High-stability dehydrogenation catalyst and preparation method thereof
By using alumina-carb alkane dehydrogenation catalyst with a combination of chromium-carbium oxide and a combination of precursors in the low-carbon alkane dehydrogenation catalyst, the problem of poor catalyst stability is solved, high stability and activity are improved, and the service life of the catalyst is extended .
Patent Information
- Application Number
- CN202411126648.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
AI Technical Summary
The existing low-carbon alkane dehydrogenation catalysts have poor stability, resulting in a short service life of domestic catalysts and cannot be compared with Clariant's products.
Alumina-carried chromium-carried dehydrogenation catalyst is prepared by precipitation and impregnation of soluble chromium salts, aluminum salts, barium salts, lanthanum salts and other salts. Combined with various precursors of Cr2O3 and CrO3, barium oxide and cerium are added. , copper, nickel and other components optimize the structure and activity of the catalyst and improve its stability.
It significantly improves the stability and activity of the catalyst, and its initial activity is better than that of domestic catalysts, and its activity decreases less after aging, and is even better than some foreign catalysts, extending the service life of the catalyst.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to a highly stable dehydrogenation catalyst and its preparation method, and more specifically, to a chromium-supported alumina dehydrogenation catalyst and a method for preparing such a catalyst. Background Technology
[0002] The dehydrogenation (ODH) of low-carbon alkanes, represented by propane, to produce propylene can convert low-value alkanes into high-value olefins, and has received widespread attention in my country's petrochemical industry in recent years. After decades of development, the industrial application of low-carbon alkane catalytic dehydrogenation technology has become increasingly mature. Five processes have been industrialized or are technologically mature: UOP's (Universal Oil Products) Oleflex process, ABB Lummus's Catofin process, Uhde's STAR process, Linde / BASF's PDH process, and Snamprogetti / Yarsintez's FBD process. Among these five methods, the Oleflex and Catofin processes are the most widely used in industrial applications.
[0003] Compared to the Oleflex process which uses a Pt catalyst, the Catofin process uses a chromium-based non-precious metal catalyst, which has lower feed requirements, no catalyst loss, and lower operating pressure (0.05 MPa) and temperature (540–640 °C). To promote continuous operation, parallel reactors operate in staggered, timed cycles. Each complete cycle typically consists of a dehydrogenation section, a regeneration section, a reduction section, and a purification section. Furthermore, to provide more favorable equilibrium conditions, the reactors are typically operated at sub-atmospheric pressure during the dehydrogenation cycle. The regeneration cycle, operating in the range of 500 °C to 700 °C, provides heat for subsequent dehydrogenation reactions. Due to such high temperatures, the effective lifetime of the dehydrogenation catalyst is typically short. Therefore, research on the high stability of chromium-based dehydrogenation catalysts is urgently needed.
[0004] Among them, Clariant's chromium-based dehydrogenation catalysts have the best stability and have been monopolized globally to date. Domestic scholars have also studied them for a long time, but their research has only been limited to literature reports, with few successful applications in industrial plants. Most problems arise from the stability of chromium-based dehydrogenation catalysts.
[0005] Chinese patent CN107398267A reports a method for preparing a catalyst by using aluminum compounds as raw materials, adding hollow hexagonal Cr(OH)3 microspheres to form a support, and then loading a co-catalyst component onto the support via an impregnation method. The evaluation shows that when approximately 10g of the catalyst is loaded into the aforementioned reactor, reacted at atmospheric pressure, with a mass hourly space velocity (WHSV) of 1.5 / h and a reaction temperature of 580℃, the resulting catalyst exhibits a conversion rate of approximately 50% and a selectivity of approximately 90%, but no stability studies were conducted.
[0006] Chinese patent CN110560038B reports a catalyst for propane dehydrogenation composed of 3-30 parts of Cr and / or W or their oxides, 0-5 parts of at least one element selected from Group VB of the periodic table or its oxide, and 69-96 parts of alumina support. Utilizing W from Group VIB, which has multiple variable valence states, Cr and / or W together can effectively alter the acid-base distribution and surface properties of the catalyst, resulting in higher catalyst activity. The catalyst obtained under these conditions achieved a propane conversion of 45% and a propylene selectivity of 90.1% in the propane dehydrogenation reaction; however, stability studies were not conducted.
[0007] According to incomplete statistics, the lifespan of domestically produced catalysts is generally only about three months, far less than Clariant's three-year lifespan. Some sources indicate that Clariant's first chromium-based dehydrogenation catalyst also had a lifespan of only about three months. Therefore, the level of domestically produced catalysts is basically on par with Clariant's first-generation catalysts developed decades ago, and no breakthrough has been achieved to date. Summary of the Invention
[0008] Given the poor stability of existing low-carbon alkane dehydrogenation catalysts, one of the technical problems this invention aims to solve is to provide a highly stable low-carbon alkane dehydrogenation catalyst. A second technical problem this invention aims to solve is to provide a catalyst preparation method corresponding to solving one of the technical problems.
[0009] To solve one of the above-mentioned technical problems, the present invention adopts the following technical solution: a highly stable low-carbon alkane dehydrogenation catalyst, the composition of which, by mass, is: Cr2O3 13~25%, Na2O 0.1~1.2%, K2O 0.3~1.8%, La2O3 0.5~1.8%, BaO 1.2~3.4%, CeO2 0.2~1.0%, ZrO2 0.5~4.5%, Mg 0.5~3.6%, Ni 0.5~2.0%, CuO 3~10%, with the remainder being Al2O3. 3。
[0010] In the above technical solution, the precursors of Cr2O3 are soluble chromium salts, Cr2O3 powder, and CrO3. The precursors of the alumina support are soluble aluminum salts and microporous boehmite. The remaining components are their respective salts.
[0011] To solve the second technical problem mentioned above, the present invention adopts the following technical solution: a highly stable dehydrogenation catalyst and its preparation method, comprising the following steps: (1) Dissolve soluble aluminum salt, soluble chromium salt, soluble copper salt, soluble barium salt, and soluble lanthanum salt in water, then add ammonia or ammonium carbonate solution dropwise. After the precipitation is complete, filter and wash until neutral, then dry at 120℃ for 2 hours, calcine at 760℃ for 24-36 hours, cool and crush to 120 mesh to obtain component A; (2) After mixing small-pore boehmite, Cr2O3 and component A, add aqueous solutions of soluble sodium salt and soluble potassium salt and nitric acid solution, knead and shape, then dry at 120℃ for 2h and calcine at 650℃ for 24h~36h to obtain component B. (3) Prepare a mixed solution of soluble cerium salt, soluble zirconium salt, soluble magnesium salt and soluble nickel salt, impregnate component B with an equal volume of the solution, and then dry at 120℃ for 2h and calcine at 650℃ for 24h~36h to obtain component C; (4) Dissolve CrO3 in water, impregnate component C with an equal volume, dry at 120℃ for 2h, then impregnate with oxidized acid solution with an equal volume, dry at 120℃ for 2h, and calcine at 650℃ for 24h~36h to obtain a highly stable dehydrogenation catalyst.
[0012] Furthermore, the proportions of the two aluminum sources used in step (1) (soluble aluminum salt) and step (2) (small-pore boehmite) to the total Al2O3 of the catalyst, based on the mass of Al2O3, are 30~70:70~30 respectively.
[0013] Furthermore, the proportions of the three chromium sources used in step (1) (soluble chromium salt), step (2) (Cr2O3), and step (4) (CrO3) in the total Cr2O3 of the catalyst, based on the mass of Cr2O3, are 30~65:30~45:5~25, respectively.
[0014] Furthermore, in step (1), the soluble aluminum salt is aluminum chloride or aluminum nitrate, the soluble chromium salt is one of chromium nitrate, chromium acetate or chromium chloride, the soluble copper salt is copper chloride or copper nitrate, the soluble barium salt is barium chloride or barium nitrate, and the soluble lanthanum salt is lanthanum nitrate.
[0015] Furthermore, the soluble sodium salt in step (2) is sodium nitrate or sodium hydroxide, and the soluble potassium salt is potassium nitrate or potassium fluoride.
[0016] In further detail, the soluble cerium salt in step (3) is cerium chloride or cerium nitrate, the soluble zirconium salt is zirconium nitrate, the soluble magnesium salt is magnesium nitrate or magnesium chloride, and the soluble nickel salt is nickel nitrate.
[0017] Furthermore, the concentration of the ascorbic acid solution in step (4) is 200~300g / L.
[0018] Compared with chromium-based catalysts prepared by existing technologies, the dehydrogenation catalyst prepared by the method provided in this invention has the following advantages: (1) Chromium is produced using three precursors, with soluble chromium salts providing Cr. 3+ The ions transform into Cr2O3, and Cr2O3 powder can ensure a high content of α-Cr2O3. CrO3 provides Cr 6+ The transformation of ions into Cr2O3, in addition, the combination of co-precipitation preparation of Cr2O3, Cr2O3 powder preparation and impregnation method to prepare Cr2O3 ensures a high Cr loading while providing abundant active Cr species. The stepwise addition of different Cr precursors also reduces the binding of Cr with the alumina support.
[0019] (2) The addition of barium oxide has multiple functions: In the preparation of dehydrogenation catalyst, the barium oxide precursor is mixed into the support preparation and then a chromium source is added, which can promote the dispersion of chromium; the interaction between barium oxide and the support reduces the binding of Cr with the alumina support and the electronic effect of barium oxide, which can promote the Cr with cracking and carbon deposition function. 6+ The deep reduction to Cr with dehydrogenation activity 3+ Barium oxide releases heat when it reacts with water during regeneration and also releases heat when it is reduced, providing an additional uniform heat source for the dehydrogenation reaction.
[0020] (3) The addition of soluble cerium salt, soluble copper salt and soluble nickel salt promotes the redox process of Cr 6+ With Cr 3+ The interconversion of these substances, along with the exothermic redox reaction that occurs during redox processes, provides an additional uniform heat source for the dehydrogenation reaction.
[0021] (4) Soluble sodium and potassium salts are added to the mixture of small-pore pseudoboehmite, Cr2O3 and component A, so that all Cr in the mixture is Cr. 3+ Instead of adding Cr to the CrO3 solution 6+ In this way, the interaction between K and Cr is avoided. 6+ The formation of potassium chromate or potassium dichromate, which are difficult to decompose, reduces the effective active Cr species and also loses the ability of sodium and potassium to regulate the acidity of the carrier.
[0022] (5) Soluble zirconium salt, soluble magnesium salt and soluble lanthanum salt can adjust the structure of the supported alumina, improve the hydrothermal stability of the catalyst, reduce the combination of Cr and alumina, and indirectly reduce the deactivation of active Cr by forming chromium aluminum spinel with alumina.
[0023] (6) The above preparation conditions can significantly reduce the interaction between Cr and the alumina support. Adding hydrazine hydrate solution further complexes Cr, further reducing the interaction between Cr and the alumina support, and simultaneously further enhances the interaction between Cr and the alumina support. 6+ It is relatively easy to reduce to Cr, which has dehydrogenation activity. 3+ . Detailed Implementation
[0024] The following provides a detailed description of the embodiments of the present invention: These embodiments are implemented based on the technical solution of the present invention, and provide detailed implementation methods and processes. However, the scope of protection of the present invention is not limited to the following embodiments. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions. Example 1
[0025] The dehydrogenation catalyst Cat-1 was prepared with the following composition by mass: 13% Cr2O3, 0.1% Na2O, 1.1% K2O, 0.5% La2O3, 1.4% BaO, 0.2% CeO2, 1.5% ZrO2, 3.6% Mg, 1.5% Ni, 10% CuO, and the remainder Al2O3. Based on the above composition, the required precursor was weighed and prepared according to the following steps: (1) Dissolve one of aluminum chloride or aluminum nitrate, chromium nitrate, chromium acetate or chromium chloride, copper chloride or copper nitrate, barium chloride or barium nitrate, or lanthanum nitrate in water, then add ammonia or ammonium carbonate solution. After precipitation is complete, filter and wash until neutral, then dry at 120°C for 2 hours, calcine at 760°C for 24 hours, cool and crush to 120 mesh to obtain component A; (2) After mixing small-pore boehmite, Cr2O3 powder and component A, add sodium nitrate or sodium hydroxide and potassium nitrate or potassium fluoride aqueous solution and nitric acid solution, knead and shape, then dry at 120℃ for 2h and calcine at 650℃ for 30h to obtain component B. (3) Prepare a mixed solution of cerium chloride or cerium nitrate, zirconium nitrate, magnesium nitrate or magnesium chloride, and nickel nitrate, and impregnate component B with an equal volume of the solution. Then dry at 120°C for 2 hours and calcine at 650°C for 28 hours to obtain component C. (4) Dissolve CrO3 in water, impregnate component C with an equal volume, dry at 120°C for 2 hours, and then impregnate with hydrazine hydrate solution with an equal volume of 200 g / L. Then dry at 120°C for 2 hours and calcine at 650°C for 36 hours to obtain a highly stable dehydrogenation catalyst.
[0026] The proportions of the two aluminum sources used in step (1) (soluble aluminum salt) and step (2) (small-pore pseudoboehmite) to the total Al2O3 of the catalyst, based on the mass of Al2O3, are 40:60.
[0027] The proportions of the three chromium sources used in step (1), step (2), and step (4), based on the mass of Cr2O3, to the total Cr2O3 in the catalyst are 30: 45: 25. Example 2
[0028] The dehydrogenation catalyst Cat-2 was prepared with the following composition by mass: 18% Cr2O3, 0.5% Na2O, 0.8% K2O, 1.8% La2O3, 1.3% BaO, 0.4% CeO2, 4.5% ZrO2, 0.6% Mg, 0.5% Ni, 8% CuO, and the remainder Al2O3. Based on the above composition, the required precursor was weighed and prepared according to the following steps: (1) Dissolve one of aluminum chloride or aluminum nitrate, chromium nitrate, chromium acetate or chromium chloride, copper chloride or copper nitrate, barium chloride or barium nitrate, or lanthanum nitrate in water, then add ammonia or ammonium carbonate solution. After the precipitation is complete, filter and wash until neutral, then dry at 120°C for 2 hours and calcine at 760°C for 26 hours. After cooling, crush to 120 mesh to obtain component A. (2) After mixing small-pore boehmite, Cr2O3 powder and component A, add sodium nitrate or sodium hydroxide and potassium nitrate or potassium fluoride aqueous solution and nitric acid solution, knead and shape, then dry at 120℃ for 2h and calcine at 650℃ for 28h to obtain component B. (3) Prepare a mixed solution of cerium chloride or cerium nitrate, zirconium nitrate, magnesium nitrate or magnesium chloride, and nickel nitrate, and impregnate component B with an equal volume of the solution. Then dry at 120°C for 2 hours and calcine at 650°C for 32 hours to obtain component C. (4) Dissolve CrO3 in water, impregnate component C with an equal volume, dry at 120°C for 2 hours, and then impregnate with hydrazine hydrate solution with an equal volume of 300 g / L. Then dry at 120°C for 2 hours and calcine at 650°C for 24 hours to obtain a highly stable dehydrogenation catalyst.
[0029] The proportions of the two aluminum sources used in step (1) (soluble aluminum salt) and step (2) (small-pore pseudoboehmite) to the total Al2O3 of the catalyst, based on the mass of Al2O3, are 70:30.
[0030] The proportions of the three chromium sources used in step (1) (soluble chromium salt), step (2) (Cr2O3), and step (4) (CrO3) in the total Cr2O3 of the catalyst, based on the mass of Cr2O3, are 45: 45:10, respectively. Example 3
[0031] The dehydrogenation catalyst Cat-3 was prepared with the following composition by mass: 25% Cr2O3, 1.2% Na2O, 1.8% K2O, 0.9% La2O3, 3.4% BaO, 0.5% CeO2, 2.3% ZrO2, 0.5% Mg, 1.0% Ni, 3% CuO, and the remainder Al2O3. Based on the above composition, the required precursor was weighed and prepared according to the following steps: (1) Dissolve one of aluminum chloride or aluminum nitrate, chromium nitrate, chromium acetate or chromium chloride, copper chloride or copper nitrate, barium chloride or barium nitrate, or lanthanum nitrate in water, then add ammonia or ammonium carbonate solution. After the precipitation is complete, filter and wash until neutral, then dry at 120°C for 2 hours, calcine at 760°C for 36 hours, cool and crush to 120 mesh to obtain component A. (2) After mixing small-pore boehmite, Cr2O3 powder and component A, add sodium nitrate or sodium hydroxide and potassium nitrate or potassium fluoride aqueous solution and nitric acid solution, knead and shape, then dry at 120℃ for 2h and calcine at 650℃ for 36h to obtain component B. (3) Prepare a mixed solution of cerium chloride or cerium nitrate, zirconium nitrate, magnesium nitrate or magnesium chloride, and nickel nitrate, and impregnate component B with an equal volume of the solution. Then dry at 120°C for 2 hours and calcine at 650°C for 24 hours to obtain component C. (4) Dissolve CrO3 in water, impregnate component C with an equal volume, dry at 120°C for 2 hours, and then impregnate with hydrazine hydrate solution with an equal volume of 230 g / L. Then dry at 120°C for 2 hours and calcine at 650°C for 24 hours to obtain a highly stable dehydrogenation catalyst.
[0032] The proportions of the two aluminum sources used in step (1) (soluble aluminum salt) and step (2) (small-pore pseudoboehmite) in the total Al2O3 of the catalyst, based on the mass of Al2O3, are 50:50.
[0033] The proportions of the three chromium sources used in step (1), step (2), and step (4), based on the mass of Cr2O3, to the total Cr2O3 in the catalyst are 65:30:5. Example 4
[0034] The dehydrogenation catalyst Cat-4 was prepared with the following composition by mass: 15% Cr2O3, 0.8% Na2O, 0.3% K2O, 1.1% La2O3, 1.2% BaO, 1.0% CeO2, 0.5% ZrO2, 1.7% Mg, 2.0% Ni, 5% CuO, and the remainder Al2O3. Based on the above composition, the required precursor was weighed and prepared according to the following steps: (1) Dissolve one of aluminum chloride or aluminum nitrate, chromium nitrate, chromium acetate or chromium chloride, copper chloride or copper nitrate, barium chloride or barium nitrate, or lanthanum nitrate in water, then add ammonia or ammonium carbonate solution. After the precipitation is complete, filter and wash until neutral, then dry at 120°C for 2 hours, calcine at 760°C for 36 hours, cool and crush to 120 mesh to obtain component A. (2) After mixing small-pore boehmite, Cr2O3 powder and component A, add sodium nitrate or sodium hydroxide and potassium nitrate or potassium fluoride aqueous solution and nitric acid solution, knead and shape, then dry at 120℃ for 2h and calcine at 650℃ for 24h to obtain component B. (3) Prepare a mixed solution of cerium chloride or cerium nitrate, zirconium nitrate, magnesium nitrate or magnesium chloride, and nickel nitrate, and impregnate component B with an equal volume of the solution. Then dry at 120°C for 2 hours and calcine at 650°C for 36 hours to obtain component C. (4) Dissolve CrO3 in water, impregnate component C with an equal volume, dry at 120°C for 2 hours, and then impregnate with hydrazine hydrate solution with an equal volume of 280 g / L. Then dry at 120°C for 2 hours and calcine at 650°C for 26 hours to obtain a highly stable dehydrogenation catalyst.
[0035] The proportions of the two aluminum sources used in step (1) (soluble aluminum salt) and step (2) (small-pore pseudoboehmite) to the total Al2O3 of the catalyst, based on the mass of Al2O3, are 30:70.
[0036] The proportions of the three chromium sources used in step (1), step (2), and step (4), based on the mass of Cr2O3, to the total Cr2O3 in the catalyst are 55:40:5.
[0037] Comparative Example 1 Cat-A, a domestically produced catalyst.
[0038] Comparative Example 2 Cat-B, a foreign catalyst.
[0039] The evaluation conditions for the catalytic dehydrogenation of isobutane are: volume hourly space velocity 300 h⁻¹ -1The reaction temperature was 580℃, and the average conversion and selectivity were measured within the first 10 minutes at atmospheric pressure. Each catalyst was evaluated for isobutane catalytic dehydrogenation after catalyst reduction.
[0040] The initial activity is the activity of the calcined catalyst without any treatment for the catalytic dehydrogenation of isobutane.
[0041] To simulate industrial conditions, two different aging conditions were established, as follows: The aging activity test involved aging the calcined catalyst in a mixed atmosphere of steam and air (20% steam - 80% air) at a space velocity of 2000 h⁻¹. -1 GHSV, aging temperature 700℃, aging time 2h.
[0042] The second aging activity was achieved by aging the calcined catalyst in a mixed atmosphere of steam and air (20% steam - 80% air) at a space velocity of 2000 h⁻¹. -1 GHSV, aging temperature is 870℃, aging time is 2h.
[0043] The activity of the aged catalyst in the catalytic dehydrogenation of isobutane was evaluated. Examples 1-4 and Comparative Examples 1-2 were evaluated, and the results are shown in Table 1.
[0044] Table 1. Activity evaluation of catalysts
[0045] As can be seen from the above examples and comparative examples, the initial activity data of the dehydrogenation catalyst prepared according to this patent is significantly better than that of domestically produced dehydrogenation catalysts, and the activity data of some examples are comparable to or better than those of foreign dehydrogenation catalysts. After two aging activity evaluations, the activity data of the dehydrogenation catalyst prepared according to this patent and the foreign dehydrogenation catalysts did not decrease significantly, while the activity data of the domestically produced dehydrogenation catalyst decreased significantly.
Claims
1. A highly stable dehydrogenation catalyst and a preparation method thereof, It is characterized in that The dehydrogenation catalyst has a composition by mass of: Cr 2 O 3 is 13~25%, Na 2 O is 0.1~1.2%, K 2 O is 0.3~1.8%, La 2 O 3 0.5~1.8%, BaO 1.2~3.4%, CeO 2 0.2~1.0%, ZrO 2 0.5~4.5%, Mg 0.5~3.6%, Ni 0.5~2.0%, CuO 3~10%, and the rest Al 2 O 3 ; The preparation method of the dehydrogenation catalyst is: (1) Dissolve soluble aluminum salt, soluble chromium salt, soluble copper salt, soluble barium salt and soluble lanthanum salt in water, then add ammonia water or ammonium carbonate solution, filter and wash until neutral after precipitation is complete, then dry at 120°C for 2h, roast at 760°C for 24h~36h, and crush to 120 mesh after cooling to obtain component A; (2) Small pore pseudo-boehmite, Cr 2 O 3 After the powder is mixed with component A, an aqueous solution of a soluble sodium salt and a soluble potassium salt and a nitric acid solution are added, kneaded and formed, and then dried at 120°C for 2h and roasted at 650°C for 24h~36h to obtain component B; (3) preparing a mixed solution of soluble cerium salt, soluble zirconium salt, soluble magnesium salt and soluble nickel salt, impregnating component B with equal volume of the mixed solution, drying at 120°C for 2h, and calcining at 650°C for 24h~36h to obtain component C; (4) CrO 3 Dissolve in water, impregnate component C with equal volume, dry at 120℃ for 2h, then impregnate with hydrazine hydrate solution with equal volume, dry at 120℃ for 2h, and calcine at 650℃ for 24h~36h to obtain a highly stable dehydrogenation catalyst.
2. The preparation method according to claim 1, It is characterized in that The amount of the two aluminum sources, the soluble aluminum salt in step (1) and the small-pore pseudo-boehmite in step (2), is calculated as follows: 2 O 3 Mass, the proportion of catalyst total Al 2 O 3 The ratios are: 30~70:70~30.
3. The preparation method according to claim 1, It is characterized in that The soluble chromium salt in step (1) and the Cr in step (2) 2 O 3 and CrO in step (4) 3 The usage of these three chromium sources is expressed as Cr 2 O 3 Mass, Cr in total catalyst 2 O 3 The ratios are: 30~65:30~45:5~25.
4. The preparation method according to claim 1, It is characterized in that The soluble aluminum salt in step (1) is aluminum chloride or aluminum nitrate, the soluble chromium salt is one of chromium nitrate, chromium acetate or chromium chloride, the soluble copper salt is copper chloride or copper nitrate, the soluble barium salt is barium chloride or barium nitrate, and the soluble lanthanum salt is lanthanum nitrate.
5. The preparation method according to claim 1, It is characterized in that The soluble sodium salt in step (2) is sodium nitrate or sodium hydroxide, and the soluble potassium salt is potassium nitrate or potassium fluoride.
6. The preparation method according to claim 1, It is characterized in that In step (3), the soluble cerium salt is cerium chloride or cerium nitrate, the soluble zirconium salt is zirconium nitrate, the soluble magnesium salt is magnesium nitrate or magnesium chloride, and the soluble nickel salt is nickel nitrate.
7. The preparation method according to claim 1, It is characterized in that The concentration of the hydrazine hydrate solution in step (4) is 200-300 g / L.