Nickel-based molecular sieve hydrocracking and isomerization catalyst as well as preparation method and application thereof
By embedding nickel metal nanoparticles into MCM-22 molecular sieve, metal-MCM-22 molecular sieve catalysts are formed, which solves the problem that existing catalysts cannot take into account both isomerization and cracking properties, and achieves efficient production and low-cost production of biodiesel.
Patent Information
- Application Number
- CN202411122716.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Existing catalysts cannot take into account the isomerization and cracking properties of biodiesel at the same time, resulting in low production efficiency of bioaerospace coal and low-cooling point biodiesel, and the preparation process is complex and costly.
By embedding nickel metal nanoparticles in situ into the MCM-22 molecular sieve, a metal-MCM-22 molecular sieve catalyst is formed, and the surface of the molecular sieve particles is modified by using nickel metal atoms to eliminate some acidic centers to prepare a catalyst with good cracking and isomerization properties. .
It achieves the isomerization and cracking properties at lower temperatures, reduces production costs, improves the activity and stability of the catalyst, and is suitable for the production of hydrocarbon-based biodiesel of C15-C18 n-alkanes.
Smart Images

Figure CN118925794A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biofuel production and molecular sieve catalyst preparation, and in particular to a nickel-based molecular sieve hydrocracking and isomerization catalyst and a preparation method and application thereof. Background Art
[0002] Biofuel refers to fuel ethanol, biodiesel and aviation biofuel produced from biological resources. It can replace gasoline and diesel produced from petroleum and is an important direction for the development and utilization of renewable energy. Compared with traditional fuels such as diesel or gasoline, it produces less harmful carbon emissions and is more environmentally friendly and energy-saving. In recent years, some researchers at home and abroad have proposed a biodiesel synthesis technology route based on catalytic hydrogenation process, forming a hydrocarbon-based biodiesel preparation technology.
[0003] Hydrocarbon-based biodiesel is mainly C 15 ~C 18 of normal alkanes. Since normal alkanes have poor cold flow properties, an isomerization depressant process is required to improve the cold flow properties of the product. Normally, in the presence of an isomerization catalyst, long-chain alkanes will undergo isomerization and cracking reactions simultaneously. If the cracking reaction is too much, the yield of the product fuel oil will be reduced; if the isomerization is insufficient, the cold flow requirements of the biofuel cannot be met. Therefore, in order to obtain as many valuable biofuel products as possible (biojet fuel and low-freezing point biodiesel), it is necessary to strictly control the hydroisomerization reaction process of bio-based long-chain alkanes, and the selectivity of isomerization and cracking is closely related to the performance of the catalyst. Since the acidic centers on the catalyst surface can simultaneously catalyze the isomerization and cracking reactions of alkanes, moderate acid strength and acid amount are the key to balancing the isomerization and cracking reactions.
[0004] The catalysts for isomerization and cracking in the prior art include: Patent CN200910188170.6 discloses a hydrodewaxing catalyst and its preparation method and application. The catalyst uses a molecular sieve carrier modified by metal additives and silicone oil. By successively depositing additives and silicone oil, the acidity and pore shape of the inner and outer surfaces of the molecular sieve carrier are adjusted, thereby increasing the isomerization rate of the raw material. However, there are the following shortcomings: 1) The catalyst preparation process is complicated, including multiple steps of impregnation and high-temperature roasting processes, and the preparation cycle is long; 2) Due to the addition of additives and silicone oil, the active metal loading is low (1% to 15%), and the reaction activity is low.
[0005] Patent CN201810935163.7 discloses a hydrocracking catalyst and its preparation method and application. The catalyst is prepared by impregnation method and contains different types of phosphorus-containing molecular sieves and non-precious metal components. It shows excellent cracking performance in the hydrocracking reaction of Saudi vacuum residue oil. However, the catalyst cannot achieve the co-production of biojet fuel and low-freezing point biodiesel and is not suitable for C15 ~C 18 Isomerization reaction of bio-based long-chain alkanes. In addition, the catalyst needs to be sulfided when used and is not suitable for processing bio-based feedstocks that are almost sulfur-free.
[0006] Patent CN201610412721.2 discloses a method for producing isomerized decondensation of bio-jet fuel and a catalyst used in the method. The catalyst is one or more medium-pore molecular sieves selected from ZSM-22, ZSM-23, ZSM-12, and SAPO-11 with silicon surface modification, and the active metal component is selected from precious metals Pt and / or Pd with a content of 0.1wt% to 5wt%.
[0007] The paper (Toward the production of renewable diesel over robust Ninanoclusters highly dispersed on a two-dimensional zeolite, NPG Asia Materials, 2023, 15, 24) discloses a method for producing biodiesel, in which the Ni-loaded ITQ-2 molecular sieve used is prepared by organic ligand chelation, impregnation and grinding. The catalyst needs to first prepare MCM-22, then obtain ITQ-2 through swelling treatment, and then obtain Ni / ITQ-2 catalyst through organic ligand chelation, impregnation and grinding. The catalyst preparation process is complicated and cumbersome, and the stability of the catalyst needs to be improved.
[0008] CN202011264516.9 discloses a method for preparing a hydroisomerization catalyst carrier, which first mechanically mixes molecular sieves, amorphous inorganic porous materials and binder powders in a container to obtain a mixed powder, then mixes an additive with deionized water and drops it into the mixed powder, and then kneads, homogenizes, dries and roasts to obtain a catalyst carrier precursor; the raw molecular sieve is treated with acid or alkali to obtain a turbid liquid containing molecular sieve fragment structural units, which is impregnated into the catalyst carrier precursor. CN202011257233.1 discloses a method for preparing a hydroisomerization catalyst and a carrier thereof, wherein the catalyst carrier is prepared by mixing a modified molecular sieve obtained by metal and / or acid impregnation modification, drying and roasting of a raw molecular sieve (including MCM-22) containing a ten-membered ring structure and an amorphous inorganic porous material and then modified again by metal and / or acid. The preparation process of the above two catalysts is complicated and cumbersome, and it is not recorded whether isomerization and cracking can be taken into account.
[0009] Similarly, patent CN202010497292.X discloses a hydroisomerization catalyst and its preparation method and application. The catalyst uses a ZSM-48 molecular sieve with a hollow spherical structure as a carrier, and the active metal component is selected from at least one of the noble metal components of Group VIII, and is prepared by an impregnation method. Patents US11603501B2 and US20240034945A1 disclose catalyst preparation methods and their applications in the production of bio-jet fuel. The catalysts used in these patents cannot take into account both isomerization and cracking, and all use noble metals as active components. Although noble metals have high low-temperature activity, the catalyst cost is relatively high and is sensitive to impurities and is easily poisoned.
[0010] Patent CN202111280384.3 discloses a method for hydrodecondensation of diesel, in which the hydrodecondensation catalyst used is a non-precious metal catalyst supported by a steam-treated ZSM-5 molecular sieve and a catalyst supported by other molecular sieve carriers, which are used in a graded loading manner. The invention content shows that the preparation process of the ZSM-5 molecular sieve carrier is complicated, energy-intensive, and prone to produce acidic and alkaline waste liquids.
[0011] It is known to those skilled in the art that there are large differences in the composition of petrochemical diesel and biodiesel. The former contains a certain amount of cycloalkanes and aromatics, and the carbon number distribution is wide; while the latter is almost entirely normal paraffins, with carbon numbers concentrated in 15 to 18. In addition, the function of the existing post-treatment catalysts for petrochemical diesel is relatively single. In order to ensure a higher diesel yield, the catalyst is more biased towards isomerization performance, and it is difficult to achieve both isomerization and cracking. The most commonly used method is to use two reactors, respectively loaded with cracking catalysts and isomerization catalysts, but this will increase equipment investment. Therefore, conventional diesel isomerization decondensation catalysts are not suitable for processing biodiesel, especially for the process of producing bio-jet fuel and producing low-condensation point biodiesel. In view of this, it is necessary to develop a nickel-based molecular sieve hydrocracking and isomerization catalyst for the simultaneous production of bio-jet fuel and low-condensation point biodiesel. Summary of the invention
[0012] In order to solve the above problems, the present application provides a nickel-based molecular sieve hydrocracking and isomerization catalyst and its preparation method and application. The method embeds nickel metal nanoparticles in situ into the MCM-22 molecular sieve through a eutectic process, and uses nickel metal atoms to modify the surface of the molecular sieve particles, eliminate some acidic centers, and form a metal-MCM-22 molecular sieve catalyst with good cracking and isomerization performance; then, the metal-MCM-22 molecular sieve catalyst is mixed and molded into a hydrocracking and isomerization catalyst, and used for the production of oil-based bio-jet fuel and low-freezing point biodiesel.
[0013] On the one hand, the present invention provides a nickel-based molecular sieve hydrocracking and isomerization catalyst. Calculated by mass fraction, the nickel-based molecular sieve hydrocracking and isomerization catalyst comprises 30-80% MCM-22 molecular sieve, 15-45% nickel metal element and γ-Al2O3, and the total mass fraction of the raw materials of MCM-22 molecular sieve, nickel metal element and γ-Al2O3 is 100%.
[0014] The preparation method of the nickel-based molecular sieve hydrocracking and isomerization catalyst comprises the following steps:
[0015] S1: prepare MCM-22 molecular sieve precursor and adjust pH to 9-13;
[0016] S2: In situ embedding nickel metal nanoparticles into the MCM-22 molecular sieve precursor obtained in step S1, adjusting the pH to 8-12, and obtaining a metal-MCM-22 molecular sieve complex;
[0017] S3: treating the metal-MCM-22 molecular sieve complex prepared in step S2 with an acid solution and / or an alkaline solution, and then filtering, washing, drying, and calcining in sequence to obtain a metal-MCM-22 molecular sieve catalyst;
[0018] S4: adding aluminum hydroxide dry rubber powder, dilute nitric acid solution and sesbania powder to the metal-MCM-22 molecular sieve catalyst obtained in step S3, and then kneading, molding, drying, roasting and reducing to obtain a nickel-based molecular sieve hydrocracking and isomerization catalyst; the metal loading is 6 to 42 wt%.
[0019] Optionally, the method for preparing the MCM-22 molecular sieve precursor in step S1 comprises the following steps:
[0020] The silicon source, the aluminum source, the sodium hydroxide and the template agent are dissolved in deionized water to obtain a viscous liquid, and the liquid is subjected to hydrothermal treatment at 30 to 80° C. to obtain an MCM-22 molecular sieve precursor;
[0021] Wherein, calculated by the mass of oxides, the chemical composition of the viscous liquid is SiO2:Al2O3:Na2O:template:H2O=(20-80):(0.5-2):(10-50):(5-30):(1000-5000). Preferably, the chemical composition of the viscous liquid is SiO2:Al2O3:Na2O:template:H2O=(20-70):(0.5-1.5):(10-40):(5-20):(1000-4000).
[0022] Furthermore, in step S1, a MCM-22 molecular sieve precursor with a specific structure is obtained, which promotes the subsequent formation of the MCM-22 molecular sieve structure and lays the foundation for the subsequent embedding of active metals.
[0023] Optionally, the method for preparing the metal-MCM-22 molecular sieve composite in step S2 comprises the following steps:
[0024] A nickel salt is added to an MCM-22 molecular sieve precursor, and a crystallization reaction is carried out at a temperature of 120 to 180° C. for 3 to 9 days, and a metal-MCM-22 molecular sieve composite in which nickel metal nanoparticles are embedded is obtained after filtering, washing and drying in sequence;
[0025] Wherein, the chemical composition of the feed is SiO2:Al2O3:NiO:Na2O:template:H2O=(20-80):(0.5-2):(5-35):(10-50):(5-30):(1000-5000) calculated by the weight of the oxide. Preferably, the chemical composition of the feed is SiO2:Al2O3:NiO:Na2O:template:H2O=(30-80):(1-2):(10-35):(20-50):(10-30):(2000-5000) calculated by the weight of the oxide.
[0026] Furthermore, in step S2, nickel metal nanoparticles are in-situ embedded in the molecular sieve through a co-hydrothermal process of nickel salt and MCM-22 molecular sieve precursor, which, on the one hand, regulates the particle size of the molecular sieve, and on the other hand, modifies the surface of the molecular sieve particles, moderately reduces the number and strength of acidic centers, and obtains a molecular sieve material with moderate cracking performance.
[0027] Optionally, the nickel salt includes one or more of nitrate, nitrite, sulfate, chloride, basic carbonate, and acetate.
[0028] Optionally, the template agent is hexamethyleneimine.
[0029] Optionally, the method for preparing the metal-MCM-22 molecular sieve catalyst in step S3 comprises the following steps:
[0030] The metal-MCM-22 molecular sieve composite is treated with an acid solution at a temperature of 40 to 60° C., and then the treated material is filtered, washed with water, dried, and calcined at 450 to 600° C. to obtain a metal-MCM-22 molecular sieve catalyst;
[0031] And / or using an alkaline solution to treat the metal-MCM-22 molecular sieve complex at a temperature of 50-80°C, and then filtering, washing, drying, and calcining the treated material at 450-600°C in sequence to obtain a metal-MCM-22 molecular sieve catalyst.
[0032] Furthermore, the preparation method of the metal-MCM-22 molecular sieve catalyst in step S3 may include the following steps: firstly treating the metal-MCM-22 molecular sieve composite at 40-70° C. with an acid solution, and then filtering, washing, and drying the treated material in sequence; then treating the metal-MCM-22 molecular sieve composite at 50-80° C. with an alkaline solution, and then filtering, washing, drying, and calcining the treated material at 450-600° C. to obtain the metal-MCM-22 molecular sieve catalyst;
[0033] Or firstly, the metal-MCM-22 molecular sieve complex is treated with an inorganic alkali solution at a temperature of 50-80°C, and then the treated material is filtered, washed with water, and dried in sequence; then, the metal-MCM-22 molecular sieve complex is treated with an acid solution at a temperature of 40-70°C, and then the treated material is filtered, washed with water, dried, and calcined at 450-600°C to obtain a metal-MCM-22 molecular sieve catalyst.
[0034] Furthermore, in step S3, the template agent is removed by high temperature treatment, which can improve the thermal stability and chemical stability of the molecular sieve.
[0035] Optionally, in step S4, the mass ratio of the metal-MCM-22 molecular sieve catalyst, aluminum hydroxide dry rubber powder, dilute nitric acid solution and sesbania powder is (30-70): (2-4): (2-4): (10-30). Preferably, in step S4, the mass ratio of the metal-MCM-22 molecular sieve catalyst, aluminum hydroxide dry rubber powder, dilute nitric acid solution and sesbania powder is (30-50): (2-4): (2-4): (10-20).
[0036] Optionally, the properties of the metal-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 200 to 500 m 2 , the total pore volume is 0.30~0.90cm 3 / g, SiO2:Al2O3 molar ratio = 15~80.
[0037] Optionally, the acid solution includes one or more of hydrochloric acid, phosphoric acid, nitric acid, acetic acid, tartaric acid, and citric acid; the concentration of the acid solution is 0.1 to 0.5 mol / L; preferably, the acid solution is a mixed acid solution of hydrochloric acid and phosphoric acid, and the mass ratio of hydrochloric acid to phosphoric acid is 1:1.
[0038] Optionally, the alkaline solution includes one or more of sodium hydroxide, potassium hydroxide, and ammonia water; the concentration of the alkaline solution is 0.1-0.5 mol / L; preferably, the alkaline solution is a mixed alkaline solution of sodium hydroxide and ammonia water, and the mass ratio of sodium hydroxide to ammonia water is 1:1.
[0039] Optionally, the silicon source includes one or two of silica sol, white carbon black, sodium silicate and kaolin.
[0040] Optionally, the aluminum source includes one or two of aluminum sulfate, aluminum nitrate, aluminum chloride, and sodium aluminate.
[0041] Another aspect of the present invention provides an application of a nickel-based molecular sieve hydrocracking and isomerization catalyst in the hydroisomerization / cracking reaction of a bio-based long-chain alkane, wherein the bio-based long-chain alkane is derived from a bio-oil hydrodeoxygenation process and is composed of C 15 ~C 18 A mixture of straight chain alkanes with a sulfur content of <3ppmw.
[0042] Furthermore, for C 15 ~C 18 For hydrocarbon-based biodiesel of normal alkanes, the existing catalyst structure is relatively simple, and the acid strength and acid amount of the catalyst are unevenly distributed, resulting in the inability to simultaneously take into account the isomerization and cracking performance during hydrogenation isomerization or cracking. In the preparation process, the present application uses nickel metal atoms to induce the growth of MCM-22 molecular sieve precursors, and modifies the surface of molecular sieve particles to eliminate some acid centers, thereby forming a metal-MCM-22 molecular sieve catalyst with good cracking and isomerization performance. Application in C 15 ~C 18 For the hydrocarbon-based biodiesel of normal alkanes, the cracking rate is not less than 43% and the isomerization rate is not less than 42% under mild conditions (e.g., 260°C), and both isomerization and cracking performance can be taken into account. Preferably, when reacting at an elevated temperature (e.g., 300°C), the cracking rate is not less than 61% and the isomerization rate is not less than 52%.
[0043] Optionally, the hydrocracking and isomerization reaction conditions are: reaction temperature 200-300°C, reaction pressure 3-8MPa, liquid hourly space velocity 0.2-3.0h -1 , hydrogen to oil volume ratio is 400~800.
[0044] Optionally, the bio-oil is selected from waste oils and / or natural oils such as kitchen waste oil, sewage oil, palmitic acid oil, soybean oil, rapeseed oil, palm oil, cottonseed oil, tung oil, peanut oil, tallow or lard.
[0045] Compared with the prior art, the present invention achieves at least one of the following beneficial effects:
[0046] (1) For the first time, nickel metal nanoparticles and MCM-22 molecular sieves were combined to prepare catalysts for use in hydrocracking and isomerization reactions.
[0047] The prepared metal (nickel)-MCM-22 molecular sieve catalyst can have both isomerization and cracking properties, overcoming the technical obstacle that the catalyst in the prior art cannot have both isomerization and cracking properties at the same time. The reason is that the present application embeds a specific amount of nickel metal nanoparticles into the MCM-22 molecular sieve in an in-situ embedding manner through a eutectic process, realizes nickel metal atom modification of the MCM-22 molecular sieve particle surface, eliminates some acidic centers, and obtains a metal-MCM-22 molecular sieve catalyst having both isomerization and cracking properties.
[0048] Furthermore, the selectivity of the isomerization and cracking performance of the metal-MCM-22 zeolite catalyst can be adjusted by changing the nickel and zeolite content, thereby improving the flexibility of the entire production process, and the ratio of bio-jet fuel and biodiesel can be flexibly adjusted according to market demand.
[0049] (2) The catalyst of the present invention is a reduced catalyst, which does not need to be sulfurized before use and does not need to be supplemented with sulfur during use. It will neither affect the sulfur content of the product nor produce sulfur-containing waste gas, thus avoiding environmental pollution. The catalyst prepared by the present invention does not contain precious metals, has a production cost much lower than that of precious metal catalysts, and has stronger tolerance to raw materials.
[0050] (3) The catalyst obtained by the preparation method of the present invention is a non-supported catalyst, and the active metal content is 2 to 3 times that of a conventional supported catalyst. The nickel metal loading in the catalyst prepared by the present invention can be as high as 42%, showing a higher catalytic activity, and the reaction can be carried out at a lower temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0052] Figure 1 The scanning electron microscope energy spectrum of the metal-MCM-22 molecular sieve catalyst in Example 1 of the present invention is shown;
[0053] Figure 2 The gas chromatogram of the liquid product obtained when the metal-MCM-22 molecular sieve catalyst in Example 2 of the present invention is applied to the hydrocracking and isomerization (260° C.) of hydrocarbon-based biodiesel is shown;
[0054] Figure 3 A photograph of the metal-MCM-22 molecular sieve catalyst of Example 3 of the present invention is shown. DETAILED DESCRIPTION
[0055] In order to more clearly illustrate the overall concept of the present invention, a detailed description is given below in an exemplary manner in conjunction with the accompanying drawings.
[0056] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0057] Example 1
[0058] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 65% MCM-22 molecular sieve, 25% nickel element and 10% gamma-Al2O3.
[0059] The preparation method of the nickel-based molecular sieve hydrocracking and isomerization catalyst comprises the following steps:
[0060] S1: Dissolve a silicon source (silica sol), an aluminum source (aluminum sulfate), sodium hydroxide and a template (hexamethyleneimine) in deionized water to obtain a viscous liquid. Calculated by the mass of the oxides, the feed ratio is SiO2:Al2O3:Na2O:template:H2O=60:1:30:10:4000; then perform a hydrothermal treatment at 60°C for 5 hours to obtain an MCM-22 molecular sieve precursor; adjust the pH to 9.
[0061] S2: Nickel nitrate was added to the MCM-22 molecular sieve precursor, and ultrasonic-assisted crystallization was carried out at a temperature of 150°C and a power of 300 W for 4 days. The pH was adjusted to 8, and the mixture was filtered, washed and dried in sequence to obtain a Ni-MCM-22 molecular sieve composite in which nickel metal nanoparticles were embedded. The chemical composition of the feed, calculated by the mass of oxides, was SiO2:Al2O3:NiO:Na2O:template:H2O=60:1:20:30:10:4000.
[0062] S3: Add the Ni-MCM-22 molecular sieve complex to a mixed solution of 0.15 mol / L hydrochloric acid and phosphoric acid, with a mass ratio of 1:1, and treat at 60°C for 6 hours; wash the acid-treated complex to neutrality, then dry and calcine at 450°C for 4 hours to obtain the Ni-MCM-22 molecular sieve catalyst. The properties of the Ni-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 472m 2 , the total pore volume is 0.81cm 3 / g, SiO2:Al2O3 (molar ratio) = 66.
[0063] S4: Take 30g Ni-MCM-22 molecular sieve catalyst, 5g aluminum hydroxide dry rubber powder, 2g dilute nitric acid solution and 10g sesbania powder, then mix, shape, dry, calcine at 500℃ for 4 hours, and reduce at 500℃ for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 25wt%.
[0064] Example 2
[0065] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 65% MCM-22 molecular sieve, 25% nickel element and 10% gamma-Al2O3.
[0066] S1: Dissolve the silicon source (kaolin), aluminum source (aluminum chloride), sodium hydroxide and template (hexamethyleneimine) in deionized water to obtain a viscous liquid. The feed ratio is SiO2:Al2O3:Na2O:template:H2O=60:1:30:10:4000, calculated by the mass of the oxides. Then, perform hydrothermal treatment at 30°C for 5 hours to obtain an MCM-22 molecular sieve precursor, and adjust the pH to 10.5.
[0067] S2: Nickel sulfate was added to the MCM-22 molecular sieve precursor, and ultrasonic-assisted crystallization was carried out at a temperature of 130°C and a power of 300 W for 6 days. The pH was adjusted to 12, and the mixture was filtered, washed and dried in sequence to obtain a Ni-MCM-22 molecular sieve composite in which nickel metal nanoparticles were embedded. The chemical composition of the feed, calculated by the mass of oxides, was SiO2:Al2O3:NiO:Na2O:template:H2O=60:1:20:30:10:4000.
[0068] S3: Add the Ni-MCM-22 molecular sieve complex to a mixed solution of 0.15 mol / L hydrochloric acid and phosphoric acid, with a mass ratio of 1:1, and treat at 50°C for 6 hours; wash the acid-treated complex to neutrality, then dry and calcine at 500°C for 4 hours to obtain the Ni-MCM-22 molecular sieve catalyst. The properties of the Ni-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 289m 2 , the total pore volume is 0.53 cm 3 / g, SiO2:Al2O3 (molar ratio) = 67.
[0069] In step S4: 30 g of Ni-MCM-22 molecular sieve catalyst, 5 g of aluminum hydroxide dry rubber powder, 2 g of dilute nitric acid solution and 10 g of sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 25 wt%.
[0070] Example 3
[0071] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 65% MCM-22 molecular sieve, 25% nickel element and 10% gamma-Al2O3.
[0072] S1: Dissolve a silicon source (sodium silicate), an aluminum source (sodium aluminate), sodium hydroxide and a template (hexamethyleneimine) in deionized water to obtain a viscous liquid. The feed ratio is SiO2:Al2O3:Na2O:template:H2O=60:1:30:10:4000, calculated by the mass of the oxides. Then, perform hydrothermal treatment at 80°C for 5 hours to obtain an MCM-22 molecular sieve precursor, and adjust the pH to 13.
[0073] S2: Nickel acetate was added to the MCM-22 molecular sieve precursor, and ultrasonic-assisted crystallization was carried out at 170°C and 300 W for 3 days. The pH was adjusted to 9.5, and the mixture was filtered, washed and dried to obtain a Ni-MCM-22 molecular sieve composite in which nickel metal nanoparticles were embedded. The chemical composition of the feed was SiO2:Al2O3:NiO:Na2O:template:H2O=60:1:20:30:10:4000, calculated by the mass of the oxides.
[0074] S3: Add the Ni-MCM-22 molecular sieve complex to a mixed solution of 0.15 mol / L hydrochloric acid and phosphoric acid, with a mass ratio of 1:1, and treat at 40°C for 6 hours; wash the acid-treated complex to neutrality, then dry and calcine at 600°C for 4 hours to obtain the Ni-MCM-22 molecular sieve catalyst. The properties of the Ni-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 314m 2 , the total pore volume is 0.62cm 3 / g, SiO2:Al2O3 (molar ratio) = 65. The obtained catalyst sample is shown in Figure 3 .
[0075] In step S4: 30 g of Ni-MCM-22 molecular sieve catalyst, 5 g of aluminum hydroxide dry rubber powder, 2 g of dilute nitric acid solution and 10 g of sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 25 wt%.
[0076] Example 4
[0077] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 52% MCM-22 molecular sieve, 38% nickel element and 10% gamma-Al2O3.
[0078] Based on Example 1, the main difference is that in step S2: calculated by the mass of oxides, the chemical composition of the feed is SiO2:Al2O3:NiO:Na2O:template:H2O=60:1:30:40:20:3500.
[0079] In step S3: the properties of the Ni-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 285m 2 , the total pore volume is 0.46 cm 3 / g, SiO2:Al2O3 (molar ratio) = 64.
[0080] In step S4: 30 g of Ni-MCM-22 molecular sieve catalyst, 5 g of aluminum hydroxide dry rubber powder, 2 g of dilute nitric acid solution and 10 g of sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 38 wt%.
[0081] Example 5
[0082] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 71% MCM-22 molecular sieve, 19% nickel element and 10% gamma-Al2O3.
[0083] Based on Example 1, the main difference is that in step S2: calculated by the mass of oxides, the chemical composition of the feed is SiO2:Al2O3:NiO:Na2O:template:H2O=60:1:15:25:25:3000.
[0084] In step S3: the properties of the Ni-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 348m 2 , the total pore volume is 0.39 cm 3 / g, SiO2:Al2O3 (molar ratio) = 68.
[0085] In step S4: 30 g of Ni-MCM-22 molecular sieve catalyst, 5 g of aluminum hydroxide dry rubber powder, 2 g of dilute nitric acid solution and 10 g of sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 19 wt%.
[0086] Example 6
[0087] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 64% MCM-22 molecular sieve, 26% nickel element and 10% gamma-Al2O3.
[0088] Based on Example 1, the main difference is that
[0089] In step S3: adding a mixed solution of 0.15 mol / L sodium hydroxide and ammonia water, wherein the mass ratio of sodium hydroxide to ammonia water is 1:1, and treating at 60° C. for 6 hours; washing the alkali-treated composite to neutrality, and then drying and calcining at 450° C. for 4 hours to obtain a Ni-MCM-22 molecular sieve catalyst;
[0090] The properties of Ni-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 372m 2 , the total pore volume is 0.34 cm 3 / g, SiO2:Al2O3 (molar ratio) = 58.
[0091] In step S4: 30 g of Ni-MCM-22 molecular sieve catalyst, 2 g of aluminum hydroxide dry rubber powder, 2 g of dilute nitric acid solution and 10 g of sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 26 wt%.
[0092] Example 7
[0093] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 66% MCM-22 molecular sieve, 24% nickel element and 10% gamma-Al2O3.
[0094] Based on Example 1, the main difference is that
[0095] In step S3: adding the Ni-MCM-22 molecular sieve composite to a mixed solution of 0.15 mol / L hydrochloric acid and phosphoric acid, wherein the mass ratio of hydrochloric acid to phosphoric acid is 1:1, and treating at 60° C. for 6 hours; washing the composite after acid treatment to neutrality, and then drying;
[0096] The Ni-MCM-22 molecular sieve complex was then added to a mixed solution of 0.15 mol / L sodium hydroxide and ammonia water, with a mass ratio of sodium hydroxide to ammonia water of 1:1, and treated at 60°C for 6 hours; the alkali-treated complex was washed to neutrality, and then dried and calcined at 450°C for 4 hours to obtain a Ni-MCM-22 molecular sieve catalyst.
[0097] The properties of Ni-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 295m 2 , with a total pore volume of 0.45 cm 3 / g, SiO2:Al2O3 (molar ratio) = 64.
[0098] In step S4: 30 g of Ni-MCM-22 molecular sieve catalyst, 5 g of aluminum hydroxide dry rubber powder, 2 g of dilute nitric acid solution and 10 g of sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 24 wt%.
[0099] Example 8
[0100] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 65% MCM-22 molecular sieve, 25% nickel element and 10% gamma-Al2O3.
[0101] Based on Example 1, the main difference is that
[0102] In step S3: adding the Ni-MCM-22 molecular sieve composite to a mixed solution of 0.15 mol / L sodium hydroxide and ammonia water, wherein the mass ratio of sodium hydroxide to ammonia water is 1:1, and treating at 60° C. for 6 hours; washing the composite after the alkali treatment to neutrality, and then drying;
[0103] The Ni-MCM-22 molecular sieve complex was then added to a mixed solution of 0.15 mol / L hydrochloric acid and phosphoric acid, with a mass ratio of hydrochloric acid to phosphoric acid of 1:1, and treated at 60°C for 6 hours; the acid-treated complex was washed to neutrality, and then dried and calcined at 450°C for 4 hours to obtain a Ni-MCM-22 molecular sieve catalyst.
[0104] The properties of Ni-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 286m 2 , the total pore volume is 0.42 cm 3 / g, SiO2:Al2O3 (molar ratio) = 65.
[0105] In step S4: 30 g of Ni-MCM-22 molecular sieve catalyst, 5 g of aluminum hydroxide dry rubber powder, 2 g of dilute nitric acid solution and 10 g of sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 25 wt%.
[0106] Example 9
[0107] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 66% MCM-22 molecular sieve, 24% nickel element and 10% gamma-Al2O3.
[0108] Based on Example 1, the main difference is that
[0109] In step S2: nickel nitrate is added to the MCM-22 molecular sieve precursor, and mechanical stirring is performed for crystallization at a temperature of 150° C. and a speed of 120 rpm for 4 days, the pH is adjusted to 8, and the Ni-MCM-22 molecular sieve composite in which nickel metal nanoparticles are embedded is obtained after filtering, washing and drying in sequence; the chemical composition of the feed is SiO2:Al2O3:NiO:Na2O:template:H2O=60:1:20:30:10:4000, calculated by the mass of the oxides.
[0110] In step S3: the properties of the Ni-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 226 m 2 , the total pore volume is 0.32cm 3 / g, SiO2:Al2O3 (molar ratio) = 65.
[0111] In step S4: 30 g of Ni-MCM-22 molecular sieve catalyst, 5 g of aluminum hydroxide dry rubber powder, 2 g of dilute nitric acid solution and 10 g of sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 24 wt%.
[0112] Comparative Example 1
[0113] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 65% MCM-22 molecular sieve, 25% nickel element and 10% gamma-Al2O3.
[0114] The preparation method of the catalyst comprises the following steps:
[0115] S1: Dissolve a silicon source (silica sol), an aluminum source (aluminum sulfate), sodium hydroxide and a template (hexamethyleneimine) in deionized water to obtain a viscous liquid. Each component is calculated according to the mass of the oxide. The chemical composition of the feed is SiO2:Al2O3:Na2O:template:H2O=60:1:30:10:4000; then perform hydrothermal treatment at 60°C for 5 hours to obtain an MCM-22 molecular sieve precursor, and adjust the pH to 9.
[0116] S2: The MCM-22 molecular sieve precursor was crystallized by ultrasound at 150° C. and 300 W for 4 days, the pH was adjusted to 8, and the MCM-22 molecular sieve was obtained after filtering, washing and drying.
[0117] S3: Add the MCM-22 molecular sieve into a mixed solution of 0.15 mol / L hydrochloric acid and phosphoric acid, with a mass ratio of hydrochloric acid to phosphoric acid of 1:1, and treat at 60°C for 6 hours; wash the acid-treated complex to neutrality, and then dry and calcine at 500°C for 4 hours to obtain the MCM-22 molecular sieve.
[0118] S4: Take 30g of MCM-22 molecular sieve, 5g of aluminum hydroxide dry rubber powder, 2g of dilute nitric acid solution and 10g of sesbania powder, then mix, shape, dry and calcine at 500°C for 4 hours to obtain a molecular sieve carrier.
[0119] S5: Prepare nickel nitrate aqueous solution, load nickel nitrate on MCM-22 molecular sieve carrier by equal volume impregnation method, dry, calcine at 500℃ for 4 hours, reduce at 500℃ for 4 hours to obtain Ni / MCM-22 cracking and isomerization catalyst with nickel loading of 25wt%. The properties of Ni / MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 316m 2 , the total pore volume is 0.30cm 3 / g, SiO2:Al2O3 (molar ratio) = 66.
[0120] Comparative Example 2
[0121] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 89.5% MCM-22 molecular sieve, 0.5% platinum element and 10% gamma-Al2O3.
[0122] Based on Comparative Example 1, the main difference is that
[0123] In step S5: prepare a chloroplatinic acid aqueous solution, load chloroplatinic acid on the carrier by an equal volume impregnation method, dry, calcine at 400°C for 4 hours, and reduce at 400°C for 4 hours to obtain a cracking and isomerization catalyst Pt / MCM-22 with a Pt loading of 0.5wt%. The properties of the Pt / MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 319m 2 , the total pore volume is 0.33 cm 3 / g, SiO2:Al2O3 (molar ratio) = 66.
[0124] Comparative Example 3
[0125] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 67% MCM-22 molecular sieve, 23% nickel element and 10% gamma-Al2O3.
[0126] S1: Dissolve a silicon source (silica sol), an aluminum source (aluminum sulfate), sodium hydroxide, a template (hexamethyleneimine) and a nickel source (nickel nitrate) in deionized water to obtain a viscous liquid. Calculated by the mass of the oxides, the chemical composition of the feed is SiO2:Al2O3:NiO:Na2O:template:H2O=60:1:20:30:10:4000; crystallize under ultrasound assistance at a temperature of 150°C and a power of 300W for 4 days, adjust the pH to 8, and obtain a metal-MCM-22 molecular sieve complex in which nickel metal nanoparticles are embedded after filtering, washing and drying in sequence.
[0127] S2: Add the metal-MCM-22 molecular sieve complex to a mixed solution of 0.15 mol / L hydrochloric acid and phosphoric acid, with a mass ratio of 1:1, and treat at 60°C for 6 hours; wash the acid-treated complex to neutrality, then dry and calcine at 450°C for 4 hours to obtain a metal-MCM-22 molecular sieve catalyst. The properties of the metal-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 241m 2 , the total pore volume is 0.28 cm 3 / g, SiO2:Al2O3 (molar ratio) = 69.
[0128] S3: Take 30g of metal-MCM-22 molecular sieve catalyst, 5g of aluminum hydroxide dry rubber powder, 2g of dilute nitric acid solution and 10g of sesbania powder, then mix, shape, dry, calcine at 500℃ for 4 hours, and reduce at 500℃ for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 23wt%.
[0129] Comparative Example 4
[0130] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 65% of MCM-22 molecular sieve, 25% of iron element and 10% of gamma-Al2O3.
[0131] The difference from Example 1 is that
[0132] In step S2: the nickel salt is replaced with an iron salt (ferric nitrate), and the rest is the same as in Example 1.
[0133] In step S3: the properties of the Fe-MCM-22 molecular sieve catalyst are as follows: BET specific surface area is 376m 2 , the total pore volume is 0.52cm 3 / g, SiO2:Al2O3 (molar ratio) = 66.
[0134] In step S4: 30 g of Fe-MCM-22 molecular sieve, 5 g of aluminum hydroxide dry rubber powder, 2 g of dilute nitric acid solution and 10 g of sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with an iron content of 25 wt%.
[0135] Comparative Example 5
[0136] A nickel-based molecular sieve hydrocracking and isomerization catalyst consists of the following components by mass fraction: 65% ZSM-22 molecular sieve, 25% nickel element and 10% gamma-Al2O3.
[0137] The difference from Example 1 is that the molecular sieve is different, and ZSM-22 molecular sieve is used.
[0138] In step S1, the template agent hexamethyleneimine is replaced with hexamethylenediamine, and the rest is the same as in Example 1 to obtain a ZSM-22 molecular sieve precursor.
[0139] In step S3: obtain a Ni-ZSM-22 molecular sieve catalyst, and the preparation process is the same as in Example 1. The properties of the Ni-ZSM-22 molecular sieve catalyst are as follows: BET specific surface area is 366m 2 , the total pore volume is 0.57 cm 3 / g, SiO2:Al2O3 (molar ratio) = 66.
[0140] In step S4: 30 g Ni-ZSM-22 molecular sieve, 5 g aluminum hydroxide dry powder, 2 g dilute nitric acid solution and 10 g sesbania powder are taken, and then mixed, molded, dried, calcined at 500° C. for 4 hours, and reduced at 500° C. for 4 hours to obtain a cracking and isomerization catalyst with a nickel content of 25 wt%.
[0141] Experimental Example 1
[0142] The catalysts prepared in the examples and comparative examples were respectively loaded into a high-pressure fixed-bed reactor, sealed and treated at 200°C for 4 hours under normal pressure hydrogen atmosphere to remove water and other gas impurities adsorbed in the catalyst. Afterwards, the hydrogen pressure of the reactor was raised to 4 MPa, and after the tail gas flow rate after the back pressure valve was stable, the reactor was programmed to heat up to 260°C. Then, the feed was started for isomerization reaction, with a volume space velocity of 1.5 h -1 , hydrogen oil volume ratio 800:1. The raw material used in the reaction is C 15 -C 18 The performance of the straight chain alkane mixture is tested, as shown in Table 1.
[0143] The stability in the table below indicates the time during which the catalytic performance of the catalyst remains essentially unchanged during the catalytic reaction in a high-pressure fixed bed reactor.
[0144] Table 1 Catalytic performance of bio-oil on different catalysts and properties of the obtained products (reaction temperature 260℃)
[0145]
[0146] Table 1
[0147]
[0148] Table 1
[0149]
[0150] As shown in Table 1, when the nickel-based molecular sieve catalyst of the present invention is applied to hydrocracking and isomerization of hydrocarbon-based biodiesel, the ideal effect can be achieved at a relatively low reaction temperature, wherein the liquid yield is not less than 95%, the product condensation point is not higher than -20°C, the cracking rate is not less than 38%, and the isomerization rate is not less than 42%. Comparing Example 1 with Examples 2, 3, 4, and 5, the change in metal content can significantly affect the performance (activity, yield, cracking rate, isomerization rate, stability) of the catalyst. With the increase of nickel content, the activity of the catalyst is significantly improved, but too much loaded metal nickel can affect the pore structure, acid properties, and dispersion of nickel metal of the molecular sieve, thereby reducing the cracking rate and isomerization rate of the raw material.
[0151] Comparing Example 1 with Examples 6, 7, and 8, the acid-base treatment can significantly affect the structure and reaction performance (activity, yield, cracking rate, isomerization rate, and stability) of the catalyst. The acid-base treatment can also partially remove the aluminum and silicon in the molecular sieve to form more mesoporous structures, which is conducive to the diffusion of the reaction, thereby improving the catalyst activity. Compared with the alkali treatment, the cracking rate and isomerization rate of the acid-treated catalyst are significantly improved, because the acid treatment can remove the nickel metal with a higher degree of aggregation and poorer activity, thereby obtaining a nickel metal with high dispersion.
[0152] Comparing Example 1 with Example 9, the molecular sieve catalyst obtained by ultrasound-assisted crystallization is superior to the molecular sieve catalyst obtained by mechanical stirring-assisted crystallization in terms of activity, cracking rate and isomerization rate.
[0153] Compared with Example 1, the metal dispersion of the catalyst prepared by the conventional impregnation method is lower than that by the in-situ embedding method, forming a large amount of nickel metal with high aggregation and poor activity, and too much metal will cover a large number of acidic centers on the surface of the molecular sieve carrier, resulting in a significant decrease in the catalyst activity, cracking, isomerization and stability.
[0154] Comparative Example 2 and Example 1 show that the non-precious metal catalyst prepared by the present invention shows a relatively higher raw material conversion rate than the precious metal catalyst, and although the cracking performance is relatively low, the product yield is higher. The non-precious metal catalyst prepared by the present invention can also achieve an effect that is not inferior to that of the precious metal catalyst.
[0155] Compared with Example 1 and Comparative Example 3, the non-precious metal catalyst prepared by the precursor method adopted in the present invention shows relatively higher raw material conversion rate, yield, cracking rate, isomerization rate and stability than directly crystallizing after mixing all the materials.
[0156] Comparative Example 4 and Example 1 show that the Ni-MCM-22 catalyst used in the present invention shows higher feedstock conversion rate, yield, cracking rate and isomerization rate than Fe-MCM-22.
[0157] Compared with Example 1 and Comparative Example 5, the Ni-MCM-22 catalyst used in the present invention shows higher raw material conversion rate, yield, cracking rate, isomerization rate and stability than Ni-ZSM-22, which is attributed to the unique layered structure and rich mesoporous structure of the MCM-22 molecular sieve.
[0158] Experimental Example 2
[0159] The catalysts prepared in the examples and comparative examples were respectively loaded into a high-pressure fixed-bed reactor, sealed and treated at 200°C for 4 hours under normal pressure hydrogen atmosphere to remove water and other gas impurities adsorbed in the catalyst. Afterwards, the hydrogen pressure of the reactor was raised to 4 MPa, and after the tail gas flow rate after the back pressure valve was stable, the reactor was programmed to heat up to 300°C. Then, the feed was started for isomerization reaction, with a volume space velocity of 1.5 h -1 , hydrogen to oil volume ratio 800:1. The raw material used in the reaction is C obtained by hydrogenation deoxygenation of sewage oil. 15 -C 18 The performance of the straight chain alkane mixture is tested, as shown in Table 2.
[0160] The stability in the table below indicates the time during which the catalytic performance of the catalyst remains essentially unchanged during the catalytic reaction in a high-pressure fixed bed reactor.
[0161] Table 2 Catalytic performance of bio-oil on different catalysts and properties of the obtained products (reaction temperature 300℃)
[0162]
[0163] Table 2
[0164]
[0165]
[0166] Table 2
[0167] Referring to Table 2, it can be seen that when the nickel-based molecular sieve catalyst of the present invention is applied to hydrocracking and isomerization of hydrocarbon-based biodiesel, when reacting at a higher reaction temperature (such as 300°C), the liquid yield is not less than 85%, the freezing point is not higher than -31°C, the cracking rate is not less than 61%, and the isomerization rate is not less than 52%. Increasing the reaction temperature can increase the reaction activity of the catalyst and the cracking rate and isomerization rate of normal alkanes, but high temperature will significantly reduce the yield of the product and produce more gas. Therefore, for the same catalyst, a moderate reaction temperature can obtain more target products. Straight-chain alkane raw materials from different raw material sources have little effect on the reaction process.
[0168] refer to Figure 1 As shown, a scanning electron microscope energy spectrum of the metal-MCM-22 molecular sieve catalyst in Example 1 of the present application is shown. It can be seen from the figure that in the composite catalyst prepared by in-situ embedding, the metal nickel is evenly dispersed inside the molecular sieve, which can provide more metal active centers and is beneficial to the activation of CH bonds in the raw material molecules.
[0169] refer to Figure 2 As shown in the figure, the gas chromatogram of the liquid product obtained by using the metal-MCM-22 molecular sieve catalyst in Example 2 of the present application is shown. It can be seen from the figure that the product is composed of normal and isomeric alkanes with different carbon numbers, which are concentrated in the C8~C 16 The jet fuel components, combined with the freezing point of the products in Table 2, show that the nickel-based molecular sieve catalyst prepared by the present invention exhibits excellent cracking and isomerization performance, and is very suitable for the production of bio-jet fuel products.
[0170] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A nickel-based molecular sieve hydrocracking and isomerization catalyst, characterized in that: Calculated by mass fraction, the nickel-based molecular sieve hydrocracking and isomerization catalyst includes 30-80% MCM-22 molecular sieve, 15-45% nickel metal element, and the rest is γ-Al2O3, and the total mass fraction of the raw materials of MCM-22 molecular sieve, nickel metal element and γ-Al2O3 is 100%.
2. A method for preparing the nickel-based molecular sieve hydrocracking and isomerization catalyst as claimed in claim 1, characterized in that: The following steps are involved: S1: prepare MCM-22 molecular sieve precursor and adjust pH to 9-13; S2: In situ embedding of nickel metal nanoparticles into the MCM-22 molecular sieve precursor obtained in step S1, adjusting the pH to 8-12, and obtaining a metal-MCM-22 molecular sieve composite with a high metal loading; S3: treating the metal-MCM-22 molecular sieve complex prepared in step S2 with an acid solution and / or an alkaline solution, and then filtering, washing, drying, and calcining in sequence to obtain a metal-MCM-22 molecular sieve catalyst; S4: adding aluminum hydroxide dry rubber powder, dilute nitric acid solution and sesbania powder to the metal-MCM-22 molecular sieve catalyst obtained in step S3, and then kneading, molding, drying, roasting and reducing to obtain a nickel-based molecular sieve hydrocracking and isomerization catalyst, wherein the metal loading is 6 to 42 wt%.
3. The method for preparing the nickel-based molecular sieve hydrocracking and isomerization catalyst according to claim 2, characterized in that: The method for preparing the MCM-22 molecular sieve precursor in step S1 comprises the following steps: The silicon source, the aluminum source, the sodium hydroxide and the template agent are dissolved in deionized water to obtain a viscous liquid, and the liquid is subjected to hydrothermal treatment at 30 to 80° C. to obtain an MCM-22 molecular sieve precursor; Wherein, calculated by the mass of oxides, the chemical composition of the viscous liquid is SiO2:Al2O3:Na2O:template:H2O=(20-80):(0.5-2):(10-50):(5-30):(1000-5000).
4. The method for preparing the nickel-based molecular sieve hydrocracking and isomerization catalyst according to claim 2, characterized in that: The method for preparing the metal-MCM-22 molecular sieve composite in step S2 comprises the following steps: A nickel salt is added to an MCM-22 molecular sieve precursor, and a crystallization reaction is carried out at a temperature of 120 to 180° C. for 3 to 9 days, and a metal-MCM-22 molecular sieve composite in which nickel metal nanoparticles are embedded is obtained after filtering, washing and drying in sequence; The crystallization reaction process also includes any one of ultrasonic assistance, mechanical stirring, and no mechanical stirring; Calculated by the mass of oxides, the chemical composition of the feed is SiO2:Al2O3:NiO:Na2O:template:H2O=(20~80):(0.5~2):(5-35):(10~50):(5-30):(1000~5000).
5. The method for preparing the nickel-based molecular sieve hydrocracking and isomerization catalyst according to claim 2, characterized in that: The preparation method of the metal-MCM-22 molecular sieve catalyst in step S3 comprises the following steps: The metal-MCM-22 molecular sieve composite is treated with an acid solution at a temperature of 40 to 70° C., and then the treated material is filtered, washed with water, dried, and calcined at 450 to 600° C. to obtain a metal-MCM-22 molecular sieve catalyst; And / or using an alkaline solution to treat the metal-MCM-22 molecular sieve complex at a temperature of 50-80°C, and then filtering, washing, drying, and calcining the treated material at 450-600°C in sequence to obtain a metal-MCM-22 molecular sieve catalyst.
6. The method for preparing the nickel-based molecular sieve hydrocracking and isomerization catalyst according to claim 2, characterized in that: The properties of the metal-MCM-22 molecular sieve catalyst obtained in step S4 are as follows: BET specific surface area is 200 to 500 m 2 , the total pore volume is 0.30~0.90cm 3 / g, SiO2:Al2O3 molar ratio = 15~80.
7. The method for preparing the nickel-based molecular sieve hydrocracking and isomerization catalyst according to claim 2, characterized in that: The acid solution includes one or more of hydrochloric acid, phosphoric acid, nitric acid, acetic acid, tartaric acid, and citric acid; the concentration of the acid solution is 0.1 to 0.5 mol / L; preferably, the acid solution is a mixed acid solution of hydrochloric acid and phosphoric acid, and the mass ratio of hydrochloric acid to phosphoric acid is 1:1; And / or the alkaline solution includes one or more of sodium hydroxide, potassium hydroxide, and ammonia water; the concentration of the alkaline solution is 0.1-0.5 mol / L; preferably, the alkaline solution is a mixed alkaline solution of sodium hydroxide and ammonia water, and the mass ratio of sodium hydroxide to ammonia water is 1:
1.
8. The method for preparing the nickel-based molecular sieve hydrocracking and isomerization catalyst according to claim 3, characterized in that: The silicon source includes one or two of silica sol, sodium silicate, kaolin and white carbon black; and / or the aluminum source includes one or two of aluminum sulfate, aluminum nitrate, aluminum chloride, and sodium aluminate; And / or the template agent is hexamethyleneimine.
9. The method for preparing the nickel-based molecular sieve hydrocracking and isomerization catalyst according to claim 4, characterized in that: The nickel salt includes one or more of nitrate, nitrite, sulfate, chloride, basic carbonate and acetate.
10. A use of the nickel-based molecular sieve hydrocracking and isomerization catalyst as claimed in claim 1 in the hydroisomerization / cracking reaction of bio-based long-chain alkanes, wherein the bio-based long-chain alkanes are derived from the hydrodeoxygenation process of bio-oils and are composed of C 15 ~C 18 A mixture of straight chain alkanes with a sulfur content of <3ppmw.
Citation Information
Patent Citations
Hydrogenation catalyst and preparation method thereof
CN108262063A
Hydrogenation catalyst support and preparation method thereof
CN108262066A
Preparation method and application of isomerization pour point depressing catalyst
CN113617384A
Bifunctional catalyst for packaging Ni-coated H-MCM-22 molecular sieve and preparation method of bifunctional catalyst
CN117772270A
Method for in-situ preparation of high-dispersion nickel-based molecular sieve catalyst
CN118304927A