Antifouling coating process for PRTV insulator
By optimizing cleaning, antifouling coating preparation, electric field pressure immersion and curing processes, the problems of poor cleaning effect, insufficient coating formula and inaccurate process in the existing PRTV insulator antifouling coating process are solved, and more efficient insulators are achieved Anti-fouling performance and more stable coating quality improve the safe and stable operation of the power system.
Patent Information
- Application Number
- CN202411253942.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
AI Technical Summary
The existing PRTV insulator anti-fouling coating process has poor results during the cleaning process, there are shortcomings in the anti-fouling coating formulation and preparation process, the electric field pressure immersion control is not accurate, the curing process efficiency and stability need to be improved, which affects the performance and reliability of the insulator.
Optimize the cleaning process, use mechanical grinding and plasma surface treatment to remove surface residues and pollution; reasonably prepare anti-fouling coatings, adopt high-speed stirring and staged temperature control technology; use electric field pressure immersion system and ultrasonic assisted immersion, and combine with intelligent control system to accurately control Process parameters; adopt a staged temperature controlled drying and curing process to ensure efficient curing of the coating.
It significantly improves the cleanliness of the insulator surface and the adhesion of the anti-fouling coating, enhances anti-fouling, water-repellent, anti-fouling flash and thermal stability, extends the service life of the coating, and improves the operating reliability and safety of the insulator. sex.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of insulators, and in particular to an anti-fouling coating process for PRTV insulators. Background Art
[0002] With the continuous development of power systems, insulators, as an important component of power transmission and transformation equipment, have a performance that is directly related to the safe and stable operation of power systems. In outdoor environments, insulators are easily affected by various pollutants, such as dust, oil, salt spray, etc. These pollutants will reduce the insulation performance of insulators and increase the probability of flashover accidents.
[0003] Traditional anti-pollution measures for insulators mainly include regular cleaning and silicone oil application, but these methods have problems such as high maintenance costs and short-term effects. In recent years, PRTV (Persistent In-Place Anti-pollution Flashover Composite Coating) insulator anti-pollution coating technology has been widely used. PRTV coating has excellent anti-pollution performance, hydrophobicity, anti-pollution flashover performance and thermal stability, which can effectively improve the operating reliability of insulators.
[0004] However, the existing PRTV insulator anti-fouling coating process still has some shortcomings. For example, during the cleaning process, the cleaning effect is not ideal, and residual impurities may affect the adhesion of the coating; the formula and preparation process of the anti-fouling coating need to be further optimized to improve its performance; during the electric field pressure impregnation process, the control of the impregnation effect and process parameters is not accurate enough; the curing process also needs to be more efficient and stable to ensure the quality of the coating. For this reason, the present invention proposes an improved PRTV insulator anti-fouling coating process. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a PRTV insulator anti-fouling coating process, which improves the performance and quality of the PRTV insulator anti-fouling coating by optimizing and innovating the cleaning, anti-fouling coating preparation, electric field pressure impregnation and curing processes, thereby providing better protection for the safe and stable operation of the power system.
[0006] The present invention provides the following technical solution: a PRTV insulator anti-fouling coating process, comprising the following steps:
[0007] S1. Cleaning: Place the insulator in an automatic cleaning platform in a 15-20m3 solvent tank. The solvent is a cleaning liquid. The cleaning steps include preheating, soaking, rinsing, spraying, dehydration and drying to complete the cleaning of the insulator.
[0008] S2. Preparation of antifouling coating: PRTV antifouling coating is composed of the following raw materials in parts by weight: 30-55 parts of antifouling functional material, 40-70 parts of silicone rubber, 2-10 parts of coupling agent, and 5-20 parts of curing agent; the antifouling functional material and silicone rubber are added to a high-speed mixer in proportion, heated to 80°C and stirred for 10 minutes, and then cooled to 60°C; in the above blending system, after adding the coupling agent, continue stirring at 60°C for 10 minutes; finally, add the curing agent, stir for 10-30 minutes, and then discharge the material;
[0009] S3. Electric field pressure impregnation: put the insulator into the electric field pressure impregnation system, inject the anti-fouling coating and then evacuate. After two times of pressure impregnation, the anti-fouling coating on the surface of the insulator can be impregnated. The injection pressure is 0.1-0.3MPa and the vacuum pressure is 0.1MPa.
[0010] S4, curing: After taking the insulator out of the electric field pressure impregnation system, place it in an oven to cure the anti-fouling coating, and evenly scrape off the outside of the insulator by mechanical demoulding;
[0011] S5. Use the voltage step method to test the anti-pollution performance, hydrophobicity, anti-pollution flashover performance and thermal stability of insulators.
[0012] Preferably, the insulator is first mechanically polished to remove surface residues and loose impurities before cleaning, and the insulator is first subjected to plasma surface treatment before mechanical polishing, using high-energy active particles of the plasma to bombard and activate the insulator surface, thereby increasing the surface energy and roughness, enhancing the adhesion of subsequent cleaning fluids and anti-fouling coatings, and removing surface organic pollutants and oxide layers.
[0013] Preferably, the cleaning solution in S1 is composed of the following components in mass fractions: 50-50% acetone, 40-45% ethanol, 1.5-3% dimethyl carbonate, 1.5-2.5% pyridine, and the remainder is purified water.
[0014] Preferably, the antifouling functional material in S2 is composed of the following materials in weight percentage: 8-12% water repellent, 0.8-2% silicone modified microspheres, 0.1-0.5% metal nanoparticles, 8-12% nano-TiO2, 0.5-1% ultraviolet absorber, and the balance is deionized water.
[0015] Preferably, in S3, an ultrasonic assisted impregnation function is added to the electric field pressure impregnation system, and the cavitation effect and mechanical action of ultrasound are used to promote the penetration and filling of the anti-fouling coating on the surface of the insulator. At the same time, an intelligent control system is used to monitor parameters such as pressure, temperature and time during the impregnation process in real time, and automatically adjust the process parameters according to actual conditions.
[0016] Preferably, during the curing process in S4, a staged temperature-controlled drying and curing process is adopted, and the uniform film layer formed by dipping is first kept at a temperature of 80-90° C. for 8 minutes, and then kept at a temperature of 170-190° C. for another 20 minutes.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) Mechanical grinding and plasma surface treatment are performed before cleaning to further remove surface residues, loose impurities, organic pollutants and oxide layers, thereby improving the roughness and adhesion of the insulator surface and ensuring a more thorough cleaning effect. A multi-stage cleaning process is adopted, including preheating, wetting, rinsing, spraying, dehydration and drying, which can completely remove various pollutants on the insulator surface and provide a clean surface for the subsequent adhesion of the anti-fouling coating;
[0019] (2) The antifouling coating has a reasonable formula, which gives the coating excellent antifouling performance, hydrophobicity, anti-fouling flashover performance and thermal stability. The coating preparation process adopts high-speed stirring and staged temperature control to ensure that all components are fully mixed, which improves the performance stability of the coating. The addition of ultraviolet absorbers can effectively reduce the damage of ultraviolet rays to the antifouling coating and extend the service life of the coating;
[0020] (3) The electric field pressure impregnation system is used, and the injection pressure and vacuum pressure are precisely controlled, so that the anti-fouling coating can fully fill the fine pores on the surface of the insulator, improve the density and adhesion of the coating, and add the ultrasonic assisted impregnation function. The cavitation effect and mechanical action of the ultrasonic wave are used to promote the penetration and filling of the anti-fouling coating on the surface of the insulator, further improving the impregnation effect;
[0021] (4) The staged temperature-controlled drying and curing process enables the antifouling coating to be gradually cured at different temperatures, thereby improving the curing quality and performance of the coating. The coating is initially cured at a lower temperature and then deeply cured at a higher temperature, thereby avoiding the adverse effects of sudden temperature changes on the coating and improving the curing efficiency. DETAILED DESCRIPTION
[0022] In order to make the objectives, technical solutions and advantages of the embodiments of the present disclosure clearer, the technical solutions of the embodiments of the present disclosure are clearly and completely described. In order to keep the following description of the embodiments of the present disclosure clear and concise, the present disclosure omits detailed descriptions of known functions and known components to avoid unnecessary confusion of the concepts of the present invention.
[0023] 1. Cleaning
[0024] 1. First, place the insulator that needs to be treated with anti-fouling coating at a distance of 15 to 20 meters. 3In the automatic cleaning platform in the solvent tank, the cleaning solution is composed of 50% acetone, 40-45% ethanol, 1.5-3% dimethyl carbonate, 1.5-2.5% pyridine and the balance is pure water.
[0025] 2. Preheating section: Use appropriate heating methods to gradually increase the temperature of the cleaning liquid to prepare for subsequent cleaning steps.
[0026] 3. Wetting section: Soak the insulator in cleaning liquid at a temperature of 80°C, so that the cleaning liquid can fully soak the surface of the insulator to dissolve and loosen the pollutants.
[0027] 4. Rinse section: Rinse the insulator with clean cleaning fluid to remove residual contaminants and cleaning fluid.
[0028] 5. Spraying section: Spray the insulators at a spraying pressure of 4MPa to further remove stubborn pollutants.
[0029] 6. Dehydration section: Use centrifugal or other dehydration methods to remove most of the moisture on the surface of the insulator.
[0030] 7. Drying section: Use 150°C nitrogen to blow dry the surface of the insulator to ensure that the surface of the insulator is dry and free of moisture.
[0031] 2. Preparation of antifouling coating
[0032] 1. Prepare antifouling functional materials according to weight percentage, including 8-12% of water repellent, 0.8-2% of silicone modified microspheres, 0.1-0.5% of metal nanoparticles, 8-12% of nano-TiO2, 0.5-1% of ultraviolet absorber and the balance of deionized water.
[0033] 2. Add 30-55 parts of antifouling functional material and 40-70 parts of silicone rubber into a high-speed mixer in proportion, heat to 80°C and stir for 10 minutes.
[0034] 3. Then cool down to 60°C, add 2 to 10 parts of coupling agent to the above blending system, and continue stirring at 60°C for 10 minutes.
[0035] 4. Finally, add 5 to 20 parts of curing agent and stir for 10 to 30 minutes, then discharge the material for later use.
[0036] 3. Electric field pressure impregnation
[0037] 1. Place the insulator into the electric field pressure impregnation system.
[0038] 2. After injecting the antifouling paint, the system is evacuated to a vacuum pressure of -0.1MPa.
[0039] 3. Add ultrasonic assisted impregnation function, and use the cavitation effect and mechanical action of ultrasound to promote the penetration and filling of anti-fouling coating on the surface of insulator.
[0040] 4. Perform two pressurized impregnations with an injection pressure of 0.1-0.3 MPa. At the same time, an intelligent control system is used to monitor the pressure, temperature, time and other parameters during the impregnation process in real time, and automatically adjust the process parameters according to the actual situation.
[0041] 4. Curing
[0042] 1. Take the insulator out of the electric field pressure impregnation system and place it in an oven.
[0043] 2. Use a staged temperature-controlled drying and curing process. First, stay at a temperature of 80-90°C for 8 minutes to initially cure the uniform film layer formed by dipping.
[0044] 3. Then stay at 170-190℃ for another 20 minutes for deep curing. After curing, use mechanical demoulding to evenly scrape the outside of the insulator to ensure a smooth coating surface.
[0045] 5. Performance Testing
[0046] The voltage step method is used to test the anti-pollution performance, hydrophobicity, anti-pollution flashover performance, and thermal stability of the insulators. At the same time, in order to more comprehensively evaluate the performance of the insulators, a weather resistance test is also carried out. The insulators coated with anti-pollution coatings are placed in a natural environment. After a certain period of natural aging process such as wind, sun, and rain, the performance test is carried out again.
[0047] In the process of implementing the present invention, firstly, the residue and loose impurities on the surface of the insulator are removed by mechanical grinding before cleaning, and the insulator is first subjected to plasma surface treatment before mechanical grinding, and the high-energy active particles of the plasma are used to bombard and activate the surface of the insulator, thereby increasing the surface energy and roughness, enhancing the adhesion of the subsequent cleaning liquid and anti-fouling coating, and removing the surface organic pollutants and the oxide layer.
[0048] The above embodiments are only exemplary embodiments of the present invention and are not intended to limit the present invention. The protection scope of the present invention is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.
Claims
1. A PRTV insulator anti-fouling coating process, characterized in that: The following steps are involved: S1. Cleaning: Place the insulator in an automatic cleaning platform in a 15-20m3 solvent tank. The solvent is a cleaning liquid. The cleaning steps include preheating, soaking, rinsing, spraying, dehydration and drying to complete the cleaning of the insulator. S2. Preparation of antifouling coating: PRTV antifouling coating is composed of the following raw materials in parts by weight: 30-55 parts of antifouling functional material, 40-70 parts of silicone rubber, 2-10 parts of coupling agent, and 5-20 parts of curing agent; the antifouling functional material and silicone rubber are added to a high-speed mixer in proportion, heated to 80°C and stirred for 10 minutes, and then cooled to 60°C; in the above blending system, after adding the coupling agent, continue stirring at 60°C for 10 minutes; finally, add the curing agent, stir for 10-30 minutes, and then discharge the material; S3. Electric field pressure impregnation: put the insulator into the electric field pressure impregnation system, inject the anti-fouling coating and then evacuate. After two times of pressure impregnation, the anti-fouling coating on the surface of the insulator can be impregnated. The injection pressure is 0.1-0.3MPa and the vacuum pressure is 0.1MPa. S4, curing: After taking the insulator out of the electric field pressure impregnation system, place it in an oven to cure the anti-fouling coating, and evenly scrape off the outside of the insulator by mechanical demoulding; S5. Use the voltage step method to test the anti-pollution performance, hydrophobicity, anti-pollution flashover performance and thermal stability of insulators.
2. The PRTV insulator anti-fouling coating process according to claim 1 is characterized in that: First, before cleaning, the insulators are mechanically polished to remove surface residues and loose impurities. Before mechanical polishing, the insulators are first subjected to plasma surface treatment, using high-energy active particles of the plasma to bombard and activate the insulator surface, thereby increasing the surface energy and roughness, enhancing the adhesion of subsequent cleaning fluids and anti-fouling coatings, and removing surface organic pollutants and oxide layers.
3. The PRTV insulator anti-fouling coating process according to claim 1 is characterized in that: The cleaning solution in S1 is composed of the following components in mass fractions: 50-50% acetone, 40-45% ethanol, 1.5-3% dimethyl carbonate, 1.5-2.5% pyridine, and the remainder is pure water.
4. The PRTV insulator anti-fouling coating process according to claim 3 is characterized by: The antifouling functional material in S2 is composed of the following materials in weight percentage: 8-12% of water repellent, 0.8-2% of organosilicon modified microspheres, 0.1-0.5% of metal nanoparticles, 8-12% of nano-TiO2, 0.5-1% of ultraviolet absorber, and the balance is deionized water.
5. The PRTV insulator anti-fouling coating process according to claim 3 is characterized by: In S3, an ultrasonic-assisted impregnation function is added to the electric field pressure impregnation system, using the cavitation effect and mechanical action of ultrasound to promote the penetration and filling of anti-fouling coatings on the surface of insulators. At the same time, an intelligent control system is used to monitor parameters such as pressure, temperature and time during the impregnation process in real time, and automatically adjust process parameters according to actual conditions.
6. The PRTV insulator anti-fouling coating process according to claim 1 is characterized by: During the curing process in S4, a staged temperature-controlled drying and curing process is adopted. First, the uniform film layer formed by dipping is kept at a temperature of 80-90°C for 8 minutes, and then kept at a temperature of 170-190°C for another 20 minutes.
Citation Information
Cited By
Technical method for cleaning surface of non-oriented silicon steel through plasma in laboratory
CN121519068A