Polypropylene / covalent organic framework hybrid hollow fiber oxygenation membrane with gradient structure and preparation method thereof
The hybrid hollow fiber oxygenated film with gradient structure was prepared by physical blending of covalent organic frame and polypropylene and thermally induced phase separation method, which solved the contradiction between plasma leakage and gas transmission performance of oxygenated films, and achieved efficient oxygen and carbon dioxide Transmission and prolonged anti-plasma leakage.
Patent Information
- Application Number
- CN202411022880.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing polypropylene oxygenated films are prone to plasma leakage during the oxygenation process, resulting in insufficient life of the oxygenated film and deterioration of gas transmission performance when improving anti-plasma leakage.
The covalent organic frame is physically blended with polypropylene, and a hybrid hollow fiber oxygenated film with a gradient structure is prepared by thermal phase separation. The covalent organic frame is distributed gradiently within the film, providing additional oxygen and carbon dioxide transmission channels. , and entangle with polypropylene molecular chains to improve mechanical properties.
The gas permeability and anti-plasma leakage of oxygen and carbon dioxide are significantly improved. The carbon dioxide transmission capacity is 9 times that of the prior art, the oxygen transmission capacity is 6 times, and the anti-plasma leakage time is extended to 124 hours.
Smart Images

Figure CN118925515A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of membrane technology, and specifically relates to a hybrid hollow fiber oxygenation membrane with a gradient structure based on a covalent organic framework and a preparation method thereof. Background Art
[0002] Extracorporeal Membrane Oxygenator (ECMO) is mainly used to provide continuous extracorporeal respiration and circulation for patients with severe cardiopulmonary failure, also known as artificial lung. The ideal ECMO membrane material should have high air permeability and good resistance to plasma leakage. Polypropylene (PP) has the advantages of low cost, high gas permeability, good biocompatibility and high surface hydrophobicity, and is one of the commercial oxygenation membrane materials. However, most of the PP membranes prepared by the prior art are homogeneous structures, and their high porosity and large pore surface are easily wetted by liquid, which increases the risk of plasma leakage and causes the life of the oxygenation membrane to be less than 6 hours. Therefore, unlike the homogeneous porous structure of the prior art, it is of great significance to develop a PP membrane with a gradient structure consisting of a dense cortex and a porous support layer to prevent plasma leakage while maintaining high gas permeability.
[0003] At present, covalent organic framework materials are developing rapidly. They have the characteristics of large specific surface area, high density of functional groups and high mechanical properties. They have water stability, high thermal stability, solvent stability, high mechanical properties and have interpenetrating, uniform, connected and stable regular mass transfer channels. They are widely used in separation systems. Their porous channels are conducive to the permeation of oxygen and carbon dioxide, and polar groups can interact with polar carbon dioxide; hybridizing two-dimensional covalent organic framework materials with polypropylene can make the covalent organic framework materials have a gradient distribution, increase the polymer concentration on the membrane surface, and provide additional channels for the rapid transmission of oxygen and carbon dioxide. The molecular chains of the two are intertwined to improve the mechanical properties of the oxygenation membrane, achieving the goal of improving the clinical performance of the hybrid hollow fiber oxygenation membrane.
[0004] Therefore, in view of the contradictory problems of gas permeability and plasma leakage resistance in the current commercial oxygenation membranes, the present invention prepares hybrid membranes by physically blending covalent organic frameworks with polypropylene via thermally induced phase separation (TIPS), which is expected to solve these problems and promote the development of the oxygenation membrane field. Summary of the invention
[0005] The purpose of the present application is to provide a hybrid hollow fiber oxygenation membrane with a gradient structure based on a covalent organic framework and a preparation method thereof, so as to solve the problem in the prior art that micropores exist on the surface of polypropylene oxygenation membranes and plasma leakage easily occurs during the oxygenation process.
[0006] To achieve the above purpose, a technical solution adopted in this application is:
[0007] Polypropylene / covalent organic framework hybrid hollow fiber oxygenation membrane with gradient structure; Hybrid hollow fiber oxygenation membrane is a hollow fiber oxygenation membrane based on the hybridization of covalent organic framework and polypropylene material. The oxygenation membrane is a gradient structure that gradually increases from the dense cortex on the surface to the loose porous main body. The covalent organic framework presents a gradient distribution in the membrane. The content gradually decreases from the surface to the main body. The schematic diagram of the membrane structure is shown in Figure 1 shown.
[0008] The preparation method of the polypropylene / covalent organic framework hybrid hollow fiber oxygenation membrane with a gradient structure comprises the following steps: firstly ultrasonically dispersing the covalent organic framework material for 5-20 minutes, then crushing the cells for 5-20 minutes and uniformly dispersing the materials in a diluent to obtain a dispersion liquid; then adding polypropylene to the dispersion liquid, heating and stirring the dispersion liquid and allowing the dispersion liquid to stand to obtain a casting liquid; and then using the casting liquid as a raw material and spinning the fibers by a thermally induced phase separation method to obtain a hybrid hollow fiber oxygenation membrane.
[0009] The mass ratio of the covalent organic framework material to polypropylene is (0.3-1.5):100.
[0010] The diluent comprises one or more combinations of dibutyl phthalate, dioctyl phthalate, trioctyl acetyl citrate, tributyl citrate and trioctyl citrate; the mass ratio of the covalent organic framework material to the diluent is (0.3-1.5):150.
[0011] The conditions for standing still after heating and stirring are: heating to 180-210° C. and stirring for 6-12 hours, stopping stirring and heating to 190-220° C. and standing still for degassing for 6-12 hours to obtain the casting solution.
[0012] The thermally induced phase separation spinning method is as follows: the casting liquid is kept at a constant temperature of 220-240°C, and the casting liquid is extruded through a spinneret and introduced into a water coagulation bath at room temperature for solidification and forming. The spinning speed is 40000-70000 mm / min, and the core liquid flow rate is 1.8-3 ml / min.
[0013] In the preparation method of the present invention, the hybrid hollow fiber oxygenation membrane is fully immersed in an extracting liquid to extract and remove the diluent, and then dried; the extracting liquid includes one or more of anhydrous ethanol, isopropanol, n-heptane, and n-hexane.
[0014] The polypropylene / covalent organic framework hybrid hollow fiber oxygenation membrane with a gradient structure of the present invention is used as an oxygenation membrane in the process of extracorporeal membrane oxygenation.
[0015] Different from the prior art, the beneficial effects of this application are:
[0016] 1. The hybrid dispersed covalent organic framework material in the hybrid hollow fiber oxygenation membrane of the present application has the characteristics of large specific surface area, high density functional groups and high mechanical properties. The covalent organic framework material in the hybrid hollow fiber oxygenation membrane of the present application is distributed in a gradient, which changes the membrane pore structure, so that the oxygenation membrane presents a gradient structure with dense surface and porous interior, which is different from the prior art, and effectively prevents plasma leakage. The embedding of the covalent organic framework provides additional adsorption and transmission channels for oxygen and carbon dioxide; the entanglement of the covalent organic framework and the polypropylene molecular chain improves the mechanical properties of the hybrid hollow fiber oxygenation membrane, while avoiding the reduction in gas transmission performance caused by the current production of polypropylene oxygenation membranes to increase the service life of the membrane. The hybrid hollow fiber oxygenation membrane of the present application has excellent oxygen and carbon dioxide gas permeability and anti-plasma leakage, and its carbon dioxide transmission capacity is 65.3ml / (min·cm 2 bar), which is the carbon dioxide transmission capacity of the unhybridized polypropylene membrane in the prior art, 7.12 ml / (min·cm 2 ·bar); oxygen transmission capacity is 53.5ml / (min·cm 2 ·bar), which is the oxygen transmission capacity of the unhybridized polypropylene membrane in the prior art, 8.33 ml / (min·cm 2 ·bar), and the anti-plasma leakage time is 124h, which is about 21 times that of the 6h of the existing non-hybridized polypropylene membrane. [1] .
[0017] 2. The preparation method of the present application disperses the covalent organic framework material in the casting solution and spins it by thermally induced phase separation. The prepared hybrid hollow fiber oxygenation membrane has strong competitiveness in the oxygenation membrane applied to extracorporeal membrane oxygenation.
[0018] [1]J.Li,T.He,H.Chen,Y.Cheng,E.Drioli,Z.Wang,Z.Cui,Preparation ofHyflon AD / Polypropylene Blend Membrane for Artificial Lung,Membranes 13(2023)665.https: / / doi.org / 10.3390 / membranes13070665. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a schematic diagram of the cross-sectional structure of a polypropylene / covalent organic framework hybrid hollow fiber oxygenation membrane with a gradient structure.
[0020] Figure 2 This is a morphology diagram of the prepared polypropylene / covalent organic framework hybrid hollow fiber oxygenation membrane with gradient structure.
[0021] Figure 3 It is a comparison chart of oxygen and carbon dioxide permeation rate performance of the membranes prepared by the preparation methods of Examples 1-4 and the polypropylene membrane of the prior art. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0023] Weigh the materials according to the formula, the mass percentage in the material formula: the mass percentage of the covalent organic framework is 0.3-1.5% of the polypropylene, and the mass ratio of the covalent organic framework to the diluent is (0.3-1.5):150; first add part of the materials, add the covalent organic framework material to the diluent, ultrasonically disperse and disrupt the cells, and then add the polypropylene after the ultrasonic covalent organic framework material is evenly dispersed, heat to 180-210°C and stir for 6-12h to fully dissolve the polypropylene to avoid large crystals and agglomeration, stop stirring, heat to 190-220°C, stand and degas for 6-12h to obtain a casting solution;
[0024] The casting liquid is used as raw material and a twin-screw spinning machine is used for spinning, and the casting liquid is extruded and introduced into a water coagulation bath at room temperature. The twin screw is kept at a constant temperature of 165-175°C, the spinneret is kept at a constant temperature of 155-165°C, the outer diameter and inner diameter of the annular spinneret are 1.2 mm and 0.7 mm respectively, the distance between the spinneret and the water coagulation bath liquid surface is 2 cm, the spinning speed is 40000-70000 mm / min, and the core liquid flow rate is 1.8-3 ml / min.
[0025] The formed hollow fiber membrane is added to the solvent, the solvent is renewed every 8-12 hours, and the solvent is exchanged and extracted for 2-3 days;
[0026] The hollow fiber membrane obtained after extraction is placed in a room temperature oven for 1-2 days to dry.
[0027] Embodiment 1:
[0028] A hybrid hollow fiber oxygenation membrane is prepared by the following steps:
[0029] Weigh 18g of dioctyl phthalate, 6mg of covalent organic framework COF-316, and 2g of polypropylene. Add the weighed dioctyl phthalate and covalent organic framework COF-316 into a 50ml three-necked flask, and ultrasonicate for 5min until the covalent organic framework COF-316 is evenly dispersed to obtain a light gray suspension. After the suspension cells are broken and ultrasonicated for 5min, 2g of polypropylene is added to the suspension, and the suspension is placed in the reactor of the hollow fiber membrane spinning machine and stirred at 180℃ for 6h. The stirred casting solution is heated to 190℃ and allowed to stand for 6h, ready for use in the preparation of hollow fiber membranes.
[0030] The casting solution was used as the raw material and spun by a hollow fiber membrane spinning machine. The casting solution was extruded and introduced into a water coagulation bath at room temperature. The twin screw was kept at a constant temperature of 165°C, the spinneret was kept at a constant temperature of 155°C, the outer diameter and inner diameter of the annular spinneret were 1.2 mm and 0.7 mm respectively, the distance between the spinneret and the water coagulation bath surface was 2 cm, the spinning speed was 40000 mm / min, and the core liquid flow rate was 1.8 ml / min.
[0031] The formed hollow fiber membrane was extracted in anhydrous ethanol for 2 days to ensure the removal of the diluent, during which the anhydrous ethanol was replaced twice, and then dried in an oven for 1 day.
[0032] Embodiment 2:
[0033] A hybrid hollow fiber oxygenation membrane is prepared by the following steps:
[0034] Weigh 8g of dioctyl phthalate, 10mg of covalent organic framework COF-300, and 2g of polypropylene. Add the weighed dioctyl phthalate and covalent organic framework COF-300 into a 50ml three-necked flask, and ultrasonically treat for 10 minutes until the covalent organic framework COF-300 is evenly dispersed to obtain a light gray suspension. After the suspension cells are broken and ultrasonicated for 10 minutes, 2g of polypropylene is added to the suspension, and the suspension is placed in the reactor of the hollow fiber membrane spinning machine and stirred at 190°C for 8 hours. The stirred casting solution is heated to 200°C and left to stand for 8 hours, ready for use in the preparation of hollow fiber membranes.
[0035] The casting solution was used as the raw material and spun by a hollow fiber membrane spinning machine. The casting solution was extruded and introduced into a water coagulation bath at room temperature. The twin screw was kept at a constant temperature of 170°C, the spinneret was kept at a constant temperature of 160°C, the outer diameter and inner diameter of the annular spinneret were 1.2 mm and 0.7 mm respectively, the distance between the spinneret and the water coagulation bath surface was 2 cm, the spinning speed was 50000 mm / min, and the core liquid flow rate was 2.2 ml / min.
[0036] The formed hollow fiber membrane was extracted in anhydrous ethanol for 2 days to ensure the removal of the diluent, during which the anhydrous ethanol was replaced twice, and then dried in an oven for 1 day.
[0037] Embodiment 3:
[0038] A hybrid hollow fiber oxygenation membrane is prepared by the following steps:
[0039] Weigh 4.6667g of dioctyl phthalate, 20mg of covalent organic framework COF-LZU1, and 2g of polypropylene. Add the weighed dioctyl phthalate and covalent organic framework COF-LZU1 into a 50mL three-necked flask, and ultrasonically treat for 15 minutes until the covalent organic framework COF-LZU1 is evenly dispersed to obtain a light gray suspension. After the suspension cells are broken and ultrasonicated for 15 minutes, 2g of polypropylene is added to the suspension, and the suspension is placed in the reactor of the hollow fiber membrane spinning machine and stirred at 200°C for 10 hours. The stirred casting solution is heated to 210°C and allowed to stand for 10 hours, ready for use in the preparation of hollow fiber membranes.
[0040] The casting solution was used as the raw material and spun by a hollow fiber membrane spinning machine. The casting solution was extruded and introduced into a water coagulation bath at room temperature. The twin screw was kept at a constant temperature of 175°C, the spinneret was kept at a constant temperature of 165°C, the outer diameter and inner diameter of the annular spinneret were 1.2 mm and 0.7 mm respectively, the distance between the spinneret and the water coagulation bath surface was 2 cm, the spinning speed was 60000 mm / min, and the core liquid flow rate was 2.6 ml / min.
[0041] The formed hollow fiber membrane was extracted in anhydrous ethanol for 3 days to ensure the removal of the diluent, during which the anhydrous ethanol was replaced twice, and then dried in an oven for 2 days.
[0042] Embodiment 4:
[0043] A hybrid hollow fiber oxygenation membrane is prepared by the following steps:
[0044] Weigh 3g of dioctyl phthalate, 40mg of covalent organic framework JUC-521, and 2g of polypropylene. Add the weighed dioctyl phthalate and covalent organic framework JUC-521 into a 50mL three-necked flask, and ultrasonically treat for 20 minutes until the covalent organic framework JUC-521 is evenly dispersed to obtain a light gray suspension. After the suspension cells are broken and ultrasonicated for 20 minutes, 2g of polypropylene is added to the suspension, and the suspension is placed in the reactor of the hollow fiber membrane spinning machine and stirred at 210°C for 12 hours. The stirred casting solution is heated to 220°C and allowed to stand for 12 hours, ready for use in the preparation of hollow fiber membranes.
[0045] The casting solution was used as the raw material and spun by a hollow fiber membrane spinning machine. The casting solution was extruded and introduced into a water coagulation bath at room temperature. The twin screw was kept at a constant temperature of 180°C, the spinneret was kept at a constant temperature of 170°C, the outer diameter and inner diameter of the annular spinneret were 1.2 mm and 0.7 mm respectively, the distance between the spinneret and the water coagulation bath surface was 2 cm, the spinning speed was 70000 mm / min, and the core liquid flow rate was 3 ml / min.
[0046] The formed hollow fiber membrane was extracted in anhydrous ethanol for 3 days to ensure the removal of the diluent, during which the anhydrous ethanol was replaced twice, and then dried in an oven for 2 days.
[0047] The hybrid hollow fiber oxygenation membrane prepared in Example 1 was characterized and analyzed by scanning electron microscopy, and the Figure 2 . Figure 2 This is a scanning electron microscope image of the hybrid hollow fiber oxygenation membrane of Example 1 of the present application.
[0048] like Figure 2 As shown, the hybrid hollow fiber oxygenation membrane prepared in Example 1 has a gradient structure with gradually increasing looseness and pores from the dense cortex on the surface to the main body.
[0049] The membrane thickness of the hybrid hollow fiber oxygenation membrane is about 500 μm, the cross section of the support layer is a loose porous structure, and the surface is dense.
[0050] Test Example 1 Test of oxygen and carbon dioxide transmission performance of hybrid hollow fiber membrane
[0051] The hybrid hollow fiber oxygenation membranes prepared in Examples 1 to 4 and the hollow fiber membranes prepared in the comparative example were respectively encapsulated into membrane modules with epoxy resin AB glue, 1 bar of oxygen or carbon dioxide was introduced into the membrane modules, the gas flow was measured with a soap film flowmeter, and the oxygen permeation rate and carbon dioxide permeation rate of each fiber membrane were calculated to obtain the data in the following table.
[0052] Table 1 Gas permeation properties of membranes modified by different covalent organic framework conditions
[0053]
[0054] like Figure 3 To test the carbon dioxide permeation rate and oxygen permeation rate under pressure, the carbon dioxide and oxygen transmission rates of the hybrid membrane with the addition of the covalent organic framework are significantly better than those of the polypropylene membrane without the addition of the covalent organic framework. This is mainly due to the fact that the covalent organic framework itself has a high content of imine, benzene ring groups, high-density pores and a large specific surface area, which enhances the dissolution-diffusion process of oxygen and carbon dioxide molecules through the membrane. Furthermore, the good interaction and compatibility between the covalent organic framework nanoparticles and polypropylene enhance the free volume of the membrane and reduce the gas transmission resistance in the membrane. The coordination of multiple action mechanisms enables the prepared hybrid membrane to have efficient gas transmission performance. Overall, the hybrid membrane of Example 2 has the best oxygen and carbon dioxide gas permeability, and its carbon dioxide transmission capacity is 65.3ml / (min·cm 2 bar), which is the carbon dioxide transmission capacity of the unhybridized polypropylene membrane in the prior art, 7.12 ml / (min·cm 2 ·bar); oxygen transmission capacity is 53.5ml / (min·cm2 ·bar), which is the oxygen transmission capacity of the unhybridized polypropylene membrane in the prior art, 8.33 ml / (min·cm 2 ·bar), and the anti-plasma leakage time is 124h, which is about 21 times that of the 6h of the prior art non-hybridized polypropylene membrane.
[0055] Although the present invention has been described above in conjunction with the accompanying drawings, the present invention is not limited to the above-mentioned specific embodiments, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can make many modifications without departing from the purpose of the present invention, all of which are within the protection of the present invention.
Claims
1. A polypropylene / covalent organic framework hybrid hollow fiber oxygenation membrane with a gradient structure; characterized in that: The hybrid hollow fiber oxygenation membrane is a hollow fiber oxygenation membrane based on the hybridization of a covalent organic framework and a polypropylene material. The oxygenation membrane is a gradient structure that gradually increases from a dense cortex on the surface to a loose and porous main body, and the covalent organic framework presents a gradient distribution in the membrane.
2. The method for preparing the polypropylene / covalent organic framework hybrid hollow fiber oxygenation membrane with gradient structure according to claim 1, characterized in that: The covalent organic framework material is first ultrasonically dispersed for 5-20 minutes, and then the cells are broken for 5-20 minutes and uniformly dispersed in a diluent to obtain a dispersion liquid; polypropylene is added to the dispersion liquid, and the dispersion liquid is heated and stirred and then allowed to stand to obtain a casting liquid. The casting liquid is used as a raw material and spun by a thermally induced phase separation method to obtain a hybrid hollow fiber oxygenation membrane.
3. The preparation method as claimed in claim 2, characterized in that The mass ratio of the covalent organic framework material to polypropylene is (0.3-1.5):
100.
4. The preparation method according to claim 2, characterized in that The diluent includes one or more combinations of dibutyl phthalate, dioctyl phthalate, trioctyl acetyl citrate, tributyl citrate, and trioctyl citrate; the mass ratio of the covalent organic framework material to the diluent is (0.3-1.5):
150.
5. The preparation method according to claim 2, characterized in that The conditions for standing still after heating and stirring are: heating to 180-210° C. and stirring for 6-12 hours, stopping stirring, heating to 190-220° C. and standing still for degassing for 6-12 hours to obtain the casting solution.
6. The preparation method according to claim 2, characterized in that Thermally induced phase separation spinning is as follows: the casting solution is kept at The casting liquid is extruded through a spinneret at a constant temperature of 220-240°C and introduced into a water coagulation bath at room temperature for solidification and forming. The spinning speed is 40000-70000 mm / min and the core liquid flow rate is 1.8-3 ml / min.
7. The preparation method according to claim 2, characterized in that The hybrid hollow fiber oxygenation membrane is fully immersed in the extraction liquid to extract and remove the diluent, and then air-dried.
8. The preparation method according to claim 7, characterized in that The extracting liquid includes one or more of anhydrous ethanol, isopropanol, n-heptane and n-hexane.
9. Use of the polypropylene / covalent organic framework hybrid hollow fiber oxygenation membrane with gradient structure according to claim 1 as an oxygenation membrane in an extracorporeal membrane oxygenation process.
Citation Information
Patent Citations
Composite hollow fiber membrane as well as preparation method and application thereof
CN113522052A
Poly(4-methyl-1-pentene) hollow fiber membrane and preparation method thereof
CN113546525A
Mixed matrix hollow fiber oxygenation membrane based on framework material and preparation method of mixed matrix hollow fiber oxygenation membrane
CN114887503A
Preparation method of permanent hydrophilic polyether sulfone hollow fiber membrane with gradient structure
CN115475536A
Hybrid hollow fiber oxygenation membrane and preparation method thereof
CN116059853A
Cited By
COF-doped mixed matrix membrane, preparation method and application in ECCO2R system
CN119524656A