Sodium alginate-based sponge-like body as well as preparation method and application thereof
By using polyazanecyclopropane and polysaccharide dialdehyde derivatives as crosslinking agents, stable sodium alginate-based cavernosomes are formed, the cytotoxicity and environmental pollution of glutaraldehyde are solved, and efficient heavy metal adsorption is achieved and environmentally friendly water pollution treatment.
Patent Information
- Application Number
- CN202411022302.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the use of glutaraldehyde as a chemical crosslinking agent for sodium alginate has the risk of cytotoxicity and environmental pollution, and it is difficult to achieve green and environmentally friendly water pollution treatment.
Polyazane and polysaccharide dialdehyde derivatives are used as crosslinking agents to form stable sodium alginate-based caverns through reaction and double crosslinking under specific pH conditions, which are used for water pollution control.
A solid structure, loose and porous sodium alginate-based cavernosate was obtained, with good heavy metal adsorption ability, and the material itself was green and environmentally friendly. It was suitable for water pollution control projects, reducing the difficulty and cost of the preparation process.
Smart Images

Figure CN118925682A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of heavy metal ion adsorbents, and in particular to a sodium alginate-based sponge and a preparation method and application thereof. Background Art
[0002] Sodium alginate is a polysaccharide carbohydrate extracted from algae such as brown algae or green algae. It is rich in hydroxyl and carboxyl groups and can react with various pollutants in water. Therefore, it is widely used in water pollution control engineering. However, due to its poor mechanical properties, low stability in application, and easy breakage, sodium alginate cannot be widely used. Generally, it is necessary to improve the stability of sodium alginate through modification methods such as physical cross-linking and chemical cross-linking so that it can be better used in the field of water treatment.
[0003] In the prior art, glutaraldehyde (GA) is commonly used as a chemical crosslinking agent for sodium alginate-based materials. For example, the invention patent with application number CN201610432403.2, based on the effect of glutaraldehyde, grafts and crosslinks sodium alginate to the surface of attapulgite by covalent bonds. The two have strong binding force. During use, sodium alginate is not easy to fall off from the surface of the carrier and freely agglomerates, showing good adsorption performance for heavy metal pollution. Another example is another invention patent with application number CN202111484023.0, in which kaolin and polyacrylamide are added to sodium alginate and polyvinyl alcohol solution, stirred to obtain a mixed solution, and then the surface is sprayed with CaCl2 aqueous solution for ion penetration crosslinking and shaping, and finally crosslinked and cured with glutaraldehyde.
[0004] However, glutaraldehyde has certain cytotoxicity, and inhalation, ingestion or percutaneous absorption is harmful. Inhalation can cause inflammation of the larynx and bronchus, chemical pneumonia, pulmonary edema, etc.; it has a strong irritation to the eyes, skin and mucous membranes; and it is harmful to the environment and can pollute water bodies. And it is difficult to completely remove residual glutaraldehyde by washing, and the material prepared using glutaraldehyde as a cross-linking agent has a greater harm for the treatment of water pollution, which is contrary to the original intention of the green and pollution-free biomass material. Therefore, finding a more environmentally friendly cross-linking agent is a problem that needs to be solved urgently. Summary of the invention
[0005] The object of the present invention is to provide a sodium alginate-based sponge and a preparation method and application thereof in view of the above-mentioned problems.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a method for preparing a sodium alginate-based sponge, comprising the following steps:
[0008] (1) adding deionized water to the polyaziridine solution, mixing evenly, and adjusting the pH to 6-7 to prepare a diluted polyaziridine solution;
[0009] (2) dispersing sodium alginate in deionized water and homogenizing for 5-10 minutes to prepare a sodium alginate paste;
[0010] (3) under continuous stirring, adding the diluted polyethylenimine solution obtained in step (1) to the sodium alginate paste obtained in step (2) in 5 portions, with the same amount added each time and the same interval between two adjacent additions. After the addition of the diluted polyethylenimine solution is completed, continuing to homogenize for a certain period of time to obtain a mixed solution;
[0011] (4) allowing the mixed solution obtained in step (3) to stand at room temperature for 24-48 hours to initially cross-link to obtain a sodium alginate / polyaziridine structure hydrogel;
[0012] (5) dissolving the polysaccharide powder in anhydrous ethanol and adding ammonium persulfate solution, reacting for 6 to 8 hours under stirring, then adding sodium bisulfite under continuous stirring, and heating in a water bath while stirring for 0.5 to 1 hour, and then dialyzing with deionized water for 3 to 4 days to prepare a polysaccharide dialdehyde derivative solution;
[0013] (6) adding the sodium alginate / polyethylenimine structure hydrogel prepared in step (4) to the polysaccharide dialdehyde derivative solution prepared in step (5), shaking for 24-48 hours, and after double cross-linking, washing and drying to obtain a sodium alginate-based sponge.
[0014] Preferably, in the above preparation method, the mass fraction of the diluted polyaziridine solution in step (1) is 3% to 6%;
[0015] Preferably, in the above preparation method, nitric acid or hydrochloric acid is added in step (1) to adjust the pH value.
[0016] Preferably, in the above preparation method, the mass fraction of the sodium alginate paste prepared in step (2) is 0.6% to 1%.
[0017] Preferably, in the above preparation method, in step (3), the diluted polyaziridine solution is added dropwise every 10 seconds, and after the addition is completed, the slurry is stirred for 10-20 seconds to obtain a mixed solution.
[0018] Preferably, in the above preparation method, in step (5), the polysaccharide powder is sodium alginate powder, chitosan powder, dextran powder or plant starch powder.
[0019] Preferably, in the above preparation method, in step (5), the mass of anhydrous ethanol is 4-5 times the mass of the polysaccharide powder; the mass fraction of ammonium persulfate solution is 4% to 6%, and its mass is 1.25-1.3 times that of anhydrous ethanol; and the mass of sodium bisulfite is 0.02-0.05 times that of anhydrous ethanol.
[0020] The present invention also provides a sodium alginate-based sponge prepared by the preparation method.
[0021] In addition, the sodium alginate-based sponge has good heavy metal adsorption capacity and can be used as an adsorbent in water pollution control projects.
[0022] In summary, due to the adoption of the above technical solution, the present invention has the following beneficial effects:
[0023] 1. The present invention uses sodium alginate as a matrix, first mixes sodium alginate with a polyaziridine solution under specific pH conditions, initially cross-links to form a sodium alginate gel, and then uses a self-made polysaccharide dialdehyde derivative solution cross-linking agent to react with the sodium alginate gel, and double cross-links to strengthen the three-dimensional structure of the material to form a sodium alginate-based sponge. The self-made polysaccharide dialdehyde derivative solution of the present invention has low biological toxicity, and the aldehyde group thereon can undergo a cross-linking reaction with the amino group in the polyaziridine, which provides good conditions for producing a sodium alginate-based sponge with a stable structure and loose porous. The sodium alginate-based sponge prepared by the present invention can be used as an adsorbent in water pollution control projects, has strong plasticity and can adapt to different scenarios, has no secondary pollution and is easy to separate solids and liquids. In addition, the preparation method of the present invention is simple, the raw materials are green and environmentally friendly, easy to obtain, and have strong scalability.
[0024] 2. The present invention uses ammonium persulfate as an oxidant and initiator to interrupt the long-chain molecules on the polysaccharide molecular chain and oxidize to obtain aldehyde groups, which fully react with the amino groups on polyaziridine to form a stable structure, thereby successfully cross-linking polyaziridine and sodium alginate to obtain a high-strength sodium alginate-based sponge. At the same time, ammonium persulfate is used as an oxidant and initiator, which has the advantages of low cost and no environmental pollution, avoids the use of highly toxic substances such as glutaraldehyde, and solves the situation where the scope of use is limited due to the cytotoxicity of chemical cross-linking agents. The preparation method provided by the present invention improves the stability and plasticity of the adsorption material, reduces the difficulty of the existing preparation process, and the prepared sodium alginate-based sponge has a good adsorption effect on some heavy metals (the adsorption efficiency of Cr (VI) is 95%), while the adsorption material itself is more green and environmentally friendly.
[0025] 3. The present invention preliminarily forms a sponge-like body through the full reaction of sodium alginate and polyaziridine. The operation is simple and convenient. The raw materials are green and environmentally friendly, easy to obtain, highly safe, and highly scalable. The preparation process is suitable for mass production. The prepared sodium alginate-based sponge-like body has a three-dimensional network structure with better stability, strong plasticity, and can be applied to various scenarios. It has broad application prospects in the field of water pollution control engineering. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM image of the sodium alginate-based sponge prepared in the present invention.
[0027] Figure 2 This is a Fourier infrared spectrum of the sodium alginate-based sponge prepared by the present invention.
[0028] Figure 3 This is the Langmuir fitting curve of sodium alginate sponge material.
[0029] Figure 4 This is a picture of the finished product of sodium alginate sponge material. DETAILED DESCRIPTION
[0030] The invention provides a sodium alginate-based sponge-like body, which can be used as an adsorbent in water pollution control projects.
[0031] The method for preparing the sodium alginate-based sponge comprises the following steps:
[0032] (1) adding deionized water to the polyethylenimine solution, mixing evenly, adding nitric acid or hydrochloric acid to adjust the pH to 6-7, and preparing a diluted polyethylenimine solution, wherein the mass fraction of the diluted polyethylenimine solution is 3% to 6%;
[0033] (2) dispersing sodium alginate in deionized water and homogenizing for 5-10 minutes to prepare a paste of sodium alginate with a mass fraction of 0.6% to 1%;
[0034] (3) under continuous stirring, adding the diluted polyethylenimine solution obtained in step (1) to the sodium alginate paste obtained in step (2) in 5 portions, adding the diluted polyethylenimine solution dropwise every 10 seconds, with the same amount added each time. After the diluted polyethylenimine solution is added, stirring the slurry for 10-20 seconds to obtain a mixed solution;
[0035] (4) quickly pouring the mixed solution obtained in step (3) into a template container, wherein the template container can be selected as a rectangular container or a cylindrical container as needed, and the external shape of the sponge-like body varies according to the template container; then placing the template container at room temperature for 24-48 hours to obtain a sodium alginate / polyaziridine structure hydrogel by preliminary cross-linking;
[0036] (5) dissolving polysaccharide powder in anhydrous ethanol, wherein the polysaccharide powder used includes but is not limited to sodium alginate, chitosan, dextran, plant starch, etc., the mass of anhydrous ethanol is 4-5 times the mass of sodium alginate, and adding a 4%-6% ammonium persulfate solution as a strong oxidant, the mass of which is 0.8 times the mass of anhydrous ethanol, and reacting for 6-8 hours under stirring; then adding sodium bisulfite under continuous stirring, the mass of which is 0.02-0.05 times the mass of anhydrous ethanol, and heating in a water bath while stirring for 0.5-1 hour; then using a dialysis membrane with a molecular weight cutoff of 8000-14000MW to make a dialysis bag for deionized water dialysis, the dialysis bag needs to reserve at least 3-4 times the volume of the liquid poured into the bag; changing the water in the dialysis bag at least 3 times a day, for 3-4 days, and after the dialysis is completed, taking out the prepared polysaccharide dialdehyde derivative solution from the dialysis bag and sealing it for storage;
[0037] (6) adding the sodium alginate / polyethylenimine structure hydrogel prepared in step (4) to the polysaccharide dialdehyde derivative solution prepared in step (5), shaking for 24-48 hours, double cross-linking, washing, and drying to obtain a sodium alginate / polyethylenimine sponge;
[0038] Among them, drying can be carried out by vacuum freeze drying or natural air drying; vacuum freeze drying requires that the moisture content of the sodium alginate-based sponge with a water content of 60%-70% be controlled below 5%; the operating steps of natural air drying are: placing the washed sodium alginate-based sponge in a fume hood at room temperature for 3-5 days.
[0039] The finished product of the prepared sodium alginate sponge material is shown in the figure Figure 4 shown.
[0040] In order to express the present invention more clearly, the present invention is further described below through specific examples.
[0041] 1. Preparation Example
[0042] Example 1
[0043] This embodiment provides a method for preparing a sodium alginate-based sponge, comprising the following steps:
[0044] (1) adding deionized water to the polyaziridine solution, mixing well, adding nitric acid to adjust the pH to 6, and preparing 25 g of a 3% polyaziridine solution;
[0045] (2) dispersing 0.6 g of sodium alginate in ionized water, stirring the mixture for 5 minutes using a homogenizer to uniformly distribute the mixture, and preparing 100 g of sodium alginate paste having a mass fraction of 0.6%;
[0046] (3) stirring the sodium alginate paste prepared in step (2) using a homogenizer, and under continuous stirring, adding the 3% polyaziridine solution obtained in step (1) dropwise in 5 portions, 5 g each time, with an interval of 10 seconds between each addition. After the addition is completed, stirring is continued for 10 seconds using a homogenizer to obtain a mixed solution;
[0047] (4) quickly pouring the mixed solution obtained in step (3) into a template container, wherein the template container is a rectangular container or a cylindrical container, and template containers of different shapes can be selected according to the needs of the sponge-like external shape; and placing the template container at room temperature for 24 hours to initially cross-link and obtain a sodium alginate / polyaziridine structure hydrogel;
[0048] (5) dissolving ammonium persulfate in deionized water to prepare 20 g of an ammonium persulfate solution with a mass fraction of 4%; then dissolving sodium alginate powder in anhydrous ethanol to prepare 25 g of a sodium alginate solution with a mass fraction of 20%, and adding the ammonium persulfate solution, stirring and reacting at room temperature for 6 hours, then adding 0.5 g of sodium bisulfite under continuous magnetic stirring, and heating in a water bath for 0.5 hours while stirring, and then dialyzing the reaction solution against deionized water for 3 days using a dialysis membrane with a molecular weight cutoff of 8000-14000 MW, changing the water in the dialysis bag at least 3 times a day, and after the dialysis is completed, taking out the prepared polysaccharide dialdehyde derivative solution from the dialysis bag and sealing it for storage;
[0049] (6) taking out the sodium alginate / polyethylenimine structure hydrogel obtained in step (4), washing it with deionized water, pouring it into a mold containing 300 ml of the polysaccharide dialdehyde derivative solution, placing it on a shaker at a speed of 50 rpm to fully shake and react for 24 hours; washing it with deionized water, and then freeze-drying it to obtain a sodium alginate / polyethylenimine sponge, that is, the sodium alginate-based sponge.
[0050] The sodium alginate / polyethylenimine sponge was scanned by electron microscope and the following results were obtained: Figure 1 As shown in the SEM image, several wrinkles and holes can be seen on its surface.
[0051] Figure 2The Fourier transform infrared spectrum (FTIR) of the sodium alginate-based sponge is shown in Figure 1, with the main peak at 3250 cm -1 (overlapping NH and OH stretching vibrations), 2930 cm -1 (CH stretching vibration), 1590cm -1 (NH bending and C=N vibration), 1410cm -1 (COO-symmetrical extension), 1300cm -1 (CN stretch vibration), 1090cm -1 and 1030cm -1 (CO stretch vibration) and 947cm -1 (CH deformation). It is worth noting that 1592cm -1 The peak at confirms that the sodium alginate-based sponge prepared by the present invention has the structure of Schiff base, indicating that the polysaccharide dialdehyde derivatives are successfully cross-linked with polyaziridine, indicating that the use of low-toxic cross-linking agents can allow the sodium alginate-based sponge to have an adsorption effect that is no less than that of using glutaraldehyde as a cross-linking agent.
[0052] Example 2
[0053] This embodiment provides a method for preparing a sodium alginate-based sponge, comprising the following steps:
[0054] (1) Add deionized water to the polyaziridine solution, mix well, add hydrochloric acid to adjust the pH to 6.5, and prepare 25 g of a 4% polyaziridine solution;
[0055] (2) dispersing sodium alginate in deionized water, stirring for 10 minutes with a homogenizer to make it evenly distributed, and preparing 100 g of sodium alginate paste with a mass fraction of 0.7%;
[0056] (3) stirring the sodium alginate paste prepared in step (2) using a homogenizer, and under continuous stirring, adding the 4% polyaziridine solution obtained in step (1) dropwise in 5 portions, 5 g each time, with an interval of 10 seconds between each addition. After the addition is completed, stirring is continued for 10 seconds using a homogenizer to obtain a mixed solution;
[0057] (4) quickly pouring the mixed solution obtained in step (3) into a template container, wherein the template container is a rectangular container or a cylindrical container, and template containers of different shapes can be selected according to the needs of the sponge-like external shape; and placing the template container at room temperature for 36 hours to initially cross-link and obtain a sodium alginate / polyaziridine structure hydrogel;
[0058] (5) dissolving 1 g of ammonium persulfate in deionized water to prepare 20 g of 5% ammonium persulfate solution; then dissolving chitosan powder in anhydrous ethanol to prepare 25 g of 24% chitosan solution, adding the ammonium persulfate solution, stirring and reacting at room temperature for 8 h, then adding 0.5 g of sodium bisulfite under continuous magnetic stirring, and heating in a water bath for 1 h while stirring, then dialyzing the reaction solution against deionized water for 4 days using a dialysis membrane with a molecular weight cutoff of 8000-14000 MW, changing the water in the dialysis bag at least 3 times a day, and taking out the prepared polysaccharide dialdehyde derivative solution from the dialysis bag after the dialysis is completed, and sealing and storing;
[0059] (6) Take out the sodium alginate / polyethylenimine structure hydrogel obtained in step (4), wash it with deionized water, pour it into a mold containing 300 ml of the polysaccharide dialdehyde derivative solution, and place it on a shaker at a speed of 50 rpm to fully shake and react for 24 hours; wash it with deionized water, and then place it in a ventilated place to dry naturally, thereby obtaining a sodium alginate-based sponge.
[0060] Example 3
[0061] This embodiment provides a method for preparing a sodium alginate-based sponge, comprising the following steps:
[0062] (1) adding deionized water to the polyaziridine solution, mixing well, adding nitric acid to adjust the pH to 7, and preparing 25 g of a 5% polyaziridine solution;
[0063] (2) dispersing sodium alginate in ionized water, stirring for 5-10 minutes with a homogenizer to make it evenly distributed, and preparing 100 g of sodium alginate paste with a mass fraction of 0.8%;
[0064] (3) stirring the sodium alginate paste prepared in step (2) using a homogenizer, and under continuous stirring, adding the 5% polyaziridine solution obtained in step (1) dropwise in 5 portions, 5 g each time, with an interval of 10 seconds between each addition. After the addition is completed, stirring is continued for 10 seconds using a homogenizer to obtain a mixed solution;
[0065] (4) quickly pouring the mixed solution obtained in step (3) into a template container, wherein the template container is a rectangular container or a cylindrical container, and template containers of different shapes can be selected according to the needs of the sponge-like external shape; and placing the template container at room temperature for 48 hours to initially cross-link and obtain a sodium alginate / polyaziridine structure hydrogel;
[0066] (5) dissolving ammonium persulfate in deionized water to prepare 20 g of an ammonium persulfate solution with a mass fraction of 4%; then dissolving dextran powder in anhydrous ethanol to prepare 25 g of a dextran solution with a mass fraction of 25%, and adding the ammonium persulfate solution, stirring and reacting at room temperature for 6 hours, then adding 1.25 g of sodium bisulfite under continuous magnetic stirring, and heating in a water bath for 0.5 hours while stirring, and then dialyzing the reaction solution against deionized water for 3 days using a dialysis membrane with a molecular weight cutoff of 8000-14000 MW, changing the water in the dialysis bag at least 3 times a day, and after the dialysis is completed, taking out the prepared polysaccharide dialdehyde derivative solution from the dialysis bag and sealing it for storage;
[0067] (6) Take out the sodium alginate / polyethylenimine structure hydrogel obtained in step (4), wash it with deionized water, pour it into a mold containing 300 ml of the polysaccharide dialdehyde derivative solution, and place it on a shaker at a speed of 50 rpm to fully shake and react for 36 hours; wash it with deionized water, and then place it in a ventilated place to dry naturally, thereby obtaining a sodium alginate-based sponge.
[0068] Example 4
[0069] This embodiment provides a method for preparing a sodium alginate-based sponge, comprising the following steps:
[0070] (1) adding deionized water to the polyaziridine solution, mixing well, adding nitric acid to adjust the pH to 6.5, and preparing 25 g of a 6% polyaziridine solution;
[0071] (2) dispersing sodium alginate in ionized water, stirring for 5-10 minutes with a homogenizer to make it evenly distributed, and preparing 100 g of sodium alginate paste with a mass fraction of 0.9%;
[0072] (3) stirring the sodium alginate paste prepared in step (2) using a homogenizer, and under continuous stirring, adding the 6% polyaziridine solution obtained in step (1) dropwise in 5 portions, 5 g each time, with an interval of 10 seconds between each addition. After the addition is completed, stirring is continued for 10 seconds using a homogenizer to obtain a mixed solution;
[0073] (4) quickly pouring the mixed solution obtained in step (3) into a template container, wherein the template container is a rectangular container or a cylindrical container, and template containers of different shapes can be selected according to the needs of the sponge-like external shape; and placing the template container at room temperature for 24 hours to initially cross-link and obtain a sodium alginate / polyaziridine structure hydrogel;
[0074] (5) dissolving ammonium persulfate in deionized water to prepare 25 g of an ammonium persulfate solution with a mass fraction of 4.8%; then dissolving corn starch powder in anhydrous ethanol to prepare 25 g of a corn starch solution with a mass fraction of 20%, and adding the ammonium persulfate solution, stirring and reacting at room temperature for 6 hours, then adding 1.25 g of sodium bisulfite under continuous magnetic stirring, and heating in a water bath while stirring for 0.5 hours, then dialyzing the reaction solution against deionized water using a dialysis membrane with a molecular weight cutoff of 8000-14000 MW for 4 days, changing the water in the dialysis bag at least 3 times a day, and after the dialysis is completed, taking out the prepared polysaccharide dialdehyde derivative solution from the dialysis bag and sealing it for storage;
[0075] (6) Take out the sodium alginate / polyethylenimine structure hydrogel obtained in step (4), wash it with deionized water, pour it into a mold containing 300 ml of the polysaccharide dialdehyde derivative solution, and place it on a shaker at a speed of 50 rpm to fully shake and react for 48 hours; wash it with deionized water, and then place it in a ventilated place to dry naturally, thereby obtaining a sodium alginate-based sponge.
[0076] Example 5
[0077] This embodiment provides a method for preparing a sodium alginate-based sponge, comprising the following steps:
[0078] (1) adding deionized water to the polyaziridine solution, mixing well, adding nitric acid to adjust the pH to 6.5, and preparing 25 g of a 6% polyaziridine solution;
[0079] (2) dispersing 1 g of sodium alginate in ionized water, stirring for 5-10 minutes with a homogenizer to make it evenly distributed, and preparing 100 g of sodium alginate paste with a mass fraction of 1%;
[0080] (3) stirring the sodium alginate paste prepared in step (2) using a homogenizer, and under continuous stirring, adding the 6% polyaziridine solution obtained in step (1) dropwise in 5 portions, 5 g each time, with an interval of 10 seconds between each addition. After the addition is completed, stirring is continued for 10 seconds using a homogenizer to obtain a mixed solution;
[0081] (4) quickly pouring the mixed solution obtained in step (3) into a template container, wherein the template container is a rectangular container or a cylindrical container, and template containers of different shapes can be selected according to the needs of the sponge-like external shape; and placing the template container at room temperature for 24 hours to initially cross-link and obtain a sodium alginate / polyaziridine structure hydrogel;
[0082] (5) dissolving ammonium persulfate in deionized water to prepare 25 g of an ammonium persulfate solution with a mass fraction of 5%; then dissolving sodium alginate powder in anhydrous ethanol to prepare 25 g of a sodium alginate solution with a mass fraction of 22%, and adding the ammonium persulfate solution, stirring and reacting at room temperature for 6 hours, then adding 1.25 g of sodium bisulfite under continuous magnetic stirring, and heating in a water bath for 0.5 hours while stirring, and then dialyzing the reaction solution against deionized water using a dialysis membrane with a molecular weight cutoff of 8000-14000 MW for 4 days, changing the water in the dialysis bag at least 3 times a day, and after the dialysis is completed, taking out the prepared polysaccharide dialdehyde derivative solution from the dialysis bag and sealing it for storage;
[0083] (6) Take out the sodium alginate / polyethylenimine structure hydrogel obtained in step (4), wash it with deionized water, pour it into a mold containing 300 ml of the polysaccharide dialdehyde derivative solution, and place it on a shaker at a speed of 50 rpm to fully shake and react for 36 hours; wash it with deionized water, and then place it in a ventilated place to dry naturally, thereby obtaining a sodium alginate-based sponge.
[0084] Example 6
[0085] This embodiment provides a method for preparing a sodium alginate-based sponge, comprising the following steps:
[0086] (1) Add deionized water to the polyaziridine solution, mix well, add nitric acid to adjust the pH to 6.5, and prepare 25 g of a polyaziridine solution with a mass fraction of 3%;
[0087] (2) dispersing sodium alginate in ionized water, stirring for 5-10 minutes with a homogenizer to make it evenly distributed, and preparing 100 g of sodium alginate paste with a mass fraction of 0.8%;
[0088] (3) stirring the sodium alginate paste prepared in step (2) using a homogenizer, and under continuous stirring, adding the 3% polyaziridine solution obtained in step (1) dropwise in 5 portions, 5 g each time, with an interval of 10 seconds between each addition. After the addition is completed, stirring is continued for 10 seconds using a homogenizer to obtain a mixed solution;
[0089] (4) quickly pouring the mixed solution obtained in step (3) into a template container, wherein the template container is a rectangular container or a cylindrical container, and template containers of different shapes can be selected according to the needs of the sponge-like external shape; and placing the template container at room temperature for 24 hours to initially cross-link and obtain a sodium alginate / polyaziridine structure hydrogel;
[0090] (5) dissolving ammonium persulfate in deionized water to prepare 25 g of an ammonium persulfate solution with a mass fraction of 6%; then dissolving sodium alginate powder in anhydrous ethanol to prepare 40 g of an ammonium persulfate solution with a mass fraction of 25% and adding the ammonium persulfate solution, stirring and reacting at room temperature for 6 hours, then adding 1.25 g of sodium bisulfite under continuous magnetic stirring, and heating in a water bath for 0.5 hours while stirring, then dialyzing the reaction solution against deionized water for 3 days using a dialysis membrane with a molecular weight cutoff of 8000-14000 MW, changing the water in the dialysis bag at least 3 times a day, and after the dialysis is completed, taking out the prepared polysaccharide dialdehyde derivative solution from the dialysis bag and sealing it for storage;
[0091] (6) Take out the sodium alginate / polyethylenimine structure hydrogel obtained in step (4), wash it with deionized water, pour it into a mold containing 300 ml of the polysaccharide dialdehyde derivative solution, and place it on a shaker at a speed of 50 rpm to fully shake and react for 24 hours; wash it with deionized water, and then perform vacuum freeze-drying to obtain a sodium alginate-based sponge.
[0092] Comparative Example 1
[0093] This comparative example provides a method for preparing a sodium alginate-based sponge. The difference between this comparative example and Example 1 is that potassium permanganate solution is used instead of ammonium persulfate solution in step (5), and ethylene glycol is used instead of sodium bisulfite. The other steps are the same as those in Example 1.
[0094] The specific operation of step (5) of this comparative example is as follows: potassium permanganate is dissolved in deionized water to prepare 25g of potassium permanganate solution with a mass fraction of 6.4%; then sodium alginate is used as a raw material, sodium alginate powder is dissolved in anhydrous ethanol to prepare 25g of sodium alginate solution with a mass fraction of 20%, and the potassium permanganate solution is added, and the reaction is stirred at room temperature for 6h, and then 5ml of ethylene glycol is added under continuous magnetic stirring, and heated in a water bath while stirring for 0.5h, and then the reaction solution is dialyzed against deionized water for 3 days using a dialysis membrane with a molecular weight cutoff of 8000-14000MW, and the water in the dialysis bag is changed at least 3 times a day. After the dialysis is completed, the prepared polysaccharide dialdehyde derivative solution is taken out from the dialysis bag and sealed for storage.
[0095] Comparative Example 2
[0096] This comparative example provides a method for preparing a sodium alginate-based sponge. This comparative example can be prepared in only 5 steps, wherein steps (1) to (4) are the same as those in Example 1, except that in step (5) of this comparative example, glutaraldehyde solution is used instead of polysaccharide dialdehyde derivative solution to react with sodium alginate / polyethylenimine structure hydrogel to obtain a sodium alginate-based sponge.
[0097] The specific operation of step (5) of this comparative example is as follows: dissolving glutaraldehyde in deionized water to prepare 500 g of a glutaraldehyde solution with a mass fraction of 0.5%; placing the sodium alginate / polyethylenimine structure hydrogel in the glutaraldehyde solution, placing it on a shaker with a rotation speed of 50 rpm and fully shaking the reaction for 24 hours; washing it with deionized water, and then placing it in a ventilated place to dry naturally, thereby obtaining a sodium alginate-based sponge.
[0098] 2. Performance Test
[0099] 1. Adsorption rate experiment at different concentrations
[0100] (1) A total of 8 groups of experiments were conducted. In each group of experiments, 8 50 ml centrifuge tubes were taken. 30 mg of sodium alginate-based sponges prepared by Examples 1-6, Comparative Example 1 or the sodium alginate sponges prepared using glutaraldehyde as a cross-linking agent (referred to as Comparative Example 2) were added to each centrifuge tube. Then, heavy metal chromium ion Cr(VI) wastewater with a concentration of 10, 20, 40, 80, 100, 150, 250, and 350 mg / L was added to the 8 centrifuge tubes of each group of experiments, respectively. The tubes were placed in a shaker and continuously shaken at a constant temperature of 25 degrees Celsius for 3 days. After sampling, the concentration of the simulated heavy metal wastewater after treatment was measured using an ultraviolet spectrophotometer.
[0101] The adsorption capacity of various sodium alginate-based sponges for different concentrations of Cr(VI) at the optimal pH is shown in Table 1.
[0102] Table 1 Comparison of the adsorption of different concentrations of Cr(VI) by various sodium alginate-based sponges
[0103]
[0104]
[0105] As can be seen from Table 1, the sodium alginate-based sponge prepared by the present invention has an adsorption rate at high concentration that is significantly higher than that of the sodium alginate sponges obtained in Comparative Examples 1 and 2, indicating that the sodium alginate-based sponge prepared by the present invention not only reduces the toxicity caused by the use of glutaraldehyde, but also has better heavy metal adsorption capacity; in addition, the sodium alginate sponge prepared by using ammonium persulfate as an oxidant has a stronger adsorption capacity than that using other oxidants; indicating that the sodium alginate sponge prepared by the embodiment of the present invention has a better application prospect in the field of water treatment.
[0106] (3) Figure 3 This is the Langmuir fitting curve of the sodium alginate sponge material in Example 1. The good fitting indicates that the adsorption may follow a monolayer adsorption mechanism.
[0107] 2. Adsorption effect experiment at different pH
[0108] A total of 8 groups of experiments were conducted, and 5 50ml centrifuge tubes were taken in each group of experiments. 30mg of sodium alginate-based sponges prepared by Examples 1-6, Comparative Example 1 or the sodium alginate sponges prepared using glutaraldehyde as a cross-linking agent (referred to as Comparative Example 2) were added to each centrifuge tube, and then heavy metal chromium ion Cr(VI) wastewater with a concentration of 50mg / L and a pH value of 1, 2, 3, 4, and 5 was added to the 5 centrifuge tubes in each group of experiments, respectively. The tubes were placed in a shaker and continuously shaken at a constant temperature of 25 degrees Celsius for 3 days, and then samples were taken, and the concentration of the simulated heavy metal wastewater after treatment was measured using an ultraviolet spectrophotometer.
[0109] When the initial concentration was 50 mg / L, the adsorption amount of Cr(VI) by each sodium alginate-based sponge at different pH values is shown in Table 2.
[0110] Table 2 Comparison of the adsorption of Cr(VI) by various sodium alginate-based sponges at different pH values
[0111]
[0112] As can be seen from Table 2, the sodium alginate-based sponge prepared in the embodiment of the present invention has a higher adsorption capacity at each pH value than the sodium alginate-based sponge prepared by using potassium permanganate as an oxidant and the sodium alginate-based sponge prepared by using glutaraldehyde as a cross-linking agent, indicating that the sodium alginate sponge prepared in the embodiment of the present invention has a higher adsorption capacity at different pH values and has a better application prospect in the field of water treatment.
[0113] 3. Stability test
[0114] 30 mg of the modified sodium alginate sponges prepared in Examples 1-6 and Comparative Example 1 were put into a polyethylene bottle with 50 ml of industrial wastewater, placed on a shaker and shaken vigorously for three days. After the end, the sodium alginate sponges were naturally air-dried and then compared with the mass of the sodium alginate sponges before shaking. It was found that the mass losses of the sodium alginate sponges prepared in Examples 1-6 were all below 3%, while the mass loss of the sodium alginate sponges prepared in Comparative Example 1 exceeded 5%, indicating that ammonium persulfate was used as an oxidant and initiator to interrupt the long-chain molecules on the polysaccharide molecular chain and oxidize them to obtain aldehyde groups, which fully reacted with the amino groups on the polyaziridine to form a stable structure, thereby successfully cross-linking polyaziridine and sodium alginate, and obtaining a high-strength sodium alginate-based sponge with strong stability and strong practical value; while the sodium alginate-based sponges prepared using other oxidants have poor stability and insufficient practicality.
[0115] 3. Application of Sodium Alginate Sponge
[0116] 30 mg of the sodium alginate sponges prepared in Example 1, Example 2, Example 3, Example 4, Example 5, and Example 6 were added to 50 ml centrifuge tubes, and 50 ml of industrial wastewater containing chromium (Cr) was added respectively. The tubes were placed on a shaker at a constant temperature of 25° C. and continuously shaken for 3 days. The concentration of the chromium-containing industrial wastewater before and after treatment was measured using an ultraviolet spectrophotometer, and the adsorption efficiency of the sodium alginate sponges for Cr(VI) was found to be 95%, while the adsorption rate of the sodium alginate sponges prepared using glutaraldehyde as a cross-linking agent was less than 90%.
[0117] It shows that the sodium alginate-based sponge prepared by the present invention not only reduces the toxicity caused by the use of glutaraldehyde, but also has better heavy metal adsorption capacity, and has better application prospects in the field of water treatment.
[0118] The above description is a detailed description of the preferred feasible embodiments of the present invention, but the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modified changes completed under the technical spirit suggested by the present invention should fall within the patent scope covered by the present invention.
Claims
1. A method for preparing a sodium alginate-based sponge, characterized in that: The following steps are involved: (1) adding deionized water to the polyaziridine solution, mixing evenly, and adjusting the pH to 6-7 to prepare a diluted polyaziridine solution; (2) dispersing sodium alginate in deionized water and homogenizing for 5-10 minutes to prepare a sodium alginate paste; (3) under continuous stirring, adding the diluted polyethylenimine solution obtained in step (1) to the sodium alginate paste obtained in step (2) in 5 portions, with the same amount added each time and the same interval between two adjacent additions. After the addition of the diluted polyethylenimine solution is completed, continuing to homogenize for a certain period of time to obtain a mixed solution; (4) allowing the mixed solution obtained in step (3) to stand at room temperature for 24-48 hours to initially cross-link to obtain a sodium alginate / polyaziridine structure hydrogel; (5) dissolving the polysaccharide powder in anhydrous ethanol and adding ammonium persulfate solution, reacting for 6 to 8 hours under stirring, then adding sodium bisulfite under continuous stirring, and heating in a water bath while stirring for 0.5 to 1 hour, and then dialyzing with deionized water for 3 to 4 days to prepare a polysaccharide dialdehyde derivative solution; (6) adding the sodium alginate / polyethylenimine structure hydrogel prepared in step (4) to the polysaccharide dialdehyde derivative solution prepared in step (5), shaking for 24-48 hours, and after double cross-linking, washing and drying to obtain a sodium alginate-based sponge.
2. The preparation method according to claim 1, characterized in that: The mass fraction of the diluted polyaziridine solution in step (1) is 3% to 6%.
3. The preparation method according to claim 1, characterized in that: In step (1), nitric acid or hydrochloric acid is added to adjust the pH value.
4. The preparation method according to claim 1, characterized in that: The mass fraction of the sodium alginate paste prepared in step (2) is 0.6% to 1%.
5. The preparation method according to claim 1, characterized in that: In step (3), the amount of diluted polyaziridine used is 5% of the mass of the sodium alginate paste.
6. The preparation method according to claim 1, characterized in that: In step (3), the diluted polyaziridine solution is added dropwise every 10 seconds, and after the addition is completed, the slurry is stirred for 10-20 seconds to obtain a mixed solution.
7. The preparation method according to claim 1, characterized in that: In step (5), the polysaccharide powder is sodium alginate powder, chitosan powder, dextran powder or plant starch powder.
8. The preparation method according to claim 1, characterized in that: In step (5), the mass of anhydrous ethanol is 4-5 times the mass of the polysaccharide powder; the mass fraction of ammonium persulfate solution is 4% to 6%, and its mass is 1.25-1.3 times that of anhydrous ethanol; and the mass of sodium bisulfite is 0.02-0.05 times that of anhydrous ethanol.
9. The sodium alginate-based sponge prepared by the preparation method according to any one of claims 1 to 8.