Sulfur dioxide low-temperature adsorbent as well as preparation method and application thereof

By using a mixture carrier of aluminum hydroxide and zirconium hydroxide and active components of metal copper and potassium in sulfur dioxide adsorbent, a low-temperature sulfur dioxide adsorbent was prepared, which solved the high energy consumption and adsorption capacity in the prior art. The problem of insufficient achieves efficient and low-cost sulfur dioxide adsorption effect.

CN118925656AActive Publication Date: 2024-11-12PETROCHINA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310522235.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

The lack of sulfur dioxide adsorbents in the prior art is low in operating temperature and good adsorption capacity, resulting in high energy consumption and increased equipment investment costs.

Method used

Using a mixture of aluminum hydroxide and zirconium hydroxide as the carrier, combined with metal copper and/or metal potassium as the active component, sulfur dioxide low-temperature adsorbent is prepared through impregnation reaction and high-temperature calcination to ensure uniform distribution of active metals and reduce the activation of sulfur dioxide and adsorbents. able.

Benefits of technology

High-efficiency sulfur dioxide adsorption is achieved at an operating temperature of 280℃, with a sulfur capacity of more than 95mg/g, reducing energy consumption and equipment investment costs, and simplifying the preparation process and production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the technical field of gas adsorbents, and particularly relates to a sulfur dioxide low-temperature adsorbent as well as a preparation method and application thereof. The sulfur dioxide low-temperature adsorbent comprises a carrier and an active component loaded on the carrier, the carrier is a mixture of aluminum hydroxide and zirconium hydroxide, and the mass ratio of the aluminum hydroxide to the zirconium hydroxide is 4: 1-4; the active component is metal copper and / or metal potassium; the mass ratio of the carrier to the active component is 100: (4-15). The sulfur dioxide low-temperature adsorbent provided by the invention can effectively adsorb sulfur dioxide in flue gas at the working temperature of 280 DEG C, and the sulfur capacity reaches 95 mg / g or above, so that the sulfur dioxide low-temperature adsorbent has the advantages of low working temperature, low energy consumption and high sulfur dioxide adsorption efficiency. The preparation process is simple and easy to operate, the production flow is short, and the production cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of gas adsorbents, and in particular relates to a sulfur dioxide low-temperature adsorbent, a preparation method and application thereof. Background Art

[0002] Sulfur dioxide is a common air pollutant. Reducing sulfur dioxide emissions and controlling air pollution have become one of the important issues in my country's environmental protection. At present, the main technologies for sulfur dioxide treatment can be divided into wet treatment technology and dry treatment technology. The wet treatment technologies mainly include limestone-gypsum desulfurization, calcium-sodium double alkali desulfurization and wet ammonia desulfurization; the dry treatment technologies mainly include activated carbon adsorption, plasma and microwave desulfurization. The equipment or facilities currently in operation show that wet desulfurization has major problems such as high investment costs, large floor space and easy corrosion of equipment, which affect the normal operation of enterprises and make it difficult to meet the national requirements for total sulfur emissions. Dry treatment technology has attracted great attention from various research institutions and enterprises due to its advantages such as small footprint, less equipment requirements and less investment.

[0003] The working temperature of the commonly used sulfur dioxide adsorbents is mostly greater than 500°C, and a heating unit needs to be set up separately, which consumes a lot of energy. CN104190432A discloses an activated carbon catalyst with high efficiency and low temperature denitrification and synergistic desulfurization, with SnCl 4 and V 2 O 5 As the active component, activated carbon is used as the carrier, and Fe 2 O 3 and CeO 2 As an auxiliary agent, the catalyst has a nitrogen oxide purification efficiency of more than 85% in the range of 70-200°C, but its sulfur capacity is relatively low, only 36 mg / g.

[0004] Therefore, the existing technology lacks a sulfur dioxide adsorbent with low working temperature and good adsorption capacity, which becomes a technical problem that needs to be solved urgently. Summary of the invention

[0005] In view of the above problems, the present invention provides a sulfur dioxide low-temperature adsorbent, a preparation method and application thereof. The sulfur dioxide low-temperature adsorbent can achieve efficient adsorption of sulfur dioxide at a relatively low operating temperature, greatly reducing the energy consumption and equipment investment cost during the adsorption process.

[0006] In a first aspect of the present invention, a sulfur dioxide low-temperature adsorbent is provided, which comprises a carrier and an active component supported on the carrier; the carrier is a mixture of aluminum hydroxide and zirconium hydroxide, and the mass ratio of the aluminum hydroxide to the zirconium hydroxide is 1 to 4:4; the active component is metallic copper and / or metallic potassium; the mass ratio of the carrier to the active component is 100:4 to 15. Further, the active component is metallic copper and metallic potassium; further, the molar ratio of the metallic copper to the metallic potassium is 1:0.5 to 3.

[0007] The second aspect of the present invention provides a method for preparing the aforementioned sulfur dioxide low-temperature adsorbent, comprising the following steps:

[0008] S1. Take aluminum hydroxide coarse powder and zirconium hydroxide coarse powder, dry, grind and sieve them respectively to obtain aluminum hydroxide fine powder and zirconium hydroxide fine powder;

[0009] S2. The copper source solution, potassium source solution, aluminum hydroxide fine powder and zirconium hydroxide fine powder are mixed for impregnation reaction, and then solid-liquid separation, drying and high-temperature calcination are performed to obtain the product.

[0010] Furthermore, in step S1, the drying temperature is 70-80° C., the drying time is 3-4 hours, and the sieving is performed to 200-300 meshes.

[0011] Furthermore, in step S2, the copper source is copper sulfate, and the mass concentration of the copper source in the copper source solution is 8-15%; the potassium source is potassium chloride, and the mass concentration of the potassium source in the potassium source solution is 10-20%.

[0012] Furthermore, in step S2, the mass volume ratio of the copper source solution, the potassium source solution, the aluminum hydroxide fine powder and the zirconium hydroxide fine powder is 50 mL: 50 mL: 20-30 g: 30-80 g.

[0013] Furthermore, in step S2, the temperature of the impregnation reaction is 40-70° C., and the time of the impregnation reaction is 2-3 hours.

[0014] Furthermore, in step S2, the drying temperature is 60-80°C, and the drying time is 2-3 hours.

[0015] Furthermore, in step S2, the temperature of the high temperature calcination is 300-400° C., and the time of the high temperature calcination is 3-4 hours.

[0016] The third aspect of the present invention provides the use of the aforementioned sulfur dioxide low-temperature adsorbent in reducing the sulfur dioxide emission concentration in flue gas.

[0017] The beneficial effects of the present invention are:

[0018] 1. The sulfur dioxide low-temperature adsorbent provided by the present invention has active metals that can be evenly distributed on the carrier, and the complex formed by the active metals and the carrier can reduce the activation energy of the reaction between sulfur dioxide and the active sites of the adsorbent, and can effectively adsorb sulfur dioxide in flue gas at an operating temperature of 280°C, with a sulfur capacity of more than 95 mg / g. Therefore, it has the advantages of low operating temperature, low energy consumption and high sulfur dioxide adsorption efficiency.

[0019] 2. The preparation process of the sulfur dioxide low-temperature adsorbent provided by the present invention is simple and easy to operate, with a short production process and low production cost. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] The present embodiment provides a sulfur dioxide low-temperature adsorbent, which is prepared by the following method: 100g aluminum hydroxide coarse powder and 100g zirconium hydroxide coarse powder are dried at 80°C for 3h, ground into fine powder with a mortar, sieved, and set aside. 200mL of 8% copper sulfate aqueous solution is prepared, 30g of 200-mesh zirconium hydroxide fine powder and 30g of 200-mesh aluminum hydroxide fine powder are added to 100mL of 8% copper sulfate aqueous solution, stirred at 40°C for 3h to obtain a uniform mixture, and then filtered to obtain a slurry, the slurry is dried at 60°C in a drying oven for 3h, and then roasted at 300°C for 3h to obtain.

[0023] Example 2

[0024] The present embodiment provides a sulfur dioxide low-temperature adsorbent, which is prepared by the following method: 100g aluminum hydroxide coarse powder and 100g zirconium hydroxide coarse powder are dried at 70°C for 4h, ground into fine powder with a mortar, sieved, and set aside. 200mL of 15% copper sulfate aqueous solution is prepared, 40g of 300-mesh zirconium hydroxide fine powder and 30g of 300-mesh aluminum hydroxide fine powder are added to 100mL of 15% copper sulfate aqueous solution, stirred at 70°C for 2h to obtain a uniform mixture, and then filtered to obtain a slurry, the slurry is dried at 70°C in a drying oven for 3h, and then roasted at 400°C for 3h.

[0025] Example 3

[0026] The present embodiment provides a sulfur dioxide low-temperature adsorbent, which is prepared by the following method: 100g of aluminum hydroxide coarse powder and 100g of zirconium hydroxide coarse powder are dried at 80°C for 3h, ground into fine powder with a mortar, sieved, and set aside. Prepare 200mL of 15% copper sulfate aqueous solution and 200mL of 10% potassium chloride aqueous solution, take 50mL of the two solutions and mix them evenly to obtain a mixed solution. Take 30g of 300-mesh zirconium hydroxide fine powder and 30g of 200-mesh aluminum hydroxide fine powder and add them to 100mL of the mixed solution, stir at 50°C for 3h to obtain a uniform mixture, and then filter to obtain a slurry, dry the slurry at 80°C in a drying oven for 2h, and then roast at 400°C for 3h.

[0027] Example 4

[0028] The present embodiment provides a sulfur dioxide low-temperature adsorbent, which is prepared by the following method: 100g of aluminum hydroxide coarse powder and 100g of zirconium hydroxide coarse powder are dried at 80°C for 3h, ground into fine powder with a mortar, sieved, and set aside. Prepare 200mL of 15% copper sulfate aqueous solution and 200mL of 20% potassium chloride aqueous solution, take 50mL of the two solutions and mix them evenly to obtain a mixed solution. Take 80g of 300-mesh zirconium hydroxide fine powder and 20g of 300-mesh aluminum hydroxide fine powder and add them to the mixed solution, stir at 50°C for 3h to obtain a uniform mixture, and then filter to obtain a slurry, dry the slurry at 80°C in a drying oven for 3h, and then roast at 400°C for 4h.

[0029] Comparative Example 1

[0030] The comparative example provides a sulfur dioxide low-temperature adsorbent, which is prepared by the following method: drying 100g of ferric hydroxide coarse powder at 80°C for 3h, grinding it into fine powder with a mortar, sieving it, and setting it aside. Preparing 200mL of 8% copper sulfate aqueous solution, taking 60g of 200-mesh ferric hydroxide fine powder and adding it to 100mL of 8% copper sulfate aqueous solution, stirring at 40°C for 3h to obtain a uniform mixture, and then filtering to obtain a slurry, drying the slurry at 60°C in a drying oven for 3h, and then roasting at 300°C for 3h to obtain the slurry.

[0031] Comparative Example 2

[0032] The comparative example provides a sulfur dioxide low-temperature adsorbent, which is prepared by the following method: 100g aluminum hydroxide coarse powder and 100g zirconium hydroxide coarse powder are dried at 80°C for 3h, ground into fine powder with a mortar, sieved, and set aside. 200mL of 8% magnesium chloride aqueous solution is prepared, 30g of 200-mesh zirconium hydroxide fine powder and 30g of 200-mesh aluminum hydroxide fine powder are added to 100mL of 8% magnesium chloride aqueous solution, stirred at 40°C for 3h to obtain a uniform mixture, and then filtered to obtain a slurry, the slurry is dried at 60°C in a drying oven for 3h, and then calcined at 300°C for 3h to obtain.

[0033] Test example

[0034] The sulfur dioxide low temperature adsorbent prepared in Examples 1 to 4 and Comparative Examples 1 to 2 was subjected to an adsorption regeneration evaluation experiment, wherein the adsorption temperature was controlled to be 280°C. The sulfur dioxide low temperature adsorbent was loaded into a fixed bed reactor, and when the sulfur dioxide concentration at the outlet of the fixed bed reactor was greater than 100 mg / m 3 When the adsorption process is completed, the sulfur content of the adsorbent is measured by using a gas chromatograph equipped with a TCD detector to detect the concentration of sulfur-containing gas in the outlet gas of the fixed bed reactor (filled with adsorbent). The SO 2 In determining the SO 2 When the adsorption capacity of sulfur is 100%, the gas composition other than water is SO 2 Concentration 1.5%, O 2 Concentration 3%, CO 2 The concentration is 25%, the balance is N 2 . SO 2 The specific calculation formula for the adsorption sulfur capacity is as follows:

[0035]

[0036] Among them, C is SO 2 The concentration of (in mol / L), V is the volume of gas passing through the adsorbent (in L), and 64 is SO 2 The molar mass of SO is 22.4. 2 The molar volume of the adsorbent is , and M is the mass of the adsorbent (in g).

[0037]

[0038] As can be seen from the above table, the sulfur capacity of the sulfur dioxide low-temperature adsorbents of Examples 1-4 of the present invention is above 95 mg / g, which is comparable to the sulfur capacity of existing common sulfur dioxide adsorbents, and has stable performance. The sulfur capacity of the adsorbents of Comparative Examples 1 to 2 is significantly lower than that of the adsorbents of Examples 1-4, which shows that the carrier and active component composition of the limited composition of the present invention can further improve the sulfur dioxide adsorption effect, and is conducive to the preparation of a sulfur dioxide adsorbent with better adsorption performance. In addition, compared with the adsorption temperature of existing common sulfur dioxide adsorbents generally above 500°C, the adsorption temperature (280°C) of the sulfur dioxide adsorbent prepared in the embodiment of the present invention is significantly lower, which is conducive to reducing energy consumption and production costs.

[0039] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

Claims

1. A sulfur dioxide low-temperature adsorbent, characterized in that: It comprises a carrier and an active component loaded on the carrier; the carrier is a mixture of aluminum hydroxide and zirconium hydroxide, the mass ratio of the aluminum hydroxide to the zirconium hydroxide is 1-4:4; the active component is metal copper and / or metal potassium; the mass ratio of the carrier to the active component is 100:4-15.

2. The sulfur dioxide low-temperature adsorbent according to claim 1, characterized in that: The active components are metallic copper and metallic potassium; preferably, the molar ratio of the metallic copper to the metallic potassium is 1:0.5-3.

3. The method for preparing the sulfur dioxide low-temperature adsorbent according to claim 2, characterized in that: The steps include: S1. Take aluminum hydroxide coarse powder and zirconium hydroxide coarse powder, dry, grind and sieve them respectively to obtain aluminum hydroxide fine powder and zirconium hydroxide fine powder; S2. The copper source solution, potassium source solution, aluminum hydroxide fine powder and zirconium hydroxide fine powder are mixed for impregnation reaction, and then solid-liquid separation, drying and high-temperature calcination are performed to obtain the product.

4. The method for preparing the sulfur dioxide low-temperature adsorbent according to claim 3, characterized in that: In step S1, the drying temperature is 70-80°C, the drying time is 3-4 hours, and the sieving is performed to 200-300 meshes.

5. The method for preparing the sulfur dioxide low-temperature adsorbent according to claim 3, characterized in that: In step S2, the copper source is copper sulfate, and the mass concentration of the copper source in the copper source solution is 8-15%; the potassium source is potassium chloride, and the mass concentration of the potassium source in the potassium source solution is 10-20%.

6. The method for preparing the sulfur dioxide low-temperature adsorbent according to claim 3, characterized in that: In step S2, the mass volume ratio of the copper source solution, the potassium source solution, the aluminum hydroxide fine powder and the zirconium hydroxide fine powder is 50 mL: 50 mL: 20-30 g: 30-80 g.

7. The method for preparing the sulfur dioxide low-temperature adsorbent according to claim 3, characterized in that: In step S2, the temperature of the impregnation reaction is 40-70° C., and the time of the impregnation reaction is 2-3 hours.

8. The method for preparing the sulfur dioxide low-temperature adsorbent according to claim 3, characterized in that: In step S2, the drying temperature is 60-80°C, and the drying time is 2-3 hours.

9. The method for preparing the sulfur dioxide low-temperature adsorbent according to claim 3, characterized in that: In step S2, the temperature of the high temperature calcination is 300-400°C, and the time of the high temperature calcination is 3-4 hours.

10. Use of the sulfur dioxide low-temperature adsorbent according to claim 1 or 2 in reducing the sulfur dioxide emission concentration in flue gas.

Citation Information

Patent Citations

  • Claus tail gas SO2 sorbent and preparation and use thereof

    CN104209084A

  • Method for preparing modified mesoporous alumina adsorbent for desulfurization and denitration

    CN104785196A

  • Desulfurization and denitrification catalyst with magnesium aluminum hydrotalcite as carriers and preparing method and application thereof

    CN106362744A

  • Production technology of gas desulfurizer

    CN107569966A

  • Mesoporous alumina-based adsorbent as well as preparation method and application thereof

    CN111330534A