Mosquito-repelling silicon dioxide aerogel microspheres, and preparation method and application thereof

By filling and wrapping the mosquito repellent with silica aerogel microspheres, the existing mosquito repellent has solved the problem of irritation and short age, achieving sustained release effect and efficient preparation, and is suitable for a variety of mosquito repellent products.

CN118923669APending Publication Date: 2024-11-12NINGBO DILATO MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410979596.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The chemicals of existing mosquito repellents may irritate the skin or cause digestive tract discomfort, and strong volatility leads to poor effect and short age. The mechanical properties and thermal stability of traditional organic polymer packaging are insufficient.

Method used

Silica aerogel microspheres containing dense outer layer and porous inner layer are filled with mosquito repellent in the porous inner layer and wrapped by the dense outer layer to form a sustained release effect and stabilize in water through prepolymerization and polymerization steps. The emulsion avoids the addition of surfactants and stabilizers, and the process is simple and the cost is low.

Benefits of technology

It realizes the sustained release effect of mosquito repellent, improves safety and convenience of use, enhances mechanical properties and thermal stability, and is suitable for the preparation of mosquito repellent liquid, spray, bracelets and fabrics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118923669A_ABST
    Figure CN118923669A_ABST
Patent Text Reader

Abstract

The invention relates to silicon dioxide aerogel microspheres for repelling mosquitoes as well as a preparation method and application of the silicon dioxide aerogel microspheres. The silicon dioxide aerogel microsphere for repelling mosquitoes comprises a silicon dioxide skeleton and a mosquito repellent filled in the silicon dioxide skeleton, the silicon dioxide skeleton is optionally modified by an organic group, and the size of the aerogel microsphere is 0.5-100 [mu] m. The silica skeleton has a porous inner layer containing pores having a size of 1-800 nm and a dense outer layer containing pores having a size of 0.5-50 nm. The holes of the porous inner layer are filled with the mosquito repellent, and the compact outer layer is used for wrapping the mosquito repellent, so that the mosquito repellent can be slowly released. The silicon dioxide aerogel microspheres provided by the invention can be used for preparing mosquito repellent liquid, mosquito repellent spray, mosquito repellent bracelets or mosquito repellent fabrics and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to silicon dioxide aerogel microspheres for repelling mosquitoes and a preparation method thereof. Background Art

[0002] Mosquito bites can spread diseases such as malaria, dengue fever, Japanese encephalitis, and chikungunya fever. They are the pests that pose the greatest threat to human health. According to statistics from the World Health Organization (WHO), about 725,000 people die from mosquito bites each year. Therefore, the prevention and treatment of mosquito bites is very important. At present, mosquito repellents are the most widely used and the most direct way to reduce mosquito bites. However, currently widely used mosquito repellents such as N,N-diethyl-m-toluamide, N,N-diethyl-3-methylbenzamide, and toluene may irritate the skin or cause symptoms such as digestive tract discomfort when in direct contact with the human body. On the other hand, if mosquito repellents are used directly, they are highly volatile and may also lead to poor effects and short mosquito repellent effects.

[0003] Special encapsulation processes, such as microcapsule encapsulation and porous material wrapping, can effectively avoid direct contact between mosquito repellent and human body, thus improving the safety of mosquito repellent. Moreover, the encapsulated mosquito repellent can be formed into solid particles, which is convenient for processing and can be prepared into various products, such as mosquito repellent spray, mosquito repellent bracelet, mosquito repellent fabric, etc.

[0004] Traditional encapsulation technology mostly uses organic polymers as encapsulation materials. For example, patent CN115943968 discloses the use of gelatin, gum arabic and other materials to encapsulate mosquito repellents, and patent CN115633682 discloses the use of chitosan to encapsulate mosquito repellents. However, the use of such organic polymers to encapsulate mosquito repellents has poor mechanical properties and low thermal stability, and the related microcapsules will be limited in further application.

[0005] Compared with organic polymers, silica has better mechanical properties, thermal stability, solvent tolerance, etc., and is highly biosafe. However, the technology of using silica microspheres to encapsulate mosquito repellents, especially the technology of using high-porosity silica aerogel microspheres to encapsulate mosquito repellents, has not been reported. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the inventors found after in-depth research that the mosquito repellent silica aerogel microspheres of the present invention can form a slow release of the mosquito repellent by filling the pores of the porous inner layer with a dense outer layer containing pores of 0.5 to 50 nm in size and a silica skeleton containing a porous inner layer containing pores of 1 to 800 nm in size, and wrapping the mosquito repellent with the dense outer layer. In addition, the silica aerogel microspheres provided by the present invention have a size of submicron to micron, which is different from traditional block aerogels, does not need to be crushed, is easy to use, and does not affect the basic properties of the material when compounded with other materials.

[0007] The present invention provides the following technical solutions:

[0008] [1] Silica aerogel microspheres for mosquito repellent, the aerogel microspheres comprising a silica skeleton and a mosquito repellent filled in the silica skeleton, wherein the silica skeleton is optionally modified with an organic group.

[0009] The size of the aerogel microspheres is 0.5 to 100 μm.

[0010] The silica skeleton has a porous inner layer containing pores with a size of 1 to 800 nm and a dense outer layer containing pores with a size of 0.5 to 50 nm.

[0011] [2] The mosquito repellent silica aerogel microspheres according to [1], wherein the silica content in the aerogel microspheres is 5 to 99% and the mosquito repellent content is 1 to 95% by mass.

[0012] [3] The mosquito repellent silica aerogel microspheres according to [1], wherein the organic group is at least one non-hydrolyzable group selected from an alkyl group, a vinyl alkyl group, an epoxy alkyl group, a styryl alkyl group, a (meth)acryloxy alkyl group, an amino alkyl group, a urea alkyl group, a chloropropyl alkyl group, a haloalkyl group, an isocyanate alkyl group or a hydroxyalkyl group.

[0013] [4] The method for preparing mosquito repellent silica aerogel microspheres according to any one of [1] to [3] is characterized by comprising the following steps:

[0014] Prepolymerization step: fully mixing silane, a hydroxyl-containing hydrophilic compound, an organic solvent, and water, adding a catalyst, heating and reacting the mixture completely, and then removing the solvent to obtain a polyalkoxysiloxane prepolymer;

[0015] Polymerization step: fully mix the polyalkoxysiloxane prepolymer obtained in the prepolymerization step, the mosquito repellent and water to obtain a white emulsion, add alkali to adjust the pH to 7-12 and continue the reaction to obtain a dispersion of silica aerogel microspheres wrapped with the mosquito repellent.

[0016] [5] The method for preparing mosquito repellent silica aerogel microspheres according to [4] further comprises the following separation, washing and / or drying steps:

[0017] Separation and washing step: after separating the silica aerogel microspheres encapsulating the mosquito repellent from the dispersion of the silica aerogel microspheres encapsulating the mosquito repellent obtained in the polymerization step, washing with water until the dispersion is neutral, the separation is centrifugal separation, filtration, ultrafiltration or dialysis;

[0018] Drying step: drying to obtain powder of silica aerogel microspheres encapsulating mosquito repellent.

[0019] [6] The method for preparing mosquito repellent silica aerogel microspheres according to [4], wherein the silane used in the prepolymerization step is a monomer having the following chemical formula, or a polysiloxane precursor having a silica content of less than 60%;

[0020] R 1 n -Si-(OR 2 ) (4-n)

[0021] Among them, R 1 is at least one non-hydrolyzable group selected from unsubstituted alkyl, vinyl alkyl, epoxy alkyl, styryl alkyl, (meth)acryloxy alkyl, amino alkyl, urea alkyl, chloropropyl alkyl, haloalkyl, isocyanate alkyl or hydroxyalkyl, R 2 is an alkyl group having 1 to 6 carbon atoms; n is 0, 1 or 2; each R 2 are the same or different from each other; when n is 2, each R 1 The same as or different from each other.

[0022] [7] The method for preparing mosquito repellent silica aerogel microspheres according to [4], wherein the organic solvent in the prepolymerization step is at least one selected from methanol, ethanol, isopropanol, butanol, ethylene glycol, ethylene glycol butyl ether, propylene glycol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, acetone, and butanone, and the weight ratio of the organic solvent to the silane is (0.1-10):1;

[0023] The catalyst in the prepolymerization step is at least one selected from hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, acidic cation exchange resin, aluminum trichloride, boron trifluoride, and alkoxytitanium;

[0024] The molar concentration of the catalyst is 0.01-10 mol / L, and the weight ratio of the catalyst to the silane is (0.001-0.2):1.

[0025] [8] The method for preparing mosquito repellent silica aerogel microspheres according to [4], wherein in the prepolymerization step, the temperature of the heating reaction is 30 to 100°C, the reaction time is 1 to 24 hours, and the distillation is selected from one of atmospheric distillation, reduced pressure distillation, thin film evaporation or rotary evaporation, or a combination thereof.

[0026] [9] The method for preparing silica aerogel microspheres for mosquito repellent according to [4], wherein the mosquito repellent in the polymerization step is at least one selected from N,N-diethyl-m-toluamide, isobutyl hydroxyethyl piperidine carboxylate, ethyl butyl acetylaminopropionate, plant essential oil mosquito repellents, and pyrethroids.

[0027]

[10] Use of the mosquito repellent silica aerogel microspheres described in any one of [1] to [3] for preparing mosquito repellent liquid, mosquito repellent spray, mosquito repellent bracelet or mosquito repellent fabric.

[0028] Effects of the Invention

[0029] The silica aerogel microspheres provided by the present invention utilize a silica skeleton of a dense outer layer and a porous inner layer to fill the mosquito repellent in the pores of the porous inner layer, and utilize the dense outer layer to wrap the mosquito repellent, so as to form a slow release of the mosquito repellent. In addition, the silica aerogel microspheres provided by the present invention are submicron to micron-sized, which is different from traditional block aerogels, does not need to be crushed, is easy to use, and does not affect the basic properties of the material when compounded with other materials. The silica aerogel microspheres provided by the present invention can be used to prepare mosquito repellent liquid, mosquito repellent spray, mosquito repellent bracelet or mosquito repellent fabric, etc.

[0030] The preparation method of the silica aerogel microspheres for mosquito repellent provided by the present invention does not require the addition of surfactants or stabilizers, and the mosquito repellent can be stabilized in water to form a stable emulsion by using an amphiphilic polyalkoxysiloxane prepolymer, with few by-products and high preparation efficiency. In addition, the preparation method of the silica aerogel microspheres for mosquito repellent provided by the present invention does not require the use of a supercritical drying process, and has a simple process flow, low cost, and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope photograph of the silica aerogel microspheres encapsulated with mosquito repellent prepared in Example 1.

[0032] Figure 2 This is a scanning electron microscope photograph of the internal structure of the silica aerogel microspheres coated with mosquito repellent prepared in Example 1 after being crushed.

[0033] Figure 3 This is the thermal gravimetric curve of the silica aerogel microspheres encapsulated with mosquito repellent prepared in Example 1.

[0034] Figure 4 This is the thermal gravimetric curve of the silica aerogel microspheres encapsulated with mosquito repellent prepared in Example 2.

[0035] Figure 5 This is the thermal gravimetric curve of the silica aerogel microspheres encapsulated with mosquito repellent prepared in Example 3.

[0036] Figure 6 This is the thermal gravimetric curve of the silica aerogel microspheres encapsulated with mosquito repellent prepared in Example 4. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the scope of the present invention is not limited in any way. Unless otherwise stated, the reagents used in the specific examples can be obtained through commercial means or conventional experimental means.

[0038] [Silica aerogel microspheres for mosquito repellent]

[0039] The silica aerogel microspheres for repelling mosquitoes comprise a silica skeleton and a mosquito repellent filled in the silica skeleton.

[0040] The aforementioned silica skeleton may be optionally modified by an organic group. Examples of such organic groups include alkyl, vinylalkyl, epoxyalkyl, styrylalkyl, (meth)acryloxyalkyl, aminoalkyl, ureaalkyl, chloropropylalkyl, haloalkyl, isocyanatealkyl or hydroxyalkyl groups. By having such an organic group on the silica skeleton, the effect of adjusting the surface properties of the prepolymer can be obtained, and further functionalization in downstream applications can also be facilitated.

[0041] The size of the aforementioned aerogel microspheres is 0.5 to 100 μm, preferably 1 to 50 μm, and more preferably 2 to 20 μm. The shape of the aforementioned aerogel microspheres is spherical or approximately spherical.

[0042] The aforementioned silica skeleton has: a porous inner layer containing pores of 1 to 800 nm in size and a dense outer layer containing pores of 0.5 to 50 nm in size. By having such a porous inner layer and a dense outer layer with different pore sizes, the mosquito repellent is filled in the pores of the porous inner layer, and the mosquito repellent is wrapped by the dense outer layer, so that the mosquito repellent can be slowly released.

[0043] In the aerogel microspheres, the content of the silica skeleton is 5 to 99% by mass, and the content of the mosquito repellent is 1 to 95%. The ratio of the aforementioned silica skeleton to the mosquito repellent can be adjusted according to practical applications. Generally, the higher the content of the mosquito repellent, the higher the porosity of the silica aerogel is required, and thus the specific gravity of the silica skeleton is lower. Preferably, in the aerogel microspheres, the content of the silica skeleton is 5 to 99% by mass, and the content of the mosquito repellent is 1 to 95%.

[0044] The silica aerogel microspheres may be in the form of powder or in the form of a dispersion, and the dispersion may be an aqueous dispersion, an organic solvent dispersion, or a mixed solvent dispersion of water and an organic solvent.

[0045] [Preparation method of silica aerogel microspheres for mosquito repellent]

[0046] The preparation method of silica aerogel microspheres for mosquito repellent comprises the following steps:

[0047] Prepolymerization step: fully mixing silane, a hydroxyl-containing hydrophilic compound, an organic solvent, and water, adding a catalyst, heating and reacting the mixture completely, and then removing the solvent to obtain a polyalkoxysiloxane prepolymer;

[0048] Polymerization step: fully mix the polyalkoxysiloxane prepolymer obtained in the prepolymerization step, the mosquito repellent and water to obtain a white emulsion, add alkali to adjust the pH to 7-12 and continue the reaction to obtain a dispersion of silica aerogel microspheres wrapped with the mosquito repellent.

[0049] The silane used in the aforementioned prepolymerization step refers to a precursor that eventually forms silicon dioxide through hydrolysis and condensation, including monomer compounds and low molecular weight polymers. Preferably, the aforementioned silane can be a monomer having the following chemical formula,

[0050] R 1 n -Si-(OR 2 ) (4-n)

[0051] Among them, R 1 is at least one non-hydrolyzable group selected from unsubstituted alkyl, vinyl alkyl, epoxy alkyl, styryl alkyl, (meth)acryloxy alkyl, amino alkyl, urea alkyl, chloropropyl alkyl, haloalkyl, isocyanate alkyl or hydroxyalkyl, R 2 is an alkyl group having 1 to 6 carbon atoms; n is 0, 1 or 2; each R 2 are the same or different from each other; when n is 2, each R 1 The same as or different from each other.

[0052] In addition, the silane mentioned above may also be a commercially available polysiloxane prepolymer having a silicon dioxide content of 60% or less. Examples of such polysiloxane prepolymers include Silicon 40, Silicon 48, and Silicon 53. These may be used alone or in combination of two or more.

[0053] The main function of the hydroxyl-containing hydrophilic compound added in the above-mentioned prepolymerization step is to impart hydrophilicity to the polyalkoxysiloxane prepolymer, thereby promoting the synthesized polyalkoxysiloxane prepolymer and the mosquito repellent to be emulsified into emulsion droplets in the aqueous phase. Such a hydroxyl-containing hydrophilic compound is preferably polyethylene glycol, polyethylene glycol monoether, a copolymer of ethylene glycol and propylene glycol, polyvinyl alcohol, polyglycerol, etc., and one of them can be used, or a combination of multiple of them can be used.

[0054] The molecular weight of the hydroxyl group-containing hydrophilic compound is preferably 200 to 10,000, more preferably 300 to 5,000, and even more preferably 500 to 2,500.

[0055] The mass ratio of the hydroxyl-containing hydrophilic compound to the silane is preferably (0.01 to 1):1, more preferably (0.03 to 0.7):1, and even more preferably (0.05 to 0.5):1.

[0056] The organic solvent in the prepolymerization step is an organic agent for dissolving / dispersing silane and a hydroxyl-containing hydrophilic compound. Examples of such organic solvents include methanol, ethanol, isopropanol, butanol, ethylene glycol, ethylene glycol butyl ether, propylene glycol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, acetone, butanone, and the like. One of these can be used, or a plurality of these can be mixed and used. Preferably, it is at least one selected from methanol, ethanol, isopropanol, and propylene glycol methyl ether, and more preferably, it is at least one selected from ethanol and propylene glycol methyl ether.

[0057] The weight ratio of the organic solvent to the silane may be, for example, (0.1 to 10):1.

[0058] The water added in the prepolymerization step is used to hydrolyze and condense the silane. Preferably, the weight ratio of the added water to the silane is (0.01-1):1, more preferably (0.05-0.5):1, and even more preferably (0.1-0.3):1.

[0059] The purpose of adding a catalyst in the aforementioned prepolymerization step is to promote the hydrolysis and condensation of the alkoxy groups in the silane and improve the efficiency of the reaction. The aforementioned catalyst can be listed as protonic acids such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, solid acids such as acidic cation exchange resins, or Lewis acids such as aluminum chloride, boron trifluoride, alkoxytitanium, but are not limited to these. The molar concentration of the aforementioned catalyst can be, for example, 0.01 to 10 mol / L. The mass ratio of the aforementioned catalyst to silane is, for example, (0.001 to 0.2):1.

[0060] In some embodiments of the method for preparing silica aerogel microspheres for mosquito repellent, preferably, in the aforementioned prepolymerization step, the temperature of the heating reaction is 30 to 100° C., more preferably 50 to 90° C., and further preferably 70 to 80° C. In the aforementioned prepolymerization step, the heating reaction time is 1 to 24 hours, preferably 5 to 15 hours.

[0061] In the aforementioned prepolymerization step, the purpose of removing the solvent is to remove excess solvent and residual catalyst from the generated polyalkoxysiloxane prepolymer to avoid affecting the formation of aerogel microspheres in the subsequent polymerization step. Preferably, the method for removing the solvent is one of atmospheric distillation, reduced pressure distillation, thin film evaporation or rotary evaporation, or a combination thereof.

[0062] In the preparation method of silica aerogel microspheres for mosquito repellent in some embodiments, the mosquito repellent in the aforementioned polymerization step is a synthetic substance or natural substance that has been fully proven to have a mosquito repellent effect. As such a mosquito repellent, it can be a composition of one or more selected from N, N-diethyl-m-toluamide, hydroxyethyl piperidine carboxylic acid isobutyl ester, butyl acetylamino propionate, plant essential oil mosquito repellent, pyrethroids, etc. The mass ratio of the aforementioned mosquito repellent to the aforementioned polysiloxane prepolymer is preferably, for example, (0.001-20): 1. If the amount of mosquito repellent exceeds the prepolymer by too much, it may lead to problems such as decreased packaging efficiency.

[0063] In the aforementioned polymerization step, the method of mixing the polyalkoxysiloxane prepolymer, mosquito repellent and water can be adopted in a manner well known to those skilled in the art, for example, magnetic stirring, mechanical stirring, ultrasonic dispersion, emulsification by an emulsifier and the like can be adopted. The purpose of adding alkali in the aforementioned polymerization step is to further promote the hydrolysis and condensation of the polyalkoxysiloxane, and quickly form a silica structure with a certain mechanical strength. As the aforementioned alkali, at least one of sodium hydroxide, potassium hydroxide and ammonia water can be used. After adding the alkali, the reaction is continued for a period of time to fully complete the hydrolysis and condensation, thereby further increasing the mechanical strength of the silica. In addition, it has been proven that extending the reaction time will not damage the various properties of the silica aerogel microspheres finally obtained.

[0064] The mosquito repellent silica aerogel microspheres obtained by the above polymerization step are in the form of a dispersion liquid. Depending on the situation, such a dispersion liquid can be used directly.

[0065] In some embodiments, the method for preparing silica aerogel microspheres for mosquito repellent may further include a separation washing step and / or a drying step.

[0066] In the separation and washing step, the silica aerogel microspheres are separated from the aqueous dispersion of the mosquito repellent silica aerogel microspheres obtained in the polymerization step, and then washed with water until the dispersion is neutral. The separation can be performed, for example, by centrifugation, filtration, ultrafiltration, dialysis, etc., and one of these methods can be used, or a combination of multiple methods can be used.

[0067] The alkali added in the polymerization step can be removed by the aforementioned separation and washing, and preferably the pH value of the dispersion is neutral. Here, "neutral" means adjusting the pH value to about 7, that is, adjusting the pH value to the range of 7±0.5, preferably adjusting the pH value to the range of 7±0.3, and more preferably adjusting the pH value to the range of 7±0.1. Adjusting the pH value of the dispersion to neutral by washing can remove by-products and facilitate further applications.

[0068] In addition, the solvent used for washing may be optionally changed to change the solvent of the dispersion liquid to a desired solvent.

[0069] The aforementioned drying may be, for example, oven drying, freeze drying, or spray drying, etc., without particular limitation. Through the aforementioned drying, the silica aerogel microspheres may be prepared into a powder form.

[0070] Example

[0071] Example 1

[0072] 200 g of tetraethyl orthosilicate, 65 g of ethanol, and 10 g of polyethylene glycol (average molecular weight 750) were mixed evenly until transparent, and then 6.5 g of concentrated hydrochloric acid (mass fraction 37%) and 5 g of deionized water were added and mixed evenly. After stirring for 5 minutes, the temperature was raised to 70° C. and the reaction was continued for 4 hours. The solvent in the system was quickly removed by reduced pressure distillation to obtain a flowable and transparent polyalkoxysiloxane prepolymer with a certain viscosity.

[0073] Take 30g of polyalkoxysiloxane prepolymer and 25g of mosquito repellent (ethyl butyl acetylaminopropionate) and add them to 250g of deionized water, stir rapidly to obtain a uniform white emulsion, then add 25g of ammonia water (mass concentration 25%), and continue stirring for 5 hours to obtain a milky white dispersion of silica aerogel microspheres coated with mosquito repellent.

[0074] The silica aerogel microsphere dispersion is centrifuged to remove the upper clear liquid, and the lower white solid is washed with water, and this process is repeated until the dispersion is neutral or nearly neutral. After further centrifugation, the lower solid is freeze-dried to obtain silica aerogel microsphere powder coated with mosquito repellent.

[0075] The scanning electron microscope photo of the prepared silica aerogel microspheres wrapped with mosquito repellent is shown in FIG. Figure 1 As shown in the figure, the average size is about 10 to 15 μm, the size distribution is uniform, the spherical structure is complete, and the surface is closed. The aerogel microspheres were crushed by mortar and observed for their internal structure. Figure 2 As shown, it can be seen that there are a large number of pore structures inside the aerogel microspheres, which can wrap the mosquito repellent.

[0076] The thermal gravimetric analysis (TGA) of silica aerogel microspheres wrapped with mosquito repellent was measured at different temperatures to evaluate the amount and efficiency of the aerogel microspheres encapsulating the mosquito repellent. The aforementioned encapsulation amount refers to the mass percentage of the mosquito repellent in the entire aerogel microsphere, and the encapsulation efficiency refers to the proportion of the mosquito repellent encapsulated by the aerogel microspheres to the initial amount of mosquito repellent. The TGA results are shown in Figure 2. Figure 3 As shown, the weight loss of the entire aerogel microsphere is about 84.5%, of which the thermal weight loss of the mosquito repellent accounts for 66.55%, indicating that the aerogel encapsulates 66.55% of the mosquito repellent. By calculating the feed ratio, it can be concluded that the encapsulation efficiency of the aerogel for the mosquito repellent is close to 100%. From the downward trend of the TGA curve, it can also be judged that the mosquito repellent is slowly released through the micropores and mesopores on the shell of the aerogel microsphere. This shows that the aerogel microspheres obtained in this embodiment have excellent thermal stability and high mechanical properties, and further illustrates that the release of the mosquito repellent is achieved through the micropores or mesopores on the surface of the microspheres rather than by the breakage of the microspheres.

[0077] Example 2

[0078] The difference between Example 2 and Example 1 is that 10 g of polyethylene glycol (average molecular weight 750) is replaced by 5 g of polyethylene glycol (average molecular weight 300). 6.5 g of concentrated hydrochloric acid (mass fraction 37%) and 5 g of deionized water in step (1) are replaced by 10 g of concentrated hydrochloric acid (mass fraction 37%) and 7.5 g of deionized water, respectively, and the reduced pressure distillation is replaced by thin film evaporation.

[0079] Thermogravimetric analysis (TGA) was used to evaluate the encapsulation effect of silica aerogel on mosquito repellent, such as Figure 4As shown, the weight loss of the mosquito repellent accounts for 66.93%, indicating that the aerogel encapsulates 66.93% of the mosquito repellent. By calculating the feed ratio, it can be concluded that the encapsulation efficiency of the aerogel for the mosquito repellent is close to 100%. From the downward trend of the TGA curve, it can also be judged that the mosquito repellent is slowly released through the micropores and mesopores on the aerogel microsphere shell.

[0080] Example 3

[0081] The difference between Example 3 and Example 1 is that the 200g tetraethyl orthosilicate used in the prepolymerization step is replaced by 180g tetraethyl orthosilicate and 20g methyltriethoxysilane; 10g polyethylene glycol (average molecular weight 750) is replaced by 25g polyethylene glycol (average molecular weight 500). The 25g mosquito repellent (ethyl butyl acetylaminopropionate) used in the polymerization step is replaced by 20g mosquito repellent (ethyl butyl acetylaminopropionate). The freeze drying in the drying step is replaced by spray drying, and the rest is the same as Example 1.

[0082] Thermogravimetric analysis (TGA) was used to evaluate the encapsulation effect of silica aerogel on mosquito repellent. Figure 5 As shown. Figure 5 It can be seen that the weight loss of the mosquito repellent accounts for 56.03%, indicating that the aerogel encapsulates 56.03% of the mosquito repellent. By calculating the feed ratio, it can be concluded that the encapsulation efficiency of the aerogel for the mosquito repellent is close to 100%. From the downward trend of the TGA curve, it can also be judged that the mosquito repellent is slowly released through the micropores and mesopores on the aerogel microsphere shell.

[0083] Example 4

[0084] The difference between Example 4 and Example 1 is that 10 g of polyethylene glycol (average molecular weight 750) used in the prepolymerization step is replaced by 5 g of polyethylene glycol (average molecular weight 500), and concentrated hydrochloric acid is replaced by 20 grams of macroporous strong acid cation exchange resin; 25 g of mosquito repellent (ethyl butyl acetylaminopropionate) used in the polymerization step is replaced by 16 g of mosquito repellent (N, N-diethyl-m-toluamide); and freeze-drying in the drying step is replaced by oven drying (temperature 45°C, time 24 hours).

[0085] Thermogravimetric analysis (TGA) was used to evaluate the encapsulation effect of silica aerogel on mosquito repellent. Figure 6 As shown. Figure 6 It can be seen that the weight loss of the mosquito repellent accounts for 40.73%, indicating that the aerogel encapsulates 40.73% of the mosquito repellent. By calculating the feed ratio, it can be concluded that the encapsulation efficiency of the aerogel for the mosquito repellent is close to 95%. From the downward trend of the TGA curve, it can also be judged that the mosquito repellent is slowly released through the micropores and mesopores on the aerogel microsphere shell.

[0086] For those skilled in the art, other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all of these changes and deformations should fall within the scope of protection of the claims of the present invention. After considering the specification and practicing the invention disclosed herein, it will be easy to think of other embodiments of the present invention. The present invention is intended to cover any variation, use or adaptive change of the present invention, which follows the general principles of the present invention and includes common knowledge or customary technical means in the technical field not disclosed by the present invention.

Claims

1. Silica aerogel microspheres for mosquito repellent, characterized in that: The aerogel microspheres comprise a silica skeleton and a mosquito repellent filled in the silica skeleton, wherein the silica skeleton is optionally modified by an organic group. The size of the aerogel microspheres is 0.5 to 100 μm. The silica skeleton has a porous inner layer containing pores with a size of 1 to 800 nm and a dense outer layer containing pores with a size of 0.5 to 50 nm.

2. The mosquito repellent silica aerogel microspheres according to claim 1, wherein: In the aerogel microspheres, the content of silicon dioxide is 5-99% and the content of mosquito repellent is 1-95% by mass ratio.

3. The mosquito repellent silica aerogel microspheres according to claim 1, wherein: The organic group is at least one non-hydrolyzable group selected from an alkyl group, a vinylalkyl group, an epoxyalkyl group, a styrylalkyl group, a (meth)acryloxyalkyl group, an aminoalkyl group, an urethane group, a chloropropylalkyl group, a haloalkyl group, an isocyanatealkyl group or a hydroxyalkyl group.

4. The method for preparing the mosquito repellent silica aerogel microspheres according to any one of claims 1 to 3, characterized in that: The steps include: Prepolymerization step: fully mixing silane, a hydroxyl-containing hydrophilic compound, an organic solvent, and water, adding a catalyst, heating and reacting the mixture completely, and then removing the solvent to obtain a polyalkoxysiloxane prepolymer; Polymerization step: fully mix the polyalkoxysiloxane prepolymer obtained in the prepolymerization step, the mosquito repellent and water to obtain a white emulsion, add alkali to adjust the pH to 7-12 and continue the reaction to obtain a dispersion of silica aerogel microspheres wrapped with the mosquito repellent.

5. The method for preparing mosquito repellent silica aerogel microspheres according to claim 4, further comprising the following separation, washing and / or drying steps: Separation and washing step: after separating the silica aerogel microspheres encapsulating the mosquito repellent from the dispersion of the silica aerogel microspheres encapsulating the mosquito repellent obtained in the polymerization step, washing with water until the dispersion is neutral, the separation is centrifugal separation, filtration, ultrafiltration or dialysis; Drying step: drying to obtain powder of silica aerogel microspheres encapsulating mosquito repellent.

6. The method for preparing silica aerogel microspheres for mosquito repellent according to claim 4, wherein: The silane used in the prepolymerization step is a monomer having the following chemical formula, or a polysiloxane precursor having a silicon dioxide content of less than 60%; R 1 n -Si-(OR 2 ) (4-n) Among them, R 1 is at least one non-hydrolyzable group selected from unsubstituted alkyl, vinyl alkyl, epoxy alkyl, styryl alkyl, (meth)acryloxy alkyl, amino alkyl, urea alkyl, chloropropyl alkyl, haloalkyl, isocyanate alkyl or hydroxyalkyl, R 2 is an alkyl group having 1 to 6 carbon atoms; n is 0, 1 or 2; each R 2 are the same or different from each other; when n is 2, each R 1 The same as or different from each other.

7. The method for preparing mosquito repellent silica aerogel microspheres according to claim 4, wherein: The organic solvent in the prepolymerization step is at least one selected from methanol, ethanol, isopropanol, butanol, ethylene glycol, ethylene glycol butyl ether, propylene glycol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, acetone, and butanone, and the weight ratio of the organic solvent to the silane is (0.1-10):1; The catalyst in the prepolymerization step is at least one selected from hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, acidic cation exchange resin, aluminum trichloride, boron trifluoride, and alkoxytitanium; The molar concentration of the catalyst is 0.01-10 mol / L, and the weight ratio of the catalyst to the silane is (0.001-0.2):

1.

8. The method for preparing mosquito repellent silica aerogel microspheres according to claim 4, wherein: In the prepolymerization step, the temperature of the heating reaction is 30-100° C., the reaction time is 1-24 hours, and the distillation is selected from one of atmospheric distillation, reduced pressure distillation, thin film evaporation or rotary evaporation or a combination thereof.

9. The method for preparing mosquito repellent silica aerogel microspheres according to claim 4, wherein: The mosquito repellent in the polymerization step is at least one selected from N,N-diethyl-m-toluamide, isobutyl hydroxyethyl piperidine carboxylate, ethyl butyl acetylaminopropionate, plant essential oil mosquito repellents, and pyrethroids.

10. Use of the mosquito repellent silica aerogel microspheres according to any one of claims 1 to 3 in preparing mosquito repellent liquid, mosquito repellent spray, mosquito repellent bracelet or mosquito repellent fabric.

Citation Information

Cited By

  • Anti-mosquito fabric finishing agent as well as preparation method and application thereof

    CN120192534A