TiO2 / xonotlite composite catalyst and preparation method thereof

By preparing TiO2/hard silicate composite catalyst, the problem of low activity and difficult treatment of photocatalysts under natural light is solved, efficient photodegradation and harmful gas treatment are achieved, and catalytic performance and stability are improved.

CN118925703APending Publication Date: 2024-11-12CHINA BUILDING MATERIAL TEST & CERT GRP (ZIBO) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985799.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing photocatalysts have low activity under natural light, difficulty in handling nano-scale powders, affect light transmittance, and have not yet achieved satisfactory results in the catalytic performance and resource utilization of pollutants.

Method used

TiO2/hard silicate composite catalyst is used to dissolve inorganic titanium salts and organic sulfur-containing compounds, adjust the pH value, and carry out hydrothermal reaction preparation, improve photocatalytic activity and pore size, and enhance light energy utilization and cyclic stability.

Benefits of technology

It significantly improves the photodegradation ability, improves the treatment efficiency of the harmful gas formaldehyde, increases the pore size, improves the light energy utilization and cycle stability, and improves the catalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925703A_ABST
    Figure CN118925703A_ABST
Patent Text Reader

Abstract

The invention provides a TiO2 / xonotlite composite catalyst preparation method, which comprises: 1, dissolving an inorganic titanium salt solution, and carrying out magnetic stirring to completely dissolve the inorganic titanium salt solution; 2, weighing a certain amount of an organic sulfur-containing compound, and adding the organic sulfur-containing compound into the solution obtained in the step 1; 3, dropwise adding a sodium hydroxide solution into the inorganic titanium salt and thiourea mixed solution obtained in the step 2, and adjusting the pH value of the mixed solution to 1.5-3; 4, adding a certain amount of xonotlite into the mixed solution obtained in the step 3, and further adjusting the pH value of the solution to 3-6 by adopting a sodium hydroxide solution; 5, the solution obtained in the step 4 is magnetically stirred and then subjected to a hydrothermal reaction in a high-pressure reaction kettle, centrifugal washing and drying are carried out, and the TiO2 / xonotlite composite catalyst is obtained and has the advantages that the light degradation capacity is improved, the good photocatalytic activity is achieved, the aperture size is increased, the light energy utilization rate is improved, the degradation efficiency of harmful gas formaldehyde is improved, and the application prospect is wide. For example, the formaldehyde treatment efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of environmentally friendly catalysts, and in particular to a TiO 2 / Xonotlite composite catalyst and preparation method thereof. Background Art

[0002] The textile, paper, leather and coating industries produce a large amount of toxic and harmful organic wastewater. If it is not handled properly, it will not only seriously damage the ecological environment, but also pose a serious threat to human health. In particular, printing and dyeing wastewater has the characteristics of dark color, high toxicity, high chemical oxygen content, high salt content, etc., and is carcinogenic, corrosive and mutagenic.

[0003] In order to prevent the further deterioration of environmental pollution caused by printing and dyeing wastewater, there are many studies on its treatment methods. The use of strong oxides produced by semiconductor materials under light to destroy the color-developing groups in printing and dyeing wastewater is currently considered to have great prospects. Titanium dioxide is widely used in water treatment as a photocatalyst because of its safety, non-toxicity, high reactivity, and relatively thorough reaction. It has also been a hot topic in the field of photocatalysis. However, due to its wide energy band width, it can only have photodegradation activity under ultraviolet light, and the utilization rate of natural light is low; nano-powder samples are not conducive to recovery, subsequent treatment is difficult, and the suspension system affects the light transmittance and reduces the light activity. These factors limit its application in actual water treatment.

[0004] In response to the current problems in this field, some loading, doping and other methods have been proposed in the prior art. However, the catalytic performance of photocatalysts prepared by the existing methods on pollutants and resource utilization need to be further improved. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a TiO 2 / xonotlite composite catalyst and preparation method thereof, the prepared TiO 2 The quartz / xonotlite composite catalyst has good photocatalytic activity, the pore size is enlarged, the light energy utilization rate is increased, and the cycle stability is improved.

[0006] In order to achieve the above object, the present invention provides a TiO 2 / The preparation method of xonotlite composite catalyst comprises the following steps:

[0007] Step 1: Dissolve the inorganic titanium salt solution and stir it magnetically to fully dissolve it;

[0008] Step 2: Weigh a certain amount of organic sulfur-containing compound and add it to the solution obtained in step 1;

[0009] Step 3: adding sodium hydroxide solution dropwise to the mixed solution of inorganic titanium salt and thiourea obtained in step 2, and adjusting the pH value of the mixed solution to 1.5-3;

[0010] Step 4: adding a certain amount of xonotlite to the mixed solution obtained in step 3, and further adjusting the pH value of the solution to 3-6 with sodium hydroxide solution;

[0011] Step 5: The solution obtained in step 4 is subjected to magnetic stirring, hydrothermal reaction in a high pressure reactor, centrifugal washing, and drying to obtain TiO 2 / xonotlite composite catalyst.

[0012] In some embodiments, the inorganic titanium salt in step 1 is a mixture of titanium sulfate and titanous sulfate.

[0013] In some embodiments, the mass ratio of titanium sulfate to titanous sulfate is 5:2-9:2.

[0014] In some embodiments, the concentration of the titanium sulfate and titanous sulfate mixture is 0.4 mol / L-0.7 mol / L.

[0015] In some embodiments, the organic sulfur-containing compound in step 2 is a mixture of thiourea and mercaptan.

[0016] In some embodiments, the mass ratio of thiourea to mercaptan is 3:1-7:1.

[0017] In some embodiments, the magnetic stirring time in step 1 is 2-3 hours.

[0018] In some embodiments, the reaction time of the hydrothermal reaction in step 5 is 8-12 hours.

[0019] In some embodiments, the reaction temperature of the hydrothermal reaction in step 5 is 150-280°C.

[0020] The present invention also provides a TiO 2 / xonotlite composite catalyst, comprising the above TiO 2 The catalyst is prepared by a method for preparing a composite catalyst of calcium notoginseng / xonotlite.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] The invention uses titanium sulfate and titanium sulfate as titanium sources, organic sulfur-containing compounds as sulfur sources, and xonotlite fiber as a carrier to prepare TiO by a hydrothermal method. 2 / xonotlite composite catalyst, the prepared TiO 2The photodegradation ability of the TiO2 / xonotlite composite catalyst is improved, for example, the degradation rate of methyl orange is improved, the pore size is increased, the light energy utilization rate is improved, and the cycle stability is improved; the prepared TiO 2 / The degradation efficiency of harmful gases by the hard calcium silicate composite catalyst is improved, for example, the efficiency of formaldehyde treatment is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The TiO prepared in Example 1 of the present invention 2 SEM image of / xonotlite composite catalyst. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments to further understand the purpose, solution and effect of the present invention, but it is not intended to limit the scope of protection of the claims attached to the present invention.

[0025] Example 1

[0026] A TiO 2 / The preparation method of xonotlite composite catalyst comprises the following steps:

[0027] Step 1: dissolving a mixture of titanium sulfate and titanous sulfate to obtain a solution, wherein the mass ratio of titanium sulfate to titanous sulfate is 7:2, the concentration of the mixture of titanium sulfate and titanous sulfate is 0.5 mol / L, and magnetic stirring is performed for 2.5 hours to fully dissolve the mixture;

[0028] Step 2: Weigh a certain amount of a mixture of thiourea and thiol and add it to the solution obtained in step 1, wherein the mass ratio of thiourea to thiol is 5:1;

[0029] Step 3: adding sodium hydroxide solution dropwise to the mixed solution obtained in step 2 to adjust the pH value of the mixed solution to 2;

[0030] Step 4: adding a certain amount of xonotlite to the mixed solution obtained in step 3, and further adjusting the pH value of the solution to 5 with a sodium hydroxide solution;

[0031] Step 5: The solution obtained in step 4 was subjected to hydrothermal reaction in a high pressure reactor for 10 h after magnetic stirring at a temperature of 200°C, and then centrifuged, washed and dried to obtain TiO 2 / xonotlite composite catalyst.

[0032] Example 2

[0033] Compared with Example 1, the difference is that the mass ratio of titanium sulfate to titanium sulfate in step 1 is 5:2.

[0034] Example 3

[0035] Compared with Example 1, the difference is that the mass ratio of titanium sulfate to titanium sulfate in step 1 is 9:2.

[0036] Example 4

[0037] Compared with Example 1, the difference is that the concentration of the titanium sulfate and titanous sulfate mixed solution in step 1 is 0.4 mol / L.

[0038] Example 5

[0039] Compared with Example 1, the difference is that the concentration of the titanium sulfate and titanous sulfate mixed solution in step 1 is 0.7 mol / L.

[0040] Example 6

[0041] Compared with Example 1, the difference is that the mass ratio of thiourea to thiol in step 2 is 3:1.

[0042] Example 7

[0043] Compared with Example 1, the difference is that the mass ratio of thiourea to mercaptan in step 2 is 7:1.

[0044] Comparative Example 1

[0045] Compared with Example 1, the difference is that the inorganic titanium salt solution in step 1 is titanium sulfate.

[0046] Comparative Example 2

[0047] Compared with Example 1, the difference is that the mass ratio of titanium sulfate to titanium sulfate in the step 1 is 2:1.

[0048] Comparative Example 3

[0049] Compared with Example 1, the difference is that the mass ratio of titanium sulfate to titanium sulfate in step 1 is 5:1.

[0050] Comparative Example 4

[0051] Compared with Example 1, the difference is that the concentration of the titanium sulfate and titanous sulfate mixed solution in step 1 is 0.3 mol / L.

[0052] Comparative Example 5

[0053] Compared with Example 1, the difference is that the concentration of the titanium sulfate and titanous sulfate mixed solution in step 1 is 0.8 mol / L.

[0054] Comparative Example 6

[0055] Compared with Example 1, the difference is that the organic sulfur-containing compound in step 2 is thiourea.

[0056] Comparative Example 7

[0057] Compared with Example 1, the difference is that the mass ratio of thiourea to mercaptan in step 2 is 2:1.

[0058] Comparative Example 8

[0059] Compared with Example 1, the difference is that the mass ratio of thiourea to mercaptan in step 2 is 8:1.

[0060] Performance Testing

[0061] The performance tests of Examples 1-7 and Comparative Examples 1-8 were carried out, specifically:

[0062] a. Select the catalyst samples prepared in each embodiment and comparative example, and conduct photodegradation experiments on them; select methyl orange as the target degradation product. Weigh a certain amount of methyl orange powder to prepare a methyl orange solution with a concentration of 20 mg / L, weigh 10 mg of the photocatalyst sample and 10 ml of the methyl orange solution in a 50 ml beaker, and place it under a high-pressure mercury lamp to simulate visible light for photodegradation experiments. Take samples every two hours, 5 ml each time, take the upper clear liquid in a quartz cuvette after centrifugation, and measure the absorbance value at the maximum absorption wavelength (about 463 nm) of methyl orange in a UV-visible spectrophotometer. Calculate the degradation rate of methyl orange based on the absorbance value, and then judge the strength of the degradation ability. The calculation formula of the methyl orange degradation rate is as follows:

[0063]

[0064] In the formula, Dp: degradation rate of methyl orange;

[0065] A: absorbance of methyl orange solution after t hours of illumination;

[0066] A 0 : absorbance of methyl orange solution at initial concentration;

[0067] C: methyl orange concentration after t hours of illumination;

[0068] C 0 : Initial concentration of methyl orange.

[0069] b. Select the catalyst samples prepared in each embodiment and comparative example, test their treatment efficiency for harmful gas formaldehyde and make statistics. Weigh 40 mg of the material to be evaluated and place it in a formaldehyde gas with a concentration of 3 ppm. Under the irradiation of a xenon lamp for 120 minutes, use a treatment device to treat formaldehyde, pass through a formaldehyde detection system, and calculate the formaldehyde treatment effect, that is, obtain the formaldehyde degradation efficiency. Among them, the calculation formula for the formaldehyde treatment efficiency is = (initial concentration of formaldehyde V 0 - Final concentration of formaldehyde V 1 ) / initial concentration of formaldehyde V 0 ×100%.

[0070] (1) The performance test results of Examples 1-3 and Comparative Examples 1-3 were statistically analyzed to obtain the following table:

[0071] Degradation rate of methyl orange Efficiency of treating formaldehyde Example 1 100% 98% Example 2 99% 96% Example 3 98% 97% Comparative Example 1 82% 44% Comparative Example 2 91% 68% Comparative Example 3 89% 77%

[0072] It can be found from the analysis of Examples 1-3 and Comparative Example 1 that in TiO 2 / In the preparation process of the xonotlite composite catalyst, when titanium sulfate and titanous sulfate were used as titanium sources, the degradation rate of methyl orange by the prepared composite catalyst was as high as over 98%, and the treatment efficiency of formaldehyde was also over 96%. When titanium sulfate was used alone as the titanium source, the degradation rate of methyl orange by the prepared composite catalyst was about 80%, and it was found that its treatment efficiency of formaldehyde was only 44%. Therefore, when titanium sulfate and titanous sulfate were used as titanium sources, the prepared TiO 2 The photocatalytic performance of the / xonotlite composite catalyst has been significantly improved, the degradation rate of methyl orange has been increased, and the treatment efficiency of formaldehyde is also very high.

[0073] At the same time, referring to Examples 1-3 and Comparative Examples 2-3, it can be found that within the range of 5:2-9:2 of the mass ratio of titanium sulfate to titanium sulfate provided by the present invention, the degradation rate of methyl orange by the prepared catalyst can reach nearly 100%, while exceeding this range, the degradation rate can only reach about 90%; and within the range of 5:2-9:2 of the mass ratio of titanium sulfate to titanium sulfate provided by the present invention, the treatment efficiency of the prepared catalyst for formaldehyde reaches about 97%, while the treatment efficiency for formaldehyde outside this range is only about 70%.

[0074] (2) The performance test results of Example 1, Examples 4-5 and Comparative Examples 4-5 were statistically analyzed to obtain the following table:

[0075] Degradation rate of methyl orange Example 1 100% Example 4 98% Example 5 99% Comparative Example 4 91% Comparative Example 5 92%

[0076] It can be found that in TiO 2 / During the preparation of the xonotlite composite catalyst, when the concentration of the titanium sulfate and titanous sulfate mixed solution is 0.4 mol / L-0.7 mol / L, the degradation rate of methyl orange by the prepared composite catalyst is relatively high. When it exceeds this range, although the degradation rate can reach about 90%, it is still relatively low.

[0077] (3) The performance test results of Example 1, Examples 6-7 and Comparative Examples 6-8 were statistically analyzed to obtain the following table:

[0078] Degradation rate of methyl orange Efficiency of treating formaldehyde Example 1 100% 98% Example 6 100% 98% Example 7 99% 96% Comparative Example 6 99% 56% Comparative Example 7 97% 78% Comparative Example 8 97% 80%

[0079] It can be found from the analysis of Examples 1, 6-7 and Comparative Examples 6-8 that in TiO 2 In the preparation method of the composite catalyst of xonotlite, thiourea and mercaptan with a mass ratio of 3:1-7:1 are used as sulfur doping to prepare TiO 2 When thiourea is used as the sulfur source alone, the degradation rate of methyl orange is still high, but the formaldehyde treatment efficiency is significantly reduced, reaching only 56%.

[0080] The TiO prepared in Examples 1, 6-7 and Comparative Examples 6-8 was further calculated by the Barrett-Joyner-Halenda (BJH) model. 2 / The pore size of the xonotlite composite catalyst is as follows:

[0081] Average pore size Example 1 6.875nm Example 6 6.233nm Example 7 6.452nm Comparative Example 6 4.658nm Comparative Example 7 5.871nm Comparative Example 8 5.989nm

[0082] It can be seen that in the preparation method provided by the present invention, thiourea and mercaptan in a mass ratio of 3:1-7:1 are used as sulfur doping to prepare TiO 2 The average pore size of the / xonotlite composite catalyst increases, and a larger pore size is more conducive to the transport and adsorption of reactants than a smaller pore size.

[0083] Furthermore, the TiO prepared in Example 1 2 / Xonotlite composite catalyst was tested by SEM, see Figure 1 It can be clearly seen from the figure that almost the entire field of view is filled with xonotlite fibers, and the fibers are interconnected. This may be the result of the addition of titanium dioxide, which loads titanium dioxide on the surface of xonotlite and connects the xonotlite fibers to each other.

[0084] In summary, the photocatalytic activity of the composite catalyst prepared by the TiO2 / xonotlite composite catalyst preparation method provided by the present invention is improved, the catalytic performance is enhanced, the pore size is increased, and it has a good treatment effect on the harmful gas formaldehyde.

[0085] The above description is only a preferred embodiment of the present invention and does not limit the present invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes and apply it to other fields. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a TiO2 / xonotlite composite catalyst, characterized in that: The steps include: Step 1: Dissolve the inorganic titanium salt solution and stir it magnetically to fully dissolve it; Step 2: Weigh a certain amount of organic sulfur-containing compound and add it to the solution obtained in step 1; Step 3: adding sodium hydroxide solution dropwise to the mixed solution of inorganic titanium salt and thiourea obtained in step 2, and adjusting the pH value of the mixed solution to 1.5-3; Step 4: adding a certain amount of xonotlite to the mixed solution obtained in step 3, and further adjusting the pH value of the solution to 3-6 with sodium hydroxide solution; Step 5: The solution obtained in step 4 is subjected to hydrothermal reaction in a high-pressure reactor after magnetic stirring, and then centrifugally washed and dried to obtain a TiO2 / xonotlite composite catalyst.

2. The method for preparing the TiO2 / xonotlite composite catalyst according to claim 1, characterized in that: The inorganic titanium salt in step 1 is a mixture of titanium sulfate and titanous sulfate.

3. The method for preparing the TiO2 / xonotlite composite catalyst according to claim 2, characterized in that: The mass ratio of titanium sulfate to titanous sulfate is 5:2-9:

2.

4. The method for preparing the TiO2 / xonotlite composite catalyst according to claim 2, characterized in that: The concentration of the titanium sulfate and titanous sulfate mixed solution is 0.4 mol / L-0.7 mol / L.

5. The method for preparing the TiO2 / xonotlite composite catalyst according to claim 1, characterized in that: The organic sulfur-containing compound in step 2 is a mixture of thiourea and mercaptan.

6. The method for preparing the TiO2 / xonotlite composite catalyst according to claim 5, characterized in that: The mass ratio of thiourea to mercaptan is 3:1-7:

1.

7. The method for preparing the TiO2 / xonotlite composite catalyst according to claim 1, characterized in that: The magnetic stirring time in step 1 is 2-3 hours.

8. The method for preparing the TiO2 / xonotlite composite catalyst according to claim 1, characterized in that: The reaction time for the hydrothermal reaction in step 5 is 8-12 hours.

9. The method for preparing the TiO2 / xonotlite composite catalyst according to claim 1, characterized in that: The reaction temperature of the hydrothermal reaction in step 5 is 150-280°C.

10. A TiO2 / xonotlite composite catalyst, characterized in that: The catalyst is prepared by the method for preparing the TiO2 / xonotlite composite catalyst according to any one of claims 1 to 9.