Composition containing fluorine-based hydrocarbon compound

By contacting specific zeolites, the problem of removing moisture and impurities in fluorine-based hydrocarbon compounds such as HFC-134a is solved, and a high-purity fluorine-based hydrocarbon compound is achieved, which is suitable for the etching gas requirements in semiconductor manufacturing.

CN118925459APending Publication Date: 2024-11-12DAIKIN INDUSTRIES LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410988037.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-11-28
Filing Date
2020-11-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove moisture and impurities in fluorine hydrocarbon compounds such as HFC-134a. Especially when the purity requirements of etching gases in semiconductor manufacturing processes are high, the presence of moisture and impurities will lead to reduced purity and corrosion of the device. .

Method used

By contacting the composition containing the fluorine-based hydrocarbon compound with a zeolite or chazeite type, mordenite type, beta type and Y type zeolite having a silica alumina ratio of 5 or more, moisture and impurities, including HFC-134 , ensure that the moisture content and HFC-134 content of the dehydrated composition are less than 3 ppmwt.

Benefits of technology

Highly efficient dehydration and impurity removal of fluorine-based hydrocarbon compounds such as HFC-134a are achieved, the purity of the composition is improved, the device corrosion and purity reduction is prevented, and it is suitable for etching gases in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958038840000241
    Figure BDA0004958038840000241
  • Figure BDA0004958038840000251
    Figure BDA0004958038840000251
  • Figure BDA0004958038840000261
    Figure BDA0004958038840000261
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method for dehydrating a composition containing a fluorine-based hydrocarbon compound such as HFC-134a. The dehydration method includes a step of bringing a composition containing a fluorine-based hydrocarbon compound into contact with zeolite.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This case is filed on November 26, 2020 、Application No. 202080082290.2(PCT / JP2020 / 044095) 、The name of the invention is Dehydration method of fluorinated hydrocarbon compounds Divisional application. Technical Field

[0002] The present invention relates to a method for dehydrating fluorine-based hydrocarbon compounds. Background Art

[0003] Fluorinated hydrocarbon compounds such as difluoromethane (HFC-32) are widely used as etching gases in semiconductor manufacturing processes.

[0004] Currently, fluorinated hydrocarbon compounds such as HFC-32 are dehydrated by adsorbing water using type A zeolite (for example, Patent Document 1).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 5446710 Summary of the invention

[0008] Technical problem to be solved by the invention

[0009] An object of the present invention is to provide a method for dehydrating a composition containing a fluorinated hydrocarbon compound such as HFC-134a.

[0010] Technical means for solving technical problems

[0011] The present invention includes the following configurations.

[0012] Item 1. A method for dehydrating a composition containing a fluorinated hydrocarbon compound, wherein the fluorinated hydrocarbon compound is at least one compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf), and the dehydration method comprises mixing the composition containing the fluorinated hydrocarbon compound with silica alumina (SiO 2 / Al 2 O 3 ) ratio is 5 or more zeolite contacting step.

[0013] Item 2. A method for dehydrating a composition containing a fluorine-containing hydrocarbon compound, wherein the fluorine-containing hydrocarbon compound is at least one compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf), and the dehydration method comprises a step of contacting the composition containing the fluorine-containing hydrocarbon compound with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite.

[0014] Item 3. The dehydration method according to Item 1 or 2 above, wherein the step is performed so that the moisture content of the composition after dehydration is less than 3 ppmwt.

[0015] Item 4. The dehydration method according to any one of Items 1 to 3, further comprising the step of contacting the composition containing a fluorinated hydrocarbon compound with the zeolite to remove 1,1,2,2-tetrafluoroethane (HFC-134).

[0016] In the dehydration method, the above step preferably causes the HFC-134 content in the dehydrated composition to be less than 3 ppmwt.

[0017] In addition, the content (ppm) of HFC-134 is, for example, the following value: when mass analysis is performed by gas chromatography / mass spectrometry (GC / MS) using gas chromatography, and then structural analysis is performed using NMR using NMR spectrum, the volume fraction obtained by dividing the content (volume) of HFC-134 contained in the composition containing the fluorine-based hydrocarbon compound by the volume of the composition containing the fluorine-based hydrocarbon compound, that is, ppmvol (volume / volume).

[0018] For example, in other words, the HFC-134 content (ppm) is less than 3 ppmvol.

[0019] Item 5. A method for producing a composition containing a fluorinated hydrocarbon compound, wherein the fluorinated hydrocarbon compound is at least one compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf), and the method comprises reacting the composition containing the fluorinated hydrocarbon compound with silica alumina (SiO 2 / Al 2 O 3 ) ratio is 5 or more zeolite contacting step.

[0020] Item 6. A method for producing a composition containing a fluorine-containing hydrocarbon compound, wherein the fluorine-containing hydrocarbon compound is at least one compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf), and the above-mentioned production method includes a step of contacting the above-mentioned composition containing a fluorine-containing hydrocarbon compound with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite.

[0021] Item 7. The production method according to Item 5 or 6, wherein the moisture content of the composition after contacting with the zeolite is less than 3 ppmwt.

[0022] Item 8. The production method according to any one of Items 5 to 7, further comprising the step of contacting the fluorinated hydrocarbon compound-containing composition with the zeolite to remove 1,1,2,2-tetrafluoroethane (HFC-134).

[0023] In the production method, the composition after contacting with the zeolite preferably has an HFC-134 content of less than 3 ppmwt.

[0024] Item 9. A method for producing a high-purity fluorine-based hydrocarbon compound, characterized in that it comprises: mixing a composition containing at least one fluorine-based hydrocarbon compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf) with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio is 5 or more to remove impurities contained in the fluorinated hydrocarbon compound.

[0025] Item 10. A method for producing high-purity fluorine-containing hydrocarbon compounds, characterized in that it includes: a step of contacting a composition containing at least one fluorine-containing hydrocarbon compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf) with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite to remove impurities contained in the fluorine-containing hydrocarbon compounds.

[0026] Item 11. The dehydration method according to Item 9 or 10, wherein the impurity is at least one component selected from water and 1,1,2,2-tetrafluoroethane (HFC-134).

[0027] Item 12. The production method according to any one of Items 9 to 11, wherein the water concentration in the fluorinated hydrocarbon compound after the impurities are removed is less than 3 ppmwt.

[0028] In the production method, the concentration of HFC-134 contained in the fluorinated hydrocarbon compound after the above-mentioned impurities have been removed is preferably less than 3 ppmwt of HFC-134.

[0029] Item 13. A composition containing fluorine-containing hydrocarbon compounds, wherein the fluorine-containing hydrocarbon compounds include at least one compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf), and the moisture content is less than 3 ppmwt and / or the HFC-134 content is less than 3 ppmwt.

[0030] Item 14. The composition according to Item 13 above, which is used as an etching gas, a refrigerant, a heat transfer medium, a deposition gas, a building block for organic synthesis, or a cleaning gas.

[0031] Effects of the Invention

[0032] According to the present invention, a method for dehydrating a composition containing a fluorine-based hydrocarbon compound such as HFC-134a can be provided. DETAILED DESCRIPTION

[0033] For etching gases in semiconductor manufacturing processes, the removal of moisture is very important.

[0034] The inventors of the present invention have conducted intensive research and found that when dehydrating a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, by mixing the composition containing a fluorine-containing hydrocarbon compound such as HFC-134a with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio (molar ratio) of 5 or more, or in contact with chabazite-type zeolite, with regard to the water adsorbed on the zeolite, even if the dehydration treatment time has passed, the release of water from the zeolite is suppressed, and the water is well removed (dehydrated) from the composition containing fluorine-based hydrocarbon compounds such as HFC-134a.

[0035] The present invention has been completed through further research based on such findings.

[0036] The present invention includes the following embodiments.

[0037] (1) Dehydration method of a composition containing a fluorinated hydrocarbon compound

[0038] The dehydration method of the composition containing fluorine-containing hydrocarbon compounds of the present invention comprises: mixing the composition containing fluorine-containing hydrocarbon compounds with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio is 5 or more zeolite contacting step.

[0039] The method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention comprises the step of contacting the fluorine-containing hydrocarbon compound composition with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite.

[0040] The method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention preferably further comprises a step of contacting the fluorine-containing hydrocarbon compound composition with the zeolite to remove 1,1,2,2-tetrafluoroethane (HFC-134).

[0041] In the dehydration method of a composition containing a fluorine-containing hydrocarbon compound of the present invention, the fluorine-containing hydrocarbon compound includes at least one compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf).

[0042] In the present invention, the above process is performed so that the maximum water content in the dehydrated composition is about 10 ppmwt (mass / mass), preferably less than 3 ppmwt. In the present invention, the minimum water content in the dehydrated composition is about 0.1 ppmwt.

[0043] In the present invention, the above process is set so that the maximum content of HFC-134 in the dehydrated composition is about 10 ppmwt (mass / mass), and preferably the content of HFC-134 is less than 3 ppmwt. In the present invention, the minimum content of HFC-134 in the dehydrated composition is about 0.1 ppmwt.

[0044] In the present invention, with regard to the above steps, it is more preferred that the moisture content in the dehydrated composition is less than 3 ppmwt, and the HFC-134 content is less than 3 ppmwt.

[0045] In addition, in the present invention, the content (ppm) of HFC-134 is, for example, the following value: when measuring by mass analysis by gas chromatography / mass spectrometry (GC / MS) using gas chromatography, and then structural analysis using NMR using NMR spectrum, the content (volume) of HFC-134 contained in the composition containing fluorine-based hydrocarbon compounds is divided by the volume of the composition containing fluorine-based hydrocarbon compounds to obtain the volume fraction, i.e., ppmvol (volume / volume).

[0046] For example, in other words, the HFC-134 content (ppm) is less than 3 ppmvol.

[0047] In the dehydration method of a composition containing fluorine-containing hydrocarbon compounds of the present invention, when dehydrating fluorine-containing hydrocarbon compounds such as HFC-134a, by using a specific zeolite, the water adsorbed to the zeolite is suppressed from being released from the zeolite even after the passage of time, which has the advantage of being able to well remove water from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a, and more preferably, the advantage of being able to well remove HFC-134 from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a.

[0048] (1-1) Composition containing fluorinated hydrocarbon compound

[0049] Fluorinated hydrocarbon compounds such as HFC-134a are used as etching gases for silicon oxide and related materials in the manufacture of semiconductors. Fluorinated hydrocarbon compounds such as HFC-134a used in the semiconductor industry require extremely high purity. For etching gases in semiconductor manufacturing processes, the removal of moisture is particularly important.

[0050] In the method for dehydrating a composition containing a fluorine-based hydrocarbon compound of the present invention, the fluorine-based hydrocarbon compound includes at least one compound selected from the group consisting of HFC-134a, HFC-125, HFC-32 and HFO-1234yf.

[0051] Compositions containing fluorinated hydrocarbon compounds such as HFC-134a contain impurities mixed in when producing fluorinated hydrocarbon compounds such as HFC-134a. Such impurities include intermediates, isomers, by-products (e.g., hydrogen fluoride, hydrofluorocarbons, hydrochlorofluorocarbons, chlorofluorocarbons, fluoroolefins, etc.).

[0052] In addition, the composition containing fluorinated hydrocarbon compounds such as HFC-134a contains impurities mixed in when using fluorinated hydrocarbon compounds such as HFC-134a. When fluorinated hydrocarbon compounds such as HFC-134a are used as etching gases for semiconductor manufacturing, the impurities include water, acid components such as HF, fluorinated hydrocarbons, non-condensable gases (N 2 , CO 2 , CO, CH4 , O 2 ) etc. When used as a refrigerant for a refrigerator, water is present as an impurity.

[0053] Compositions containing fluorinated hydrocarbon compounds such as HFC-134a contain 1,1,2,2-tetrafluoroethane (HFC-134) as impurities other than water.

[0054] If water, hydrogen fluoride, etc. are present as impurities in a composition containing a fluorinated hydrocarbon compound such as HFC-134a, the fluorinated compound may deteriorate (decompose, polymerize, isomerize, etc.) and fall into a vicious cycle that further reduces the purity, especially when the fluorinated compound is chemically unstable due to reasons such as having reactive sites such as double bonds.

[0055] In the present invention, the impurities removed by adsorption by zeolite include, in particular, impurities containing water, impurities containing hydrogen fluoride, impurities containing hydrocarbons, impurities containing halogenated carbon compounds, impurities containing halogenated hydrocarbon compounds (such as HFC-134), and impurities containing isomers of fluorine-containing compounds that come into contact with the zeolite, such as positional isomers of carbon-carbon double bonds, cyclic isomers, and the like.

[0056] Specific examples of the impurities include heptafluorobutene, chloroheptafluorobutene, methyl iodide, and chlorotrifluoroethylene.

[0057] In the semiconductor industry, it is particularly important to remove water from compositions containing fluorinated hydrocarbon compounds such as HFC-134a.

[0058] (1-2) Zeolite

[0059] The method for dehydrating a composition containing a fluorine-containing hydrocarbon compound of the present invention comprises a step of bringing the composition containing a fluorine-containing hydrocarbon compound such as HFC-134a into contact with a specific zeolite.

[0060] Zeolite is a type of clay mineral, and is composed of a rigid anionic skeleton having regular channels (tubular pores) and cavities (holes), and is a hydrous aluminosilicate containing an alkali or alkaline earth metal.

[0061] Zeolites are generally represented by the following composition, where the cations compensate for the negative charge of the aluminosilicate framework.

[0062] (M I ,M II 1 / 2 ) m (Al m Si n O 2(m+n) )·xH 2 O, (n≥m)

[0063] (M I :Li + 、Na + , K + etc., M II :Ca 2+ Mg 2+ , Ba 2+ wait)

[0064] There is no particular limitation on the type of cation in the zeolite, and H + , Li + 、Na + , K + , Ca 2+ Mg 2+ , Ba 2 + wait.

[0065] The basic unit of the structure is a tetrahedral structure of SiO4 or AlO4 (collectively referred to as TO4 tetrahedron), which is infinitely continuous in three dimensions to form a crystal. In zeolite, the crystal is porous, and the diameter of the pores is usually 0.2nm to 1.0nm. Zeolite has a molecular sieve effect that prevents molecules larger than the pore size of the zeolite from entering. In addition to the molecular sieve effect brought about by the pores of its skeleton structure, zeolite also has solid acidity, ion exchange performance, catalytic performance, adsorption performance and other characteristics.

[0066] In the present invention, contacting a composition containing a fluorinated hydrocarbon compound such as HFC-134a with a specific zeolite means passing the fluorinated hydrocarbon compound such as HFC-134a through a column filled with zeolite or filling the fluorinated hydrocarbon compound in a container filled with zeolite.

[0067] In the present invention, the use form of the zeolite used is not particularly limited. The composition containing fluorine-containing hydrocarbon compounds such as HFC-134a can be circulated in a device filled with zeolite, and the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a can be filled into a container filled with zeolite, and after a predetermined time, the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a after dehydration treatment is taken out.

[0068] The dehydration method of the composition containing fluorine-containing hydrocarbon compounds of the present invention comprises: mixing the composition containing fluorine-containing hydrocarbon compounds with the following silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more, and / or a step of contacting it with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite.

[0069] The ratio of silicon dioxide to aluminum oxide (SiO 2 / Al 2 O 3 Zeolite with a ratio of 5 or more

[0070] In the present invention, from the viewpoint of being able to efficiently perform dehydration treatment from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, and being able to well suppress the release of water from the zeolite even after the dehydration treatment time has passed, and from the viewpoint of being able to more efficiently remove HFC-134 from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, a zeolite having a ratio of silica to alumina (SiO 2 / Al 2 O 3 In the present invention, the SiO of the zeolite used is 5 or more. 2 / Al 2 O 3 The ratio is preferably 5.5 or more, more preferably 6 or more.

[0071] In the present invention, the SiO 2 / Al 2 O 3 The ratio is preferably 50 or less, more preferably 45 or less, and further preferably 40 or less.

[0072] In the present invention, SiO 2 / Al 2 O 3 When the ratio is less than 5, the polarity of the zeolite becomes high, and when it is greater than 50, the polarity of the zeolite becomes low. Therefore, it is preferable to use SiO 2 / Al 2 O 3 The ratio of zeolite is 5 to 50.

[0073] In the present invention, SiO 2 / Al 2 O 3 When the ratio is less than 5, the polarity of the zeolite becomes high. 2 / Al 2 O 3 When the ratio is greater than 50, the polarity of the zeolite becomes low, so it is preferred to use SiO 2 / Al 2 O 3 Zeolite with a ratio of 5 to 50.

[0074] (i) Chabazite-type zeolite

[0075] Chabazite (CHA) has a three-dimensional pore structure with a pore diameter of about 0.38 nm. There is a larger cage inside.

[0076] In the present invention, from the aspect that a dehydration treatment can be efficiently performed from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, even after the dehydration treatment time has passed, the release of water from the zeolite can be well suppressed, and from the aspect that HFC-134 can be more preferably efficiently removed from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, a chabazite type (CHA type) zeolite is used. In the present invention, a specific chabazite type zeolite can be used among commercially available products.

[0077] The genus Chabazite includes sodium chabazite type, erionite type, levynite type, chabazite type, and the like.

[0078] In the present invention, the so-called chabazite-type zeolite means a zeolite included in the genus Chabazite, and preferably a zeolite having at least one type selected from the group consisting of Chabazite-type, sodium Chabazite-type, erionite-type, and intercalated Chabazite-type is used. In the present invention, as the chabazite-type zeolite, it is more preferred to use a chabazite-type zeolite, or a mixed zeolite (synthetic zeolite) including chabazite-type and sodium Chabazite-type, erionite-type, and intercalated Chabazite-type, which are other chabazite-type zeolites, and it is further preferred to use a mixed zeolite (synthetic zeolite) including chabazite-type and erionite-type, which are other chabazite-type zeolites.

[0079] In the present invention, specifically, as the chabazite-type zeolite, it is preferred to use a synthetic zeolite whose crystal system is a mixture of natural minerals chabazite and erionite, that is, a mixture of a chabazite-type synthetic zeolite (chabazite-type zeolite) and an erionite-type synthetic zeolite (erionite-type zeolite).

[0080] The silica / alumina ratio (SiO 2 / Al 2 O 3 ) is usually about 2, but the silica / alumina ratio (SiO 2 / Al 2 O 3 ) is around 6.1 to 6.7.

[0081] (ii) Mordenite-type zeolite

[0082] Mordenite is also called morden zeolite, and its chemical formula is (Ca, K 2 ,Na 2 )〔AlSi 5 O 12 〕 2 7H 2 O, is a silicate mineral. Mordenite type zeolite structure is usually composed of SiO 4 and AlO 4The zeolite having a pore structure composed of oxygen 12-membered rings and oxygen 8-membered rings bonded by sharing oxygen has a pore diameter of about 0.67 nm×0.70 nm for oxygen 12-membered rings and about 0.29 nm×0.57 nm for oxygen 8-membered rings.

[0083] In the present invention, mordenite-type zeolite is used from the viewpoint that dehydration treatment can be efficiently performed from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a, and even after the dehydration treatment time has passed, the release of water from the zeolite can be well suppressed, and more preferably, HFC-134 can be efficiently removed from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a. In the present invention, a specific mordenite-type zeolite can be used from commercially available products.

[0084] (iii) β-zeolite

[0085] Beta zeolite is a type of crystalline aluminosilicate containing Si and Al, and has a three-dimensional pore structure including pores containing a 12-membered oxygen ring.

[0086] In the present invention, beta zeolite is used from the viewpoint that dehydration treatment can be efficiently performed from a composition containing fluorine hydrocarbon compounds such as HFC-134a, and even after the dehydration treatment time has passed, the release of water from the zeolite can be well suppressed, and more preferably, HFC-134 can be efficiently removed from a composition containing fluorine hydrocarbon compounds such as HFC-134a. In the present invention, a specific beta zeolite can be used among commercially available products.

[0087] (iv) Y-type zeolite

[0088] Y-type zeolite has pore entrances with a diameter of about 0.74 nm, and is the zeolite having the largest pores among commercially available zeolites.

[0089] In the present invention, Y-type zeolite is used from the viewpoint that dehydration treatment can be efficiently performed from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a, and even after the dehydration treatment time has passed, the release of water from the zeolite can be well suppressed, and more preferably, HFC-134 can be efficiently removed from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a. In the present invention, a specific Y-type zeolite can be used among commercially available products.

[0090] Pore ​​diameter of zeolite

[0091] In the present invention, from the viewpoint of being able to efficiently perform dehydration treatment from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, being able to well suppress the release of water from the zeolite even after the dehydration treatment time has passed, and from the viewpoint of being able to more efficiently remove HFC-134 from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, it is preferred to use a zeolite having In the present invention, the average pore diameter of the zeolite used is more preferably Particularly preferably, The average pore diameter of zeolite is

[0092] In the present invention, zeolite is preferably porous.

[0093] In the present invention, the average pore diameter of the zeolite used is When the fluorinated hydrocarbon compound contained in the composition is preferably a compound having 2 carbon atoms (C2 compound) to a compound having 8 carbon atoms (C8 compound), and more preferably a C2 compound to a C4 compound, it has the advantage of being able to efficiently carry out a dehydration treatment from a composition containing a fluorinated hydrocarbon compound such as HFC-134a, and more preferably being able to efficiently remove HFC-134 from a composition containing a fluorinated hydrocarbon compound such as HFC-134a.

[0094] Zeolite cation types

[0095] In the present invention, from the viewpoint of being able to efficiently perform dehydration treatment from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, and being able to well suppress the release of water from the zeolite even after the dehydration treatment time has passed, and from the viewpoint of being able to more efficiently remove HFC-134 from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, the cationic species (cationic species) of the zeolite that can be preferably used is preferably H + , Li + 、Na + , K + , Ca 2+ Mg 2+ , Ba 2+ etc., more preferably H + 、Na + Zeolites with the same cationic species as above.

[0096] In the present invention, the cations in the zeolite interact electrostatically with water, thereby making it possible to more efficiently perform the dehydration treatment.

[0097] Surface area of ​​zeolite

[0098] In the present invention, from the viewpoint of being able to efficiently perform dehydration treatment from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, and being able to well suppress the release of water from the zeolite even after the dehydration treatment time has passed, and from the viewpoint of being able to more efficiently remove HFC-134 from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, the specific surface area of ​​the zeolite measured by the BET method (hereinafter also referred to as the BET specific surface area) is preferably 50 m 2 / g~3,000m 2 / g, more preferably 100m 2 / g~1,000m 2 / g, more preferably 200m 2 / g~800m 2 / g, particularly preferably 250m 2 / g~700m 2 / g.

[0099] In the present invention, when the BET specific surface area of ​​the zeolite catalyst is within such a range, the density of the zeolite particles will not be too small, and therefore, there is an advantage of being able to efficiently perform a dehydration treatment, and more preferably, an advantage of being able to efficiently remove HFC-134 from a composition containing a fluorinated hydrocarbon compound such as HFC-134a.

[0100] Properties of Zeolite

[0101] The zeolite used in the present invention is preferably porous.

[0102] In the present invention, the zeolite used can be used in powder, granular, or pellet form, or can be used as a molded body. The zeolite used is preferably used as a molded body in industry. The shape of the molded body is not particularly limited, for example, a cylindrical molded body with a diameter of about 0.5 mm to 5 mm and a length of about 1 mm to 15 mm, or a spherical molded body with a diameter of about 0.5 mm to 10 mm is preferably used.

[0103] In the present invention, the method for producing the zeolite molded body is not particularly limited, and for example, a conventionally known method using kaolin-based clay as a binder can be employed.

[0104] The zeolite used in the present invention can be obtained through commercial channels.

[0105] Preferred zeolites

[0106] In the present invention, from the viewpoint that a dehydration treatment can be efficiently performed from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, and that the release of water from the zeolite can be well suppressed even after the dehydration treatment time has passed, and from the viewpoint that HFC-134a can be more efficiently removed from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a, it is preferred to use a zeolite having a ratio of 1:1 silica to 1:1 (SiO 2 / Al 2 O 3 The present invention relates to a zeolite having a molar ratio (ratio) of 5 or more and at least one zeolite selected from the group consisting of chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite.

[0107] (1-3) Step of contacting a composition containing a fluorinated hydrocarbon compound with zeolite

[0108] The dehydration method of the composition containing fluorine-containing hydrocarbon compounds of the present invention comprises: mixing the composition containing fluorine-containing hydrocarbon compounds with silicon dioxide alumina (SiO 2 / Al 2 O 3 The dehydration method preferably further comprises the step of contacting the composition containing the fluorine-containing hydrocarbon compound with the zeolite to remove HFC-134.

[0109] In the present invention, bringing the composition into contact with the zeolite means passing the composition through a column or the like filled with the zeolite, or filling the composition in a container filled with the zeolite.

[0110] In the present invention, the zeolite is used as a water removing material (dehydrating agent), and the composition containing the fluorinated hydrocarbon compound is brought into contact with (passed through) the zeolite to remove the water contained in the composition. The dehydration method preferably also removes HFC-134 contained in the composition.

[0111] In the present invention, in order to effectively remove water (dehydration), and further, preferably to effectively remove HFC-134, the composition containing fluorine-containing hydrocarbon compounds and the above-mentioned zeolite are preferably contacted at a mass ratio (composition containing fluorine-containing hydrocarbon compounds: zeolite) of about 100:1 to 1:10, more preferably at a ratio of about 50:1 to 1:5, and further preferably at a ratio of about 10:1 to 1:3. In the present invention, regarding the amount of the above-mentioned zeolite used, for example, the composition containing fluorine-containing hydrocarbon compounds can be contacted in a range of about 10g to 100g relative to 10g of the zeolite filling (stainless steel cylinder, etc.).

[0112] In the present invention, the zeolite may be activated before use. The activation conditions include: preferably in a vacuum (10 -1 mmHg~10 -3 mmHg), or a drying treatment such as heating overnight at a temperature in the range of 150°C to 300°C as a temperature range capable of maintaining the crystal structure of the zeolite under the flow of an inert gas such as nitrogen.

[0113] In the present invention, zeolite which has not been subjected to the above-mentioned activation treatment can also be suitably used.

[0114] In the present invention, the use form of the zeolite used is not particularly limited. The composition containing the fluorine-containing hydrocarbon compound can be circulated into the device filled with the above-mentioned zeolite, and the composition containing the fluorine-containing hydrocarbon compound can be filled into the container filled with the above-mentioned zeolite, and the above-mentioned composition can be taken out after a predetermined time.

[0115] In the present invention, the temperature at which the composition containing fluorine-containing hydrocarbon compounds is brought into contact with the above-mentioned zeolite is not particularly limited. It can be determined by taking into account the boiling point of fluorine-containing hydrocarbon compounds such as HFC-134a contained in the composition containing fluorine-containing hydrocarbon compounds. From the perspective of suppressing side reactions such as isomerization of fluorine-containing hydrocarbon compounds during contact, it is generally preferred to contact at low temperatures. Preferably, it is in the range of about -50°C to 100°C.

[0116] In the present invention, the time for which the composition containing a fluorine-based hydrocarbon compound is brought into contact with the zeolite is not particularly limited.

[0117] Preferred contacting process

[0118] In the dehydration method of the composition containing fluorine-containing hydrocarbon compounds of the present invention, the contacting step may be to contact the composition (i) containing fluorine-containing hydrocarbon compounds such as HFC-134a with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more, and (ii) contacting with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite, or (iii) contacting with silica-alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more, and a step of contacting with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite.

[0119] In the method for dehydrating a composition containing a fluorine-containing hydrocarbon compound of the present invention, the contacting step may be a step of contacting the composition (iv) containing a fluorine-containing hydrocarbon compound such as HFC-134a with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio is 5 or more and at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite is contacted.

[0120] (1-4) Contact process in gas phase

[0121] In the method for dehydrating a composition containing a fluorine-containing hydrocarbon compound, the composition containing a fluorine-containing hydrocarbon compound is mixed with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more, a step of contacting with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite, and / or a step of contacting with silica-alumina (SiO 2 / Al 2 O 3 In the step of contacting the zeolite with at least one zeolite selected from the group consisting of chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite with a ) ratio of 5 or more, the step is preferably carried out in a gas phase.

[0122] In the dehydration method of the composition containing fluorine-based hydrocarbon compounds of the present invention, the contacting step is preferably carried out in the gas phase, particularly in a gas phase continuous flow method using a fixed bed reactor. When the gas phase continuous flow method is carried out, the device, operation, etc. can be simplified and it is also economically advantageous.

[0123] Temperature of the contact process in the gas phase

[0124] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, the temperature at which the fluorine-containing hydrocarbon compound composition is brought into contact with the specific zeolite in a gas phase is not particularly limited.

[0125] In the above-mentioned contact step in the present invention, the lower limit of the contact temperature in the gas phase is preferably -30°C, and more preferably -20°C, from the perspective of being able to efficiently carry out dehydration treatment from the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a and being able to well suppress the release of water from the zeolite even after the dehydration treatment time has passed, and from the perspective of being able to more efficiently remove HFC-134 from the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a.

[0126] In the contact step of the present invention, the upper limit of the contact temperature in the gas phase is about 100°C.

[0127] In the contact step of the present invention, the contact temperature in the gas phase is preferably low temperature because of strong adsorption. In the contact step of the present invention, the contact temperature in the gas phase is most preferably room temperature in consideration of the operation and handling of the equipment.

[0128] Time of the contact process in the gas phase

[0129] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, the time for which the fluorine-containing hydrocarbon compound composition is brought into contact with the specific zeolite in the gas phase is not particularly limited.

[0130] In the dehydration method of a composition containing fluorine-containing hydrocarbon compounds of the present invention, when carried out in the gas phase, by appropriately adjusting the reaction temperature and reaction time (contact time) of the above-mentioned contact, it is possible to efficiently carry out dehydration treatment from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a, and even after the dehydration treatment time has passed, it is possible to well suppress the release of water from the zeolite, and more preferably, it is possible to efficiently remove HFC-134 from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a.

[0131] Pressure of the contact process in the gas phase

[0132] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, the pressure at which the fluorine-containing hydrocarbon compound composition is brought into contact with a specific zeolite in a gas phase is not particularly limited.

[0133] In the step of carrying out the chlorination reaction of the present invention, the contact pressure is preferably -0.05 MPa to 2 MPa, more preferably -0.01 MPa to 1 MPa, and further preferably normal pressure to 0.5 MPa, from the viewpoint of being able to efficiently carry out dehydration treatment from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a and being able to well suppress the release of water from the zeolite even after the dehydration treatment time has passed, and from the viewpoint of being able to more efficiently remove HFC-134 from a composition containing a fluorine-containing hydrocarbon compound such as HFC-134a.

[0134] In the present invention, when there is no indication regarding pressure, it is assumed to be gauge pressure.

[0135] Container for contact process in gas phase

[0136] In the dehydration method of the composition containing fluorine hydrocarbon compounds of the present invention, as a reactor for contacting the composition containing fluorine hydrocarbon compounds with a specific zeolite in the gas phase, as long as it can withstand the above temperature and pressure, the shape and structure are not particularly limited. As the above reactor, for example, a vertical reactor, a horizontal reactor, a multi-tube reactor, etc. can be listed. As the material of the reactor, for example, glass, stainless steel, iron, nickel, iron-nickel alloy, etc. can be listed.

[0137] Example of contact step in gas phase

[0138] In the dehydration method of the composition containing fluorine-containing hydrocarbon compounds of the present invention, the composition containing fluorine-containing hydrocarbon compounds is continuously contacted with a specific zeolite in the above reactor in the gas phase, and the dehydrated fluorine-containing hydrocarbon compounds are continuously taken out from the reactor in either a flow-through method or a batch method. It is preferably implemented in a flow-through method so that the dehydrated fluorine-containing hydrocarbon compounds do not remain in the reactor.

[0139] In the dehydration method of the composition containing fluorine-containing hydrocarbon compounds of the present invention, it is preferred to carry out the step of contacting the composition containing fluorine-containing hydrocarbon compounds with a specific zeolite in the gas phase, especially in a gas phase continuous flow type using a fixed bed reactor. When the gas phase continuous flow type is carried out, the device, operation, etc. can be simplified, and it is also economically advantageous.

[0140] In the dehydration method of the composition containing fluorine hydrocarbon compounds of the present invention, the atmosphere when the dehydration treatment is carried out in the gas phase can be carried out in the presence of an inert gas from the perspective of suppressing the deterioration of the zeolite. The inert gas is preferably at least one selected from nitrogen, helium, argon and carbon dioxide. Among these inert gases, nitrogen is more preferred from the perspective of suppressing costs. The concentration of the inert gas is preferably set to 0 to 50 mol% of the gas component introduced into the reactor.

[0141] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, the dehydration treatment is preferably performed in the absence of an inert gas as the atmosphere in the gas phase.

[0142] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, the fluorine-containing hydrocarbon compound composition is brought into contact with a specific zeolite in a gas phase and then, if necessary, purified by a conventional method to obtain a dehydrated fluorine-containing hydrocarbon compound.

[0143] In the dehydration method of a composition containing fluorine-containing hydrocarbon compounds of the present invention, by bringing the above-mentioned composition containing fluorine-containing hydrocarbon compounds into contact with a specific zeolite in a gas phase, it is possible to efficiently perform a dehydration treatment from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a, and even after the dehydration treatment time has passed, it is possible to well suppress the release of water from the zeolite, and more preferably, it is possible to efficiently remove HFC-134 from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a.

[0144] (1-5) Contact process in liquid phase

[0145] In the present invention, in the dehydration method of the composition containing fluorine-containing hydrocarbon compounds, the composition containing fluorine-containing hydrocarbon compounds is mixed with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more, a step of contacting with chabazite-type zeolite, and / or a step of contacting with silica alumina (SiO 2 / Al 2 O 3 In the step of contacting the chabazite-type zeolite with a carbonyl group-containing zeolite having a carbonyl group-containing zeolite ratio of 5 or more, the step is preferably carried out in a liquid phase.

[0146] Solvent for the contact process in the liquid phase

[0147] In the dehydration method of the fluorine-containing hydrocarbon compound composition of the present invention, when the method is carried out in a liquid phase, a solvent is not particularly required if the fluorine-containing hydrocarbon compound is in a liquid state.

[0148] Temperature of the contact process in the liquid phase

[0149] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, the temperature at which the fluorine-containing hydrocarbon compound composition is brought into contact with the specific zeolite in a liquid phase is not particularly limited.

[0150] In the above-mentioned contact step of the present invention, the lower limit of the contact temperature in the liquid phase is preferably -30°C, and more preferably -20°C, from the perspective of being able to efficiently carry out dehydration treatment from the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a and being able to well suppress the release of water from the zeolite even after the dehydration treatment time has passed, and from the perspective of being able to more efficiently remove HFC-134 from the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a.

[0151] In the contact step of the present invention, the upper limit of the contact temperature in the liquid phase is about 100°C.

[0152] In the contact step of the present invention, the contact temperature in the liquid phase is preferably low temperature because of strong adsorption. In the contact step of the present invention, the contact temperature in the liquid phase is most preferably room temperature in consideration of the operation and handling of the equipment.

[0153] Pressure of the contact process in the liquid phase

[0154] In the dehydration method of the composition containing fluorine hydrocarbon compounds of the present invention, there is no limitation on the reactor as long as the composition containing fluorine hydrocarbon compounds can be brought into contact with a specific zeolite in the liquid phase. The liquid phase conditions can be any conditions as long as the composition containing fluorine hydrocarbon compounds can be well liquefied, and can be a reaction under the saturated vapor pressure of the fluorine hydrocarbon compounds.

[0155] Closed reaction system and / or pressurized reaction system in liquid phase

[0156] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, there is no particular limitation on the pressure in the reactor as long as the fluorine-containing hydrocarbon compound composition can be brought into contact with a specific zeolite in a liquid phase.

[0157] In the dehydration method of the composition containing fluorine-containing hydrocarbon compounds of the present invention, the step of contacting the composition containing fluorine-containing hydrocarbon compounds with a specific zeolite in a liquid phase is preferably carried out in a closed reaction system and / or a pressurized reaction system from the viewpoint that the dehydration treatment can be efficiently carried out from the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a, and the release of water from the zeolite can be well suppressed even after the dehydration treatment time has passed, and from the viewpoint that HFC-134a can more preferably be efficiently removed from the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a.

[0158] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, the shape and structure of the reactor for contacting the fluorine-containing hydrocarbon compound composition with the specific zeolite in a liquid phase is not particularly limited as long as it can withstand the reaction.

[0159] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, it is preferred to use a batch-type pressure-resistant reaction vessel as a closed reaction system in a liquid phase to seal the reaction system and conduct the reaction.

[0160] In the dehydration method of the fluorine-containing hydrocarbon compound composition of the present invention, the reaction pressure is preferably set to be equal to or higher than the saturated vapor pressure of the target fluorine-containing hydrocarbon compound as a pressurized reaction system in a liquid phase to enable liquefaction.

[0161] In the present invention, unless otherwise specified, the reaction pressure is a gauge pressure.

[0162] In the dehydration method of the composition containing fluorine hydrocarbon compounds of the present invention, in the closed reaction system and / or pressurized reaction system in the liquid phase, there is no restriction on the reactor. For example, it is preferred to put the above-mentioned composition containing fluorine hydrocarbon compounds into a pressure vessel such as an autoclave, heat it to an appropriate reaction temperature with a heater, and react for a certain time under stirring. As the material of the reactor, for example, glass, stainless steel, iron, nickel, iron-nickel alloy, etc. can be listed. As the reaction atmosphere, it is preferred to react in an atmosphere of inert gases such as nitrogen, helium, carbonic acid gas. For example, it is preferred to use a batch-type pressure-resistant reaction vessel (autoclave, etc.) to make the reaction system airtight and react. As the material of the reactor, for example, glass, stainless steel, iron, nickel, iron-nickel alloy, etc. can be listed.

[0163] In the dehydration method of the composition containing fluorine hydrocarbon compounds of the present invention, the reaction pressure of the pressurized reaction system in the liquid phase is the pressure inside the reaction container used for the pressurized reaction system. In the dehydration method of the composition containing fluorine hydrocarbon compounds of the present invention, regarding the reaction pressure of bringing the composition containing fluorine hydrocarbon compounds into contact with a specific zeolite, it is preferred to react under conditions that enable liquefaction, more preferably at a pressure of 0.5 MPa or more, further preferably at a pressure of 0.7 MPa or more, and particularly preferably at a pressure of 1.0 MPa or more, from the perspective of being able to efficiently perform dehydration treatment from the composition containing fluorine hydrocarbon compounds such as HFC-134a, and being able to well suppress the release of water from the zeolite even after the dehydration treatment time has passed.

[0164] In the dehydration method of the composition containing fluorine hydrocarbon compounds of the present invention, from the same aspect as above, the upper limit of the reaction pressure for contacting the composition containing fluorine hydrocarbon compounds with a specific zeolite in the liquid phase is usually about 1.0 MPa. Regarding pressurization, the pressure in the reaction system can be increased by introducing an inert gas such as nitrogen, helium, carbon dioxide, etc. into the reaction system.

[0165] In the dehydration method of the composition containing fluorine-containing hydrocarbon compounds of the present invention, in the step of contacting the above-mentioned composition containing fluorine-containing hydrocarbon compounds with a specific zeolite in the liquid phase, the liquid can be taken out while the product is vaporized and taken out by connecting a back pressure valve to a continuous phase tank reactor (CSTR), etc., so as to carry out the reaction in a continuous and pressurized manner.

[0166] In the method for dehydrating a fluorine-containing hydrocarbon compound composition of the present invention, the fluorine-containing hydrocarbon compound composition is brought into contact with a specific zeolite in a liquid phase and then, if necessary, purified by a conventional method to obtain a dehydrated fluorine-containing hydrocarbon compound.

[0167] In the dehydration method of a composition containing fluorine-containing hydrocarbon compounds of the present invention, by contacting the above-mentioned composition containing fluorine-containing hydrocarbon compounds with a specific zeolite in a liquid phase in a closed reaction system and / or a pressurized reaction system, it has the advantages of being able to efficiently perform a dehydration treatment from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a, and being able to well suppress the release of water from the zeolite even after the dehydration treatment time has passed, and more preferably being able to efficiently remove HFC-134 from a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a. (1-6) The moisture content and / or HFC-134 content is lower than 3ppmwt

[0168] According to the dehydration method of the composition containing fluorine-containing hydrocarbon compounds of the present invention, when dehydrating the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a, the above-mentioned silica alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more, and / or at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite, can suppress the release of water adsorbed to the zeolite even after the passage of time.

[0169] According to the dehydration method of the composition containing fluorine hydrocarbon compounds of the present invention, in the dehydrated composition, that is, in the composition after contact with the above-mentioned zeolite, the water content in the composition containing fluorine hydrocarbon compounds such as HFC-134a can be lower than about 10ppmwt (mass / mass), preferably lower than about 3ppmwt. In the present invention, the minimum value of the water content in the dehydrated composition is about 0.1ppmwt.

[0170] According to the dehydration method of the composition containing fluorine hydrocarbon compounds of the present invention, in the dehydrated composition, that is, in the composition after contact with the above-mentioned zeolite, the content of HFC-134 in the composition containing fluorine hydrocarbon compounds such as HFC-134a can be made lower than about 10ppmwt (mass / mass), preferably lower than about 3ppmwt. In the present invention, in the dehydrated composition, the minimum content of HFC-134 is about 0.1ppmwt.

[0171] According to the method for dehydrating a composition containing a fluorine-containing hydrocarbon compound of the present invention, it is more preferable to reduce the water content in the composition containing a fluorine-containing hydrocarbon compound such as HFC-134a to less than about 3 ppmwt and reduce the HFC-134 content to less than about 3 ppmwt.

[0172] According to the present invention, by effectively dehydrating (removing) the water content in the composition containing fluorine-based hydrocarbon compounds such as HFC-134a, the fluorine-based hydrocarbon compounds such as HFC-134a from which the water has been dehydrated (removed), more preferably the fluorine-based hydrocarbon compounds such as HFC-134a from which HFC-134 has been removed, can be suitably used as etching gas for semiconductor manufacturing. In addition, corrosion and early degradation of the device can also be suppressed.

[0173] (2) Method for producing a composition containing a fluorinated hydrocarbon compound

[0174] In the method for producing a composition containing a fluorine-containing hydrocarbon compound of the present invention, the fluorine-containing hydrocarbon compound comprises at least one compound selected from HFC-134a, HFC-125, HFC-32 and HFO-1234yf, and the method comprises reacting the composition containing the fluorine-containing hydrocarbon compound with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio is 5 or more zeolite contacting step.

[0175] In the method for producing a composition containing a fluorine-containing hydrocarbon compound of the present invention, the fluorine-containing hydrocarbon compound comprises at least one compound selected from HFC-134a, HFC-125, HFC-32 and HFO-1234yf, and the method comprises the step of contacting the composition containing the fluorine-containing hydrocarbon compound with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite.

[0176] Preferably, the method for producing a fluorine-containing hydrocarbon compound composition of the present invention further comprises a step of contacting the fluorine-containing hydrocarbon compound composition with the zeolite to remove HFC-134.

[0177] The step of bringing the fluorinated hydrocarbon compound-containing composition into contact with various zeolites can employ the step in the above-described dehydration method.

[0178] In the method for producing a composition containing a fluorine-containing hydrocarbon compound of the present invention, the moisture content of the composition after contacting with the zeolite is less than about 10 ppmwt, preferably less than about 3 ppmwt. In the present invention, the minimum value of the moisture content in the composition is about 0.1 ppmwt.

[0179] In the method for producing a composition containing a fluorine-containing hydrocarbon compound of the present invention, the content of HFC-134 in the composition after contacting with the above-mentioned zeolite is less than about 10 ppmwt, preferably less than about 3 ppmwt. In the present invention, the minimum content of HFC-134 in the above-mentioned composition is about 0.1 ppmwt.

[0180] In the method for producing a fluorine-containing hydrocarbon compound composition of the present invention, the composition after contacting with the zeolite preferably has a moisture content of less than about 3 ppmwt and an HFC-134 content of less than about 3 ppmwt.

[0181] The production method of the present invention is a production method of a high-purity fluorine-based hydrocarbon compound, characterized in that it comprises the steps of: mixing at least one fluorine-based hydrocarbon compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf) with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio is 5 or more to remove impurities contained in the fluorinated hydrocarbon compound.

[0182] The manufacturing method of the present invention is a manufacturing method for high-purity fluorine-based hydrocarbon compounds, characterized in that it includes a step of contacting at least one fluorine-based hydrocarbon compound selected from 1,1,1,2-tetrafluoroethane (HFC-134a), 1,1,1,2,2-pentafluoroethane (HFC-125), difluoromethane (HFC-32) and 2,3,3,3-tetrafluoropropylene (HFO-1234yf) with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite to remove impurities contained in the fluorine-based hydrocarbon compound.

[0183] The impurities are preferably at least one component selected from the group consisting of water and HFC-134.

[0184] The step of bringing the fluorinated hydrocarbon compound-containing composition into contact with various zeolites can employ the step in the above-described dehydration method.

[0185] In the manufacturing method of the present invention, the impurities removed are, for example, the water described above. Regarding the water concentration contained in the fluorine hydrocarbon compound after the impurities are removed, the water content is less than about 10ppmwt, preferably less than about 3ppmwt. In the present invention, the minimum value of the water content is about 0.1ppmwt.

[0186] In the manufacturing method of the present invention, the impurities to be removed are, for example, the HFC-134 described above. With regard to the concentration of HFC-134 contained in the fluorine-based hydrocarbon compound after the impurities are removed, the content of HFC-134 is less than about 10 ppmwt, preferably less than about 3 ppmwt. In the present invention, the minimum content of HFC-134 is about 0.1 ppmwt.

[0187] The water content and HFC-134 content in the fluorinated hydrocarbon compound after the above impurities have been removed are more preferably less than about 3 ppmwt of water and less than about 3 ppmwt of HFC-134.

[0188] In the present invention, in the above step, it is preferred that water is adsorbed on the above zeolite from the composition containing the fluorine-containing hydrocarbon compound to dehydrate the composition before contacting the zeolite. In the present invention, in the above step, it is even more preferred to remove HFC-134 from the composition containing the fluorine-containing hydrocarbon compound.

[0189] In the method for producing a composition containing a fluorine-containing hydrocarbon compound of the present invention, the contacting step may be to contact the composition containing a fluorine-containing hydrocarbon compound such as HFC-134a with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more, and at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite. 2 / Al 2 O 3 ) ratio of 5 or more, and a step of contacting with at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite.

[0190] In the method for producing a composition containing a fluorine-containing hydrocarbon compound of the present invention, the contacting step may be to contact the composition containing a fluorine-containing hydrocarbon compound such as HFC-134a with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio is 5 or more and at least one zeolite selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite is contacted.

[0191] In the present invention, the water content in the composition after contacting the zeolite, particularly in the composition containing a fluorinated hydrocarbon compound such as HFC-134a, can be preferably reduced to less than 3 ppmwt.

[0192] In the present invention, the content of HFC-134 in the composition after contacting the zeolite, particularly in the composition containing a fluorinated hydrocarbon compound such as HFC-134a, can be preferably reduced to less than 3 ppmwt.

[0193] In the method for producing a composition containing fluorine-containing hydrocarbon compounds of the present invention, the composition containing fluorine-containing hydrocarbon compounds to be dehydrated, the zeolite used, the step of contacting the composition containing fluorine-containing hydrocarbon compounds with the zeolite, the contact step in the gas phase, the contact step in the liquid phase, making the water content less than 3ppmwt, making the HFC-134 content less than 3ppmwt, etc. are as described in the above-mentioned method for dehydrating a composition containing fluorine-containing hydrocarbon compounds of the present invention.

[0194] (3) Compositions containing fluorinated hydrocarbon compounds

[0195] In the fluorine-containing hydrocarbon compound composition of the present invention, the fluorine-containing hydrocarbon compound includes at least one compound selected from HFC-134a, HFC-125, HFC-32 and HFO-1234yf, and the water content is less than 3 ppmwt.

[0196] In the fluorine-containing hydrocarbon compound composition of the present invention, the fluorine-containing hydrocarbon compound comprises at least one compound selected from HFC-134a, HFC-125, HFC-32 and HFO-1234yf, and the content of HFC-134 is less than 3 ppmwt.

[0197] The fluorine-containing hydrocarbon compound composition of the present invention more preferably has a moisture content of less than 3 ppmwt and an HFC-134 content of less than 3 ppmwt.

[0198] Determination of water content

[0199] The moisture content of the composition containing fluorine-containing hydrocarbon compounds of the present invention is the moisture content measured using a Karl Fischer titrator, and is the moisture content obtained based on the Karl Fischer method. Specifically, it refers to the value measured by titration by adding 1 g of the composition containing fluorine-containing hydrocarbon compounds (liquefied gas) to the Karl Fischer titrator, trapping water in the solvent.

[0200] The moisture content (ppm) is a mass fraction obtained by dividing the moisture content (mass) contained in the composition containing a fluorine-containing hydrocarbon compound by the mass of the composition containing a fluorine-containing hydrocarbon compound, that is, ppmwt (mass / mass).

[0201] Determination of HFC-134 content

[0202] The HFC-134 content of the fluorine-based hydrocarbon compound-containing composition of the present invention can be measured based on mass analysis and structural analysis.

[0203] The HFC-134 content of the composition containing a fluorine-based hydrocarbon compound of the present invention can be measured, for example, by mass analysis by gas chromatography / mass spectrometry (GC / MS) using a gas chromatograph (e.g., manufactured by Shimadzu Corporation, trade name "GC-2014"), and then by structural analysis using an NMR spectrum using an NMR spectrum (e.g., manufactured by JEOL, trade name "400YH").

[0204] In the present invention, the HFC-134 content (ppm) when using these devices is the volume fraction obtained by dividing the HFC-134 content (volume) contained in the composition containing the fluorine-containing hydrocarbon compound by the volume of the composition containing the fluorine-containing hydrocarbon compound, that is, ppmvol (volume / volume).

[0205] In other words, the content (ppm) of HFC-134 can be expressed as, for example, less than 3 ppmvol.

[0206] The composition containing a fluorine-based hydrocarbon compound of the present invention is preferably used as an etching gas, a refrigerant or a heat transfer medium for forming the most advanced microstructures such as semiconductors and liquid crystals, similar to HFC-134a, HFC-125, HFC-32, HFO-1234yf, etc. In addition, the composition containing a fluorine-based hydrocarbon compound of the present invention can be effectively used in various applications such as deposition gas, building blocks for organic synthesis, and cleaning gas in addition to being used as an etching gas.

[0207] The fluorine-containing hydrocarbon compound composition of the present invention is preferably used as an etching gas, a refrigerant, a heat transfer medium, a deposition gas, a building block for organic synthesis, or a cleaning gas.

[0208] The above-mentioned deposition gas is a gas for depositing an etching resistant polymer layer.

[0209] The organic synthesis building block is a substance that can be a precursor of a compound having a highly reactive skeleton. 3 Si(CH 3 ) 3 Fluorine-containing organic silicon compounds react to introduce CF 3 The fluoroalkyl radicals such as fluoroalkyl radicals can be converted into substances that can become cleaning agents and fluorinated pharmaceutical intermediates.

[0210] Although the embodiments of the present invention have been described above, various modifications may be made to the embodiments and details without departing from the spirit and scope of the claims.

[0211] Example

[0212] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to these Examples in any way.

[0213] Determination of water content in compositions containing fluorinated hydrocarbon compounds

[0214] The moisture content was measured using the following measuring apparatus, conditions, and method.

[0215] Measuring device: Karl Fischer titrator

[0216] Determination conditions: Coulometric titration

[0217] The moisture content of the composition containing a fluorinated hydrocarbon compound is the moisture content measured using a Karl Fischer titrator, and is the moisture content obtained by a coulometric titration method based on the Karl Fischer method. Specifically, 1 g of the composition containing a fluorinated hydrocarbon compound is put into the Karl Fischer titrator, and moisture is collected in a solvent, and the value measured by the titration method is used.

[0218] The moisture content (ppm) is a mass fraction obtained by dividing the moisture content (mass) contained in the composition containing a fluorine-containing hydrocarbon compound by the mass of the composition containing a fluorine-containing hydrocarbon compound, that is, ppmwt (mass / mass).

[0219] (1) Dehydration method of the composition containing fluorine-containing hydrocarbon compound of the embodiment (liquid phase)

[0220] Fluorinated hydrocarbon compounds: HFC-134a

[0221] The composition containing HFC-134a is mixed with silica alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more, chabazite-type zeolite (Example 1), mordenite-type zeolite (Example 2), β-type zeolite (Example 3), or Y-type zeolite (Example 4).

[0222] A stainless steel cylinder with a capacity of 75 mL was filled with 1 g of each zeolite (dehydrating agent) shown in Table 1. A composition containing a predetermined amount (10 g) of HFC-134a was filled in the cylinder. The mixture was stirred appropriately, and the water content of the liquid phase was measured by Karl Fischer method 24 hours (24 hr), 48 hours (48 hr), 72 hours (72 hr), and 96 hours (96 hr) after the start of dehydration (0 hr).

[0223] [Table 1]

[0224]

[0225] The moisture content of the composition after contacting with each zeolite of the examples was less than 3 ppmwt. 2 / Al2 O 3 When a chabazite-type zeolite having a ) ratio of 5 or more was used as a dehydrating agent, water was not released from the zeolite even after a period of time, and no increase in the water content in the composition containing HFC-134a was observed.

[0226] (2) Dehydration method of the fluorinated hydrocarbon compound-containing composition of the comparative example (liquid phase)

[0227] The composition containing HFC-134a is mixed with silica alumina (SiO 2 / Al 2 O 3 ) ratio is lower than 5 and is not a chabazite-type zeolite.

[0228] A stainless steel cylinder with a capacity of 75 mL was filled with 1 g of each zeolite (dehydrating agent) shown in Table 2. A composition containing a predetermined amount (10 g) of HFC-134a was filled in the cylinder. The mixture was stirred appropriately, and the water content of the liquid phase was measured by Karl Fischer method 24 hours (24 hr), 48 hours (48 hr), 72 hours (72 hr), and 96 hours (96 hr) after the start of dehydration (0 hr).

[0229] [Table 2]

[0230]

[0231] The composition after contact with each zeolite of the comparative example had a moisture content exceeding 3 ppmwt. 2 / Al 2 O 3 ) ratio of about 2 was used as a dehydrating agent, it was confirmed that the adsorbed water was released from the zeolite over time, and the water content in the composition containing HFC-134a increased.

[0232] (3) Method for dehydrating a composition containing a fluorinated hydrocarbon compound in a gas phase

[0233] Fluorinated hydrocarbon compounds: HFC-134a

[0234] This HFC-134a is a sample containing 5 ppmwt (mass / mass) of water.

[0235] The zeolites (molecular sieves (MS)) used were heated in vacuum (10 -1 mmHg~10 - 3 The zeolite was heated at 180° C. (mmHg) to remove water from the zeolite, thereby performing an activation treatment (pretreatment).

[0236] The composition (gas) containing HFC-134a is mixed with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more chabazite-type zeolite (Example 8), and silica alumina (SiO 2 / Al 2 O 3 ) ratio is less than 5 and is not a chabazite type A zeolite (Comparative Examples 9 and 10). Regarding the dehydration method in the gas phase, a gas containing HFC-134a is passed through the zeolite layer under the conditions of W / F=0.2 to 0.6 g / (cc / sec) and a flow rate of HFC-134a: 1.7 cm / sec.

[0237] [Table 3]

[0238]

[0239] The zeolite of Example 8 efficiently removed water from the composition (gas) containing HFC-134a in a short time. In addition, by subjecting the used zeolite to an activation treatment (pretreatment) before use, water was removed from the composition (gas) containing HFC-134a more efficiently and in a short time.

[0240] On the other hand, each of the zeolites of Comparative Examples 9 and 10 could not efficiently remove water from the composition (gas) containing HFC-134a.

[0241] (4) Method for removing HFC-134 from a composition containing fluorinated hydrocarbon compounds in a gas phase

[0242] Fluorinated hydrocarbon compounds: HFC-134a

[0243] This HFC-134a is a sample containing 5 ppmwt (mass / mass) of water and 500 ppmvol (volume / volume) of HFC-134.

[0244] The zeolite (molecular sieves (MS)) used was heated in vacuum (10 -1 mmHg~10 -3 The zeolite is heated at 180°C (0.4777 in 1000 μm) to remove water from the zeolite, thereby performing an activation treatment (pretreatment).

[0245] The composition (gas) containing HFC-134a is mixed with silicon dioxide alumina (SiO 2 / Al 2 O 3 ) ratio of 5 or more chabazite-type zeolite (Example 11), and silica alumina (SiO 2 / Al 2 O3 ) ratio is less than 5 and is not a chabazite type A zeolite (Comparative Examples 12 and 13). Regarding the method of removing HFC-134 in the gas phase, a gas containing HFC-134a is passed through the zeolite layer under the condition of W / F=100 g / (cc / sec) until the HFC-134 concentration is detected at the outlet.

[0246] [Table 4]

[0247]

[0248] For the zeolite of Example 11, even when a composition (gas) containing HFC-134a was circulated under the condition of W / F=100 g / (cc / sec) for 12 hours, there was no breakthrough and HFC-134 was not detected. The zeolite of Example 11 was able to remove HFC-134 efficiently in a short time. At this time, no water was detected. In addition, by subjecting the used zeolite to an activation treatment (pretreatment) before its use, HFC-134 was removed from the composition (gas) containing HFC-134a more efficiently and in a short time.

[0249] On the other hand, each zeolite of Comparative Examples 12 and 13 was penetrated within 6 minutes, HFC-134 was detected, and the amount detected continued to increase. Each zeolite of Comparative Examples 12 and 13 could not efficiently remove HFC-134 from the composition (gas) containing HFC-134a.

[0250] (5) Description of Chabazite-type (A-like) Zeolite (MS) used in Examples

[0251] The chabazite-type (A-like) zeolite used in the examples is a synthetic zeolite A-type zeolite with 5A AlO 4 Replaced by SiO 4 , a zeolite whose crystal structure has the same crystal structure as chabazite.

[0252] The chabazite-type (A-similar type) zeolite used in the examples is a mixture of natural minerals chabazite and erionite according to the results of X-ray diffraction, that is, a synthetic zeolite that is a mixture of a chabazite-type synthetic zeolite (chabazite-type zeolite) and an erionite-type synthetic zeolite (erionite-type zeolite).

[0253] (6) Summary of Dehydration Methods for Compositions Containing Fluorinated Hydrocarbon Compounds

[0254] As semiconductor integrated circuit devices become faster and more highly integrated, circuit patterns are becoming increasingly miniaturized. Fluorinated hydrocarbon compounds such as HFC-134a are essential gases for etching the finest contact holes.

[0255] In the method for dehydrating a composition containing fluorine-containing hydrocarbon compounds and the method for producing a composition containing fluorine-containing hydrocarbon compounds of the present invention, the above-mentioned specific zeolite is used when dehydrating a composition containing fluorine-containing hydrocarbon compounds such as HFC-134a. This has the advantage that the water adsorbed to the zeolite is suppressed from being released from the zeolite after a period of time, and water can be well removed from the composition containing fluorine-containing hydrocarbon compounds such as HFC-134a.

[0256] According to the dehydration method of the composition containing fluorine hydrocarbon compounds and the manufacturing method of the composition containing fluorine hydrocarbon compounds of the present invention, the water content in the composition containing fluorine hydrocarbon compounds such as HFC-134a can be reduced to less than 3ppmwt. The composition containing fluorine hydrocarbon compounds (HFC-134a, etc.) with a water content less than 3ppmwt is advantageous in etching fine contact holes for semiconductor integrated circuit devices and forming fine circuit patterns.

Claims

1. A composition containing a fluorine-based hydrocarbon compound, characterized in that: The fluorinated hydrocarbon compound includes 1,1,1,2-tetrafluoroethane (HFC-134a), The content of HFC-134 is 0.1 ppmwt or more and less than 3 ppmwt.

2. A composition containing a fluorine-based hydrocarbon compound, characterized in that: The composition is a composition obtained by the following manufacturing method, The manufacturing method comprises the step of contacting the composition containing the fluorine-based hydrocarbon compound with at least one zeolite having a silica-alumina (SiO2 / Al2O3) ratio of 5.5 or more and selected from chabazite-type zeolite, mordenite-type zeolite, β-type zeolite and Y-type zeolite, The fluorinated hydrocarbon compound includes 1,1,1,2-tetrafluoroethane (HFC-134a), The content of HFC-134 is 0.1 ppmwt or more and less than 3 ppmwt, The composition contains HFC-134a in high purity.

3. The composition according to claim 1 or 2, characterized in that: The composition is used as an etching gas, a refrigerant, a heat transfer medium, a deposition gas, a building block for organic synthesis, or a cleaning gas.

Citation Information

Patent Citations

  • CTC collection system and CTC collection method

    JP2020044095A