kV, and the tube current is set to 15mA. At this time, the diffracted X-rays are detected by a high-speed one-dimensional detector (D / teX Ultra2) through a metal plate with a thickness of 30μm and a Kβ local opening. In addition, the sampling width is set to 0.02°, the scanning speed is set to 10° / minute, the divergence slit width is set to 0.625°, the light receiving slit width is set to 13mm (OPEN), and the scattering slit width is set to 8mm. Furthermore, the crystal structure of the composite oxide can be determined based on the obtained X-ray diffraction pattern and by Rietveld analysis using the "RIETAN-FP" program (F. Izumi and K. Momma, Solid State Phenom., 130, 15-20 (2007).). It should be noted that the X-ray diffraction apparatus is not limited to the above apparatus, nor is the X-ray source. The X-ray diffraction measurement conditions are not limited to the above conditions. In addition, the analysis method of the obtained X-ray diffraction pattern is not limited to the above method.
[0030] The composite oxide having a crystal structure belonging to the space group Fm-3m is represented by the general formula: Li x TM tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, and Q is set to be 2×tm×{1-(1-f / 2) 5}, Q<1 is satisfied. Here, Q represents the number of oxygens bonded to the transition metal bonded to fluorine. In addition, for a half-cell using the composite oxide as a positive electrode active material, the ratio dV / dq of the change dV in the voltage V of the half-cell relative to the change dq in the battery capacity q of the half-cell obtained when the half-cell is charged at 25°C with a charging current of 0.1C to a termination voltage in the range of 4.7 to 4.95V, and the relationship between the charge rate SOC of the half-cell, that is, the dV / dq-SOC curve, has one or more peaks in the range of SOC 10% to 40%. By using such a composite oxide, the discharge capacity can be increased. The preparation conditions of a half-cell using a composite oxide as a positive electrode active material are described in the examples.
[0031] In the dV / dq-SOC curve of a half-cell using a composite oxide as a positive electrode active material, if there is one or more peaks in the range of SOC 10% or more and 40% or less, the number of peaks is not limited. Alternatively, there may be only one peak. In addition, it is preferred that there is no peak in the range of SOC exceeding 40%.
[0032] (dV / dq-SOC curve)
[0033] When charging of the half-cell is started under the above conditions, the battery voltage V and current value I of the half-cell are measured at predetermined intervals, and the SOC (charging rate) is calculated based on the battery voltage V. In addition, the change dq of the battery capacity (charging capacity) q of the half-cell and the change dV of the battery voltage V are calculated from the measured values of the battery voltage V and current value I at that time, and dV / dq is calculated based on these calculation results. If the SOC and dV / dq of the half-cell are calculated at predetermined intervals, a dV / dq-SOC curve showing the relationship between SOC and dV / dq can be obtained based on these calculation results. Specifically, the horizontal axis is set to the value of SOC, and the vertical axis is set to the value of dV / dq, and these values calculated at predetermined intervals are graphed, thereby obtaining a dV / dQ-SOC curve.
[0034] The composition of the composite oxide has an influence on whether there is one or more peaks in the range of SOC10% to 40% in the dV / dq-SOC curve. In the dV / dq-SOC curve, in order to have one or more peaks in the range of SOC10% to 40%, for example, it is preferred to control tm and f in the above general formula within the range of Q<1. Furthermore, in the general formula, x, tm, y and f preferably satisfy 1.75≤x+tm+y≤2, 0<f≤0.7, and preferably satisfy 1.0<x≤1.4, 0.4≤tm<1.0, 0≤y≤0.2, 0.1≤f≤0.6. It should be noted that the above crystal structure may also have pores in which Li atoms, TM atoms and M atoms are not configured. Here, having pores means that in the positive electrode active material taken out immediately after production or after disassembling a discharged secondary battery, the composite oxide has pores that are not filled with Li atoms, TM atoms, or M atoms. The molar ratio of pores is preferably 0.05 to 0.25.
[0035] In a half-cell using the composite oxide of the present embodiment, the half-cell is charged at 25° C. with a charging current of 0.1C to a cut-off voltage range of 4.7 to 4.95V, and then charged at the above cut-off voltage until the current value reaches 0.05C, and then discharged at a discharge current of 0.1C to a cut-off voltage of 3.0 to 3.5V. The discharge capacity is 100 mAh / g or more. It should be noted that the discharge capacity is the capacity per unit mass of the positive electrode active material.
[0036] In addition, in a half-cell using the composite oxide of the present embodiment, the half-cell is charged at a constant current of 0.1C at 25°C to a termination voltage in the range of 4.7 to 4.95V, and then charged at the aforementioned termination voltage until the current value reaches 0.05C. Then, the discharge capacity is 200mAh / g or more when the half-cell is discharged at a discharge current of 0.1C to a termination voltage of 2.5 to 3.0V.
[0037] For example, from the viewpoint of obtaining a high discharge capacity, the composite oxide preferably contains Mn as the transition metal (TM), and in the general formula, in tm, the molar ratio tm_Mn of Mn is preferably 0.6<tm_Mn<0.8.
[0038] For example, from the aspect of being able to obtain a high discharge capacity, the composite oxide preferably contains Mn and a transition metal other than Mn. As the transition metal other than Mn, for example, Ni, Co, Fe, Ti, Y, Zr, Nb, Mo, Sc, W, V, Gd, Ce, Ta, Ag, etc. can be listed.
[0039] Examples of the non-transition metal (M) contained in the composite oxide include Al, Mg, Sb, Bi, Ca, Sr, Mg, K, Ga, Sn, and Zn.
[0040] The composition of the composite oxide can be confirmed by, for example, Rietveld analysis of parameters obtained by inductively coupled plasma optical emission spectrometry, X-ray photoelectron spectroscopy, and powder X-ray diffraction.
[0041] The method for producing the composite oxide is not particularly limited, and may be a known method in the synthesis of the positive electrode active material, for example, it may be obtained by treating a lithium source, an additive element source, a fluorine source, etc. using a mechanochemical method. A mechanochemical method (also referred to as mechanochemical treatment, etc.) refers to a synthesis method that utilizes a mechanochemical reaction. A mechanochemical reaction refers to a chemical reaction such as a crystallization reaction, a solid solution reaction, a phase change reaction, etc., which is locally generated by mechanical energy such as friction and compression during the crushing process of a solid substance. As an apparatus for performing a mechanochemical method, a ball mill, a bead mill, a vibration mill, a turbo pulverizer, a mechanical fusion device, a disc mill, and other pulverizers / dispersing machines may be cited. Among these, a ball mill is preferred. The mechanochemical treatment may be carried out in an atmosphere of an inert gas such as argon, or in an oxygen-containing atmosphere.
[0042] Lithium sources include lithium carbonate, lithium hydroxide, etc. The added element source is a compound containing a transition metal and a compound containing a non-transition metal, such as an oxide or hydroxide containing a transition metal, an oxide or hydroxide containing a non-transition metal, a composite oxide or hydroxide containing a transition metal and a non-transition metal, etc. The fluorine source is a fluoride such as lithium fluoride, molybdenum fluoride, magnesium fluoride, etc. It should be noted that lithium fluoride can be used as a lithium source, transition metal fluorides such as molybdenum fluoride can be used as a transition metal-containing compound of an added element source, and non-transition metal fluorides such as magnesium fluoride can also be used as a non-transition metal-containing compound of an added element source.
[0043] The composite oxide obtained by the mechanochemical treatment may be subjected to a heat treatment. The heating temperature is not particularly limited, and is, for example, in the range of 500° C. to 1000° C. In addition, the heating time is not particularly limited, and is, for example, 1 hour to 20 hours. The heating may be performed in an inert gas atmosphere such as argon gas, or in an oxygen-containing atmosphere.
[0044] The positive electrode active material may be composed of the above-mentioned composite oxide alone, or may contain other active materials other than the above-mentioned composite oxide. Examples of other active materials include Li x MO y (M represents at least one transition metal) represented by a composite oxide (Li having a layered α-NaFeO2 type crystal structure) x CoO2、Li x NiO2、Li x MnO2、Li x Ni α Co (1-α) O2、Li x Ni α Mn β Co (1-α-β) O2, etc., Li with spinel crystal structure xMn2O4、Li x Ni α Mn (2-α) O4, etc.), Li w M ’ x (XO y ) z (M' represents at least one transition metal, X represents, for example, P, Si, B, V, etc.) represented by a polyanion compound (LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc.).
[0045] The content of the composite oxide is preferably 50% by mass or more, more preferably 70% by mass or more, and further preferably 90% by mass or more relative to the total mass of the positive electrode active material. The composite oxide has a crystal structure belonging to the space group Fm-3m and is represented by the general formula: Li x TM tm M y O 2-f F f In the general formula, TM is a transition metal, M is a non-transition metal, and Q is set to be 2×tm×{1-(1-f / 2) 5}, Q<1 is satisfied, and in the above dV / dq-SOC curve, there is one or more peaks in the range of SOC 10% to 40%.
[0046] Examples of the conductive material contained in the positive electrode composite material layer include carbon black, acetylene black, Ketjen black, graphite and other carbon powders, etc. These may be used alone or in combination of two or more.
[0047] As the binding material included in the positive electrode composite material layer, for example, fluorine resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), PAN, polyimide resins, acrylic resins, polyolefin resins, styrene-butadiene rubber (SBR), CMC or its salt, polyacrylic acid (PAA) or its salt (PAA-Na, PAA-K etc.), polyvinyl alcohol (PVA) etc. can be used. These can be single 1 kind, and also can be used in combination of 2 or more kinds.
[0048] <Negative electrode>
[0049] The negative electrode 12 includes a negative electrode current collector such as a metal foil, and a negative electrode composite material layer formed on the negative electrode current collector. As the negative electrode current collector, a foil of a metal such as copper that is stable within the potential range of the negative electrode, a film having the metal disposed on the surface, etc. can be used. The negative electrode composite material layer includes, for example, a negative electrode active material, a binder, etc.
[0050] As the negative electrode active material contained in the negative electrode composite material layer, there is no particular limitation as long as it is a material that can absorb / release lithium ions, for example, carbon materials, elements that can form alloys with lithium, or compounds containing the elements, etc. can be listed. As carbon materials, graphites such as natural graphite, difficult graphitization carbon, and artificial graphite, coke, etc. can be used. As elements that can form alloys with lithium and compounds containing the elements, for example, silicon, tin, silicon oxide, tin oxide, etc. formed by combining them with oxygen can be listed. In addition, in addition to the above, materials such as lithium titanate whose charge and discharge potential relative to metallic lithium is higher than that of carbon materials, etc. can also be used. As the binding material contained in the negative electrode composite material layer, the same materials as those in the case of the positive electrode can be listed.
[0051] <Separator>
[0052] For example, a porous sheet having ion permeability and insulation is used as the separator 13. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. As the material of the separator 13, olefin resins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator 13 can be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin, or a layer obtained by coating the surface of the separator 13 with aramid resin, etc.
[0053] Example
[0054] Hereinafter, the present disclosure will be further described by way of examples, but the present disclosure is not limited to these examples.
[0055] <Example 1>
[0056] [Preparation of positive electrode active material]
[0057] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gadolinium oxide (Gd2O3), and niobium oxide (Nb2O5) were weighed and mixed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Gd:Nb:F became 1.192:0.73:0.005:0.005:0.01:0.298. The mixed powder was put into a planetary ball mill (Premium-Line P7 manufactured by Fritsch, rotation speed: 600 rpm, container: 45 mL pot made of zirconia, balls: 200 g / min, 100 g / min, ... Ball), in Ar atmosphere, at room temperature for 35 hours (35 cycles of running for 1 hour and resting for 10 minutes). In this way, Li 1.192 Mn 0.73 Mg 0.005 G 0.005 Nb0.01 O 1.702 F 0.298 The composite oxide shown.
[0058] The obtained composite oxide was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 2 The crystal structure was analyzed, and it was confirmed that the crystal structure of the composite oxide belonged to the space group Fm-3m. The conditions for the powder X-ray diffraction measurement were as described above (the same conditions were also used for other examples and comparative examples).
[0059] The obtained composite oxide was used as a positive electrode active material, and a half cell was produced by the following method.
[0060] [Production of positive electrode]
[0061] The above-mentioned composite oxide was mixed in a ratio of 70 parts by mass, acetylene black was mixed in a ratio of 20 parts by mass, and polyvinylidene fluoride was mixed in a ratio of 10 parts by mass, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a slurry for a positive electrode composite material layer. Next, the slurry for the positive electrode composite material layer was applied to an aluminum foil with a thickness of 15 μm and dried, and then rolled in a manner such that the film thickness was in the range of 20 to 50 μm. Then, the mold was demolded to a size of 20 mm × 20 mm to obtain a positive electrode having a positive electrode composite material layer formed on both sides of the aluminum foil.
[0062] [Preparation of non-aqueous electrolyte]
[0063] A non-aqueous electrolyte was prepared by dissolving lithium hexafluorophosphate (LiPF6) in a mixed solvent of fluoroethylene carbonate (FEC) and methyl propionate (FMP) at a volume ratio of 1:3 at a concentration of 1 mol / L.
[0064] [Production of test battery cells]
[0065] Electrode leads were installed on the positive electrode and the metal lithium foil (thickness 0.3 mm) as the negative electrode. Next, an electrode body was prepared by sandwiching a separator between the positive electrode and the negative electrode, and the electrode body was placed in an outer shell of an aluminum laminate film, and the nonaqueous electrolyte was injected, and the outer shell was sealed. This was used as a half-cell (nonaqueous electrolyte secondary battery) of Example 1.
[0066] <Example 2>
[0067] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), and cerium oxide (CeO2) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Ce:F became 1.225:0.625:0.025:0.025:0.5. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.22 5Mn 0.625 Mg 0.025 Ce 0.025 O 1.5 F 0.5 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0068] In addition, using Li 1.225 Mn 0.625 Mg 0.025 Ce 0.025 O 1.5 F 0.5 A half cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0069] <Example 3>
[0070] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gallium oxide (Ga2O3), and niobium oxide (Nb2O5) were used as starting sources of composite oxides and weighed in such a way that the molar ratio of Li:Mn:Mg:Ga:Nb:F became 1.15:0.785:0.005:0.005:0.005:0.1. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.15 Mn 0.785 Mg 0.005 Ga 0.005 Nb 0.005 O 1.9 F 0.1 The obtained composite oxide was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 3 As a result of analyzing the crystal structure, it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0071] In addition, using Li 1.15 Mn 0.785 Mg 0.005 Ga 0.005 Nb 0.005 O 1.9 F0.1 A half cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0072] <Example 4>
[0073] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gallium oxide (Ga2O3), and cerium oxide (CeO2) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Ga:Ce:F became 1.15:0.785:0.005:0.005:0.005:0.2. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.15 Mn 0.785 Mg 0.005 Ga 0.005 Ce 0.005 O 1.8 F 0.2 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0074] In addition, using Li 1.15 Mn 0.785 Mg 0.005 Ga 0.005 Ce 0.005 O 1.8 F 0.2 A half cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0075] <Example 5>
[0076] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), gadolinium oxide (Gd2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Gd:Nb:Ce:F became 1.192:0.73:0.005:0.01:0.005:0.298. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.192 Mn 0.73 G 0.005 Nb 0.01 Ce 0.005 O 1.702 F 0.298 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0077] In addition, using Li 1.192 Mn 0.73 G 0.005 Nb 0.01 Ce 0.005 O 1.702 F 0.298 A half cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0078] <Example 6>
[0079] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gallium oxide (Ga2O3), and niobium oxide (Nb2O5) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Ga:Nb:F became 1.2:0.735:0.005:0.005:0.005:0.3. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.2 Mn 0.735 Mg 0.005 Ga 0.005 Nb 0.005 O 1.7 F 0.3 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0080] In addition, using Li 1.2 Mn 0.735 Mg 0.005 Ga 0.005 Nb 0.005 O 1.7 F 0.3 A half cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0081] <Example 7>
[0082] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), niobium oxide (Nb2O5), and cerium oxide (CeO2) were used as starting sources of composite oxides and weighed in a molar ratio of Li:Mn:Mg:Nb:Ce:F of 1.15:0.785:0.005:0.005:0.005:0.2. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.15 Mn 0.785 Mg 0.005 Nb0.005 Ce 0.005 O 1.8 F 0.2 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0083] In addition, using Li 1.15 Mn 0.785 Mg 0.005 Nb 0.005 Ce 0.005 O 1.8 F 0.2 A half cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0084] <Comparative Example 1>
[0085] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), gallium oxide (Ga2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) were used as starting sources of composite oxides and weighed in a molar ratio of Li:Mn:Ga:Nb:Ce:F of 1.126:0.695:0.048:0.038:0.005:0.431. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.126 Mn 0.695 Ga 0.048 Nb 0.038 Ce 0.005 O 1.569 F 0.431 The obtained composite oxide was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 4 As a result of analyzing the crystal structure, it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0086] In addition, using Li 1.126 Mn 0.695 Ga 0.048 Nb 0.038 Ce 0.005 O 1.569 F 0.431 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0087] <Comparative Example 2>
[0088] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), gadolinium oxide (Gd2O3), and niobium oxide (Nb2O5) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Mg:Gd:Nb:F became 1.139:0.678:0.024:0.025:0.048:0.436. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.139 Mn 0.678 Mg 0.024 G 0.025 Nb 0.048 O 1.564 F 0.436 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0089] In addition, using Li 1.139 Mn 0.678 Mg 0.024 G 0.025 Nb 0.048 O 1.564 F 0.436 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0090] <Comparative Example 3>
[0091] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), gallium oxide (Ga2O3), niobium oxide (Nb2O5), and cerium oxide (CeO2) were weighed as starting sources of composite oxides so that the molar ratio of Li:Mn:Ga:Nb:Ce:F became 1.2:0.58:0.05:0.01:0.01:0.6. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.2 Mn 0.58 Ga 0.05 Nb 0.01 Ce 0.01 O 1.4 F 0.6 The obtained composite oxide was subjected to powder X-ray diffraction measurement, and the results are shown in Figure 5 As a result of analyzing the crystal structure, it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0092] In addition, using Li 1.2 Mn 0.58 Ga 0.05Nb 0.01 Ce 0.01 O 1.4 F 0.6 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0093] <Comparative Example 4>
[0094] Lithium fluoride (LiF), lithium manganate (LiMnO2), manganese (III) oxide (Mn2O3), lithium peroxide (Li2O2), magnesium oxide (MgO), niobium oxide (Nb2O5), and cerium oxide (CeO2) were used as starting sources of composite oxides and weighed in such a way that the molar ratio of Li:Mn:Mg:Nb:Ce:F became 1.217:0.696:0.015:0.01:0.005:0.596. The same operation as in Example 1 was performed except that the above was performed to obtain Li 1.217 Mn 0.696 Mg 0.015 Nb 0.01 Ce 0.005 O 1.404 F 0.596 The obtained composite oxide was subjected to powder X-ray diffraction measurement and crystal structure analysis, and it was confirmed that the crystal structure of the composite oxide belongs to the space group Fm-3m.
[0095] In addition, using Li 1.217 Mn 0.696 Mg 0.015 Nb 0.01 Ce 0.005 O 1.404 F 0.596 A test battery cell was prepared in the same manner as in Example 1 using the composite oxide shown.
[0096] [dV / dq-SOC curve]
[0097] The half-cells of each embodiment and each comparative example were charged at a constant current of 0.1C at a temperature of 25°C until the final voltage (cell voltage) reached 4.95V. During the charging, the SOC and dV / dq of the half-cell were calculated at predetermined intervals to obtain a dV / dq-SOC curve. The results are shown in Figure 6 and 7 .
[0098] like Figure 6As shown, in the dV / dq-SOC curve, the half-cells of Examples 1 and 2 have one peak in the range of SOC 10% or more and 40% or less. On the other hand, in the dV / dq-SOC curve, the half-cells of Comparative Examples 1 and 2 have one peak and two peaks in the range of SOC exceeding 40% and being 70% or less, respectively.
[0099] like Figure 7 As shown, in the half-cells of Examples 3, 5, and 6, there is one peak in the dV / dq-SOC curve within the range of SOC 10% or more and 40% or less. On the other hand, in the half-cell of Comparative Example 4, there are two peaks in the dV / dq-SOC curve within the range of SOC exceeding 40% and being 70% or less.
[0100] It should be noted that in the half-cells of Examples 4 and 7, it was confirmed that: in the dV / dq-SOC curve, there were one or more peaks in the range of SOC 10% or more and 40% or less. In addition, in the half-cell of Comparative Example 3, it was confirmed that: in the dV / dq-SOC curve, there was one peak in the range of SOC exceeding 40% and being 70% or less.
[0101] [Charge and discharge test 1]
[0102] The half-cells of each embodiment and each comparative example were charged at a constant current of 0.1C until the end voltage (battery voltage) reached 4.95V under a temperature environment of 25°C, and charged at a constant voltage of 4.95V until the current value reached 0.05C. Then, constant current discharge was performed at a constant current of 0.1C until the end voltage (battery voltage) reached 2.5V. The discharge capacity (mAh / g) during the above constant current discharge was determined.
[0103] Table 1 summarizes the composition of the composite oxide of each example and each comparative example, the composition (Li x TM tm M y O 2-f F f : TM is a transition metal, M is a non-transition metal) tm, f, Q (=2×tm×{1-(1-f / 2) 5}) values, and the results of discharge capacity.
[0104] [Table 1]
[0105]
[0106] Compared with Comparative Examples 1 to 4, Examples 1 to 7 all showed high discharge capacities. From these results, it can be seen that by using a crystal structure belonging to the space group Fm-3m and having the general formula: Lix TM tm M y O 2-f F f The composite oxide shown in the figure can obtain a high discharge capacity. In the above general formula, TM is a transition metal, M is a non-transition metal, and Q is set to be 2×tm×{1-(1-f / 2) 5}, Q<1 is satisfied, and in the dV / dq-SOC curve, which is the relationship between dV / dq and SOC of the half cell, there is one or more peaks in the range of SOC 10% to 40%.
[0107] <Example 8>
[0108] The half-cell of Example 1 was charged at a constant current of 0.1 C at a temperature of 25° C. until the final voltage (cell voltage) reached 4.7 V. During the charge, the SOC and dV / dq of the half-cell were calculated at predetermined intervals to obtain a dV / dq-SOC curve.
[0109] <Example 9>
[0110] The same operation as in Example 8 was carried out except that the half-cell of Example 5 was used to obtain a dV / dq-SOC curve.
[0111] <Comparative Example 5>
[0112] The same operation as in Example 8 was carried out except that the half-cell of Comparative Example 1 was used to obtain a dV / dq-SOC curve.
[0113] The dV / dq-SOC curves of Examples 8, 9, and Comparative Example 5 were checked. As a result, the half-cells of Examples 8 and 9 had one or more peaks in the dV / dq-SOC curves within the range of SOC 10% or more and 40% or less. On the other hand, the half-cell of Comparative Example 5 had one peak in the dV / dq-SOC curve within the range of SOC exceeding 40% and being 70% or less.
[0114] [Charge and discharge test 2]
[0115] The half-cells of Example 8, Example 9 and Comparative Example 5 were charged at a constant current of 0.1C at a temperature of 25°C until the final voltage (battery voltage) reached 4.7 V. Then, they were discharged at a constant current of 0.1C until the final voltage (battery voltage) reached 3.0 V. The discharge capacity (mAh / g) during the above constant current discharge was determined.
[0116] Table 2 summarizes the compositions of the composite oxides of Example 8, Example 9 and Comparative Example 5, the compositions (Lix TM tm M y O 2-f F f : TM is a transition metal, M is a non-transition metal) tm, f, Q (=2×tm×{1-(1-f / 2) 5}) values, and the results of discharge capacity.
[0117] [Table 2]
[0118]
[0119] Compared with Comparative Example 5, Examples 8 and 9 both showed high discharge capacity. From these results, it can be said that by using a crystal structure belonging to the space group Fm-3m and having the general formula: Li x TM tm M y O 2-f F f The composite oxide shown in the figure can obtain a high discharge capacity. In the above general formula, TM is a transition metal, M is a non-transition metal, and Q is set to be 2×tm×{1-(1-f / 2) 5}, Q<1 is satisfied, and in the dV / dq-SOC curve, which is the relationship between dV / dq and SOC of the half cell, there is one or more peaks in the range of SOC 10% to 40%.
[0120] Description of Reference Numerals
[0121] 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 battery case, 16 case body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 bulge, 23 partially opened metal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cover, 28 gasket.
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery, which has a crystal structure belonging to the space group Fm-3m and has the general formula: Li x TM tm M y O 2-f F f The composite oxide shown in the general formula, TM is a transition metal, M is a non-transition metal, and Q is set to be 2×tm×{1-(1-f / 2) 5}, Q<1, When the composite oxide is made into a half-cell by the following method, the ratio dV / dq of the change dV of the voltage V of the half-cell to the change dq of the battery capacity q of the half-cell obtained when the half-cell is charged at 25° C. with a charging current of 0.1C to a final voltage range of 4.7 to 4.95V and the charging rate SOC of the half-cell, i.e., the relationship between the ratio dV / dq of the change dV of the voltage V of the half-cell to the change dq of the battery capacity q of the half-cell and the charging rate SOC of the half-cell, i.e., the dV / dq-SOC curve has one or more peaks in the range of SOC 10% to 40%; The method is as follows: the composite oxide, acetylene black and polyvinylidene fluoride are mixed in a mass ratio of 7:2:1, dispersed using N-methyl-2-pyrrolidone, and a slurry for a positive electrode composite material layer is prepared. The slurry for the positive electrode composite material layer is coated on an aluminum foil, dried, and then rolled in a manner such that the film thickness is in the range of 20 to 50 μm, and then demolded into 20 mm×20 mm to obtain a positive electrode. The electrode body obtained by sandwiching a separator between the positive electrode and a metal lithium foil with a thickness of 0.3 mm as a negative electrode is housed in an outer shell of an aluminum laminate film, and a non-aqueous electrolyte in which LiPF6 is dissolved in a mixed solvent of fluoroethylene carbonate and methyl propionate in a volume ratio of 1:3 at a concentration of 1 mol / L is injected into the outer shell, which is sealed to produce a half-cell.
2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The half-battery is charged at a constant current of 0.1C at 25°C to a termination voltage in the range of 4.7 to 4.95V, and then charged at a constant voltage to a current value of 0.05C, and then discharged at a discharge current of 0.1C to a termination voltage of 3.0 to 3.5V, and the discharge capacity is 100mAh / g or more.
3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The half-battery is charged at a constant current of 0.1C at 25°C to a termination voltage range of 4.7 to 4.95V, and then charged at a constant voltage to a current value of 0.05C at the termination voltage. The discharge capacity is 200mAh / g or more when the half-battery is discharged at a discharge current of 0.1C to a termination voltage range of 2.5 to 3.0V.
4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein In the general formula, x, tm, y and f satisfy 1.75≤x+tm+y≤2, 0<f≤0.
7.
5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 4, wherein In the general formula, x, tm, y and f satisfy 1.0<x≤1.4, 0.4≤tm<1.0, 0≤y≤0.2, 0.1≤f≤0.
6.
6. The positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 5, wherein The composite oxide contains Mn as the transition metal (TM), In the general formula, in tm, the molar ratio of Mn tm_Mn is 0.6<tm_Mn<0.
8.
7. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 6, wherein The composite oxide contains Mn and a transition metal other than Mn as the transition metal (TM).