Novel preparation method of super-macroporous cellulose microsphere chromatographic medium
By combining pre-crosslinked bacterial cellulose and cellulose chains, micron-scale macroporous cellulose microspheres without pore preparation agents were prepared, solving the problem of too small pore size of traditional cellulose microspheres, achieving efficient adsorption and simplified operation , improves chromatographic performance and mechanical performance.
Patent Information
- Application Number
- CN202310539265.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-12
AI Technical Summary
The nano-scale pore size of traditional cellulose microspheres limits the rapid mass transfer process of adsorbents. Existing pore size expansion methods such as template method and emulsification method have the problem of using pore-making agents or toxic reagents, resulting in reduced mechanical properties and complex operation.
By pre-crosslinking the combination of bacterial cellulose with high crystallinity and high aspect ratio and dissolved cellulose chains, an ultra-large pore structure is formed. Micron-scale cellulose microspheres are prepared by one-step pre-crosslinking method, avoiding the use of pore-making agents and simplifying operations .
It realizes non-toxic, environmentally friendly, and simple operation to prepare high-strength, micron-scale macroporous cellulose microspheres, which improve adsorption capacity and specific surface area, and improve chromatographic performance.
Smart Images

Figure CN118925696A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials and relates to a new method for preparing a super-macroporous cellulose microsphere chromatographic medium. Background Art
[0002] Cellulose ((C6H 10 O5) n ) is a natural renewable polymer with huge reserves. It can be extracted from trees, straw, cotton, seaweed and bacteria, with an annual output of more than 10 12 Tons. Cellulose is a high molecular linear polysaccharide formed by the polymerization of glucose through β-1, 4 glycosidic bonds. The degree of polymerization (DP) of cellulose is related to its source and ranges from several hundred to tens of thousands. Cellulose has attracted extensive attention from scientists all over the world due to its wide sources, abundant reserves, biocompatibility, degradability, non-toxicity, good mechanical properties and low cost. Regenerated cellulose can form a porous network structure, exposing more hydroxyl groups, which is conducive to mass transfer and increasing reaction rate. It is a good matrix for preparing chromatographic media. Among them, cellulose microspheres have shown good application prospects in the fields of chromatography analysis, separation technology and adsorbents.
[0003] Cellulose microspheres are excellent chromatographic column fillers with the characteristics of simple operation and easy filling. Cellulose microspheres have been used in a variety of chromatographic systems as stationary phases for separation and purification. According to the interaction between the microspheres and the separated substances, they can be applied to affinity chromatography, ion exchange chromatography, hydrophobic interaction chromatography and hydrophobic charge induction chromatography. The physical structure (pore size distribution and porosity) of cellulose microspheres is closely related to the separation effect of liquid chromatography. However, traditional cellulose microspheres are mainly based on nanoscale pores, which hinder the rapid mass transfer of adsorbents in the medium. At present, there are two main strategies for enlarging the pore size: template method and emulsification method. However, the template method uses pore-forming agents to prepare closed pores, and the removal of pore-forming agents not only increases the experimental steps but also requires more reagents. The emulsification method requires a large amount of toxic organic reagents, and the pore size of the prepared microspheres is too large, resulting in a decrease in the mechanical properties of the microspheres and lack of practicality.
[0004] Therefore, it is of great significance to find a green and environmentally friendly method for constructing macroporous cellulose microspheres without the need for pore-forming agents to improve their chromatographic performance. The present invention develops a new method for preparing a novel ultra-macroporous cellulose microsphere chromatographic medium. This method introduces bacterial cellulose with the same chemical properties, high crystallinity, and high aspect ratio, and pre-crosslinks it with the dissolved cellulose chains, and then partially gels the solution after cross-linking. The steric hindrance generated by the gelled bacterial cellulose network during the solidification and regeneration of cellulose leads to the formation of ultra-large pores. The present invention does not use any pore-forming agents, and cellulose microspheres with ultra-large pores can be prepared by only one-step pre-crosslinking of bacterial cellulose. The preparation method is simple, which makes it have good development prospects in the field of macromolecular separation and purification. Summary of the invention
[0005] The present invention aims to overcome the defect of low mass transfer efficiency of traditional cellulose micro-mesoporous structure and proposes a new method for preparing micron-scale ultra-macroporous cellulose microsphere chromatographic medium which is simple to operate and does not require a pore-forming agent.
[0006] The specific plan is as follows: (1) Preparation of pre-cross-linked cellulose solution: Dissolve microcrystalline cellulose in NaOH / thiourea aqueous solution in an ice bath and stir vigorously to form a transparent cellulose solution. Add 2.4 g of bacterial cellulose homogenate and continue to stir vigorously for 20 min. Then, add 400 μL of epichlorohydrin and pre-cross-link at low temperature for 30 min. (2) Emulsification of cellulose solution: Weigh 5 g of span 80 and 1 g of Tween 80 and add them to 80 mL of isooctane and 40 mL of white oil as the oil phase. Take 15 mL of the cellulose dispersion obtained in step (1) and add it dropwise into the oil phase. Control the stirring speed to obtain water-in-oil emulsion droplets. Emulsify at room temperature for 20 min. (3) Regeneration of cellulose microspheres: Add 50 mL of 5% H2SO4 to the emulsion from the previous step, stir for 20 min and let stand, separate the precipitated cellulose microspheres by centrifugation, and wash with 20% ethanol and pure water to remove the residual oil phase.
[0007] Further preferably, the ultra-macroporous cellulose microsphere chromatography medium is prepared according to the following steps: (1) In the above technical scheme, the NaOH / thiourea aqueous solution used in step (1) has a NaOH concentration of 8 wt%~12 wt%, a thiourea concentration of 7 wt%~8 wt%, a vigorous stirring speed of 1500 rpm, a dissolution time of 3 min~5 min, and a prepared cellulose solution concentration of 4 wt%~6 wt%; (2) In the above technical solution, the mass ratio of bacterial cellulose homogenate to microcrystalline cellulose added in step (1) is 0.4:1.0~1.2:1.0, and the volume ratio of epichlorohydrin to cellulose solution is 400 μL:50 mL~1 mL:50 mL; (3) In the above technical solution, the ratio of isooctane to white oil used in step (2) is 1:1~2:1, the surfactant Span 80 is 4~6 times that of Tween 80, the volume ratio of the cellulose solution and the oil phase used for emulsification is 1:12~1:6, the emulsification temperature is 22℃~30℃, and the emulsification time is 20 min~120 min; (4) In the above technical solution, the regeneration conditions used in step (3) can be 70% ethanol or 5% HCl or 5% H2SO4, the regeneration time is 30 min~60 min, the centrifugation conditions are 3000 rpm~4500 rpm, and the centrifugation time is 3 min~5 min.
[0008] Compared with the prior art, the present invention has the following advantages: (1) The present invention is simple to operate, the reagents are green and environmentally friendly, and the repeatability is high, which is conducive to large-scale development; (2) The present invention uses bacterial cellulose pre-crosslinking gelation to prepare pores to prepare micron-sized macroporous and high-strength cellulose microspheres. The cellulose has low cost and good biocompatibility. (3) The ultra-large pore structure of the cellulose microspheres prepared in the present invention facilitates the rapid entry of the adsorbate into the interior of the microspheres and contact with the active functional group sites. The micro-mesopores increase the specific surface area of the microspheres, ensuring a higher adsorption capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 , Figure 2 They are respectively a scanning electron microscope photo and a local magnified photo of the ultra-macroporous cellulose microsphere chromatographic medium provided by the present invention. DETAILED DESCRIPTION
[0010] In order to better understand the present invention, the present invention will be further explained below in conjunction with the implementation examples and the accompanying drawings. However, it should be particularly noted that the implementation examples are only used to further explain the present invention, and the scope of protection claimed by the present invention is not limited to the scope represented by the implementation examples.
[0011] Example 1 Measure 50 mL of NaOH (12%) / thiourea (8%) aqueous solution, add 3 g of microcrystalline cellulose in an ice bath, stir at 1500 rpm for 3 min to obtain a colorless and transparent cellulose solution; add 1.2 g of bacterial cellulose homogenate, stir at 1500 rpm at room temperature for 20 min, add 800 μL of epichlorohydrin, and continue stirring at 10°C for 40 min; add 15 mL of this dispersion dropwise to the oil phase containing 6 g Span 80, 1 g Tween 60, 60 mL of white oil and 60 mL of isooctane, and stir at 800 rpm for 30 min at 28°C; slowly add 50 mL of 70% ethanol and stir for 30 min to regenerate the cellulose microspheres; precipitate the regenerated cellulose microspheres, and wash with 20% ethanol and pure water to remove the residual oil phase.
[0012] Example 2 Measure 50 mL of NaOH (12%) / thiourea (8%) aqueous solution, add 3 g of microcrystalline cellulose in an ice bath, stir at 1500 rpm for 5 min to obtain a colorless and transparent cellulose solution; add 2.4 g of bacterial cellulose homogenate, stir at 1500 rpm at room temperature for 20 min, add 400 μL of epichlorohydrin, and continue stirring at 25°C for 40 min; add 20 mL of this dispersion dropwise to the oil phase containing 5.5 g Span 80, 1 g Tween 60, 80 mL of white oil and 40 mL of isooctane, and stir at 800 rpm for 60 min at 28°C; slowly add 50 mL of 5% sulfuric acid and stir for 20 min to regenerate the cellulose microspheres; precipitate the regenerated cellulose microspheres, and wash with 20% ethanol and pure water to remove the residual oil phase.
Claims
1. A novel method for preparing ultra-macroporous cellulose microsphere chromatographic medium, characterized in that The steps include: (1) Preparation of pre-crosslinked cellulose solution: Dissolve microcrystalline cellulose in NaOH / thiourea aqueous solution in an ice bath and stir vigorously to form a transparent cellulose solution. Add 2.4 g of bacterial cellulose homogenate and continue to stir vigorously for 20 min. Then, add 400 μL of epichlorohydrin and pre-crosslink at low temperature for 30 min. (2) Emulsification of cellulose solution: Weigh 5 g of span 80 and 1 g of Tween 80 and add them to 80 mL of isooctane and 40 mL of white oil as the oil phase. Take 15 mL of the cellulose dispersion obtained in step (1) and add it dropwise into the oil phase. Control the stirring speed to obtain water-in-oil emulsion droplets. Emulsify at room temperature for 20 min. (3) Regeneration of cellulose microspheres: Add 50 mL of 5% H2SO4 to the emulsion from the previous step, stir for 20 min and let stand, separate the precipitated cellulose microspheres by centrifugation, and wash with 20% ethanol and pure water to remove the residual oil phase.
2. The novel method for preparing the ultra-macroporous cellulose microsphere chromatographic medium according to claim 1, characterized in that The NaOH / thiourea aqueous solution used in step (1) has a NaOH concentration of 8 wt%~12 wt%, a thiourea concentration of 7 wt%~8wt%, a vigorous stirring speed of 1500 rpm, a dissolution time of 3 min~5 min, and a prepared cellulose solution concentration of 4wt%~6wt%.
3. The novel method for preparing the ultra-macroporous cellulose microsphere chromatographic medium according to claim 1, characterized in that The mass ratio of the bacterial cellulose homogenate to the microcrystalline cellulose added in step (1) is 0.4:1.0~1.2:1.0, and the volume ratio of epichlorohydrin to the cellulose solution is 400 μL:50 mL~1 mL:50 mL.
4. The novel method for preparing the ultra-macroporous cellulose microsphere chromatographic medium according to claim 1, characterized in that The ratio of isooctane to white oil used in step (2) is 1:1~2:1, the surfactant span 80 is 4~6 times that of Tween 80, the volume ratio of the cellulose solution used for emulsification and the oil phase is 1:12~1:6, the emulsification temperature is 22℃~30℃, and the emulsification time is 20 min~120 min.
5. The novel method for preparing the ultra-macroporous cellulose microsphere chromatographic medium according to claim 1, characterized in that The regeneration conditions used in step (3) can be 70% ethanol or 5% HCl or 5% H2SO4, the regeneration time is 30 min~60 min, the centrifugation conditions are 3000 rpm~4500 rpm, and the centrifugation time is 3 min~5 min.