Monatomic silver-based ethylene epoxidation catalyst and preparation method thereof

By using boron nitride as a support to prepare a single-atom silver-based ethylene epoxidation catalyst, the problems of selectivity and precious metal usage in existing catalysts were solved, achieving a catalytic effect with high selectivity and low silver loading, thus improving the economic benefits of ethylene oxide production.

CN118925770APending Publication Date: 2024-11-12NINGBO JINYUANDONG PETROCHEM ENG TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964897.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing ethylene epoxidation catalysts have shortcomings in selectivity and the amount of precious metals used, which limits the economic benefits of ethylene oxide production.

Method used

Boron nitride was used as a support to prepare a single-atom silver-based ethylene epoxidation catalyst. By utilizing the rich pore structure and excellent physicochemical properties of boron nitride, a low amount of silver atoms were loaded to form a highly selective catalyst.

Benefits of technology

It achieved a selectivity of over 90% for ethylene oxide, reduced the amount of precious metals used, and improved the reaction performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925770A_ABST
    Figure CN118925770A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a monatomic silver-based ethylene epoxidation catalyst, which comprises the following steps: (1) dissolving a silver salt compound in a solvent to obtain a silver salt solution; (2) dispersing the boron nitride solid in a solvent to obtain a carrier dispersion; (3) under a dark condition, mixing and stirring the silver salt solution and the carrier dispersion, and after the stirring is finished, carrying out centrifugal separation, collecting and washing a solid; and (4) carrying out vacuum drying on the solid obtained in the step (3), and roasting in an inert atmosphere to obtain the monatomic silver-based ethylene epoxidation catalyst. The catalyst obtained by the method is high in selectivity and low in noble metal loading capacity, and fills the blank type of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ethylene oxide production, and in particular to a single-atom silver-based ethylene epoxidation catalyst and a preparation method thereof. Background Art

[0002] At present, the preparation method of ethylene epoxidation catalyst in the market mostly adopts the traditional impregnation thermal decomposition method, which loads the metal components onto the α-Al2O3 carrier and then prepares the ethylene oxide catalyst by high-temperature calcination. The important research direction of ethylene oxide catalyst is how to maximize the ethylene conversion rate and improve the selectivity of the catalyst, which is very important for ethylene oxide production companies to control costs and increase profits.

[0003] The catalysts used in existing ethylene oxide production equipment are mainly divided into three categories: the first is high-activity catalysts, which are characterized by high activity, good stability, and a wide range of applications, but due to their low selectivity, the economic benefits are not obvious; the second is high-selectivity catalysts, which have the advantage of high initial selectivity, but have strict requirements on the content of components in the feed gas, and the time-space yield is relatively low; the third is medium-selectivity catalysts, which are a catalyst that combines the characteristics of the first two catalysts. Due to the performance limitations of traditional catalysts and the consumption problems in the preparation process, people have to continue to explore and study new catalysts and their preparation methods.

[0004] Recently, there has been an increasing amount of research on single-atom catalysts. It has been found that the selectivity of single-atom silver catalysts for ethylene epoxidation can reach a level of ≥95%, and the Ag loading is also significantly reduced, saving precious silver metal materials and using silver metal resources in other more valuable fields.

[0005] Boron nitride, as a new type of nanomaterial with a structure similar to graphite, has excellent physical and chemical properties such as better high temperature resistance, better oxidation resistance and stronger chemical corrosion resistance than graphite materials. In addition, its rich pore structure is conducive to light absorption and charge transfer, and can provide more active sites, thereby improving catalytic reaction performance.

[0006] In view of this, the research on obtaining a new type of single-atom silver-based ethylene epoxidation catalyst can not only improve the catalyst performance, but also has positive significance for the allocation and utilization of precious metal resources. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a method for preparing a single-atom silver-based ethylene epoxidation catalyst. The catalyst obtained by the method has high selectivity and low precious metal loading, filling the blank type of catalyst.

[0008] The basic concept of the technical solution of the present invention is as follows: A method for preparing a single-atom silver-based ethylene epoxidation catalyst comprises the following steps: (1) dissolving a silver salt compound in a solvent to obtain a silver salt solution; (2) dispersing the boron nitride solid in a solvent to obtain a carrier dispersion; (3) mixing and stirring the silver salt solution and the carrier dispersion in the dark, and then centrifuging, collecting and washing the solid after completion; (4) vacuum drying the solid obtained in step (3), and then calcining it under an inert atmosphere to obtain the single-atom silver-based ethylene epoxidation catalyst.

[0009] As one embodiment, the silver salt compound is selected from one or a combination of silver nitrate or silver oxalate.

[0010] As one embodiment, the silver salt compound is silver oxalate, the solvent is deionized water, ethanolamine and ethylenediamine, and the obtained silver salt solution is a silver ammonia solution.

[0011] As one approach, the mass ratio of the silver salt compound to the boron nitride solid is (1-20):(200-1000).

[0012] As one embodiment, in step (4), the vacuum drying temperature is 20-80°C.

[0013] As one approach, in step (4), the calcination temperature is 200-400° C., and the calcination time is 1-6 h.

[0014] As a method, during calcination, the temperature is increased to 200-400°C at a rate of 2-7°C / min.

[0015] In one embodiment, the boron nitride solid is hexagonal boron nitride.

[0016] The present invention also provides a single-atom silver-based ethylene epoxidation catalyst, which is obtained according to the preparation method described in any one of the above contents.

[0017] Compared with the prior art, the present invention has the following advantages: 1. The present invention uses boron nitride as a new type of catalyst carrier to prepare a noble metal Ag single atom catalyst. When the Ag loading is not higher than 5%, a better catalytic effect can be achieved. Moreover, compared with the existing ordinary silver catalyst, the usage of the noble metal element is reduced, thereby obtaining a new type of catalyst and filling the technical gap.

[0018] 2. The boron nitride carrier used in the present invention has a rich pore structure. After loading single Ag atoms, it is beneficial to light absorption and charge transfer, provides more active sites, and improves the catalytic reaction performance. The catalyst with low Ag loading content of the present invention is evaluated using a fixed bed evaluation device, and the ethylene oxide selectivity can reach more than 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a high-angle annular dark-field scanning transmission electron microscope image of catalyst 1 prepared in Example 1 of the present invention; Figure 2 is a high-angle annular dark-field scanning transmission electron microscope image of catalyst 2 prepared in Example 2 of the present invention; Figure 3 It is a laboratory micro fixed bed reactor used in the present invention to test the performance of the catalyst.

[0020] Figure 4 yes Figure 3 Schematic diagram of the working principle of the reactor. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention is clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] The raw materials used in the present invention are common commodities purchased from the market unless otherwise specified, wherein the silver salt compound is preferably silver nitrate or silver oxalate.

[0023] High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) examinations were performed using a JEOL JEM-2200FS transmission electron microscope with an accelerating voltage of 200 kV and probe-side aberration correction, with an active area of ​​200 mm for the detector. The STEM specimens were prepared by ultrasonically dispersing the powdered sample in high-purity ethanol and then allowing a drop of the suspension to evaporate on a gold grid coated with carbon.

[0024] Example 1 (1) Dissolve 78 mg of silver nitrate in 10 ml of deionized water to obtain a silver nitrate solution; (2) dispersing 5 g of boron nitride (hexagonal boron nitride, h-BN) into 100 ml of deionized water to obtain a carrier dispersion; (3) In the dark and under continuous stirring conditions, slowly dropwise add the silver nitrate solution to the carrier dispersion; after mixing, continue stirring for 12 hours, centrifuge the suspension at a centrifugal speed of 4000 rpm; wash the separated and collected solid with deionized water, ethanol or a mixed solution; (4) Drying at 25°C for 8 h under vacuum conditions (vacuum degree of 0.08 MPa); then calcining the solid powder in a tube furnace under nitrogen atmosphere at 300°C with a heating rate of 5°C / min for 2 h to obtain a single-atom silver-based ethylene oxide catalyst, which is designated as catalyst 1.

[0025] The silver atomic loading of the obtained catalyst was 0.85% by ICP-OES analysis.

[0026] High-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) analysis showed that there were no nanoparticles or clusters in catalyst 1. Isolated bright spots against a dark background indicated that silver was atomically dispersed ( Figure 1 ).

[0027] Example 2 Compared with Example 1, silver oxalate was used instead of silver nitrate, 500 mg of silver oxalate was dissolved in 10 mL of deionized water, 3 g of ethanolamine and 10 g of ethylenediamine reagent to form a silver amine solution, ensuring that there were no obvious solid particles in the obtained silver amine solution and the overall liquid was transparent, and tin foil was used to avoid light during stirring, and the mass of the loaded boron nitride was 10 g. Other conditions were the same as in Example 1. Recorded as catalyst 2.

[0028] The silver atomic loading of the obtained catalyst was 3.1% by ICP-OES analysis.

[0029] HAADF-STEM analysis showed that the silver in catalyst 2 was mainly in an atomically dispersed state ( Figure 2 ).

[0030] Example 3 The difference from Example 1 is that the solid powder finally obtained is treated in a nitrogen atmosphere at 200° C. for 2 h. This is recorded as Catalyst 3.

[0031] Example 4 The difference from Example 1 is that the solid powder finally obtained is treated in a nitrogen atmosphere at 400° C. for 6 h. This is recorded as Catalyst 4.

[0032] Example 5 The only difference from Example 1 is that the mass ratio of the silver salt compound to the boron nitride solid is 10:200, 50 mg of silver nitrate, and 1000 mg of boron nitride. This is designated as Catalyst 5, and the silver atomic loading is 2.9% as analyzed by ICP-OES.

[0033] Example 6 The only difference from Example 1 is that the mass ratio of the silver salt compound to the boron nitride solid is 1:500, 10 mg of silver nitrate, and 5000 mg of boron nitride. It is designated as Catalyst 6, and the silver atomic loading is 0.1% as analyzed by ICP-OES.

[0034] The silver loading statistics of catalysts 1-6 are shown in Table 1.

[0035] Table 1 Catalyst name Silver content% Catalyst 1 0.85% Catalyst 2 3.1% Catalyst 3 0.84% Catalyst 4 0.82% Catalyst 5 2.9% Catalyst 6 0.1% Effect Example 1 Catalysts 1-6 were subjected to performance evaluation experiments using a laboratory micro fixed bed reactor under the same conditions. The specific method is: a stainless steel reaction tube with an inner diameter of 10 mm was used and placed in a three-stage heating furnace. The constant temperature section was ensured to be 7-10 cm, the catalyst loading amount was 1 ml, and the loading items of the reaction tube were quartz wool, quartz sand, catalyst particles, and quartz sand from bottom to top. When loading, the catalyst was ensured to be in the middle of the reaction heating furnace. The measurement conditions are shown in Table 2 below.

[0036] Table 2 When the above conditions are stably achieved, the gas composition at the reactor inlet and outlet is continuously measured by gas chromatography. After the analysis results are corrected for volume compression, the selectivity of the catalyst is calculated according to the selectivity formula, where the volume correction factor is: f = ΔEO / (ΔEO+0.5×ΔCO2)×100% f represents the coefficient of change of gas volume before and after; ΔEO: change of EO concentration in the intake gas and the product; ΔCO2: change of carbon dioxide concentration in the intake gas and the product; The calculation formula for ethylene conversion is: C EO , in: ethylene oxide inlet gas chromatography detection concentration; C EO,out : Chromatographic detection concentration of ethylene oxide in product gas; C EO =(C EO,in -C EO,out ) / C EO,in ×100% The formula for calculating the selectivity of ethylene oxide (EO) is: S EO =C EO,out / (C Eo,out +0.5(Cco 2,out -Cco 2,in ))×100% The final catalyst evaluation results are shown in Table 3.

[0037] Table 3 *: After the device has been running stably for 148 hours; From the results of catalyst activity and selectivity in Table 3: 1. The content of single silver atoms has a significant effect on the effect of ethylene epoxidation. This is mainly because single silver atoms are real active sites. Higher silver loading can provide more active sites during the reaction. The conversion rate of catalysts for ethylene epoxidation is positively correlated with the silver loading, but the selectivity of each catalyst does not vary significantly with the change of silver loading, indicating that the selectivity is mainly determined by the structure of silver atoms.

[0038] 2. The temperature and time of the calcination process have an impact on the performance of the catalyst. The catalyst of the present invention tends to be calcined in a nitrogen atmosphere at a low temperature. This is mainly because high temperature and long-term calcination will cause silver atoms to agglomerate to form nanoclusters, thereby affecting the atomic utilization of silver. The conversion of silver atoms to silver nanoclusters has an adverse effect on the selectivity and conversion rate of the catalyst.

[0039] Although the embodiments disclosed in the present invention are as above, the contents described are only embodiments adopted to facilitate understanding of the present invention and are not intended to limit the present invention. Any technician in the field to which the present invention belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in the present invention, but the patent protection scope of the present invention shall still be subject to the scope defined in the attached claims.

Claims

1. A method for preparing a single-atom silver-based ethylene epoxidation catalyst, characterized in that: The steps include: (1) dissolving a silver salt compound in a solvent to obtain a silver salt solution; (2) dispersing the boron nitride solid in a solvent to obtain a carrier dispersion; (3) mixing and stirring the silver salt solution and the carrier dispersion in the dark, and then centrifuging, collecting and washing the solids; (4) vacuum drying the solid obtained in step (3), and then calcining it under an inert atmosphere to obtain the single-atom silver-based ethylene epoxidation catalyst.

2. The method for preparing the single-atom silver-based ethylene epoxidation catalyst according to claim 1, characterized in that: The silver salt compound is selected from silver nitrate or silver oxalate, or a combination of the two.

3. The method for preparing the single-atom silver-based ethylene epoxidation catalyst according to claim 2, characterized in that: The silver salt compound is silver oxalate, the solvent is deionized water, ethanolamine and ethylenediamine, and the obtained silver salt solution is a silver ammonia solution.

4. The method for preparing the single-atom silver-based ethylene epoxidation catalyst according to claim 1, characterized in that: The mass ratio of the silver salt compound to the boron nitride solid is (1-20): (200-1000).

5. The method for preparing the single-atom silver-based ethylene epoxidation catalyst according to claim 1, characterized in that: In step (4), the vacuum drying temperature is 20-80°C.

6. The method for preparing the single-atom silver-based ethylene epoxidation catalyst according to claim 1, characterized in that: In step (4), the calcination temperature is 200-400°C and the calcination time is 1-6h.

7. The method for preparing the single-atom silver-based ethylene epoxidation catalyst according to claim 7, characterized in that: During calcination, the temperature is raised to 200-400°C at a rate of 2-7°C / min.

8. The method for preparing the single-atom silver-based ethylene epoxidation catalyst according to claim 1, characterized in that: The boron nitride solid is hexagonal boron nitride.

9. A single-atom silver-based ethylene epoxidation catalyst, characterized in that: Obtained according to the preparation method according to any one of claims 1 to 8.