Preparation and application of Co-Nx co-doped carbon nanotube for in-situ encapsulation of cobalt nanoparticles
By in situ encapsulating cobalt nanoparticles in Co-Nx co-doped carbon nanotubes, forming Co@N-CNTs and combining with PMS, the problems of low catalyst activity and poor stability are solved, and the efficient degradation of phenolic compounds is achieved and the Environmentally friendly catalytic effect.
Patent Information
- Application Number
- CN202310534931.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-12
AI Technical Summary
The existing catalysts have low activity, poor stability and metal ion dissolution problems when degrading phenolic compounds in the treatment water, resulting in environmental pollution.
Cobalt nanoparticles are encapsulated in situ in Co-Nx co-doped carbon nanotubes to form Co@N-CNTs, which are used to activate PMS under the permonosulfate system to achieve efficient degradation of phenolic compounds. The method includes preparing the precursor CoxZny-ZIF in a supercritical fluid, pyrolysis at high temperature after adding a nitrogen source to form Co@N-CNTs, and applying it to the phenolic compound solution after pickling, adding PMS to the phenolic compound solution for degradation.
The degradation rate of 95.62% to 100% of phenolic compounds is achieved, the leaching amount of cobalt ions is reduced, the stability and anti-anionic ability of the catalyst are improved, and the adaptability to a wide pH range is adapted.
Smart Images

Figure CN118925704A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of new environmental materials, and specifically relates to a Co-N x Preparation method of co-doped carbon nanotubes, prepared Co-N nanotubes with in-situ encapsulation of cobalt nanoparticles x Co-doped carbon nanotubes can efficiently degrade phenolic compounds. Background Art
[0002] Phenolic compounds are widely used in industrial production. Common phenolic compounds include phenol, bisphenol A, acetaminophen and octylphenol. Studies have found that different concentrations of phenolic compounds have been detected in rivers, soil and landfill leachate. Phenolic compounds in the environment can enter the human body through skin contact, daily diet and inhalation of dust, thus threatening human health. In the face of the harm of phenolic compounds to the natural ecological environment and human health, how to reasonably remove phenolic compounds in water bodies has become a hot topic of research.
[0003] Advanced oxidation processes (AOPs) based on peroxymonosulfate (KHSO5, Peroxymonosulfate, PMS) have attracted wide attention in the treatment of refractory organic pollutants in water environments. Advanced oxidation technology can produce reactive oxygen species (ROS) with strong oxidative ability, such as sulfate radicals (SO4 ·- ), hydroxyl radical (·OH) and singlet oxygen ( 1 O2) to decompose organic pollutants into small molecular organic matter, which are finally mineralized into CO2 and H2O, thus achieving the purpose of completely degrading organic pollutants.
[0004] In recent years, metal oxides and carbon-based materials have been widely used in the advanced oxidation process of persulfate. However, metal oxides have poor stability and serious metal ion leaching problems, which will cause secondary pollution to the environment. Carbon-based materials have good stability, but their activity is generally low. Therefore, how to combine the advantages of high catalytic activity and long-term stability in one catalyst still faces great challenges. Summary of the invention
[0005] The purpose of the present invention is to provide a Co-N in-situ encapsulated cobalt nanoparticles. x The preparation and application of co-doped carbon nanotubes solve the problems of low activity, poor stability and serious metal ion dissolution of most current catalysts, and degrade phenolic compounds in water in a persulfate system.
[0006] The technical solution of the present invention is as follows: a Co-N in-situ encapsulated cobalt nanoparticle xThe method for preparing co-doped carbon nanotubes is characterized in that cobalt nanoparticles are in situ encapsulated in carbon nanotubes, and part of the cobalt atoms are stabilized in the Co-N x Co-N encapsulated cobalt nanoparticles are formed in the structure x Co-doped carbon nanotubes are used to activate PMS to degrade phenolic compounds. The specific steps are as follows:
[0007] (1) Precursor Co x Zn y Preparation of -ZIF: Cobalt salt, zinc salt and organic ligand are reacted in supercritical fluid, washed with ethanol or methanol, and centrifuged to obtain the precursor Co x Zn y -ZIF;
[0008] (2) Intermediate Co x Zn y -ZIF / nitrogen source preparation: The precursor Co x Zn y -ZIF is mixed with a nitrogen source in an organic solvent for a period of time, and the organic solvent is evaporated and dried to obtain the intermediate Co x Zn y -ZIF / nitrogen source;
[0009] (3) In-situ encapsulation of Co-N nanoparticles x Preparation of co-doped carbon nanotubes (Co@N-CNTs-x / y): The intermediate Co x Zn y -ZIF / nitrogen source is obtained by high temperature pyrolysis under inert gas, acid washing, cleaning and drying.
[0010] (Preferably, the cobalt salt in step 1) is one or more of cobalt acetylacetonate (Co(acac)2) and cobalt nitrate hexahydrate (Co(NO3)2·6H2O), and the zinc salt is one or more of zinc acetylacetonate (Zn(acac)2) and zinc nitrate hexahydrate (Zn(NO3)2·6H2O).
[0011] (Preferably, the molar ratio of the cobalt salt, zinc salt and organic ligand in step 1) is 1:(0.5-1.8):(6-11.2).
[0012] The supercritical fluid in (preferably step 1) is one of supercritical carbon dioxide and supercritical water.
[0013] The reaction temperature in (preferably step 1) is 30-60° C., the reaction pressure is 20-40 MPa, and the reaction time is 10-60 min.
[0014] (Preferably, step 2) wherein the nitrogen source is one or more of dicyandiamide, polyvinyl pyrrolidone and urea; the precursor Cox Zn y -The mass ratio of ZIF to nitrogen source is 1:(1-4).
[0015] (Preferably, the mixing reaction time in step 2) is 12 to 24 hours; the organic solvent is one of methanol or ethanol.
[0016] (Preferably, the inert gas in step 3) is argon or nitrogen; the high temperature pyrolysis temperature is 700-1000° C., and the pyrolysis time is 2-3 hours.
[0017] The acid used for pickling in (preferably step 3) is one or more of sulfuric acid, nitric acid or hydrochloric acid, the acid concentration is 0.5 to 1.0 mol / L, and the pickling time is 8 to 10 hours.
[0018] Co-N in-situ encapsulated cobalt nanoparticles prepared by the present invention x Co-doped carbon nanotubes (Co@N-CNTs-x / y) are used to activate PMS and efficiently degrade phenolic compounds in water. The phenolic compounds are one or more of phenol, bisphenol A and acetaminophen. The specific steps are as follows:
[0019] In situ encapsulation of Co-N nanoparticles x The co-doped carbon nanotubes are placed in an aqueous solution containing a phenolic compound, and then PMS is added and reacted for 10 to 60 minutes under magnetic stirring.
[0020] The concentration of the phenolic compound solution is 0.10-0.25 g / L.
[0021] Preferably, the volume ratio of the input mass of Co@N-CNTs-x / y to the solution containing the phenolic compound is 0.03 g / L to 0.15 g / L.
[0022] Preferably, the volume ratio of the input amount of the PMS to the solution is 0.37 g / L to 0.87 g / L.
[0023] The method for detecting the concentration of phenolic compounds in water provided by the present invention is as follows:
[0024] The concentration of phenolic compounds in the solution after the reaction was detected by high performance liquid chromatography, and the results showed that the degradation rate of phenolic compounds was 95.62% to 100%.
[0025] Beneficial effects of the present invention:
[0026] (1) The present invention uses supercritical fluid as a reaction solvent to quickly and greenly synthesize the precursor Co x Zn y -ZIF, thus avoiding the use of a large amount of organic solvents, the synthesized crystals have good crystallinity, and it is an environmentally friendly and efficient synthesis method.
[0027] (2) The present invention can adjust the particle size of cobalt nanoparticles in the pyrolysis composite material and the formation of carbon nanotubes by adjusting the molar ratio of the initial cobalt salt and the zinc salt. The cobalt nanoparticles are encapsulated in situ and the Co atoms in the material are anchored to form Co-N x structure, reducing the leaching ratio of cobalt ions and solving the problems of poor stability of most catalysts and secondary pollution caused by metal ion dissolution.
[0028] (3) The present invention utilizes Co-N in situ encapsulation of cobalt nanoparticles x Co-doped carbon nanotubes achieve efficient degradation of one or more phenolic compounds such as phenol, bisphenol A and acetaminophen. This material can solve the problem of inorganic anions (Cl - 、NO3 - 、HCO3 - and H2PO4 - ) and a wide pH range (3-11).
[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The Co-N in-situ encapsulated cobalt nanoparticles of Example 2 x Scanning electron microscopy images of co-doped carbon nanotubes;
[0031] Figure 2 The Co-N in-situ encapsulated cobalt nanoparticles of Example 2 x Transmission electron microscopy image of co-doped carbon nanotubes;
[0032] Figure 3 The Co-N in-situ encapsulated cobalt nanoparticles of Example 2 x Degradation performance diagram of co-doped carbon nanotubes in anion tolerance experiment;
[0033] Figure 4 The Co-N in-situ encapsulated cobalt nanoparticles of Example 2 x Degradation performance diagram of co-doped carbon nanotubes at different initial pH. DETAILED DESCRIPTION
[0034] Example 1
[0035] A Co-N in-situ encapsulated cobalt nanoparticle x The method for degrading phenolic compounds by co-doping carbon nanotubes comprises the following steps:
[0036] (1) Precursor Co x Zn yPreparation of -ZIF: 1.0 mmol of cobalt nitrate hexahydrate, 0.5 mmol of zinc nitrate hexahydrate and 6 mmol of dimethylimidazole were reacted in supercritical carbon dioxide at 60 °C and 40 MPa for 60 min, washed with ethanol, and centrifuged to obtain the precursor Co x Zn y -ZIF;
[0037] (2) Intermediate Co x Zn y -ZIF / nitrogen source preparation: The precursor Co x Zn y -ZIF was mixed with polyvinyl pyrrolidone in methanol for 12 h, and the organic solvent was evaporated to obtain the intermediate Co x Zn y -ZIF / polyvinylpyrrolidone.
[0038] (3) In-situ encapsulation of Co-N nanoparticles x Preparation of co-doped carbon nanotubes (Co@N-CNTs-x / y): The intermediate Co x Zn y -ZIF / polyvinyl pyrrolidone was pyrolyzed at 950 °C for 3 h in a nitrogen atmosphere, washed with 0.8 mol / L nitric acid for 10 h, and then cleaned and dried to obtain Co-N nanoparticles encapsulated in situ. x Co-doped carbon nanotubes (Co@N-CNTs-x / y).
[0039] (4) Add 0.12 g / L of Co@N-CNTs-x / y prepared in step (3) to a 0.20 g / L phenol solution, then add 0.6 g / L of PMS, and react for 40 min under magnetic stirring. The solution after the reaction is filtered using a 0.22 μm filter membrane, and the concentration of phenol in the solution is determined by high performance liquid chromatography. The degradation rate of phenol is 95.62%, and the leaching amount of cobalt ions in the solution is 0.32 mg / L.
[0040] Example 2
[0041] A Co-N in-situ encapsulated cobalt nanoparticle x The method for degrading phenolic compounds by co-doping carbon nanotubes comprises the following steps:
[0042] (1) Precursor Co x Zn y Preparation of -ZIF: 1.0 mmol of cobalt acetylacetonate, 1.0 mmol of zinc acetylacetonate and 8 mmol of dimethylimidazole were reacted in supercritical carbon dioxide at 60 °C and 30 MPa for 10 min, washed with methanol, and centrifuged to obtain the precursor Co x Zn y -ZIF;
[0043] (2) Intermediate Co x Zn y -ZIF / nitrogen source preparation: The precursor Co x Zn y -ZIF was mixed with dicyandiamide in methanol for 12 h, and the organic solvent was evaporated to obtain the intermediate Co x Zn y -ZIF / dicyandiamide.
[0044] (3) In-situ encapsulation of Co-N nanoparticles x Preparation of co-doped carbon nanotubes (Co@N-CNTs-x / y): The intermediate Co x Zn y -ZIF / dicyandiamide was pyrolyzed at 900 °C for 2 h in a nitrogen atmosphere, pickled with 0.5 mol / L sulfuric acid for 8 h, and then cleaned and dried to obtain Co-N nanoparticles encapsulated in situ. x Co-doped carbon nanotubes (Co@N-CNTs-x / y).
[0045] (4) Add 0.10 g / L of Co@N-CNTs-x / y prepared in step (3) to a solution containing 0.15 g / L of bisphenol A, then add 0.615 g / L of PMS, and react for 40 min under magnetic stirring. The solution after the reaction is filtered using a 0.22 μm filter membrane, and the concentration of bisphenol A in the solution is determined by high performance liquid chromatography. The degradation rate of bisphenol A is 100%, and the leaching amount of cobalt ions is 0.27 mg / L.
[0046] Example 3
[0047] A Co-N in-situ encapsulated cobalt nanoparticle x The method for degrading phenolic compounds by co-doping carbon nanotubes comprises the following steps:
[0048] (1) Precursor Co x Zn y Preparation of -ZIF: 1.0 mmol of cobalt nitrate hexahydrate, 1.8 mmol of zinc acetylacetonate and 11.2 mmol of dimethylimidazole were reacted in supercritical carbon dioxide at 30 °C and 20 MPa for 30 min, washed with methanol, and centrifuged to obtain the precursor Co x Zn y -ZIF;
[0049] (2) Intermediate Co x Zn y -ZIF / nitrogen source preparation: The precursor Co x Zn y -ZIF was mixed with urea in methanol for 24 h, and the organic solvent was evaporated to obtain the intermediate Cox Zn y -ZIF / urea.
[0050] (3) In-situ encapsulation of Co-N nanoparticles x Preparation of co-doped carbon nanotubes (Co@N-CNTs-x / y): The intermediate Co x Zn y -ZIF / urea was pyrolyzed at 750 °C for 3 h in an argon atmosphere, pickled with 0.3 mol / L hydrochloric acid for 8 h, and then cleaned and dried to obtain Co-N nanoparticles encapsulated in situ. x Co-doped carbon nanotubes (Co@N-CNTs-x / y).
[0051] (4) Add 0.08 g / L of Co@N-CNTs-x / y prepared in step (3) to a solution containing 0.25 g / L of acetaminophen, then add 0.87 g / L of PMS, and react for 40 min under magnetic stirring. The solution after the reaction is filtered using a 0.22 μm filter membrane, and the concentration of acetaminophen in the solution is determined by high performance liquid chromatography. The degradation rate of acetaminophen is 98.2%, and the leaching amount of cobalt ions is 0.23 mg / L.
Claims
1. A Co-N in situ encapsulated cobalt nanoparticle x The method for preparing co-doped carbon nanotubes is characterized in that: The following steps are involved: (1) Cobalt salt, zinc salt and dimethylimidazole are mixed and reacted in a supercritical fluid to obtain a precursor Co x Zn y -ZIF. (2) The precursor Co obtained in step (1) x Zn y -ZIF is mixed with a nitrogen source in an organic solvent for a period of time to obtain the intermediate Co x Zn y -ZIF / nitrogen source. (3) The intermediate Co obtained in step (2) x Zn y -ZIF / nitrogen source was pyrolyzed under inert gas and acid-washed to obtain Co-N nanoparticles encapsulated in situ x Co-doped carbon nanotubes (Co@N-CNTs-x / y).
2. The Co-N encapsulated cobalt nanoparticles according to claim 1. x The method for preparing co-doped carbon nanotubes is characterized in that: The cobalt salt in step (1) is one or more of cobalt acetylacetonate (Co(acac)2) and cobalt nitrate hexahydrate (Co(NO3)2·6H2O); the zinc salt is one or more of zinc acetylacetonate (Zn(acac)2) and zinc nitrate hexahydrate (Zn(NO3)2·6H2O); and the supercritical fluid is one of supercritical carbon dioxide and supercritical water.
3. The Co-N in-situ encapsulated cobalt nanoparticles according to claim 1 x The method for preparing co-doped carbon nanotubes is characterized in that: In the step (1), the molar ratio of the cobalt salt, the zinc salt and the organic ligand is 1:(0.5-1.8):(6-11.2).
4. The Co-N in-situ encapsulated cobalt nanoparticles according to claim 1 x The method for preparing co-doped carbon nanotubes is characterized in that: The reaction temperature in step (1) is 30-60° C., the reaction pressure is 20-40 MPa, and the reaction time is 10-60 min.
5. The Co-N in-situ encapsulated cobalt nanoparticles according to claim 1 x The method for preparing co-doped carbon nanotubes is characterized in that: The nitrogen source in step (2) is one or more of dicyandiamide, polyvinyl pyrrolidone and urea, and the precursor Co x Zn y The mass ratio of -ZIF to nitrogen source is 1:(1-4), the mixing reaction time is 12-24 hours, and the organic solvent is one or more of methanol or ethanol.
6. The Co-N in-situ encapsulated cobalt nanoparticles according to claim 1 x The method for preparing co-doped carbon nanotubes is characterized in that: In the step (3), the inert gas is one or more of argon or nitrogen, the pyrolysis temperature is 700-1000° C., and the pyrolysis time is 2-3 hours.
7. The Co-N in-situ encapsulated cobalt nanoparticles according to claim 1. x The method for preparing co-doped carbon nanotubes is characterized in that: The acid used for pickling in step (3) is one or more of sulfuric acid, nitric acid or hydrochloric acid, the acid concentration is 0.5-1.0 mol / L, and the pickling time is 8-10 hours.
8. A Co-N nanoparticle in-situ encapsulated cobalt nanoparticle according to any one of claims 1 to 7 x Application of co-doped carbon nanotubes as activated peroxymonosulfate.
9. The Co-N in-situ encapsulated cobalt nanoparticles according to claim 8 x The use of co-doped carbon nanotubes as activated peroxymonosulfate is characterized in that: The application mode is as a degradation agent of phenolic compounds.
10. The Co-N in situ encapsulated nanoparticles according to claim 9. x The application of co-doped carbon nanotubes is characterized by: The phenolic compound is one or more of phenol, bisphenol A and acetaminophen.
Citation Information
Cited By
Preparation method of cobalt nitride nanowire rich in nitrogen vacancies and application of cobalt nitride nanowire in advanced treatment of antibiotic wastewater
CN119702040A