Method for preparing cerium-zirconium-aluminum composite oxide carrier through homogeneous precipitation method and application of cerium-zirconium-aluminum composite oxide carrier
The cerium-zirconium-aluminum composite oxide support was prepared by homogeneous precipitation method, combined with noble metal-supported catalysts, which solved the problem of insufficient catalytic activity, achieved efficient CO catalytic oxidation reaction, and reduced the preparation cost.
Patent Information
- Application Number
- CN202411055487.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
AI Technical Summary
The existing cerium-zirconium-aluminum composite oxide support lacks catalytic activity in catalytic oxidation reaction, and the pore structure is not conducive to the high dispersion of the active components of noble metals, resulting in the need to improve the catalytic activity.
The homogeneous precipitation method is used to prepare the cerium-zirconium-aluminum composite oxide support. Through the microwave-assisted homogeneous precipitation process, the slow growth and high dispersion of CeO2 crystallization are promoted, and the catalytic activity is improved by combining with precious metal-supported catalysts.
The CO catalytic oxidation activity of the catalyst is improved, the preparation cost is reduced, and the synergistic effect between precious metals and the support is improved, which significantly improves the catalytic activity and durability.
Smart Images

Figure CN118925707A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts and air pollution control, and in particular relates to a cerium-zirconium-aluminum composite oxide carrier for CO catalytic oxidation, and a preparation method and application thereof. Background Art
[0002] In the steel industry, the sintering process is the most serious link in producing atmospheric pollutants such as carbon monoxide and nitrogen oxides. Sintering flue gas has the characteristics of large flue gas volume, complex composition, large flue gas temperature fluctuation range, and high water content, which increases the difficulty of controlling pollutants in sintering flue gas. The problem of removing CO from sintering flue gas needs to be solved urgently, and the problem of CO emission reduction has received widespread attention from all walks of life. Therefore, the removal of CO from sintering flue gas has important application value.
[0003] At present, there are many methods for treating CO in flue gas, such as direct combustion, cryogenic separation, solution absorption, adsorption and catalytic oxidation. Among them, catalytic oxidation is to convert CO and oxygen into carbon dioxide and water at a certain temperature. Compared with other CO treatment processes, catalytic oxidation has the advantages of large treatment capacity, high purification efficiency, no secondary pollution and high safety, making it a feasible sintering flue gas treatment technology. The key to catalytic oxidation technology lies in the development of catalysts.
[0004] The catalytic oxidation method is considered to be one of the most effective and economical ways to remove CO due to its high efficiency and relatively low reaction temperature. In recent years, the catalytic oxidation removal process of nitrogen oxides and carbon monoxide in sintering flue gas has been publicly reported. For example, CN103708808A (a sintering flue gas semi-dry desulfurization ash autoclaved brick and its production method) and CN116371188A (a sintering flue gas energy-saving denitrification system and method), the technical routes disclosed in their patent applications are all catalytic oxidation removal of CO processes. At present, most of the sintering flue gas CO removal projects that have reached pilot scale use catalytic oxidation technology for the removal of CO from sintering flue gas in the test.
[0005] In the catalytic oxidation method, commonly used catalysts include precious metal catalysts (such as Pt, Au, Pd, Ag) and non-precious metal catalysts (such as Cu, Co, Mn). Precious metal catalysts have good activity and stability, but are relatively expensive. Usually, the active components are highly dispersed on the carrier to increase the catalytic active sites, thereby reducing the loading amount of the active components to control the catalyst cost. Among them, Pt is one of the most commonly used catalysts. In addition, precious metal catalysts such as Au, Pd and Ag are also widely used in CO removal reactions.
[0006] Metal oxides are one of the carriers of precious metal catalysts, among which alumina is a commonly used carrier. By doping other metal elements, such as rare earth elements or alkali metal elements, composite metal oxides can be obtained to improve the performance of the catalyst. The preparation methods of composite metal oxide carriers include hydrothermal method, coprecipitation method or sol-gel method. Cerium-zirconium-aluminum composite oxides have been widely studied and applied. Zhao Ming et al. (Preparation of CeO2-ZrO2-Al2O3 and catalytic performance of its palladium-loaded three-way catalyst,
[0007] [J]. Chin. J. Catal, 2010, 31: 429-434), the cerium zirconium aluminum composite oxide carrier prepared by coprecipitation method and the palladium-based catalyst prepared by impregnation method have a large specific surface area and a high oxygen storage capacity, but their three-way catalytic activity needs to be improved. The sample prepared by coprecipitation method has a large specific surface area, but its pore structure is not conducive to the high dispersion of the noble metal active components, and its catalytic activity needs to be improved. Summary of the invention
[0008] The object of the present invention is to provide a method for preparing a cerium-zirconium-aluminum composite oxide carrier by a homogeneous precipitation method. Through a microwave-assisted urea homogeneous precipitation process, the slow growth and high dispersion of CeO2 crystals are promoted, the synergistic effect between the noble metal and the carrier can be enhanced, and the catalyst obtained after loading the active component has high CO catalytic oxidation activity.
[0009] Another object of the present invention is to provide a noble metal supported catalyst based on the carrier and its application in CO catalytic oxidation reaction.
[0010] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0011] A method for preparing a cerium-zirconium-aluminum composite oxide support by a homogeneous precipitation method, characterized in that it comprises the following steps:
[0012] (1) mixing a cerium precursor, a zirconium precursor, Al2O3 and urea in a solvent, and heating and aging the resulting mixed solution under microwave action;
[0013] (2) The slurry obtained in step (1) is centrifuged, washed with water, and dried; the obtained solid is calcined and crushed to obtain the cerium-zirconium-aluminum composite oxide carrier.
[0014] The carrier uses urea as a precipitant, and cerium and zirconium are deposited on Al2O3 through homogeneous precipitation. The precipitation process is slow, and the slurry is highly dispersed through microwave assistance, which promotes the slow growth and high dispersion of CeO2 crystals in the Al2O3 pore structure.
[0015] Preferably, based on the mass of the mixed solution, the mass fraction of urea is 3% to 15%.
[0016] Preferably, the mixed solution is heated at a temperature of 85 to 95° C. under the action of microwaves, and the aging time is 20 to 28 hours.
[0017] Preferably, the power of the microwave is 200-300W.
[0018] The Al2O3 includes but is not limited to α alumina, γ alumina, β alumina or η alumina. The particle size of the alumina is preferably 20 μm to 400 μm. The pore size of the alumina is preferably 2 to 50 nm, more preferably 10 to 30 nm.
[0019] Preferably, the solvent includes, but is not limited to, one or more of water, methanol, ethanol, acetonitrile, hexane and cyclohexane.
[0020] Preferably, the cerium precursor includes, but is not limited to, one or more of cerium acetate, cerium chloride, cerium acetate, cerium oxalate and cerium nitrate. The zirconium precursor includes, but is not limited to, one or more of zirconium acetate, zirconium oxalate, zirconium nitrate, zirconium acetate, zirconium carbonate and zirconium oxide.
[0021] In the mixed solution, the molar ratio of metal ions to urea is 1:1-50, preferably 1:5-25.
[0022] In step (2), preferably, the drying temperature is 100-300° C., the drying time is 1-5 hours, the roasting temperature is 300-900° C., and the roasting time is 1-5 hours.
[0023] The invention also relates to a cerium-zirconium-aluminum composite oxide carrier prepared by the method.
[0024] Furthermore, the cerium-zirconium-aluminum composite oxide carrier comprises, by mass percentage, 70% to 98% Al2O3, 1% to 29% CeO2, and 1% to 29% ZrO2.
[0025] The present invention also provides a cerium / zirconium doped alumina supported Pt-based catalyst, comprising noble metal Pt and the cerium-zirconium-aluminum composite oxide carrier.
[0026] Furthermore, in the catalyst, the Pt content is 0.1% to 2% by mass.
[0027] The catalyst can be prepared by loading the precious metal Pt according to the known methods in the prior art. The catalyst can be prepared into powder or granular catalysts of various shapes, or the prepared slurry can be coated on porous materials such as honeycombs and foam metals.
[0028] The present invention also provides the use of the cerium / zirconium doped alumina supported Pt-based catalyst in CO catalytic oxidation reaction.
[0029] Beneficial effects: The method for preparing a cerium-zirconium-aluminum composite oxide carrier by a urea homogeneous precipitation method provided by the present invention, the obtained cerium-zirconium-aluminum composite oxide carrier, due to the slow precipitation process of the urea homogeneous precipitation method, the precursor of Ce ions uses Al2O3 particles as crystal nuclei, slowly grows in the Al2O3 pore structure, and microwave-assisted CeO2 crystals are highly dispersed, this highly dispersed CeO2 can promote the interaction between the carrier and the active component Pt, improve the dispersion of the active component, and Pt has a smaller particle size, thereby promoting the improvement of catalytic activity. The carrier preparation method provided by the present invention is simple, the preparation cost is low, and the catalyst obtained after loading the active component has high CO catalytic activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Example 1 TEM image of the cerium-zirconium-aluminum composite oxide support prepared by urea homogeneous precipitation method.
[0031] Figure 2 The durability test of the Pt-based catalyst supported by the cerium-zirconium-aluminum composite oxide prepared in Example 1 in the CO catalytic combustion reaction. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is described in detail below through specific embodiments. However, it is necessary to point out that the following embodiments are only used to describe the content of the present invention and do not constitute a limitation on the protection scope of the present invention.
[0033] In the following examples, the test method for the activity of the catalyst in the catalytic oxidation reaction of CO is as follows: 1% Pt is loaded on a cerium-zirconium-aluminum composite oxide carrier, and the Pt-based catalyst loaded on the obtained cerium-zirconium-aluminum composite oxide carrier is pressed, ground, and sieved to obtain 40-60 mesh catalyst small particles. Weigh 0.035g and put it into a quartz tube with an inner diameter of 9mm, and the quartz tube is placed in an electric heating furnace. Use cylinder gas to simulate a CO-containing simulated mixed gas, and the composition of the inlet reaction gas is: O2=21%, CO=5000ppm, N2 balance gas. 300mL / min of the simulated mixed gas is passed into the quartz tube containing the catalyst, and the CO concentration in the outlet gas is analyzed by online chromatography. The reaction temperature of the test is 100-300℃; the air velocity is about 510000mL·g -1 ·h -1 The reaction temperature T50 or T90 when the CO conversion rate reaches 50% or 90% is mainly used as the catalyst activity index (the lower the value of T50 or T90, the better the catalyst activity).
[0034] Example 1
[0035] A cerium-zirconium-aluminum composite oxide carrier, a Pt-based catalyst based on the carrier and a preparation method thereof, the specific steps are as follows:
[0036] Weigh 2.17g of cerous nitrate hexahydrate and 2.235g of zirconium nitrate hexahydrate and dissolve them in 100ml of deionized water. Then weigh 11.46g of γ-Al2O3 and add them to the mixed solution and stir. Add 10ml of 30wt% urea solution to the obtained mixed solution. Use microwave-assisted heating with a power of 210W to 90°C to promote urea hydrolysis and stir the reaction for 24h. Then centrifuge and wash with water 3 times, and dry the washed product at 110°C for 2h. The dried solid is calcined at 500°C for 2h to obtain a cerium-zirconium-aluminum composite oxide carrier.
[0037] The cerium-zirconium-aluminum composite oxide carrier prepared above was ground, 5 ml of 0.004 g / ml platinum nitrate and deionized water were added, and Pt was controlled to account for 1% of the total mass of the catalyst. The mixture was stirred at room temperature (25°C) for 12 hours, and the mixed solution was heated to 80°C until it was boiled dry. The material was dried in a drying oven at 110°C for 12 hours, and then heated to 450°C at 5°C / min and calcined for 2 hours. After the temperature dropped to room temperature, it was taken out to obtain the Pt-based catalyst supported on the cerium-zirconium-aluminum composite oxide carrier.
[0038] Example 2
[0039] Cerium-zirconium-aluminum composite oxide support, Pt-based catalyst and its synthesis process are as follows:
[0040] Weigh a certain amount of cerous nitrate and zirconium nitrate hexahydrate and dissolve them in water to prepare a solution, add a certain amount of Al2O3 to the mixed solution and stir to dissolve. Add urea solution to the mixed solution (the molar ratio of metal ions to urea in the solution is 1:15), use microwave-assisted heating with a power of 210W to 90°C to promote urea hydrolysis, and stir the reaction continuously for 20 to 28 hours. Then centrifuge and wash with water three times, and dry the washed product at 110°C for 2 hours. The dried solid is calcined at 500°C for 2 hours to obtain a cerium-zirconium-aluminum composite oxide carrier.
[0041] The obtained carrier was ground, and platinum nitrate solution and deionized water were added to control Pt to account for 1% of the total mass of the catalyst. The mixture was stirred at room temperature for 12 hours, and then heated to 80°C until it was dried. The material was dried in a drying oven at 110°C for 12 hours, and then heated to 450°C at 5°C / min and calcined for 2 hours. After the temperature dropped to room temperature, the material was taken out to obtain a Pt-based catalyst supported on a cerium-zirconium-aluminum composite oxide carrier.
[0042] The carriers and catalysts with different cerium-zirconium-aluminum contents were prepared, and the catalyst activity was tested. Table 1 shows the catalysts with different cerium-zirconium-aluminum contents and their activity data in the CO catalytic combustion reaction. As shown in Table 1, the mass content of cerium oxide is 5-20%, and the mass content of zirconium oxide is 5-20%, and the obtained catalysts have achieved good catalytic effects. The Pt-based catalyst supported on the cerium-zirconium-aluminum composite oxide carrier with a mass content of 7.5% cerium oxide and a mass content of 7.5% zirconium oxide has the best catalytic activity.
[0043] Table 1 Catalysts with different cerium-zirconium-aluminum contents in the support and their activities in CO catalytic oxidation reaction
[0044]
[0045] Example 3
[0046] The cerium zirconium aluminum composite oxide support and the loaded Pt-based catalyst were prepared by using different molar ratios of metal ions to urea. The preparation method was basically the same as that in Example 1. After calcination, the mass contents of cerium oxide and zirconium oxide in the cerium zirconium aluminum composite oxide support were 7.5% and 7.5%, respectively, and the balance was aluminum oxide. The molar ratios of metal ions to urea in the mixed solution were adjusted to be 1:5, 1:10, 1:15, 1:20, and 1:25, respectively.
[0047] Table 2 shows the Pt-based catalysts supported on the cerium-zirconium-aluminum composite oxide carrier obtained at different metal ion to urea molar ratios and their CO catalytic oxidation activities. From the Pt particle size (CO pulse analysis), H2-TPR minimum reduction peak temperature (α peak position) on different catalysts and their effects on the catalytic activity of CO catalytic combustion reaction, it can be seen that the prepared catalyst Pt particle size is small, and the Pt particle size is ≤2.6 in the range of metal ion to urea molar ratio of 1:5-25. When the metal ion to urea molar ratio is 1:15, the catalyst Pt particle size is about 1.9, which has the highest CO oxidation activity. The changes in properties such as Pt particle size and H2-TPR minimum reduction peak temperature are consistent with the changes in its CO catalytic combustion reaction activity.
[0048] Table 2 Catalysts prepared with different metal ion to urea molar ratios and their activities in CO catalytic oxidation reaction
[0049] Metal ion to urea molar ratio Pt particle size (nm) α peak position (℃) T50(℃) T90(℃) 1∶5 2.5 119 137 191 1∶10 2.3 113 133 177 1∶15 1.9 105 126 162 1∶20 2.2 109 135 171 1∶25 2.6 121 141 199
[0050] Example 4
[0051] The cerium zirconium aluminum composite oxide support and the loaded Pt-based catalyst were prepared using different precursors. The preparation method was basically the same as that in Example 1. In the support preparation process, cerium and zirconium nitrates, acetates and oxalates were used as precursors, respectively, and the molar ratio of metal ions to urea was 1:15. After calcination, the mass contents of cerium oxide and zirconium oxide in the cerium zirconium aluminum composite oxide support were 7.5% and 7.5%, respectively, and the balance was aluminum oxide.
[0052] Table 3 shows the Pt-based catalysts supported on cerium-zirconium-aluminum composite oxide supports prepared from different precursors and their CO catalytic oxidation activities. As shown in Table 3, the cerium-zirconium-aluminum composite oxide supports prepared from different precursors have different properties. In general, nitrate>acetate>oxalate. In addition, the changes in properties such as Pt particle size and H2-TPR minimum reduction peak temperature are consistent with the changes in its CO catalytic combustion reaction activity.
[0053] Table 3 Catalysts prepared from different precursors and their activities in CO catalytic oxidation reaction
[0054] Precursor Pt particle size (nm) α peak position (℃) T50(℃) T90(℃) Nitrates 1.9 105 126 162 Acetate 2.9 116 137 203 Oxalate 3.2 121 143 215
[0055] Example 5
[0056] The durability of the catalyst prepared in Example 1 for the catalytic combustion reaction of CO at 200°C was measured. Figure 2 As shown in the figure, within the 100h test, the activity of the catalyst for CO catalytic combustion remained nearly 100%, and no obvious catalyst activity decay was found, indicating that the catalyst has good durability.
[0057] Comparative Example 1
[0058] The preparation method in Example 1 is adopted, a certain amount of cerous nitrate and zirconium nitrate hexahydrate are weighed and dissolved in water to prepare a solution, and then a certain amount of Al2O3 is weighed and added to the mixed solution and stirred. Urea solution (the molar ratio of metal ions to urea in the solution is 1:15) is added to the mixed solution, heated to 90°C in a water bath to promote urea hydrolysis, stirred and reacted for 24 hours, and then centrifuged and washed 3 times, and the washed product is dried at 110°C for 2 hours. The dried solid is roasted at 500°C for 2 hours to obtain a cerium zirconium aluminum composite oxide carrier, wherein the mass contents of cerium oxide and zirconium oxide are 7.5% and 7.5% respectively, and the remainder is aluminum oxide. The carrier is ground, platinum nitrate solution and deionized water are added, and Pt is controlled to account for 1% of the total mass of the catalyst. It is stirred at room temperature for 12 hours, and then heated to 80°C until it is boiled dry; the material is placed in a drying oven at 110°C and dried for 12 hours, and then heated to 450°C at 5°C / min and roasted for 2 hours. After the reaction is completed, the catalyst is taken out after the temperature drops to room temperature, thereby obtaining a Pt-based catalyst supported on the cerium-zirconium-aluminum composite oxide carrier.
[0059] Comparative Example 2
[0060] The preparation method in Example 1 is adopted, a certain amount of cerous nitrate and zirconium nitrate hexahydrate are weighed and dissolved in water to prepare a solution, and then a certain amount of Al2O3 is weighed and added to the mixed solution. After stirring, an ammonia solution is added to the mixed solution (the molar ratio of metal ions to ammonia water in the solution is 1:15), and a microwave-assisted heating with a power of 210W is used to heat to 90°C to promote the hydrolysis of ammonia water, and the reaction is stirred continuously for 6 hours, and then centrifuged and washed 3 times, and the washed product is dried at 110°C for 2 hours. The dried solid is roasted at a temperature of 500°C for 2 hours to obtain a cerium-zirconium-aluminum composite carrier, in which the mass contents of cerium oxide and zirconium oxide are 7.5% and 7.5% respectively, and the remainder is aluminum oxide. The carrier is ground, platinum nitrate and water are added, and Pt is controlled to account for 1% of the total mass of the catalyst. Stir at room temperature for 12 hours, and the mixed solution is heated to 80°C until it is dried; the material is placed in a drying oven at 110°C and dried for 12 hours; the dry material is heated to 450°C at 5°C / min and roasted for 2 hours. After the reaction is completed, the catalyst is taken out after the temperature drops to room temperature, thereby obtaining a Pt-based catalyst supported on the cerium-zirconium-aluminum composite oxide carrier.
[0061] Comparative Example 3
[0062] The preparation method in Example 1 is adopted, a certain amount of cerous nitrate and zirconium nitrate hexahydrate are weighed and dissolved in water to prepare a solution, and then a certain amount of Al2O3 is weighed and added to the mixed solution. After stirring, (NH4)2CO3 solution is added to the mixed solution (the molar ratio of metal ions to (NH4)2CO3 in the solution is 1:15), and microwave-assisted heating with a power of 210W is used to promote the hydrolysis of (NH4)2CO3 to 90°C, and the reaction is stirred continuously for 6h, and then centrifuged and washed 3 times, and the washed product is dried at 110°C for 2h. The dried solid is roasted at a temperature of 500°C for 2h to obtain a cerium-zirconium-aluminum composite carrier, in which the mass contents of cerium oxide and zirconium oxide are 7.5% and 7.5% respectively, and the balance is aluminum oxide. The carrier was ground, and platinum nitrate and water were added to control the Pt content to be 1% of the total mass of the catalyst. The catalyst was stirred at room temperature for 12 hours, and then boiled at 80°C until dry. The material was placed in a drying oven at 110°C for 12 hours, and then heated to 450°C at 5°C / min and calcined for 2 hours. After the temperature dropped to room temperature, the catalyst was taken out to obtain a Pt-based catalyst supported on a cerium-zirconium-aluminum composite oxide carrier.
[0063] Comparative Example 4
[0064] The preparation method in Example 1 is adopted, a certain amount of cerous nitrate and zirconium nitrate hexahydrate are weighed and dissolved in water to prepare a solution, and then a certain amount of Al2O3 is weighed and added to the mixed solution. After stirring, NH4HCO3 solution is added to the mixed solution (the molar ratio of metal ions to NH4HCO3 in the solution is 1:15), and microwave-assisted heating with a power of 210W is used to 90°C to promote the hydrolysis of NH4HCO3, and the reaction is stirred for 6h, and then centrifuged and washed 3 times, and the washed product is dried at 110°C for 2h. The dried solid is calcined at a temperature of 500°C for 2h to obtain a cerium-zirconium-aluminum composite carrier, in which the mass contents of cerium oxide and zirconium oxide are 7.5% and 7.5% respectively, and the balance is aluminum oxide. The carrier was ground, platinum nitrate and water were added, and Pt was controlled to account for 1% of the total mass of the catalyst. The catalyst was stirred at room temperature for 12 hours, and then boiled at 80°C until dry. The material was placed in a drying oven at 110°C for 12 hours. The dry material was heated to 450°C at 5°C / min and calcined for 2 hours. After the temperature dropped to room temperature, the catalyst was taken out to obtain a Pt-based catalyst supported on a cerium-zirconium-aluminum composite oxide carrier.
[0065] Table 4 is a comparison of the CO catalytic oxidation activity of Pt-based catalysts supported on different cerium-zirconium-aluminum composite oxide supports, including properties such as Pt particle size, H2-TPR minimum reduction peak temperature, etc. The catalyst prepared in Example 1 in the table is recorded as 1Pt / CeZrAl-UW.
[0066] Table 4 Comparison of catalytic performance
[0067] Catalyst type Pt particle size (nm) α peak position (℃) T50(℃) T90(℃) 1Pt / Ce Zr Al-UW 1.9 105 126 162 Comparative Example 1 2.6 114 148 182 Comparative Example 2 3.3 117 172 205 Comparative Example 3 3.1 124 177 202 Comparative Example 4 2.9 122 174 206
[0068] The above description is only a preferred embodiment of the present invention, and does not limit the present invention in any substantial or formal sense. It should be noted that, for a person skilled in the art, several improvements can be made without departing from the purpose of the present invention, and these improvements should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a cerium-zirconium-aluminum composite oxide support by a homogeneous precipitation method, characterized in that: The following steps are involved: (1) mixing a cerium precursor, a zirconium precursor, Al2O3 and urea in a solvent, and heating and aging the resulting mixed solution under microwave action; (2) Centrifuging, washing and drying the slurry obtained in step (1); calcining and crushing the obtained solid to obtain the cerium-zirconium-aluminum composite oxide support.
2. The method for preparing a cerium-zirconium-aluminum composite oxide support by homogeneous precipitation according to claim 1, characterized in that: The mixed solution is heated at a temperature of 85 to 95° C. under the action of microwaves, and the aging time is 20 to 28 hours.
3. The method for preparing a cerium-zirconium-aluminum composite oxide support by homogeneous precipitation according to claim 1, characterized in that: In the mixed solution, the mass fraction of urea is 3% to 15%, and the molar ratio of metal ions to urea is 1:1 to 50.
4. The method for preparing a cerium-zirconium-aluminum composite oxide support by homogeneous precipitation according to claim 1, characterized in that: The Al2O3 is α-alumina, γ-alumina, β-alumina or η-alumina, with a particle size of 20 μm to 400 μm and a pore size of 2 to 50 nm.
5. The method for preparing a cerium-zirconium-aluminum composite oxide support by homogeneous precipitation according to claim 1, characterized in that: The solvent is one or more of water, methanol, ethanol, acetonitrile, hexane and cyclohexane.
6. The method for preparing a cerium-zirconium-aluminum composite oxide support by homogeneous precipitation method according to claim 1, characterized in that: The cerium precursor is selected from one or more of cerium acetate, cerium chloride, cerium acetate, cerium oxalate and cerium nitrate, and the zirconium precursor is selected from one or more of zirconium acetate, zirconium oxalate, zirconium nitrate, zirconium acetate, zirconium carbonate and zirconium oxide.
7. A cerium-zirconium-aluminum composite oxide support prepared according to the method for preparing a cerium-zirconium-aluminum composite oxide support by homogeneous precipitation method according to any one of claims 1 to 6.
8. The cerium-zirconium-aluminum composite oxide support according to claim 7, characterized in that In terms of mass percentage, it contains 70% to 98% Al2O3, 1% to 29% CeO2, and 1% to 29% ZrO2.
9. A cerium / zirconium doped alumina supported Pt-based catalyst, characterized in that: Contains the noble metal Pt and the cerium-zirconium-aluminum composite oxide support according to claim 7.
10. Use of the cerium / zirconium doped alumina supported Pt-based catalyst according to claim 9 in a CO catalytic oxidation reaction.