Flotation process for directly recycling polymetallic sulfide ore tailing water

By using the same non-yellowicide collector and masking agent in the flotation process of copper (lead) zinc polymetallic sulfide ore, the problem of difficulty in directly reusing tailings water is solved, and the direct use of polymetallic ore ore dressing water is achieved Reuse reduces the operating costs of the ore dressing plant.

CN118925944APending Publication Date: 2024-11-12CHINA ENFI ENG CORP +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411256681.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the traditional copper (lead) zinc polymetallic sulfide ore flotation process, the collectors at each flotation stage cannot be mixed, making it difficult to directly reuse tailings water, which increases the investment and operation costs of the ore dressing plant.

Method used

A flotation process for direct reuse of polymetallic sulfide tailings water is adopted. By adding masking agents in the grinding stage, the same non-yellow drug collector is used for the full process flotation treatment, including copper or lead floatation. Selection, zinc flotation and sulfur flotation ensure that the tailings water can be directly returned to the grinding service after dense treatment.

Benefits of technology

It effectively avoids the negative impact between different collectors, realizes direct reuse of polymetallic ore ore dressing water, reduces the demand for return water or return water treatment in stages, and reduces infrastructure investment and operation costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of mineral separation, in particular to a flotation process for directly recycling polymetallic sulfide ore tailing water. Copper or / and lead flotation; zinc flotation; sulfur flotation; and treating tailings. According to the method, copper (lead) sulfide, zinc sulfide and iron sulfide minerals are collected through the same collecting agent, meanwhile, a masking agent is adopted in the ore grinding process to eliminate the activation effect of activated ions (copper, iron and the like) in return water on the zinc sulfide and iron sulfide minerals, and the adverse effect that zinc sulfide and iron sulfide are difficult to restrain in the copper (lead) flotation stage is avoided; and different inhibitors or activators are combined in different mineral separation stages for synergistic cooperation, so that the purpose of directly recycling the polymetallic mineral separation water is achieved, means such as stage backwater or backwater treatment are avoided, and the capital construction investment or the operation cost of a mineral separation plant is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore dressing, and in particular to a flotation process for directly recycling tailings water of a polymetallic sulfide ore. Background Art

[0002] The common flotation process of copper (lead) zinc polymetallic sulfide ore is copper (lead) priority flotation - copper (lead) tailings zinc selection - zinc tailings sulfur selection process. In the traditional reagent system, the collectors in each flotation operation stage are not the same. The commonly used collectors for copper (lead) flotation are ester reagents (such as Z-200), black medicine reagents (such as No. 25 black medicine), etc. The commonly used collectors for zinc selection are xanthate reagents (such as butyl xanthate), sulfur nitrogen reagents (such as ethyl sulfur nitrogen), and the commonly used collectors for sulfur selection are xanthate reagents (such as butyl xanthate, pentyl xanthate, etc.). However, the collectors used in each stage have different action capabilities, and the target minerals selected are also very different. Therefore, in the traditional copper (lead) zinc polymetallic sulfide ore flotation system, the collectors in each flotation stage cannot be mixed, especially the collectors for zinc selection cannot enter the copper (lead) flotation operation section. However, the mineral processing return water will inevitably contain all types of collectors.

[0003] In order to ensure the normal use of return water, mineral processing plants currently use three methods to solve the problem: (1) Use the tailings pond return water method to utilize the return water. Xanthate and other mineral processing reagents are degraded by exposure to the tailings pond and then reused, which has little impact on the mineral processing process. (2) Use the staged return water method to avoid the adverse effects of return water. After the copper (lead) flotation operation, a thickener is installed to return the return water from the copper (lead) flotation to this section. (3) Treat the return water, degrade the residual reagents, and then return it for use. This method is often seen in many situations such as incomplete degradation of the tailings pond return water, pre-plant return water, and the inability to set up a staged return water thickener. However, the staged return water method will increase the investment of the beneficiation plant, and the return water treatment method will increase the operating cost of the beneficiation plant.

[0004] Chinese patent document CN109675714B discloses a brecciated lead-zinc sulfide ore dressing method in which the return water can be directly used. In the actual production process, with the continuous accumulation of dressing reagents, it is impossible to accurately control the residual reagents in the recovery, so it is also impossible to accurately control and adjust the dosage of reagents such as butyl xanthate for lead selection and pine oil for zinc coarse selection. The return water will inevitably disrupt the entire beneficiation process. Based on this, it is still difficult to fundamentally solve the problem that the return water cannot be directly reused. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defect that the existing polymetallic sulfide ore tailings water is difficult to directly reuse, thereby providing a flotation process for directly reusing the polymetallic sulfide ore tailings water to solve the above problem.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A flotation process for direct reuse of polymetallic sulfide ore tailings water, comprising:

[0008] Grinding: Grind the polymetallic sulfide ore and add masking agent to obtain flotation pulp;

[0009] Copper or / and lead flotation: adding zinc sulfide and iron sulfide mineral inhibitors, copper or / and lead collectors, and frothers to the flotation pulp for flotation treatment to obtain copper or / and lead concentrates and tailings;

[0010] Zinc flotation: adding iron sulfide mineral inhibitor, zinc sulfide mineral activator, zinc collector and frother to copper and / or lead flotation tailings for flotation treatment to obtain zinc concentrate and zinc tailings;

[0011] Sulfur flotation: Add iron sulfide mineral activator, iron sulfide mineral collector and frother to zinc tailings for flotation treatment to obtain sulfur concentrate and final tailings;

[0012] Tailings treatment: After the final tailings are thickened, the overflow water is directly returned to the grinding mill for use;

[0013] The copper and / or lead collector, the zinc collector and the iron sulfide mineral collector are the same and non-xanthate collectors.

[0014] Preferably, the polymetallic sulfide ore is at least one of lead-zinc sulfide ore, copper-zinc sulfide ore, and copper-lead-zinc sulfide ore;

[0015] And / or, the grinding process is performed to a particle size of -0.074 mm, accounting for 70-80%;

[0016] And / or, the mass percentage concentration of the flotation pulp is 30-40%;

[0017] And / or, the masking agent is at least one of sodium sulfide, sodium humate, sodium dimethyldithiocarbamate, and sodium trithiocarbonate;

[0018] And / or, based on the dry weight of the feed mineral, the amount of the masking agent is 100-500 g / t.

[0019] Preferably, the zinc sulfide and iron sulfide mineral inhibitors are at least two of zinc sulfate, sodium sulfite, sodium pyrosulfite, and sodium sulfate;

[0020] And / or, the iron sulfide mineral inhibitor is at least one of calcium oxide, sodium sulfite and sodium pyrosulfite.

[0021] Preferably, the zinc sulfide mineral activator is copper sulfate;

[0022] And / or, the iron sulfide mineral activator is at least one of sulfuric acid, ferrous sulfate, and an organic acid;

[0023] And / or, the foaming agent is No. 2 oil and / or methyl isobutyl carbinol.

[0024] Preferably, the collector is one of a black medicine collector, an ester collector, and an EF collector, preferably an EF collector.

[0025] Preferably, the EF collector is composed of catalytic cracking clarified oil and a thiocarbamate agent or / and a thiophosphate agent.

[0026] Preferably, the EF collector contains 5-15% catalytic cracking clarified oil, 0-85% thiocarbamate agents, and 0-85% thiophosphate agents.

[0027] Preferably, based on the dry weight of the feed mineral, in the roughing operation of the copper and / or lead flotation, the dosage of zinc sulfide and iron sulfide mineral inhibitors is 1000-3000 g / t, the dosage of copper and / or lead collector is 10-40 g / t, and the dosage of frother is 10-30 g / t.

[0028] Preferably, based on the dry weight of the feed mineral, in the roughing operation of the zinc flotation, the amount of the iron sulfide mineral depressant is 1000-3000 g / t, the amount of the zinc sulfide mineral activator is 100-400 g / t, the amount of the zinc collector is 30-60 g / t, and the amount of the frother is 10-30 g / t.

[0029] Preferably, based on the dry weight of the feed mineral, in the roughing operation of the sulfur flotation, the amount of the iron sulfide mineral activator is 1000-5000 g / t, the amount of the iron sulfide mineral collector is 20-80 g / t, and the amount of the frother is 10-40 g / t.

[0030] In the present invention, the process of copper and / or lead flotation is one stage of rough scavenging, two stages of scavenging and three stages of concentrating; the process of zinc flotation is one stage of rough scavenging, two stages of scavenging and three stages of concentrating; the process of sulfur flotation is one stage of rough scavenging, one stage of scavenging and two stages of concentrating.

[0031] In the present invention, after the final tailings are thickened, the thickener underflow is discharged into the tailings pond or other treatment.

[0032] The technical solution of the present invention has the following advantages:

[0033] 1. A flotation process for directly recycling tailings water of copper, lead and zinc polymetallic sulfide ore, comprising: grinding: grinding the polymetallic sulfide ore and adding a masking agent to obtain a flotation pulp; copper or / and lead flotation: adding zinc sulfide and iron sulfide mineral inhibitors, copper or / and lead collectors, and frothers to the flotation pulp for flotation treatment to obtain copper or / and lead concentrate and tailings; zinc flotation: adding iron sulfide mineral inhibitors, zinc sulfide to the copper or / and lead flotation tailings. Mineral activator, zinc collector, and frother are used for flotation treatment to obtain zinc concentrate and zinc tailings; sulfur flotation: add iron sulfide mineral activator, iron sulfide mineral collector, and frother to zinc tailings for flotation treatment to obtain sulfur concentrate and final tailings; tailings treatment: after the final tailings are thickened, the overflow water is directly returned to the grinding for use; wherein the copper and / or lead collector, zinc collector, and iron sulfide mineral collector are the same and non-xanthate collectors. At present, the traditional idea in the field of mineral processing technology is to use different collectors for different minerals, but there is a problem that the return water is difficult to reuse directly. In the face of this problem, the present invention uses the same collector to collect copper (lead) sulfide, zinc sulfide, and iron sulfide minerals, effectively avoiding the negative impact caused by different collectors returning to the previous operation with the return water. At the same time, a masking agent is used to eliminate the activation effect of activated ions (copper, iron, etc.) in the return water on zinc sulfide and iron sulfide minerals, avoiding the adverse effects of zinc sulfide and iron sulfide that are difficult to suppress in the copper (lead) flotation stage, and combining different inhibitors or activators in different mineral processing stages. That is, the present invention achieves the purpose of direct reuse of polymetallic mineral processing water through the synergistic cooperation between multiple means, avoids stage return water or return water treatment and other means, and reduces infrastructure investment or plant operation costs.

[0034] 2. In the flotation process of the present invention, the whole process collector can be selected from black medicine, ester medicine, EF collector, etc. Among them, the black medicine and ester medicine have relatively poor collection ability for zinc sulfide minerals and iron sulfide minerals (especially iron sulfide minerals), and the effect is obviously not as good as the EF collector. Therefore, the present invention adopts the EF collector composed of catalytic cracking clarified oil and thiocarbamate medicine or / and thiophosphate medicine for whole process collection. The function of this collector is that it can selectively collect copper, lead, zinc and sulfur minerals under the action of different targeted adjusting agents. DETAILED DESCRIPTION

[0035] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0036] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0037] Example 1

[0038] A certain lead-zinc mine contains 1.2% lead, 3.4% zinc and 8.3% sulfur. The main lead mineral is galena, the main zinc mineral is sphalerite, and the sulfur mineral is pyrite.

[0039] This embodiment provides a flotation process for directly recycling the tailings water of the polymetallic sulfide ore, and the specific steps are as follows:

[0040] (1) Grinding: Grinding the lead-zinc ore to prepare flotation pulp, adding 50 g / t of sodium sulfide (the dosage is the weight of the reagent used per ton of dry ore, the same below) and 50 g / t of sodium humate during grinding to obtain a flotation pulp with an ore particle size of -0.074 mm accounting for 75%, and a mass percentage concentration of the flotation pulp of 32%. The water used for grinding is the overflow return water obtained after the tailings obtained by this process are concentrated by sedimentation in a concentrator;

[0041] (2) Lead flotation: The flotation pulp obtained in step (1) is treated by a flotation process of one-stage roughing, two-stage scavenging and three-stage concentrating. In the roughing, 1000 g / t of zinc sulfate, 500 g / t of sodium pyrosulfite, 30 g / t of EF collector and 25 g / t of No. 2 oil are added. In the first concentrating, an appropriate amount of inhibitor (specifically 400 g / t of zinc sulfate + 200 g / t of sodium pyrosulfite) is added. The amount of subsequent concentrating is halved. In the first scavenging, an appropriate amount of EF collector (specifically 15 g / t) is added. The amount of subsequent scavenging is halved to obtain lead concentrate and lead tailings. The lead tailings enter the zinc flotation operation. Among them, the EF collector is a combined collector formed by N-allyl-O-isobutyl-thiocarbamate accounting for 80%, dimethyl phenyl sodium dithiophosphate accounting for 10%, and catalytic cracking clarified oil accounting for 10%. The same below;

[0042] (3) Zinc flotation: The lead tailings obtained in step (2) are treated by a flotation process of one-stage roughing, two-stage scavenging and three-stage cleaning. 1000 g / t of calcium oxide, 500 g / t of sodium pyrosulfite, 200 g / t of copper sulfate, 40 g / t of EF collector and 20 g / t of No. 2 oil are added in the roughing. An appropriate amount of inhibitor (specifically 200 g / t of calcium oxide + 100 g / t of sodium pyrosulfite) is added in the first cleaning, and the amount used in subsequent cleaning is halved. An appropriate amount of EF collector (specifically 15 g / t) is added in the first cleaning, and the amount used in subsequent cleaning is halved to obtain zinc concentrate and zinc tailings. The zinc tailings enter the sulfur flotation operation;

[0043] (4) Sulfur flotation: The zinc tailings obtained in step (3) are treated by a flotation process of one stage roughing, one stage scavenging and two stages concentrating. In the roughing, 2000 g / t of sulfuric acid, 60 g / t of EF collector and 40 g / t of No. 2 oil are added. In the concentrating, blank concentrating is used. In the scavenging, an appropriate amount (specifically 30 g / t) of EF collector is added to obtain sulfur concentrate and final tailings. After the final tailings are settled and concentrated by a concentrator, the overflow water is directly returned to the grinding for use. Through the above process, a lead concentrate with a lead grade of 61% and a recovery rate of 89.24% can be obtained, and the zinc content of the lead concentrate is 4.1%; a zinc concentrate with a zinc grade of 50.23% and a zinc recovery rate of 89.78% can be obtained. At the same time, a concentrate with a sulfur grade of 46.67% can be obtained.

[0044] In this embodiment, the following control group was also established:

[0045] Control group 1 replaced the collector in zinc flotation and sulfur flotation operations with the traditional agent butyrate xanthate, while the collector in lead flotation operations remained unchanged, and the return water was directly reused. At the same time, the dosage of inhibitors in lead and zinc flotation operations was increased by 50%. The grade of the lead concentrate obtained was only 50%, and the zinc content of the lead concentrate reached 10.23%.

[0046] In control group 2, the collector used in the whole process remains unchanged, that is, EF collector, but no masking agent is added in the grinding stage. The lead concentrate grade obtained is 56%, and the zinc content of the lead concentrate is 8.7%.

[0047] The schemes of control groups 1 and 2 above cause a large amount of zinc minerals to enter the lead concentrate, thereby affecting the grade of the lead concentrate and causing a relatively serious loss of zinc metal.

[0048] Example 2

[0049] The difference between this embodiment and embodiment 1 is that No. 25 black medicine is used as a collector in the whole process, and other conditions are the same as those in embodiment 1. The lead concentrate obtained in this embodiment has a grade of 60%, and the lead concentrate contains 4.2% zinc, and a zinc concentrate with a zinc grade of 50.11% and a zinc recovery rate of 87.45% can be obtained.

[0050] Example 3

[0051] The difference between this embodiment and embodiment 1 is that ethionamide is used as a collector in the whole process, and other conditions are the same as those in embodiment 1. The lead concentrate obtained in this embodiment has a grade of 58%, and the lead concentrate contains 6.8% zinc, and a zinc concentrate with a zinc grade of 50.23% and a zinc recovery rate of 87.78% can be obtained.

[0052] Example 4

[0053] A copper-zinc mine contains 0.45% copper, 3.82% zinc and 10.23% sulfur. The main copper mineral is chalcopyrite, the main zinc mineral is sphalerite, and the sulfur mineral is pyrite.

[0054] This embodiment provides a flotation process for directly recycling the tailings water of the polymetallic sulfide ore, and the specific steps are as follows:

[0055] (1) Grinding: Grinding the copper-zinc ore to prepare flotation pulp, adding 80 g / t of sodium sulfide (the dosage is the weight of the reagent used per ton of dry ore, the same below) and 40 g / t of sodium humate during grinding to obtain a flotation pulp with an ore particle size of -0.074 mm accounting for 75%, and a mass percentage concentration of the flotation pulp of 33%. The water used for grinding is the overflow return water obtained after the tailings obtained in this process are concentrated by sedimentation in a concentrator;

[0056] (2) Copper flotation: The flotation pulp obtained in step (1) is treated by a flotation process of one-stage roughing, two-stage scavenging and three-stage concentrating. In the roughing, 1000 g / t of zinc sulfate, 500 g / t of sodium pyrosulfite, 20 g / t of EF collector and 20 g / t of No. 2 oil are added. In the first concentrating, an appropriate amount of inhibitor (specifically 400 g / t of zinc sulfate + 200 g / t of sodium pyrosulfite) is added. The amount of subsequent concentrating is halved. In the first scavenging, an appropriate amount of EF collector (specifically 10 g / t) is added. The amount of subsequent scavenging is halved to obtain copper concentrate and copper tailings. The copper tailings enter the zinc flotation operation. Among them, the EF collector is a combined collector formed by stirring 45% of ethylthiocarbamate, 45% of sodium diisopropyl dithiophosphate and 10% of catalytic cracking clarified oil, the same below;

[0057] (3) Zinc flotation: The copper tailings obtained in step (2) are treated by a flotation process of one-stage roughing, two-stage scavenging and three-stage cleaning. 1200 g / t of calcium oxide, 600 g / t of sodium pyrosulfite, 200 g / t of copper sulfate, 40 g / t of EF collector and 20 g / t of No. 2 oil are added in the roughing. An appropriate amount of inhibitor (specifically 400 g / t of calcium oxide + 200 g / t of sodium pyrosulfite) is added in the first cleaning, and the amount used in subsequent cleaning is halved. An appropriate amount of EF collector (specifically 20 g / t) is added in the first cleaning, and the amount used in subsequent cleaning is halved to obtain zinc concentrate and zinc tailings. The zinc tailings enter the sulfur flotation operation;

[0058] (4) Sulfur flotation: The zinc tailings obtained in step (3) are treated by a flotation process of one stage roughing, one stage scavenging and two stages concentrating. In the roughing, 2000 g / t of sulfuric acid, 60 g / t of EF collector and 40 g / t of No. 2 oil are added. In the concentrating, blank concentrating is used. In the scavenging, an appropriate amount (specifically 25 g / t) of EF collector is added to obtain sulfur concentrate and final tailings. After the final tailings are settled and concentrated by a concentrator, the overflow water is directly returned to the grinding for use. Through the above process, a copper concentrate with a copper grade of 23% and a recovery rate of 89.56% can be obtained, and the zinc content of the copper concentrate is 4.3%; a zinc concentrate with a zinc grade of 50.56% and a zinc recovery rate of 90.23% can be obtained. At the same time, a sulfur concentrate with a sulfur grade of 47.54% can be obtained.

[0059] In this embodiment, the following control group was also established:

[0060] Control group 1 replaced the collector in zinc flotation and sulfur flotation operations with the traditional agent butyrate xanthate, while the collector in copper flotation operations remained unchanged, and the return water was directly reused. At the same time, the amount of inhibitor in copper and zinc flotation operations was increased by 50%. The grade of the copper concentrate obtained was only 16%, and the zinc content of the copper concentrate reached 11.67%.

[0061] In control group 2, the collector used in the whole process remains unchanged, that is, EF collector, but no masking agent is added in the grinding stage. The copper concentrate grade obtained is 18%, and the zinc content of the copper concentrate is 8.2%.

[0062] The solutions of the above control groups 1 and 2 cause a large amount of zinc minerals to enter the copper concentrate, thereby affecting the grade of the copper concentrate and causing a relatively serious loss of zinc metal.

[0063] Example 5

[0064] The difference between this embodiment and embodiment 4 is that No. 25 black medicine is used as a collector in the whole process, and other conditions are the same as those in embodiment 4. The copper concentrate obtained in this embodiment has a grade of 21%, and the copper concentrate contains 4.5% zinc, and a zinc concentrate with a zinc grade of 50.34% and a zinc recovery rate of 88.12% can be obtained.

[0065] Example 6

[0066] The difference between this embodiment and embodiment 4 is that ethiocarbamate is used as a collector in the whole process, and other conditions are the same as those in embodiment 4. The copper concentrate obtained in this embodiment has a grade of 20.5%, and the copper concentrate contains 5.5% zinc, and a zinc concentrate with a zinc grade of 50.45% and a zinc recovery rate of 88.78% can be obtained.

[0067] Example 7

[0068] A copper-zinc mine contains 0.45% copper, 3.82% zinc and 10.23% sulfur. The main copper mineral is chalcopyrite, the main zinc mineral is sphalerite, and the sulfur mineral is pyrite.

[0069] This embodiment provides a flotation process for directly recycling the tailings water of the polymetallic sulfide ore, and the specific steps are as follows:

[0070] (1) Grinding: Grinding the copper-zinc ore to prepare flotation pulp, adding 80 g / t of sodium sulfide (the dosage is the weight of the reagent used per ton of dry ore, the same below) and 40 g / t of sodium humate during grinding to obtain a flotation pulp with an ore particle size of -0.074 mm accounting for 70%, and a mass percentage concentration of the flotation pulp of 40%. The water used for grinding is the overflow return water obtained after the tailings obtained in this process are concentrated by sedimentation in a concentrator;

[0071] (2) Copper flotation: The flotation pulp obtained in step (1) is treated by a flotation process of one-stage roughing, two-stage scavenging and three-stage concentrating. In the roughing, 2000g / t of zinc sulfate, 1000g / t of sodium pyrosulfite, 40g / t of EF collector and 10g / t of No. 2 oil are added. In the first concentrating, an appropriate amount of inhibitor (specifically 200g / t of zinc sulfate + 100g / t of sodium pyrosulfite) is added. The amount of subsequent concentrating is halved. In the first scavenging, an appropriate amount of EF collector (specifically 10g / t) is added. The amount of subsequent scavenging is halved to obtain copper concentrate and copper tailings. The copper tailings enter the zinc flotation operation. Among them, the EF collector is a combined collector formed by stirring with 10% of ethylthiocarbamate, 85% of sodium diisopropyl dithiophosphate and 5% of catalytic cracking clarified oil, the same below;

[0072] (3) Zinc flotation: The copper tailings obtained in step (2) are treated by a flotation process of one-stage roughing, two-stage scavenging and three-stage cleaning. 700 g / t of calcium oxide, 300 g / t of sodium pyrosulfite, 400 g / t of copper sulfate, 30 g / t of EF collector and 30 g / t of No. 2 oil are added in the roughing. An appropriate amount of inhibitor (specifically 400 g / t of calcium oxide + 200 g / t of sodium pyrosulfite) is added in the first cleaning, and the amount used in subsequent cleaning is halved. An appropriate amount of EF collector (specifically 20 g / t) is added in the first cleaning, and the amount used in subsequent cleaning is halved to obtain zinc concentrate and zinc tailings. The zinc tailings enter the sulfur flotation operation;

[0073] (4) Sulfur flotation: The zinc tailings obtained in step (3) are treated by a flotation process of one stage roughing, one stage scavenging and two stages concentrating. In the roughing, 5000 g / t of sulfuric acid, 20 g / t of EF collector and 10 g / t of No. 2 oil are added. In the concentrating, blank concentrating is used. In the scavenging, an appropriate amount (specifically 25 g / t) of EF collector is added to obtain sulfur concentrate and final tailings. After the final tailings are settled and concentrated by a concentrator, the overflow water is directly returned to the grinding for use. Through the above process, a copper concentrate with a copper grade of 22% and a recovery rate of 89.73% can be obtained, and the zinc content of the copper concentrate is 4.2%; a zinc concentrate with a zinc grade of 50.38% and a zinc recovery rate of 90.34% can be obtained. At the same time, a sulfur concentrate with a sulfur grade of 47.51% can be obtained.

[0074] In this embodiment, the following control group was also established:

[0075] Control group 1 replaced the collector in zinc flotation and sulfur flotation operations with the traditional agent butyrate xanthate, while the collector in copper flotation operations remained unchanged, and the return water was directly reused. At the same time, the dosage of inhibitors in copper and zinc flotation operations was increased by 50%. The grade of the copper concentrate obtained was only 15%, and the zinc content of the copper concentrate reached 12.1%.

[0076] In control group 2, the collector used in the whole process remains unchanged, that is, EF collector, but no masking agent is added in the grinding stage. The copper concentrate grade obtained is 17%, and the zinc content of the copper concentrate is 8.5%.

[0077] The solutions of the above control groups 1 and 2 cause a large amount of zinc minerals to enter the copper concentrate, thereby affecting the grade of the copper concentrate and causing a serious loss of zinc metal.

[0078] Example 8

[0079] The difference between this embodiment and embodiment 7 is that No. 25 black medicine is used as a collector in the whole process, and other conditions are the same as those in embodiment 7. The copper concentrate obtained in this embodiment has a grade of 20.6%, and the copper concentrate contains 4.4% zinc, and a zinc concentrate with a zinc grade of 50.29% and a zinc recovery rate of 88.15% can be obtained.

[0080] Example 9

[0081] The difference between this embodiment and embodiment 7 is that ethiocarbamate is used as a collector in the whole process, and other conditions are the same as those in embodiment 7. The copper concentrate obtained in this embodiment has a grade of 20.3%, and the copper concentrate contains 6.1% zinc, and a zinc concentrate with a zinc grade of 50.43% and a zinc recovery rate of 88.56% can be obtained.

[0082] Example 10

[0083] The difference between this embodiment and embodiment 7 is that sodium diisopropyl dithiophosphate is used as a collector in the whole process, and other conditions are the same as those in embodiment 7. The copper concentrate obtained in this embodiment has a grade of 19.8%, and the copper concentrate contains 6.7% zinc, and a zinc concentrate with a zinc grade of 50.46% and a zinc recovery rate of 88.44% can be obtained.

[0084] Embodiment 11

[0085] The difference between this embodiment and embodiment 7 is that the whole process adopts EF collector (85% of ethylthiocarbamate and 15% of catalytic cracking clarified oil), and other conditions are the same as those of embodiment 7. The copper concentrate obtained in this embodiment has a grade of 21.3%, and the copper concentrate contains 4.5% zinc, and a zinc concentrate with a zinc grade of 50.30% and a zinc recovery rate of 90.18% can be obtained.

[0086] Example 12

[0087] The difference between this embodiment and embodiment 7 is that the whole process adopts EF collector (sodium diisopropyl dithiophosphate accounts for 85%, catalytic cracking clarified oil accounts for 15%), and other conditions are the same as those of embodiment 7. The copper concentrate obtained in this embodiment has a grade of 21.1%, and the copper concentrate contains 4.4% zinc, and a zinc concentrate with a zinc grade of 50.26% and a zinc recovery rate of 90.06% can be obtained.

[0088] Example 13

[0089] A copper-zinc mine contains 0.45% copper, 3.82% zinc and 10.23% sulfur. The main copper mineral is chalcopyrite, the main zinc mineral is sphalerite, and the sulfur mineral is pyrite.

[0090] This embodiment provides a flotation process for directly recycling the tailings water of the polymetallic sulfide ore, and the specific steps are as follows:

[0091] (1) Grinding: Grinding the above copper-zinc ore to prepare flotation pulp, adding 250 g / t of sodium dimethyldithiocarbamate (the dosage is the weight of the reagent used per ton of dry ore, the same below) and 250 g / t of sodium trithiocarbonate during grinding to obtain a flotation pulp with an ore particle size of -0.074 mm accounting for 80%, and a mass percentage concentration of the flotation pulp of 30%. The water used for grinding is the overflow return water obtained after the tailings obtained in this process are concentrated by sedimentation in a concentrator;

[0092] (2) Copper flotation: The flotation pulp obtained in step (1) is treated by a flotation process of one-stage roughing, two-stage scavenging and three-stage concentrating. In the roughing, 700 g / t of sodium sulfate, 300 g / t of sodium sulfite, 10 g / t of EF collector and 30 g / t of methyl isobutyl carbinol are added. In the first concentrating, an appropriate amount of inhibitor (specifically 400 g / t of zinc sulfate + 200 g / t of sodium pyrosulfite) is added. The amount of subsequent concentrating is halved. In the first scavenging, an appropriate amount of EF collector (specifically 10 g / t) is added. The amount of subsequent scavenging is halved to obtain copper concentrate and copper tailings. The copper tailings enter the zinc flotation operation. Among them, the EF collector is a combined collector formed by stirring with 10% of ethylthiocarbamate, 85% of sodium diisopropyl dithiophosphate and 10% of catalytic cracking clarified oil, the same below;

[0093] (3) Zinc flotation: The copper tailings obtained in step (2) are treated by a flotation process of one-stage roughing, two-stage scavenging and three-stage cleaning. 2000 g / t of calcium oxide, 1000 g / t of sodium pyrosulfite, 100 g / t of copper sulfate, 60 g / t of EF collector and 10 g / t of methyl isobutyl carbinol are added in the roughing. An appropriate amount of inhibitor (specifically 200 g / t of calcium oxide + 100 g / t of sodium pyrosulfite) is added in the first cleaning, and the amount used in subsequent cleaning is halved. An appropriate amount of EF collector (specifically 20 g / t) is added in the first cleaning, and the amount used in subsequent cleaning is halved to obtain zinc concentrate and zinc tailings. The zinc tailings enter the sulfur flotation operation.

[0094] (4) Sulfur flotation: The zinc tailings obtained in step (3) are treated by a flotation process of one stage roughing, one stage scavenging and two stages concentrating. In the roughing, 1000 g / t of sulfuric acid, 80 g / t of EF collector and 40 g / t of methyl isobutyl carbinol are added. In the concentrating, blank concentrating is used. In the scavenging, an appropriate amount (specifically 25 g / t) of EF collector is added to obtain sulfur concentrate and final tailings. After the final tailings are settled and concentrated by a concentrator, the overflow water is directly returned to the grinding for use. Through the above process, a copper concentrate with a copper grade of 23% and a recovery rate of 89.48% can be obtained, and the zinc content of the copper concentrate is 4.4%; a zinc concentrate with a zinc grade of 50.47% and a zinc recovery rate of 90.18% can be obtained. At the same time, a sulfur concentrate with a sulfur grade of 47.48% can be obtained.

[0095] In this embodiment, the following control group was also established:

[0096] Control group 1 replaced the collector in zinc flotation and sulfur flotation operations with the traditional agent butyrate xanthate, while the collector in copper flotation operations remained unchanged, and the return water was directly reused. At the same time, the amount of inhibitor in copper and zinc flotation operations was increased by 50%. The grade of the copper concentrate obtained was only 17%, and the zinc content of the copper concentrate reached 11.42%.

[0097] In control group 2, the collector used in the whole process remains unchanged, that is, EF collector, but no masking agent is added in the grinding stage. The copper concentrate grade obtained is 16%, and the zinc content of the copper concentrate is 8.9%.

[0098] The solutions of the above control groups 1 and 2 cause a large amount of zinc minerals to enter the copper concentrate, thereby affecting the grade of the copper concentrate and causing a relatively serious loss of zinc metal.

[0099] Embodiment 14

[0100] The difference between this embodiment and embodiment 13 is that No. 25 black medicine is used as a collector in the whole process, and other conditions are the same as those in embodiment 13. The copper concentrate obtained in this embodiment has a grade of 21%, and the copper concentrate contains 4.6% zinc, and a zinc concentrate with a zinc grade of 50.31% and a zinc recovery rate of 88.06% can be obtained.

[0101] Embodiment 15

[0102] The difference between this embodiment and embodiment 13 is that ethiocarbamate is used as a collector in the whole process, and other conditions are the same as those in embodiment 13. The copper concentrate obtained in this embodiment has a grade of 20.1%, and the copper concentrate contains 5.8% zinc, and a zinc concentrate with a zinc grade of 50.37% and a zinc recovery rate of 88.74% can be obtained.

[0103] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A flotation process for direct reuse of polymetallic sulfide ore tailings water, characterized in that: include: Grinding: Grind the polymetallic sulfide ore and add masking agent to obtain flotation pulp; Copper or / and lead flotation: adding zinc sulfide and iron sulfide mineral inhibitors, copper or / and lead collectors, and frothers to the flotation pulp for flotation treatment to obtain copper or / and lead concentrates and tailings; Zinc flotation: adding iron sulfide mineral inhibitor, zinc sulfide mineral activator, zinc collector and frother to copper and / or lead flotation tailings for flotation treatment to obtain zinc concentrate and zinc tailings; Sulfur flotation: Add iron sulfide mineral activator, iron sulfide mineral collector and frother to zinc tailings for flotation treatment to obtain sulfur concentrate and final tailings; Tailings treatment: After the final tailings are thickened, the overflow water is directly returned to the grinding mill for use; The copper and / or lead collector, the zinc collector and the iron sulfide mineral collector are the same and non-xanthate collectors.

2. The flotation process according to claim 1, characterized in that: The polymetallic sulfide ore is at least one of lead-zinc sulfide ore, copper-zinc sulfide ore, and copper-lead-zinc sulfide ore; And / or, the grinding process is performed to a particle size of -0.074 mm, accounting for 70-80%; And / or, the mass percentage concentration of the flotation pulp is 30-40%; And / or, the masking agent is at least one of sodium sulfide, sodium humate, sodium dimethyldithiocarbamate, and sodium trithiocarbonate; And / or, based on the dry weight of the feed mineral, the amount of the masking agent is 100-500 g / t.

3. The flotation process according to claim 1 or 2, characterized in that: The zinc sulfide and iron sulfide mineral inhibitors are at least two of zinc sulfate, sodium sulfite, sodium pyrosulfite, and sodium sulfate; And / or, the iron sulfide mineral inhibitor is at least one of calcium oxide, sodium sulfite and sodium pyrosulfite.

4. The flotation process according to any one of claims 1 to 3, characterized in that: The zinc sulfide mineral activator is copper sulfate; And / or, the iron sulfide mineral activator is at least one of sulfuric acid, ferrous sulfate, and an organic acid; And / or, the foaming agent is No. 2 oil and / or methyl isobutyl carbinol.

5. The flotation process according to any one of claims 1 to 4, characterized in that: The collector is one of a black medicine collector, an ester collector, and an EF collector, preferably an EF collector.

6. The flotation process according to any one of claim 5, characterized in that: The EF collector is composed of catalytic cracking clarified oil and a thiocarbamate agent or / and a thiophosphate agent.

7. The flotation process according to any one of claim 6, characterized in that: In the EF collector, catalytic cracking clarified oil accounts for 5-15%, thiocarbamate agents account for 0-85%, and thiophosphate agents account for 0-85%.

8. The flotation process according to any one of claims 1 to 7, characterized in that: Based on the dry weight of the feed minerals, in the roughing operation of the copper and / or lead flotation, the dosage of zinc sulfide and iron sulfide mineral inhibitors is 1000-3000 g / t, the dosage of copper and / or lead collector is 10-40 g / t, and the dosage of frother is 10-30 g / t.

9. The flotation process according to any one of claims 1 to 8, characterized in that: Based on the dry weight of the feed mineral, in the roughing operation of the zinc flotation, the amount of the iron sulfide mineral depressant is 1000-3000 g / t, the amount of the zinc sulfide mineral activator is 100-400 g / t, the amount of the zinc collector is 30-60 g / t, and the amount of the frother is 10-30 g / t.

10. The flotation process according to any one of claims 1 to 9, characterized in that: Based on the dry weight of the feed mineral, in the roughing operation of the sulfur flotation, the amount of the iron sulfide mineral activator is 1000-5000 g / t, the amount of the iron sulfide mineral collector is 20-80 g / t, and the amount of the frother is 10-40 g / t.

Citation Information

Cited By

  • Comprehensive utilization and recovery process for polymetallic ore

    CN119634042A

  • Flotation process for pressurizing and stirring sulphide ore

    CN119657345A