Preparation method of protein-induced polyamide nanofiltration membrane
Through protein regulation interface polymerization technology, a polyamide nanofiltration membrane with a multi-stage pore structure is formed, which solves the problem of insufficient water flux in the nanofiltration membrane in the prior art, and combines high salt cutoff and high water flux, simplifies The preparation process was carried out.
Patent Information
- Application Number
- CN202411091639.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing methods are difficult to achieve precise regulation of the pore size of the nanofiltration membrane and the formation control of the polyamide membrane, resulting in the inability to prepare a high-water flux polyamide composite nanofiltration membrane.
By using the protein-regulating interface polymerization process, by adding protein and piperazine to the aqueous phase, hydrogen bonding is used to slow down the release of piperazine, forming a thinner, defect-free polyamide film, combining the polycondensation reaction of protein and triformyl chloride to form Multi-stage pore structure, improving the water flux and salt cutoff of the membrane.
While ensuring high salt cutoff, the water flux of the nanofiltration membrane was significantly improved, from 15.46L m-2h-1bar-1 to 32.13L m-2h-1bar-1, and the membrane was added through special structure. Specific surface area simplifies the preparation process and is suitable for large-scale production.
Smart Images

Figure CN118925519A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of drinking water purification and wastewater pollution control, and specifically relates to a method for preparing a protein-induced polyamide nanofiltration membrane. Background Art
[0002] Compared with other technologies, membrane separation technology is a relatively energy-saving water treatment technology. The membrane elements on the market can be roughly divided into microfiltration membrane (MF), ultrafiltration membrane (UF), nanofiltration membrane (NF) and reverse osmosis membrane (RO). Among them, nanofiltration membrane is an important material widely used in deep water treatment, hard water softening, brackish water treatment and other fields. It can remove specific organic matter, pigments and salts in water. It is a separation membrane with a pore size between porous ultrafiltration membrane and dense reverse osmosis membrane. With its advantages of low operating pressure, high water flux, and effective retention of dissolved organic matter and hardness in water, it is widely used in the field of drinking water purification and wastewater pollution control. Among them, the polyamide composite membrane prepared with porous base membrane as the substrate is the most widely used nanofiltration membrane. Interfacial polymerization is the most widely used polyamide membrane preparation technology, which has the characteristics of controllable pore size and molecular screening, simple operation and customization.
[0003] However, there are some problems with the interfacial polymerization method, which makes it difficult to achieve precise control of pore size and control of polyamide membrane formation. The physical structure and chemical properties of the polyamide separation layer determine the separation performance of the composite membrane. By regulating the interfacial polymerization process to optimize the physical and chemical properties of the polyamide layer, the separation performance of the composite membrane can be improved. Therefore, how to regulate the interfacial polymerization process of forming the polyamide layer is the current research focus. Summary of the invention
[0004] The purpose of the present invention is to solve the problem that the existing methods are difficult to achieve precise control of pore size and control of polyamide membrane formation, and cannot prepare polyamide composite nanofiltration membranes with high water flux, and to provide a method for preparing a protein-induced polyamide nanofiltration membrane.
[0005] The present invention uses protein to regulate the interfacial polymerization process to achieve precise regulation of interfacial polymerization and prepare a polyamide composite nanofiltration membrane that can achieve high water flux while ensuring a high separation rate. Protein has rich groups and has high affinity with water and amine molecules. It is a highly potential substance that has not yet been developed for interfacial polymerization regulation.
[0006] A method for preparing a protein-induced polyamide nanofiltration membrane is completed by the following steps:
[0007] 1. Pretreatment of ultrafiltration membrane:
[0008] The ultrafiltration membrane is rinsed with deionized water for multiple times, and then the ultrafiltration membrane is immersed in anhydrous ethanol for a period of time. Before use, the ultrafiltration membrane is taken out from the anhydrous ethanol, and then the anhydrous ethanol on the surface of the ultrafiltration membrane is rinsed with deionized water to obtain a pretreated ultrafiltration membrane;
[0009] 2. Prepare aqueous solution:
[0010] The protein is dissolved in a buffer solution of a certain pH value, and then placed in a refrigerator at 3°C to 4°C for a period of time, and then piperazine is added to obtain an aqueous phase solution containing protein and piperazine;
[0011] 3. Prepare the organic phase solution:
[0012] Dissolving trimesoyl chloride in an organic solvent, stirring evenly and then standing for a period of time to obtain an organic phase solution for interfacial polymerization;
[0013] 4. Fixed ultrafiltration membrane:
[0014] Cut the pretreated ultrafiltration membrane into the same size as the glass plate, then place the pretreated ultrafiltration membrane on the glass plate to avoid the generation of bubbles, and then place the silicone pad and polytetrafluoroethylene frame on the edge of the glass plate in turn and fix them with a dovetail clip;
[0015] 5. Enrichment of aqueous solution in membrane pores:
[0016] A certain volume of aqueous solution containing protein and piperazine was poured onto the pretreated ultrafiltration membrane, allowed to stand for a certain period of time, and then the aqueous solution containing protein and piperazine was poured out. 2 The purge gun removes the excess aqueous solution visible on the surface to obtain an ultrafiltration membrane enriched with aqueous solution;
[0017] 6. Interface polymerization:
[0018] The ultrafiltration membrane enriched with aqueous phase solution is laid flat and allowed to stand for a period of time, and then a certain volume of organic phase solution for interfacial polymerization is poured onto the ultrafiltration membrane enriched with aqueous phase solution, and the organic phase solution is poured out after cross-linking at room temperature for a period of time, and then the unreacted organic phase solution is washed away with an organic solvent, and finally placed in an oven for thermal cross-linking for a period of time to obtain a protein-induced polyamide nanofiltration membrane.
[0019] Principle of the present invention:
[0020] 1. When using interfacial polymerization to prepare polyamide membranes, there is a problem that the reaction speed is fast and it is difficult to control the interfacial polymerization process from a kinetic level. At present, there are a lot of studies on the regulation of polyamide layers, such as preparing a sacrificial layer of cadmium hydroxide nanowires and preparing a hydrophilic intermediate layer. However, the present invention uses a method of adding protein to the aqueous phase to regulate the interfacial polymerization process. The regulation principle is based on the fact that protein and piperazine in the aqueous phase will attract each other through hydrogen bonds, which slows down the release of piperazine and forms a thinner, defect-free polyamide membrane to improve water flux and salt rejection rate.
[0021] 2. The present invention proves that the protein itself can also undergo a polycondensation reaction with trimesoyl chloride (TMC) in the organic phase to form a film. Therefore, the protein itself forms a film in the aqueous phase. Since the pores formed by the reaction of the protein with TMC are relatively large, the dense pores formed by the reaction with piperazine (PIP) and TMC form a multi-level pore structure, thereby forming a nanofiltration membrane with a special structure and function.
[0022] 3. The membrane structure prepared by the present invention has an obvious striped Turing structure and a special coffee ring structure, which greatly increases the specific surface area of the membrane. The two special structures provide additional water passages for the membrane, which greatly improves the water flux of the membrane while ensuring the salt rejection rate of the membrane.
[0023] The present invention has the following effects:
[0024] 1. The method used in the present invention can be implemented without changing the existing interfacial polymerization process, has strong applicability, and can increase the water flux from 15.46 L m to 25.46 L m while ensuring a high salt rejection rate. -2 h -1 bar -1 Increased to 32.13L m -2 h -1 bar -1 ;
[0025] 2. Compared with the membrane formed by conventional interfacial polymerization, the polyamide layer of the membrane prepared by the present invention has a striped Turing structure and a coffee ring structure, while the nanofiltration membrane prepared by conventional interfacial polymerization has a typical nodular structure. The two special morphologies greatly increase the specific surface area of the polyamide layer, provide additional water channels for the membrane, and thus greatly improve the water flux of the membrane;
[0026] 3. The protein-induced polyamide nanofiltration membrane prepared by the present invention has a polyamide layer with fewer defects, a reduced thickness, and significantly increased roughness;
[0027] 4. The protein-induced polyamide nanofiltration membrane prepared by the present invention greatly improves the water flux of the nanofiltration membrane while ensuring a high salt rejection rate. The preparation process has the characteristics of simple preparation method, easy operation, short cycle, and no need to change the existing interfacial polymerization process, and is suitable for large-scale nanofiltration membrane preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Figures 1 and 2 are the surface morphologies of the nanofiltration membrane prepared by the conventional interfacial polymerization method in Example 6, 1 is a low magnification image, 2 is a high magnification image, 3 and 4 are the surface morphologies of the protein-induced polyamide nanofiltration membrane in Example 3, 3 is a low magnification image, 4 is a high magnification image, 5 and 6 are the surface morphologies of the protein-induced polyamide nanofiltration membrane in Example 5, 5 is a low magnification image, and 6 is a high magnification image;
[0029] Figure 2 FTIR spectra of the films and protein powders prepared in Examples 1 to 6;
[0030] Figure 3 The atomic force microscope images of the films prepared in Example 3 and Example 6, in which 2 is the PA-L1 film prepared in Example 1, 1 is the PA-L0 film prepared in Example 6 for comparison, the upper image is a 2D image, the lower image is a 3D image, and the inset image shows the height change along the scribe line;
[0031] Figure 4 To test the water flux and salt rejection of the membranes prepared in Examples 1 to 6, the water flux was measured at 0.4 MPa after a pre-pressure of 0.5 MPa for 1 h, and the salt rejection was measured using a 1000 ppm sodium sulfate solution;
[0032] Figure 5 The salt rejection rate and water flux of the membranes prepared in Example 3 and Example 6 are compared. The bar graph is the salt rejection rate of sodium sulfate, magnesium sulfate, magnesium chloride, calcium chloride and sodium chloride. The line graph is the water flux. The concentrations of the several solutions used in the salt rejection rate test experiment are all 1000ppm. DETAILED DESCRIPTION
[0033] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the essence of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention all fall within the scope of the present invention.
[0034] Specific implementation method 1: In this implementation method, a method for preparing a protein-induced polyamide nanofiltration membrane is completed by the following steps:
[0035] 1. Pretreatment of ultrafiltration membrane:
[0036] The ultrafiltration membrane is rinsed with deionized water for multiple times, and then the ultrafiltration membrane is immersed in anhydrous ethanol for a period of time. Before use, the ultrafiltration membrane is taken out from the anhydrous ethanol, and then the anhydrous ethanol on the surface of the ultrafiltration membrane is rinsed with deionized water to obtain a pretreated ultrafiltration membrane;
[0037] 2. Prepare aqueous solution:
[0038] The protein is dissolved in a buffer solution of a certain pH value, and then placed in a refrigerator at 3°C to 4°C for a period of time, and then piperazine is added to obtain an aqueous phase solution containing the protein and piperazine;
[0039] 3. Prepare the organic phase solution:
[0040] Dissolving trimesoyl chloride in an organic solvent, stirring evenly and then standing for a period of time to obtain an organic phase solution for interfacial polymerization;
[0041] 4. Fixed ultrafiltration membrane:
[0042] Cut the pretreated ultrafiltration membrane into the same size as the glass plate, then place the pretreated ultrafiltration membrane on the glass plate to avoid the generation of bubbles, and then place the silicone pad and polytetrafluoroethylene frame on the edge of the glass plate in turn and fix them with a dovetail clip;
[0043] 5. Enrichment of aqueous solution in membrane pores:
[0044] A certain volume of aqueous solution containing protein and piperazine was poured onto the pretreated ultrafiltration membrane, allowed to stand for a certain period of time, and then the aqueous solution containing protein and piperazine was poured out. 2 The purge gun removes the excess aqueous solution visible on the surface to obtain an ultrafiltration membrane enriched with aqueous solution;
[0045] 6. Interface polymerization:
[0046] The ultrafiltration membrane enriched with aqueous phase solution is laid flat and allowed to stand for a period of time, and then a certain volume of organic phase solution for interfacial polymerization is poured onto the ultrafiltration membrane enriched with aqueous phase solution, and the organic phase solution is poured out after cross-linking at room temperature for a period of time, and then the unreacted organic phase solution is washed away with an organic solvent, and finally placed in an oven for thermal cross-linking for a period of time to obtain a protein-induced polyamide nanofiltration membrane.
[0047] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: in step 1, the ultrafiltration membrane is rinsed with deionized water for 3 to 5 times, and then the ultrafiltration membrane is immersed in anhydrous ethanol for more than 24 hours. The other steps are the same as those of specific implementation method 1.
[0048] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the ultrafiltration membrane in step 1 is a polyethersulfone membrane, a polytetrafluoroethylene membrane, a polyvinylidene fluoride membrane, a polyvinylidene fluoride membrane or a cellulose acetate membrane. The other steps are the same as those in specific implementation method 1 or 2.
[0049] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the protein in step 2 is one or a mixture of lysozyme, bovine serum albumin, β-lactoglobulin and pepsin. The other steps are the same as those of specific embodiments 1 to 3.
[0050] Specific implementation mode five: The difference between this implementation mode and specific implementation modes one to four is that: the buffer solution described in step two is HEPES buffer solution or Tris-HCl buffer solution; the concentration of the buffer solution described in step two is 10mmol / L, and the pH value is 7.0-8.5; the standing time described in step two is 8h-12h.
[0051] The other steps are the same as those in Specific Embodiments 1 to 4.
[0052] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that: the mass fraction of protein in the aqueous solution containing protein and piperazine in step 2 is 0.05wt% to 0.8wt%; the mass fraction of piperazine in the aqueous solution containing protein and piperazine in step 2 is 0.1wt% to 0.5wt%. The other steps are the same as those in specific embodiments 1 to 5.
[0053] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the mass fraction of trimesoyl chloride in the organic phase solution for interfacial polymerization described in step 3 is 0.05wt% to 0.2wt%; the organic solvent described in step 3 is n-hexane or ISOPAR-G; the standing time described in step 3 is 1h to 2h. The other steps are the same as those of specific embodiments 1 to 6.
[0054] Specific embodiment eight: The difference between this embodiment and specific embodiments one to seven is that the size of the glass plate described in step four is 14cm×10cm; in step five, 20mL of the aqueous solution containing protein and piperazine is poured onto the pretreated ultrafiltration membrane; the standing time described in step five is 10min to 20min.
[0055] The other steps are the same as those in Specific Embodiments 1 to 7.
[0056] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the volume ratio of the organic phase solution used for interfacial polymerization in step 6 to the aqueous phase solution containing protein and piperazine in step 5 is 1:1; the cross-linking time at room temperature in step 6 is 30s to 120s. The other steps are the same as those in specific embodiments 1 to 8.
[0057] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: in step 6, the ultrafiltration membrane enriched with the aqueous phase solution is placed flat for 30s to 120s; the organic solvent in step 6 is n-hexane or ISOPAR-G; the temperature of the oven in step 6 is 60°C to 80°C, and the time for thermal crosslinking is 10min to 20min. The other steps are the same as those in specific embodiments 1 to 9.
[0058] The following examples are used to verify the beneficial effects of the present invention:
[0059] Example 1: A method for preparing a protein-induced polyamide nanofiltration membrane is completed by the following steps:
[0060] 1. Pretreatment of ultrafiltration membrane:
[0061] The ultrafiltration membrane was rinsed with deionized water for 3 times, and then immersed in anhydrous ethanol for 24 hours. Before use, the ultrafiltration membrane was taken out from the anhydrous ethanol, and then the anhydrous ethanol on the surface of the ultrafiltration membrane was rinsed with deionized water to obtain a pretreated ultrafiltration membrane.
[0062] In step 1, the ultrafiltration membrane is a polyethersulfone membrane, model GC-UF0202;
[0063] 2. Prepare aqueous solution:
[0064] The protein is dissolved in a buffer solution with a certain pH value, and then placed in a refrigerator at 4°C for 8 hours, and then piperazine is added to obtain an aqueous phase solution containing the protein and piperazine;
[0065] The protein described in step 2 is lysozyme;
[0066] The buffer described in step 2 is Tris-HCl buffer; the concentration of the buffer described in step 2 is 10 mmol / L, and the pH value is 7.4;
[0067] The mass fraction of protein in the aqueous solution containing protein and piperazine in step 2 is 0.05wt%;
[0068] The mass fraction of piperazine in the aqueous solution containing protein and piperazine in step 2 is 0.1wt%;
[0069] 3. Prepare the organic phase solution:
[0070] Dissolve trimesoyl chloride in an organic solvent, stir for 6 hours at a stirring speed of 600 r / min, and then stand for 1 hour to obtain an organic phase solution for interfacial polymerization;
[0071] The mass fraction of trimesoyl chloride in the organic phase solution used for interfacial polymerization in step 3 is 0.1wt%;
[0072] The organic solvent described in step 3 is ISOPAR-G;
[0073] 4. Fixed ultrafiltration membrane:
[0074] Cut the pretreated ultrafiltration membrane into the same size as the glass plate, then place the pretreated ultrafiltration membrane on the glass plate to avoid the generation of bubbles, and then place the silicone pad and polytetrafluoroethylene frame on the edge of the glass plate in turn and fix them with a dovetail clip;
[0075] The size of the glass plate described in step 4 is 14 cm × 10 cm;
[0076] 5. Enrichment of aqueous solution in membrane pores:
[0077] Pour 20 mL of the aqueous solution containing protein and piperazine onto the pretreated ultrafiltration membrane, let it stand for 10 min, then pour out the aqueous solution containing protein and piperazine, and use N 2 The purge gun removes the excess aqueous solution visible on the surface to obtain an ultrafiltration membrane enriched with aqueous solution;
[0078] 6. Interface polymerization:
[0079] The ultrafiltration membrane enriched with aqueous phase solution was laid flat for 2 minutes, and then 20 mL of organic phase solution for interfacial polymerization was poured onto the ultrafiltration membrane enriched with aqueous phase solution. After cross-linking at room temperature for 1 minute, the organic phase solution was poured out, and the unreacted organic phase solution was washed away with an organic solvent. Finally, it was placed in an oven at 60°C for thermal cross-linking for 10 minutes to obtain a protein-induced polyamide nanofiltration membrane (named PA-L1).
[0080] The organic solvent described in step six is ISOPAR-G.
[0081] Example 2: This example is different from Example 1 in that the mass fraction of protein in the aqueous solution containing protein and piperazine in step 2 is 0.1 wt%; the protein-induced polyamide nanofiltration membrane finally obtained is named PA-L2. The other steps and parameters are the same as those in Example 1.
[0082] Example 3: The difference between this example and Example 1 is that the mass fraction of protein in the aqueous solution containing protein and piperazine in step 2 is 0.3wt%; the protein-induced polyamide nanofiltration membrane finally obtained is named PA-L3. The other steps and parameters are the same as those in Example 1.
[0083] Example 4: This example is different from Example 1 in that the mass fraction of protein in the aqueous solution containing protein and piperazine in step 2 is 0.5 wt %; the protein-induced polyamide nanofiltration membrane finally obtained is named PA-L4. The other steps and parameters are the same as those in Example 1.
[0084] Example 5: This example is different from Example 1 in that the mass fraction of protein in the aqueous solution containing protein and piperazine in step 2 is 0.8 wt %; the protein-induced polyamide nanofiltration membrane finally obtained is named PA-L5. The other steps and parameters are the same as those in Example 1.
[0085] Example 6: The differences between this example and Example 1 are: the mass fraction of protein in the aqueous solution containing protein and piperazine in step 2 is 0wt%; the mass fraction of piperazine in the aqueous solution containing protein and piperazine in step 2 is 0.1wt%; the aqueous solution is pure water, and the membrane finally prepared is named PA-L0. The other steps and parameters are the same as those in Example 1.
[0086] The membranes PA-L1 to 5 prepared in Examples 1 to 5 are mainly used to explore the effects of different lysozyme concentrations on a protein-induced polyamide nanofiltration membrane. Example 6 is a polyamide nanofiltration membrane (PA-L0) prepared without protein induction, which is mainly used for comparison with a protein-induced polyamide nanofiltration membrane.
[0087] Figure 1 Figures 1 and 2 are the surface morphologies of the nanofiltration membrane prepared by the conventional interfacial polymerization method in Example 6, 1 is a low magnification image, 2 is a high magnification image, 3 and 4 are the surface morphologies of the protein-induced polyamide nanofiltration membrane in Example 3, 3 is a low magnification image, 4 is a high magnification image, 5 and 6 are the surface morphologies of the protein-induced polyamide nanofiltration membrane in Example 5, 5 is a low magnification image, and 6 is a high magnification image;
[0088] Depend on Figure 1 It can be seen that: ordinary nanofiltration membranes present a typical nodular morphology, while the surface of a protein-induced polyamide nanofiltration membrane of the present invention presents two special morphologies, namely the special coffee ring structure shown in the SEM images (3 and 4) taken of the membrane prepared in Example 3 and the striped Turing structure shown in the SEM images taken of the membrane prepared in Example 5. Both special structures provide special water passages for the polyamide membrane, explaining why the water flux of the present invention is greatly improved in subsequent tests.
[0089] Figure 2 FTIR spectra of the films and protein powders prepared in Examples 1 to 6;
[0090] Figure 2LYZ is the infrared spectrum of lysozyme powder for comparison; Figure 2 It can be seen that: at 1500-1800cm -1 The successful immobilization of lysozyme and its integrity after cross-linking were confirmed in the fingerprint region of 1650 cm -1 The peak at 2960cm-1 gradually becomes stronger with the increase of lysozyme concentration, which is caused by the stretching vibration of C=O of peptide bond in protein; -1 The peak at 1540cm may be related to the aliphatic part of the protein; -1 The peak at 3300 cm-1 is due to the peptide bonds in the protein (NH bending and CN stretching vibrations); a peak at 3300 cm-1 was observed in all lysozyme membranes. -1 The center of the broadband and several 3000cm -1 The smaller peak centered at is related to the overlap of the stretching vibrations of N—H and -COOH formed during the interfacial polymerization and other groups (such as O—H groups) in the lysozyme layer.
[0091] The films prepared in Example 3 and Example 6 were tested by atomic force microscopy. Figure 3 ;
[0092] Figure 3 The atomic force microscope images of the films prepared in Example 3 and Example 6, in which 2 is the PA-L1 film prepared in Example 1, 1 is the PA-L0 film prepared in Example 6 for comparison, the upper image is a 2D image, the lower image is a 3D image, and the inset image shows the height change along the scribe line;
[0093] Depend on Figure 3 It can be seen that the polyamide nanofiltration membrane prepared by protein-induced interfacial polymerization has a special striped Turing structure with a height of about 15 nm. Compared with the ordinary polyamide nanofiltration membrane prepared in Example 6, the roughness increases from 3.45±0.45 to 5.09±0.30.
[0094] Figure 4 To test the water flux and salt rejection of the membranes prepared in Examples 1 to 6, the water flux was measured at 0.4 MPa after a pre-pressure of 0.5 MPa for 1 h, and the salt rejection was measured using a 1000 ppm sodium sulfate solution;
[0095] from Figure 4 It can be seen that: with the increase of lysozyme concentration, the water flux first increases and then decreases, and the salt rejection first decreases, then increases, and then decreases. Combining the water flux and the salt rejection rate, PA-L2 and PA-L3 are determined to be suitable concentrations, because at this time the water flux is greatly improved compared with the normally prepared polyamide membrane, while ensuring a high salt rejection rate.
[0096] Figure 5The salt rejection rate and water flux of the membranes prepared in Example 3 and Example 6 are compared. The bar graph is the salt rejection rate of sodium sulfate, magnesium sulfate, magnesium chloride, calcium chloride and sodium chloride. The line graph is the water flux. The concentrations of the several solutions used in the salt rejection rate test experiment are all 1000ppm.
[0097] from Figure 5 It can be seen that the membrane prepared by the protein-induced polyamide layer preparation method can increase the water flux from 15.46 L m-1 to 2.5 L m-2 while ensuring a high salt rejection rate. -2 h -1 bar -1 Increased to 32.13L m -2 h -1 bar -1 The reasons were analyzed. On the one hand, the addition of protein slowed down the release of piperazine in the aqueous phase, forming special structures of stripes and coffee rings, providing additional water channels, and greatly improving the water flux; on the other hand, the protein-induced interfacial polymerization effectively realized the control of interfacial polymerization and produced a thinner polyamide layer with fewer defects.
Claims
1. A method for preparing a protein-induced polyamide nanofiltration membrane, characterized in that The preparation method is completed according to the following steps:
1. Pretreatment of ultrafiltration membrane: The ultrafiltration membrane is rinsed with deionized water for multiple times, and then the ultrafiltration membrane is immersed in anhydrous ethanol for a period of time. Before use, the ultrafiltration membrane is taken out from the anhydrous ethanol, and then the anhydrous ethanol on the surface of the ultrafiltration membrane is rinsed with deionized water to obtain a pretreated ultrafiltration membrane; 2. Prepare aqueous solution: The protein is dissolved in a buffer solution of a certain pH value, and then placed in a refrigerator at 3°C to 4°C for a period of time, and then piperazine is added to obtain an aqueous phase solution containing the protein and piperazine; 3. Prepare the organic phase solution: Dissolving trimesoyl chloride in an organic solvent, stirring evenly and then standing for a period of time to obtain an organic phase solution for interfacial polymerization; 4. Fixed ultrafiltration membrane: Cut the pretreated ultrafiltration membrane into the same size as the glass plate, then place the pretreated ultrafiltration membrane on the glass plate to avoid the generation of bubbles, and then place the silicone pad and polytetrafluoroethylene frame on the edge of the glass plate in turn and fix them with a dovetail clip; 5. Enrichment of aqueous solution in membrane pores: A certain volume of aqueous solution containing protein and piperazine is poured onto the pretreated ultrafiltration membrane, and allowed to stand for a certain period of time, and then the aqueous solution containing protein and piperazine is poured out, and the excess aqueous solution visible on the surface is removed by a N2 purge gun to obtain an ultrafiltration membrane enriched with the aqueous solution; 6. Interface polymerization: The ultrafiltration membrane enriched with aqueous phase solution is laid flat and allowed to stand for a period of time, and then a certain volume of organic phase solution for interfacial polymerization is poured onto the ultrafiltration membrane enriched with aqueous phase solution, and the organic phase solution is poured out after cross-linking at room temperature for a period of time, and then the unreacted organic phase solution is washed away with an organic solvent, and finally placed in an oven for thermal cross-linking for a period of time to obtain a protein-induced polyamide nanofiltration membrane.
2. The method for preparing a protein-induced polyamide nanofiltration membrane according to claim 1, characterized in that In step 1, the ultrafiltration membrane is rinsed with deionized water for 3 to 5 times, and then the ultrafiltration membrane is immersed in anhydrous ethanol for more than 24 hours.
3. The method for preparing a protein-induced polyamide nanofiltration membrane according to claim 1, characterized in that In step 1, the ultrafiltration membrane is a polyethersulfone membrane, a polytetrafluoroethylene membrane, a polyvinylidene fluoride membrane, a polyvinylidene fluoride membrane or a cellulose acetate membrane.
4. A method for preparing a protein-induced polyamide nanofiltration membrane according to claim 1, 2 or 3, characterized in that The protein in step 2 is one or a mixture of lysozyme, bovine serum albumin, β-lactoglobulin and pepsin.
5. The method for preparing a protein-induced polyamide nanofiltration membrane according to claim 1, 2 or 3, characterized in that The buffer described in step 2 is HEPES buffer or Tris-HCl buffer; the concentration of the buffer described in step 2 is 10 mmol / L, and the pH value is 7.0-8.5; the standing time described in step 2 is 8h-12h.
6. A method for preparing a protein-induced polyamide nanofiltration membrane according to claim 1, 2 or 3, characterized in that The mass fraction of protein in the aqueous solution containing protein and piperazine in step 2 is 0.05wt% to 0.8wt%; the mass fraction of piperazine in the aqueous solution containing protein and piperazine in step 2 is 0.1wt% to 0.5wt%.
7. A method for preparing a protein-induced polyamide nanofiltration membrane according to claim 1, 2 or 3, characterized in that The mass fraction of trimesoyl chloride in the organic phase solution for interfacial polymerization in step 3 is 0.05wt% to 0.2wt%; the organic solvent in step 3 is n-hexane or ISOPAR-G; and the standing time in step 3 is 1h to 2h.
8. The method for preparing a protein-induced polyamide nanofiltration membrane according to claim 1, 2 or 3, characterized in that The size of the glass plate described in step 4 is 14 cm×10 cm; in step 5, 20 mL of the aqueous solution containing protein and piperazine is poured onto the pretreated ultrafiltration membrane; and the standing time described in step 5 is 10 min to 20 min.
9. The method for preparing a protein-induced polyamide nanofiltration membrane according to claim 1, 2 or 3, characterized in that The volume ratio of the organic phase solution used for interfacial polymerization in step 6 to the aqueous phase solution containing protein and piperazine in step 5 is 1:1; the cross-linking time at room temperature in step 6 is 30s to 120s.
10. The method for preparing a protein-induced polyamide nanofiltration membrane according to claim 1, 2 or 3, characterized in that In step 6, the ultrafiltration membrane enriched with the aqueous phase solution is placed flat and allowed to stand for 30s to 120s; the organic solvent in step 6 is n-hexane or ISOPAR-G; the temperature of the oven in step 6 is 60° C. to 80° C., and the thermal crosslinking time is 10min to 20min.
Citation Information
Patent Citations
High-flux composite nanofiltration membrane and preparation method thereof
CN112827370A
Preparation method of 2D protein nano interlayer nanofiltration membrane
CN118416706A
Highly selective ultrathin polymer nanofilm composite membrane and process for preparation thereof