Composition for removing CO and SO2 as well as preparation method and treatment method thereof

By preparing a composition containing components such as catalyst, magnesium oxide, calcium oxide, etc., the problems of short service life of catalysts and corrosion of toxic substances in the prior art are solved, and the efficient removal of CO and SO2 is achieved, and the characteristics of long life and environmental protection are achieved. .

CN118925712APending Publication Date: 2024-11-12CARBON BEI TECHNOLOGY (BEIJING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411137632.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art catalyst used to remove CO and SO2 in the sintering process has a short service life and there is corrosion of toxic substances on the catalyst, affecting its effectiveness.

Method used

The composition consisting of a catalyst, magnesium oxide, calcium oxide, citric acid, stearic acid, glass fiber, carboxymethyl cellulose and glycerol is prepared by dry mixing, wet mixing, molding, drying and calcining, etc., to form a A catalyst for removing CO and SO2 with a long service life.

Benefits of technology

This composition effectively improves the removal efficiency of CO and SO2, and has a certain NO removal ability, extends the service life of the catalyst, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999861930000131
    Figure BDA0004999861930000131
  • Figure FDA0004999861920000011
    Figure FDA0004999861920000011
Patent Text Reader

Abstract

The invention discloses a composition for removing CO and SO2 as well as a preparation method and a treatment method of the composition. The composition provided by the invention is prepared from the following raw materials: 1200-1700 parts by weight of a catalyst; 100 to 400 parts by weight of magnesium oxide; 100 to 400 parts by weight of calcium oxide; 20-60 parts by weight of citric acid; 10-50 parts by weight of stearic acid; 150 to 280 parts by weight of glass fiber; 10 to 25 parts by weight of carboxymethyl cellulose; and 15 to 35 parts by weight of glycerin; wherein the catalyst comprises a carrier and an active component; the carrier is titanium dioxide and aluminum oxide, and the mass ratio of the titanium dioxide to the aluminum oxide is (7-12): 1; the active components comprise manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide. The composition can be used for effectively removing CO and SO2 in flue gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composition for removing CO and SO2 and a preparation method and a treatment method thereof. Background Art

[0002] As an important step in steel smelting, the sintering process produces a large amount of flue gas. The catalytic oxidation of CO in the sintering flue gas to CO2 can effectively reduce the harm caused by CO to the ecological environment, and the heat generated during its oxidation process can also be further utilized. However, sulfur dioxide, trace heavy metal elements, and a large amount of water vapor in the sintering flue gas have a very obvious toxic effect on the CO oxidation catalyst, which will reduce the service life of the catalyst.

[0003] CN117299110A discloses a MO x -WO3 / SiO2 catalyst, MO x Water-soluble or alcohol-soluble compounds derived from one or more of Ce, Al, Zr, Fe, Mg, V, Zn, Sn, Ca, Li, Na, K, Mo, Co and Mn. MO x :WO3:SiO2=0.1-50:0.1-50:100. The catalyst is used for removing DBT and 4,6-DMDBT.

[0004] CN114602532A discloses a method for preparing a desulfurization and denitration activated coke catalyst, including raw material powder preparation, binder preparation, kneading and molding, pre-curing, carbonization, and activation. The raw material powder includes, by weight: 40 to 60 parts of coal powder, 5 to 12 parts of asphalt powder, 2 to 9 parts of copper oxide powder, 3 to 12 parts of manganese trioxide powder, 1 to 4 parts of cerium oxide powder, 1 to 5 parts of molybdenum carbide powder, 1 to 6 parts of molybdenum nitride powder, 1 to 4 parts of tungsten phosphide powder, and 1 to 3 parts of cobalt dioxide powder. The catalyst is used for desulfurization and denitration.

[0005] CN110893345A discloses a low-temperature SCR denitration catalyst with high catalytic efficiency. The main agent includes manganese composite oxide, chromium composite oxide, cerium dioxide, vanadium pentoxide, titanium dioxide, tungsten composite oxide, copper composite oxide, tin composite oxide, iron composite oxide, cerium vanadium tetraoxide, and ammonia water. The auxiliary agent includes molybdenum oxide, sodium oxide, potassium oxide, sulfur element crystal powder, glacial acetic acid, anhydrous ethanol and magnesium oxide. The catalyst is used for denitration. Summary of the invention

[0006] In view of this, an object of the present invention is to provide a composition for removing CO and SO2, which can effectively remove CO and SO2 from flue gas. Further, the composition has a certain ability to remove NO. Furthermore, the composition has a long service life.

[0007] Another object of the present invention is to provide a method for preparing a composition, which can improve the ability of the composition to remove CO and SO2. Furthermore, the preparation method can improve the service life of the composition.

[0008] Another object of the present invention is to provide a method for treating carbon-sulfur-containing gas, which can effectively remove CO and SO2 from the carbon-sulfur-containing gas.

[0009] The above purpose is achieved through the following technical solutions.

[0010] In one aspect, the present invention provides a composition for removing CO and SO2, wherein the composition is prepared from a raw material comprising the following components:

[0011] Catalyst 1200-1700 parts by weight;

[0012] 100-400 parts by weight of magnesium oxide;

[0013] 100-400 parts by weight of calcium oxide;

[0014] 20-60 parts by weight of citric acid;

[0015] 10-50 parts by weight of stearic acid;

[0016] 150-280 parts by weight of glass fiber;

[0017] 10 to 25 parts by weight of carboxymethyl cellulose; and

[0018] Glycerin 15-35 parts by weight;

[0019] The catalyst comprises a carrier and an active component; the carrier is titanium dioxide and aluminum oxide, and the mass ratio of titanium dioxide to aluminum oxide is (7-12):1;

[0020] The active components include manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide, and the molar ratio of manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide is 2:(0.3-1.5):(0.05-0.4):(0.01-0.1):(0.1-0.5); wherein manganese oxide is calculated as MnO2, cerium oxide is calculated as CeO2, lanthanum oxide is calculated as La2O3, sodium oxide is calculated as Na2O, and tungsten oxide is calculated as WO3.

[0021] According to the composition of the present invention, preferably, the loading amount of the active component is 10 to 20 wt % based on the mass of the carrier.

[0022] In another aspect, the present invention provides a method for preparing the above-mentioned composition, comprising the following steps:

[0023] (1) dry-mixing a catalyst, magnesium oxide, calcium oxide, citric acid, and stearic acid to obtain a dry material;

[0024] (2) mixing the dry material and water to obtain a first mud material;

[0025] (3) Wet-mixing the first mud material, glass fiber and carboxymethyl cellulose to obtain a second mud material;

[0026] (4) adding glycerin to the second mud material to obtain a third mud material;

[0027] (5) forming the third mud material to obtain a honeycomb green body;

[0028] (6) drying the honeycomb green body to obtain a dried honeycomb green body;

[0029] (7) The dried honeycomb green body is calcined to obtain a composite material.

[0030] According to the preparation method of the present invention, preferably, step (6) is dried under the following conditions:

[0031] Dry in the shade for 15 to 30 hours at a temperature of 15 to 35°C and a humidity of 10 to 40%; dry in an oven for 15 to 30 hours at a temperature of 35 to 70°C and a humidity of 45 to 80%; dry in an oven for 30 to 60 hours at a temperature of 70 to 100°C and a humidity of 60 to 90%.

[0032] According to the preparation method of the present invention, preferably, in step (7), the calcination temperature is 400-600° C., and the calcination time is 3-9 hours.

[0033] According to the preparation method of the present invention, preferably, step (5) comprises the following steps:

[0034] The third mud material is pre-extruded, and then vacuum-kneaded to obtain mud columns; the mud columns are extruded and formed to obtain a honeycomb green body.

[0035] The preparation method according to the present invention preferably further comprises the following steps:

[0036] (A) dry-mixing titanium dioxide and aluminum oxide, and then adding manganese acetate, cerium acetate, lanthanum nitrate, sodium nitrate and ammonium metatungstate and dry-mixing to obtain a mixed dry material;

[0037] (B) mixing the mixed dry material with water to obtain a mud material;

[0038] (C) aging the clay material to obtain aged clay material; drying and roasting the aged clay material to obtain a roasted product;

[0039] (D) The calcined product is crushed to obtain a catalyst.

[0040] According to the preparation method of the present invention, preferably, in step (C), the clay is aged for 18 to 30 hours at a temperature of 20 to 40°C and a humidity of 40 to 80%; the aged clay is dried at 120 to 180°C for 13 to 20 hours, and then calcined at 300 to 500°C for 2 to 8 hours.

[0041] In another aspect, the present invention provides a method for treating carbon-sulfur-containing gas, comprising the following steps:

[0042] contacting the carbon-sulfur-containing gas with the above composition in a fixed bed reactor;

[0043] The carbon-sulfur-containing gas contains 700-1500 mg / Nm 3 CO, 10~150mg / Nm 3 SO2.

[0044] According to the treatment method of the present invention, preferably, the air velocity is 2000-18000h -1 The carbon and sulfur-containing gas contacts the composition at a temperature of 180 to 280°C.

[0045] The composition of the present invention can effectively remove CO and SO2 from flue gas. Furthermore, the composition has a certain ability to remove NO. Furthermore, the composition has a long service life. DETAILED DESCRIPTION

[0046] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0047] <Composition>

[0048] The composition of the present invention is prepared from raw materials including the following ingredients: a catalyst, magnesium oxide, calcium oxide, citric acid, stearic acid, glass fiber, carboxymethyl cellulose and glycerol. The raw materials also include water. Preferably, the raw materials are composed of the above ingredients. The solid raw materials in the above raw materials can be used in the form of powder.

[0049] The amount of the catalyst used is 1200 to 1700 parts by weight, preferably 1400 to 1600 parts by weight, and more preferably 1500 to 1600 parts by weight, which helps to improve the removal performance of the composition for CO and NO and maintain a high removal efficiency for SO2.

[0050] The amount of magnesium oxide used is 100 to 400 parts by weight, preferably 150 to 300 parts by weight, and more preferably 200 to 250 parts by weight.

[0051] The amount of calcium oxide used is 100 to 400 parts by weight, preferably 150 to 300 parts by weight, and more preferably 200 to 250 parts by weight.

[0052] Controlling the amount of magnesium oxide and calcium oxide within the above range helps to improve the removal efficiency of the composition for SO2 and ensure the removal performance of the composition for CO and NO.

[0053] The amount of citric acid used is 20 to 60 parts by weight, preferably 30 to 50 parts by weight, and more preferably 40 to 45 parts by weight. This allows the composition of the present invention to have an appropriate pore structure, thereby improving the removal effect of the composition on CO, NO and SO2.

[0054] The amount of stearic acid used is 10 to 50 parts by weight, preferably 15 to 40 parts by weight, and more preferably 20 to 30 parts by weight. The amount of glycerol used is 15 to 35 parts by weight, preferably 20 to 30 parts by weight, and more preferably 24 to 26 parts by weight. This helps to improve the smoothness of the surface of the composition and reduce defects after molding and baking.

[0055] The amount of carboxymethyl cellulose used is 10 to 25 parts by weight, preferably 13 to 20 parts by weight, and more preferably 16 to 18 parts by weight. This allows the composition to have an appropriate pore structure and strength, thereby improving the performance and service life of the composition.

[0056] The amount of glass fiber used is 150 to 280 parts by weight, preferably 170 to 250 parts by weight, and more preferably 200 to 220 parts by weight, which helps to improve the strength of the composition and increase the service life of the composition.

[0057] The catalyst of the present invention comprises a carrier and an active component.

[0058] The carrier includes titanium dioxide and aluminum oxide. The aluminum oxide is preferably γ-type aluminum oxide. The carrier can be composed of titanium dioxide and aluminum oxide. The mass ratio of titanium dioxide to aluminum oxide is (7-12):1; preferably (8-11):1; more preferably (9-10):1.

[0059] The active components include manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide. In certain embodiments, the active components consist of manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide.

[0060] The molar ratio of manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide is 2:(0.3-1.5):(0.05-0.4):(0.01-0.1):(0.1-0.5); preferably 2:(0.8-1.2):(0.1-0.3):(0.03-0.08):(0.15-0.3); more preferably 2:1:0.2:0.05:0.2.

[0061] Based on the carrier, the loading amount of the active component is 10 to 20 wt %, preferably 12 to 18 wt %, and more preferably 15 to 16 wt %.

[0062] The combination of the carrier and the active component can improve the removal efficiency of the composition for CO and increase the service life of the composition.

[0063] <Method for preparing composition>

[0064] The preparation method of the composition of the present invention comprises the following steps: (1) a dry mixing step; (2) a step of obtaining a first clay material; (3) a step of obtaining a second clay material; (4) a step of obtaining a third clay material; (5) a molding step; (6) a drying step; and (7) a calcining step.

[0065] Dry Mixing Steps

[0066] The invention dry-mixes a catalyst, magnesium oxide, calcium oxide, citric acid and stearic acid to obtain a dry material.

[0067] The dry mixing time may be 0.2 to 5 hours, preferably 1 to 3 hours, and more preferably 1 to 2 hours. The dry mixing may be carried out in a kneader.

[0068] Steps to obtain the first mud

[0069] The present invention adds water to dry materials for wet mixing to obtain the first mud material.

[0070] The wet mixing time may be 0.5 to 5 hours, preferably 1 to 3 hours, and more preferably 1 to 2 hours. The wet mixing may be performed in a kneader.

[0071] The moisture content of the first mud material may be 10 to 25 wt %, preferably 15 to 22 wt %, and more preferably 18 to 20 wt %.

[0072] Steps for obtaining the second mud

[0073] The first mud material, glass fiber and carboxymethyl cellulose are wet mixed to obtain the second mud material. Specifically, the glass fiber is added to the first mud material in batches, and the stirring is continued; and then the carboxymethyl cellulose is added to obtain the second mud material.

[0074] The interval between each batch of glass fibers is 0.2 to 1 hour, preferably 0.3 to 0.8 hours, and more preferably 0.5 to 0.7 hours.

[0075] The wet mixing time after adding carboxymethyl cellulose is 0.2 to 1 h, preferably 0.3 to 0.8 h, and more preferably 0.5 to 0.7 h.

[0076] Steps to obtain the third mud

[0077] Glycerol is added to the second mud to obtain a third mud.

[0078] The wet mixing time of the second mud material and glycerin is 0.2 to 1 h, preferably 0.3 to 0.8 h, and more preferably 0.5 to 0.7 h.

[0079] Forming steps

[0080] The third mud material is molded to obtain a honeycomb green body. Specifically, the method comprises the following steps: pre-extruding the third mud material, and then vacuum kneading the mud to obtain mud columns; and extruding the mud columns to obtain a honeycomb green body.

[0081] The number of pre-extrusions can be one or more than one time. Preferably, the number of pre-extrusions is one time.

[0082] The vacuum mud kneading may be performed once or multiple times. Preferably, the vacuum mud kneading is performed twice.

[0083] The mud column can be extruded into shape using a vacuum honeycomb extruder.

[0084] Drying steps

[0085] The honeycomb green body is dried to obtain a dried honeycomb green body. The drying can be performed in a constant temperature and humidity chamber.

[0086] Specifically, drying can be carried out under the following conditions:

[0087] Dry in the shade for 15 to 30 hours, preferably 20 to 24 hours, at a temperature of 15 to 35°C, preferably 20 to 25°C, and a humidity of 10 to 40%, preferably 20 to 30%. Dry for 15 to 30 hours, preferably 20 to 24 hours, at a temperature of 35 to 70°C, preferably 45 to 55°C, and a humidity of 45 to 80%, preferably 50 to 60%. Dry for 30 to 60 hours, preferably 40 to 50 hours, at a temperature of 70 to 100°C, preferably 80 to 90°C, and a humidity of 60 to 90%, preferably 70 to 80%.

[0088] Roasting steps

[0089] The dried honeycomb green body is calcined to obtain a composite material. The calcination can be performed in a muffle furnace.

[0090] The calcination temperature may be 400 to 600°C, preferably 450 to 550°C, and more preferably 500 to 520°C.

[0091] The calcination time may be 3 to 9 hours, preferably 4 to 7 hours, and more preferably 5 to 6 hours.

[0092] In certain embodiments, the method further includes a step of preparing a catalyst, including (A) preparing a mixed dry material; (B) preparing a mud material; (C) obtaining a roasted product; and (D) crushing.

[0093] Steps for preparing dry mix

[0094] Titanium dioxide and aluminum oxide are dry-mixed, and then manganese acetate, cerium acetate, lanthanum nitrate, sodium nitrate and ammonium metatungstate are added and dry-mixed to obtain a mixed dry material. This can be carried out in a kneader.

[0095] The titanium dioxide and aluminum oxide are dry mixed for 0.1 to 2 hours, preferably 0.5 to 1 hour.

[0096] Add manganese acetate, cerium acetate, lanthanum nitrate, sodium nitrate and ammonium metatungstate and dry mix for 0.5 to 3 hours, preferably 1.5 to 2 hours.

[0097] Steps to prepare clay

[0098] The mixed dry materials are mixed with water to obtain mud.

[0099] Wet mixing can be carried out in a kneader. The temperature inside the kneader cavity can be 40-60°C, preferably 45-50°C.

[0100] The wet mixing time may be 0.5 to 4 hours, preferably 1 to 3 hours, and more preferably 1.5 to 2 hours.

[0101] The moisture content of the mud can be 15 to 35 wt %, preferably 20 to 30 wt %, and more preferably 25 to 28 wt %.

[0102] Steps for obtaining roasted product

[0103] The clay material is aged to obtain aged clay material; the aged clay material is dried and roasted to obtain a roasted product.

[0104] The slurry can be placed in a sealed box for aging. The aging can be carried out at a temperature of 20 to 40°C, preferably 25 to 30°C, and a humidity of 40 to 80%, preferably 50 to 70%. The aging time can be 18 to 30 hours, preferably 20 to 25 hours. The aging can be carried out in a constant temperature and humidity box.

[0105] The drying temperature may be 120 to 180° C., preferably 140 to 150° C. The drying time may be 13 to 20 hours, preferably 17 to 20 hours. The drying may be carried out in an oven.

[0106] The calcination temperature may be 300 to 500° C., preferably 350 to 450° C., and more preferably 400 to 450° C. The calcination time may be 2 to 8 hours, preferably 3 to 7 hours, and more preferably 4 to 6 hours. The calcination may be carried out in a muffle furnace.

[0107] Broken Steps

[0108] The calcined product is crushed to obtain a catalyst. The calcined product can be crushed by a crusher. The particle size of the catalyst is about 200 mesh.

[0109] <Treatment Method of Carbon and Sulfur-Containing Gas>

[0110] The treatment method of the present invention comprises the following steps: contacting the carbon-sulfur-containing gas with the above composition in a fixed bed reactor.

[0111] The carbon-sulfur-containing gas contains CO and SO2. The carbon-sulfur-containing gas may also contain NO, O2, CO2 and water vapor.

[0112] The concentration of CO is 700~1500mg / Nm 3 ; preferably 800~1300mg / Nm 3 More preferably, 1000 to 1100 mg / Nm 3 .

[0113] The concentration of SO2 is 10~150mg / Nm 3 ; preferably 20 to 120 mg / Nm 3 In some embodiments, the concentration of SO2 is 25 to 30 mg / Nm 3 In other embodiments, the concentration of SO2 is 100-110 mg / Nm 3 .

[0114] The concentration of NO is 300~900mg / Nm 3 ; preferably 400~800mg / Nm 3 More preferably, 600 to 700 mg / Nm 3 .

[0115] The concentration of CO2 is 8 to 25 vol%, preferably 10 to 20 vol%, and more preferably 15 to 18 vol%.

[0116] The concentration of O2 is 8 to 25 vol%, preferably 10 to 20 vol%, and more preferably 16 to 18 vol%.

[0117] The concentration of water vapor is 8 to 25 vol%, preferably 10 to 20 vol%, and more preferably 16 to 18 vol%.

[0118] The airspeed can be 2000~18000h -1 ; preferably 3000~15000h -1 ; More preferably 4000 to 5000 hours -1 .

[0119] The carbon-sulfur-containing gas may be contacted with the composition at a temperature of 180 to 280°C, preferably 200 to 250°C.

[0120] Preparation Example 1

[0121] After dry-mixing titanium dioxide powder and gamma-alumina powder in a kneader for 0.5 h, manganese acetate, cerium acetate, lanthanum nitrate, sodium nitrate and ammonium metatungstate were put into the kneader and dry-mixed for 1.5 h to obtain a mixed dry material.

[0122] Water was added to the mixed dry materials, the temperature inside the kneading machine cavity was maintained at 50°C, and wet mixing was performed for 1.5 hours to obtain a mud material (water content was 25wt%).

[0123] The clay material was placed in a sealed box and then aged for 24 hours in a constant temperature and humidity box at a temperature of 30°C and a humidity of 60%. The aged clay material was dried in an oven at 150°C for 17 hours and then calcined in a muffle furnace at 400°C for 5 hours to obtain a calcined product.

[0124] The calcined product was crushed into powder of about 200 meshes by a crusher to obtain a catalyst.

[0125] The catalyst uses titanium dioxide and aluminum oxide as carriers, and uses manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide as active components. The mass ratio of titanium dioxide to aluminum oxide is 9:1. The molar ratio of manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide is 2:1:0.2:0.05:0.2. Based on the carrier, the loading amount of the active components is 15wt%. Manganese oxide is calculated as MnO2, cerium oxide is calculated as CeO2, lanthanum oxide is calculated as La2O3, sodium oxide is calculated as Na2O, and tungsten oxide is calculated as WO3.

[0126] Example 1

[0127] 1200 parts by weight of the catalyst obtained by the method of Preparation Example 1, 400 parts by weight of magnesium oxide powder, 400 parts by weight of calcium oxide powder, 40 parts by weight of citric acid powder, and 30 parts by weight of stearic acid powder were placed in a kneader and dry mixed for 1 hour to obtain a dry material.

[0128] Water was added to the dry material and mixed for 1 hour to obtain the first mud material (with a water content of 18 wt%).

[0129] 200 parts by weight of glass fiber with a length of 3 mm were added to the first mud in batches, each time with an interval of 0.5 h and continuous stirring; then 16 parts by weight of carboxymethyl cellulose were added and wet mixed for 0.5 h to obtain the second mud.

[0130] 24 parts by weight of glycerin was added to the second mud material and wet-mixed for 0.5 hours to obtain a third mud material. The third mud material was pre-extruded once and vacuum-mixed twice to obtain a mud column.

[0131] The mud column is extruded and formed by a vacuum honeycomb extruder to obtain a honeycomb green body.

[0132] The honeycomb green body was dried in a constant temperature and humidity chamber at a temperature of 25°C and a humidity of 30% for 24 hours; dried at a temperature of 50°C and a humidity of 60% for 24 hours; dried at a temperature of 90°C and a humidity of 70% for 48 hours to obtain a dry honeycomb green body.

[0133] The dried honeycomb green body was calcined in a muffle furnace at 500° C. for 6 hours to obtain a composite.

[0134] Example 2

[0135] The same procedures as in Example 1 were followed except that the amount of the catalyst was 1400 parts by weight, the amount of calcium oxide was 300 parts by weight, and the amount of magnesium oxide was 300 parts by weight.

[0136] Example 3

[0137] The same procedures as in Example 1 were followed except that the amount of the catalyst was 1600 parts by weight, the amount of calcium oxide was 200 parts by weight, and the amount of magnesium oxide was 200 parts by weight.

[0138] Comparative Example 1

[0139] The same procedures as in Example 1 were followed except that the amount of the catalyst was 1000 parts by weight, the amount of calcium oxide was 500 parts by weight, and the amount of magnesium oxide was 500 parts by weight.

[0140] Experimental example

[0141] The removal performance of the composition for CO, SO2 and NO was tested using the following method:

[0142] The composition was formed into a module unit of 150mm×150mm×300mm. The module unit was placed in a fixed bed reactor and tested at a temperature of 200-250°C for 168 hours. The inlet flue gas composition and air velocity are shown in Table 1. The composition of the flue gas was tested using an industrial flue gas analyzer produced by MRU, Germany. The CO removal efficiency was calculated using the following formula:

[0143] CO removal efficiency = (C CO入口 -C CO出口 ) / C CO入口 ×100wt%

[0144] Among them, C CO入口 Indicates the CO content in the flue gas at the reactor inlet, in mg / Nm 3 ;

[0145] Among them, C CO出口 Indicates the CO content in the flue gas at the reactor outlet, in mg / Nm 3 .

[0146] The properties of the composition are shown in Table 2.

[0147] Table 1

[0148] project airspeed Oxygen concentration CO concentration <![CDATA[SO2 concentration]]> NO concentration <![CDATA[CO2 concentration]]> Moisture content Condition 1 <![CDATA[8000h -1 ]]> 16vol% <![CDATA[1000mg / Nm 3 ]]> <![CDATA[25mg / Nm 3 ]]> <![CDATA[600mg / Nm 3 ]]> 15vol% 16vol% Condition 2 15000h-1 16vol% <![CDATA[1000mg / Nm 3 ]]> <![CDATA[25mg / Nm 3 ]]> <![CDATA[600mg / Nm 3 ]]> 15vol% 16vol% Condition three 4000h-1 16vol% <![CDATA[1000mg / Nm 3 ]]> <![CDATA[100mg / Nm 3 ]]> <![CDATA[600mg / Nm 3 ]]> 15vol% 16vol%

[0149] Table 2

[0150]

[0151] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A composition for removing CO and SO2, characterized in that: The composition is prepared from raw materials including the following ingredients: The catalyst comprises a carrier and an active component; the carrier is titanium dioxide and aluminum oxide, and the mass ratio of titanium dioxide to aluminum oxide is (7-12):1; The active components include manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide, and the molar ratio of manganese oxide, cerium oxide, lanthanum oxide, sodium oxide and tungsten oxide is 2:(0.3-1.5):(0.05-0.4):(0.01-0.1):(0.1-0.5); wherein manganese oxide is calculated as MnO2, cerium oxide is calculated as CeO2, lanthanum oxide is calculated as La2O3, sodium oxide is calculated as Na2O, and tungsten oxide is calculated as WO3.

2. The composition according to claim 1, characterized in that Based on the mass of the carrier, the loading amount of the active component is 10-20 wt%.

3. The method for preparing the composition according to any one of claims 1 to 2, characterized in that: The steps include: (1) dry-mixing a catalyst, magnesium oxide, calcium oxide, citric acid, and stearic acid to obtain a dry material; (2) mixing the dry material and water to obtain the first mud material; (3) wet-mixing the first mud material, glass fiber, and carboxymethyl cellulose to obtain a second mud material; (4) adding glycerin to the second mud material to obtain a third mud material; (5) forming the third mud material to obtain a honeycomb green body; (6) drying the honeycomb green body to obtain a dried honeycomb green body; (7) The dried honeycomb green body is calcined to obtain a composite.

4. The preparation method according to claim 3, characterized in that Step (6) is dried under the following conditions: Dry in the shade for 15 to 30 hours at a temperature of 15 to 35°C and a humidity of 10 to 40%; dry in an oven for 15 to 30 hours at a temperature of 35 to 70°C and a humidity of 45 to 80%; and dry in an oven for 30 to 60 hours at a temperature of 70 to 100°C and a humidity of 60 to 90%.

5. The preparation method according to claim 3, characterized in that In step (7), the calcination temperature is 400-600° C., and the calcination time is 3-9 hours.

6. The preparation method according to claim 3, characterized in that Step (5) includes the following steps: The third mud material is pre-extruded, and then vacuum-kneaded to obtain mud columns; the mud columns are extruded and formed to obtain a honeycomb green body.

7. The preparation method according to claim 3, characterized in that The following steps are also included: (A) dry-mixing titanium dioxide and aluminum oxide, and then adding manganese acetate, cerium acetate, lanthanum nitrate, sodium nitrate and ammonium metatungstate and dry-mixing to obtain a mixed dry material; (B) mixing the dry material with water to obtain a mud material; (C) aging the clay material to obtain aged clay material; drying and roasting the aged clay material to obtain a roasted product; (D) The calcined product is crushed to obtain a catalyst.

8. The preparation method according to claim 7, characterized in that In step (C), the clay is aged at a temperature of 20-40° C. and a humidity of 40-80% for 18-30 hours; the aged clay is dried at 120-180° C. for 13-20 hours, and then calcined at 300-500° C. for 2-8 hours.

9. A method for treating carbon-sulfur-containing gas, characterized in that: The steps include: contacting a carbon and sulfur-containing gas with the composition according to any one of claims 1 to 2 in a fixed bed reactor; The carbon and sulfur-containing gas contains 700-1500 mg / Nm 3 CO, 10-150 mg / Nm 3 SO2.

10. The processing method according to claim 9, characterized in that: Airspeed is 2000~18000h -1 The carbon and sulfur-containing gas contacts the composition at a temperature of 180 to 280°C.