Preparation method of nanofiber adsorption material for removing dichromate radicals and dichromate radical wastewater recycling technology

By preparing nanofiber adsorption materials containing nitrogen-containing adsorption sites, the problems of low removal efficiency and high treatment cost in the prior art are solved, efficient removal and resource utilization are achieved, and the risk of secondary pollution is reduced.

CN118925685APending Publication Date: 2024-11-12CHONGQING UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411115218.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing nanofibers have low removal efficiency for dichromate, high processing cost, low recycling efficiency for chromium metal resources, and a risk of secondary pollution.

Method used

Nanofibers are prepared by raw materials such as polyvinyl alcohol, polyvinyl chloride, polyacrylonitrile and polyvinylidene fluoride. By introducing nitrogen-containing adsorption sites and oxidizing agents to react, an efficient nanofiber adsorption material is formed to remove dichromate. And the resource utilization of sodium chromate is achieved through the desorption solution.

Benefits of technology

It improves the removal efficiency of dichromate, reduces the treatment cost, reduces the risk of secondary pollution, and realizes the resource utilization of chromate ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925685A_ABST
    Figure CN118925685A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nanofiber adsorption materials, and particularly discloses a preparation method of a nanofiber adsorption material for dichromate radical removal, and the preparation method comprises the following steps: respectively dissolving polyvinyl alcohol, polyvinyl chloride, polyacrylonitrile and polyvinylidene fluoride; adding an oxidizing agent into the polyvinyl alcohol solution for reaction, and aminating to introduce nitrogen-containing adsorption sites; the method comprises the following steps: adding an amido-containing compound into a polyvinyl chloride solution, polyacrylonitrile or polyvinylidene fluoride solution, and aminating to introduce nitrogen-containing adsorption sites; preparing a spinning solution under homogeneous reaction; processing and forming nano-fibers, washing and drying to obtain the nano-fiber adsorption material for removing dichromate radicals. According to the method, the removal and recycling efficiency of the dichromate ions is improved, the treatment cost is reduced, meanwhile, the risk of secondary pollution is reduced, and the method has higher selectivity and affinity for the dichromate ions. The recycling of the dichromate radical wastewater is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanofiber adsorption materials, and in particular to a method for preparing a nanofiber adsorption material for removing dichromate and a dichromate wastewater resource recovery technology. Background Art

[0002] At present, nanofiber adsorption material is a material with strong adsorption capacity made by utilizing the characteristics of nanofibers. Nanofibers, as a new type of fiber material with a diameter at the nanometer level, have extremely high length and specific surface area, which makes nanofibers have significant advantages in adsorption, filtration, and enhancement. The large specific area and surface activity of nanofibers give them strong adsorption capacity, which can be used to remove harmful substances and heavy metal pollutants in water.

[0003] However, in the prior art, ordinary nanofibers have low removal efficiency for dichromate, high processing costs, low recovery efficiency for chromium metal resources, and a risk of secondary pollution. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a nanofiber adsorption material for dichromate removal and a dichromate wastewater resource recovery technology, aiming to solve the technical problems in the prior art that ordinary nanofibers have low dichromate removal efficiency, high treatment costs, low chromium metal resource recovery efficiency, and the risk of secondary pollution.

[0005] To achieve the above object, the present invention adopts a method for preparing a nanofiber adsorbent material for dichromate removal, comprising the following steps: Step 1: using polyvinyl alcohol, polyvinyl chloride, polyacrylonitrile and polyvinylidene fluoride as raw materials, and dissolving the polyvinyl alcohol, polyvinyl chloride, polyacrylonitrile and polyvinylidene fluoride respectively; Step 2: Add an oxidant to the polyvinyl alcohol solution to react, oxidize the alcohol hydroxyl group to a carbonyl group, and then add an amine-containing compound to introduce the nitrogen-containing adsorption site. The reaction temperature is 50-100°C and the reaction time is 4-48 hours. Add an amine-containing compound to a polyvinyl chloride solution, a polyacrylonitrile solution or a polyvinylidene fluoride solution to introduce nitrogen-containing adsorption sites. The reaction temperature is 80-140°C and the reaction time is 2-48 hours. Step 3: purifying the polyvinyl alcohol solution, polyvinyl chloride solution, polyacrylonitrile solution and polyvinylidene fluoride solution after the reaction and adding a spinning aid to obtain a spinning solution; Step 4: using the spinning solution prepared above as a raw material, processing and shaping into nanofibers by means of electrospinning equipment, and after washing and drying, obtaining a nanofiber adsorption material for dichromate removal; Step 5: The nanofibers prepared as described above are used as adsorbents, activated by an activation solution, and then filled into an adsorption column, and the dichromate-containing wastewater is pumped into the adsorption column from bottom to top, so as to remove the dichromate ions in the wastewater; Step 6: After the nanofibers are saturated with adsorption, a desorption solution is introduced to desorb the dichromate ions and obtain a high-concentration sodium chromate solution with a concentration of 5~240g / L.

[0006] Step 7: The desorption liquid desorbs the dichromate ions on the surface of the nanofibers to achieve enrichment, and then the sodium chromate product is obtained after concentration, cooling, crystallization, filtration and drying.

[0007] Wherein, the polyvinyl alcohol is dissolved in water at a temperature of 80-95°C.

[0008] Wherein, the polyvinyl chloride is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

[0009] Wherein, the polyacrylonitrile is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

[0010] Wherein, when the polyvinylidene fluoride is dissolved in N,N-dimethylacetamide, 0.5-5% of sodium carbonate or potassium carbonate is added, and the temperature is 70-105°C.

[0011] Wherein, the oxidant is any one of sodium periodate, hydrogen peroxide and potassium permanganate, and the usage amount of the oxidant is 1-15% of the weight of the polyvinyl alcohol.

[0012] Wherein, the amine-containing compound is any one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethyleneimine and 2-thiopheneethylamine.

[0013] Wherein, the activation solution is a 0.5-2 mol / L hydrochloric acid aqueous solution, and the desorption solution is a 1-4 mol / L sodium hydroxide solution.

[0014] The beneficial effects of the nanofiber adsorption material preparation method for dichromate removal and the dichromate wastewater resource technology of the present invention are as follows: the prepared nanofiber adsorption material has a large specific surface area and a very high surface area / volume ratio, which provides a strong adsorption capacity for it, can effectively adsorb dichromate ions in wastewater, and improve the removal efficiency of dichromate ions. When wastewater containing dichromate ions passes through the nanofiber adsorption material, the dichromate ions will be effectively trapped on the nitrogen-containing adsorption sites exposed on the surface of the nanofiber, and efficient removal is achieved. The nanofiber adsorption material can be recycled, which reduces the processing cost and the risk of secondary pollution. It has higher selectivity and affinity for dichromate ions. Finally, the dichromate wastewater can be treated by column adsorption, and the sodium chromate product can also be prepared by a high-concentration desorption liquid to recycle the dichromate wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0016] Figure 1 These are the SEM images and mapping images of the nanofiber adsorbent material for dichromate removal prepared in Example 1 of the present invention.

[0017] Figure 2 This is an infrared spectrum of the nanofiber adsorption material for dichromate removal prepared in Example 1 of the present invention.

[0018] Figure 3 It is a dynamic adsorption penetration curve diagram of the nanofiber adsorption material for dichromate removal prepared in Example 2 of the present invention.

[0019] Figure 4 It is a practical operation flow chart of the dichromate wastewater resource recovery technology according to Example 3 of the present invention.

[0020] Figure 5 This is the XRD diagram of the sodium chromate product of the heavy acid radical wastewater resource recovery technology in Example 4 of the present invention. DETAILED DESCRIPTION

[0021] The present invention provides a method for preparing a nanofiber adsorption material for dichromate removal, comprising the following steps: Step 1: using polyvinyl alcohol, polyvinyl chloride, polyacrylonitrile and polyvinylidene fluoride as raw materials, and dissolving the polyvinyl alcohol, polyvinyl chloride, polyacrylonitrile and polyvinylidene fluoride respectively; Step 2: Add an oxidant to the polyvinyl alcohol solution to react, oxidize the alcohol hydroxyl group to a carbonyl group, and then add an amine-containing compound to introduce the nitrogen-containing adsorption site. The reaction temperature is 50-100°C and the reaction time is 4-48 hours. Add an amine-containing compound to a polyvinyl chloride solution, a polyacrylonitrile solution or a polyvinylidene fluoride solution to introduce nitrogen-containing adsorption sites. The reaction temperature is 80-140°C and the reaction time is 2-48 hours. Step 3: purifying the polyvinyl alcohol solution, polyvinyl chloride solution, polyacrylonitrile solution and polyvinylidene fluoride solution after the reaction and adding a spinning aid to obtain a spinning solution; Step 4: Using the spinning solution prepared above as a raw material, the spinning solution is processed into nanofibers by means of electrospinning equipment. After washing and drying, the nanofiber adsorption material for dichromate removal is obtained.

[0022] Step 5: The nanofibers prepared as described above are used as adsorbents, activated by an activation solution, and then filled into an adsorption column, and the dichromate-containing wastewater is pumped into the adsorption column from bottom to top, so as to remove the dichromate ions in the wastewater; Step 6: After the nanofibers are saturated with adsorption, a desorption solution is introduced to desorb the dichromate ions and obtain a high-concentration sodium chromate solution with a concentration of 5~240g / L.

[0023] Step 7: The desorption liquid desorbs the dichromate ions on the surface of the nanofibers to achieve enrichment, and then the sodium chromate product is obtained after concentration, cooling, crystallization and filtration.

[0024] Furthermore, the polyvinyl alcohol is dissolved in water at a temperature of 80-95°C.

[0025] Furthermore, the polyvinyl chloride is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

[0026] Furthermore, the polyacrylonitrile is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

[0027] Furthermore, when the polyvinylidene fluoride is dissolved in N,N-dimethylacetamide, 0.5-5% of sodium carbonate or potassium carbonate is added at a temperature of 70-105°C.

[0028] Furthermore, the oxidant is any one of sodium periodate, hydrogen peroxide and potassium permanganate, and the amount of the oxidant used is 1-15% of the weight of the polyvinyl alcohol.

[0029] Furthermore, the amine-containing compound is any one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethyleneimine and 2-thiopheneethylamine.

[0030] Furthermore, the activation solution is a 0.5-2 mol / L hydrochloric acid aqueous solution, and the desorption solution is a 1-4 mol / L sodium hydroxide solution.

[0031] In the present embodiment, the nanofiber has a very large specific surface area and a very high surface area / volume ratio, which provides a strong adsorption capacity, can effectively adsorb the dichromate ions in the wastewater, improve the removal efficiency of the dichromate ions, and secondly, the excellent aspect ratio structure of the nanofiber has a small flow resistance in the dynamic adsorption formation, which is convenient for desorption and regeneration activation. When the wastewater containing dichromate ions passes through the nanofiber adsorbent material, the dichromate ions can be effectively trapped on the adsorption sites on the surface of the nanofiber, and efficient removal is achieved. The nanofiber adsorbent material can be recycled, which reduces the processing cost, reduces the risk of secondary pollution, and has higher selectivity and affinity for dichromate ions. Finally, the hexavalent chromium ions can be enriched by column adsorption and converted into sodium chromate products, realizing the resource utilization of dichromate ions. Example 1, the present invention also provides a method for preparing a nanofiber adsorption material for dichromate removal and a dichromate wastewater resource recovery technology, comprising the following steps: Using polyvinyl chloride as raw material and dissolving the polyvinyl chloride; A 10% polyvinyl chloride solution was obtained at 90°C, 20 mL was taken and transferred to the reactor, and 5 mL of polyethyleneimine was added to introduce nitrogen adsorption sites. The reaction temperature was 90°C and the reaction time was 12 h. Then add 1.2g of polyvinyl chloride and fully dissolve it to prepare a spinning solution; The spinning solution prepared as above is used as raw material, and is processed into nanofibers by means of electrostatic spinning equipment. After drying, the nanofiber adsorption material for dichromate removal is obtained.

[0032] The SEM image and mapping image of the nanofiber adsorbent material for dichromate removal prepared in Example 1 are shown in Figure 1 , infrared spectrum see Figure 2 .

[0033] Example 2: 2.0 g of the nanofiber adsorption material for dichromate removal prepared in Example 1 was loaded into an adsorption column with a diameter of 10 mm and a height of 100 mm. A peristaltic pump was used to control the chromium-containing wastewater to pass through the adsorption column at a flow rate of 1 mL / min. The effluent was taken at different times and its chromium ion concentration was determined.

[0034] The results of the test are as follows Figure 3 As shown, no dichromate was detected in the effluent before 1200 min.

[0035] Example 3, large-scale treatment of actual dichromate wastewater such as Figure 4As shown, the dichromate ion wastewater needs to pass through the filtration system and be pumped from bottom to top into the chromium-containing wastewater adsorption treatment system. By controlling the water stop valve, two working adsorption columns are always connected in series, and one adsorption column is a spare column after desorption / regeneration. The desorption / regeneration circulation system is controlled to pump the desorption / regeneration activation liquid from top to bottom into the adsorption saturated column, which becomes a spare column after desorption / regeneration. The desorption enrichment liquid is processed to prepare sodium chromate products, thereby realizing the continuous treatment and resource utilization of dichromate wastewater.

[0036] Example 4: The circulating desorption enriched liquid obtained in Example 2 is concentrated, cooled, crystallized, filtered and dried to obtain a sodium chromate product, thereby realizing the resource utilization of dichromate ion wastewater. The XRD pattern of sodium chromate is shown in Figure 5 .

[0037] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A method for preparing a nanofiber adsorption material for dichromate removal, It is characterized in that The steps include: Step 1: using polyvinyl alcohol, polyvinyl chloride, polyacrylonitrile and polyvinylidene fluoride as raw materials, and dissolving the polyvinyl alcohol, polyvinyl chloride, polyacrylonitrile and polyvinylidene fluoride respectively; Step 2: Add an oxidant to the polyvinyl alcohol solution to react, oxidize the alcohol hydroxyl group to a carbonyl group, and then add an amine-containing compound to introduce the nitrogen-containing adsorption site. The reaction temperature is 50-100°C and the reaction time is 4-48 hours. Add an amine-containing compound to a polyvinyl chloride solution, a polyacrylonitrile solution or a polyvinylidene fluoride solution to introduce nitrogen-containing adsorption sites. The reaction temperature is 80-140°C and the reaction time is 2-48 hours. Step 3: purifying the reacted aminated polyvinyl alcohol solution, polyvinyl chloride solution, polyacrylonitrile solution and polyvinylidene fluoride solution and adding a spinning aid to obtain a spinning solution; Step 4: The spinning solution prepared above is used as a raw material, and is processed into nanofibers by means of an electrospinning device. After washing and drying, the nanofiber adsorption material for dichromate removal is obtained. Step 5: The nanofibers prepared in step 4 above are used as adsorbents, and after activation by an activation solution, they are filled into an adsorption column, and the wastewater containing dichromate is pumped into the adsorption column from bottom to top, so as to remove the dichromate ions in the wastewater; Step 6: After the nanofibers are saturated with adsorption, the desorption liquid is introduced to desorb the dichromate ions and obtain a high-concentration sodium chromate solution with a concentration of 5-240 g / L. Step 7: The desorption liquid desorbs the dichromate ions on the surface of the nanofibers to achieve enrichment, and then the sodium chromate product is obtained after concentration, cooling, crystallization, filtration and drying.

2. A method for preparing a nanofiber adsorption material for dichromate removal as described in claim 1, Features: The polyvinyl alcohol is dissolved in water at a temperature of 80-95°C.

3. A method for preparing a nanofiber adsorption material for dichromate removal according to claim 1, Features: The polyvinyl chloride is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

4. The method for preparing a nanofiber adsorption material for dichromate removal according to claim 1, Features: The polyacrylonitrile is dissolved in N,N-dimethylacetamide at a temperature of 70-105°C.

5. The method for preparing a nanofiber adsorption material for dichromate removal according to claim 1, Features: When the polyvinylidene fluoride is dissolved in N,N-dimethylacetamide, 0.5-5% of sodium carbonate or potassium carbonate is added at a temperature of 70-105°C.

6. A method for preparing a nanofiber adsorption material for dichromate removal according to claim 1, Features: The oxidant is any one of sodium periodate, hydrogen peroxide and potassium permanganate, and the amount of the oxidant used is 1-15% of the weight of the polyvinyl alcohol.

7. A method for preparing a nanofiber adsorption material for dichromate removal according to claim 1, Features: The amine-containing compound is any one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyethyleneimine and 2-thiopheneethylamine.

8. The dichromate wastewater resource recovery technology according to claim 1, Features: The activation solution is a 0.5-2 mol / L hydrochloric acid aqueous solution, and the desorption solution is a 1-2 mol / L sodium hydroxide solution.

Citation Information

Patent Citations

  • Method for modifying activity of polyvinyl alcohol

    CN103288990A

  • Method for treating hexavalent chromium wastewater with weak base ion exchange fiber

    CN103663621A

  • Method for treating waste water containing vanadium and chromium

    CN104556522A

  • Amine modified fibrous membrane adsorption material and preparation method thereof

    CN105195110A

  • Chemical grafting modification method and application of polyvinylidene fluoride

    CN116970105A