Working roll shifting method for improving local high point position of strip steel
By optimizing the position and rolling model of the working roller, the cold rolling rib defects caused by local high points in the cross section of hot-rolled strip are solved, and the negative adaptability of cold-rolled intermediate rollers and the edge distance of the strip are improved, and the Production stability.
Patent Information
- Application Number
- CN202410996584.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
There are local high points in the cross-sectional profile of hot-rolled strip, which leads to rib defects and downstream production stability problems during cold rolling, affecting the lamination effect and electromagnetic performance of silicon steel.
By collaboratively optimizing the position of the working rollers, avoiding the rollers staying near the zero position, improving the local high point position of the cross-section of the strip steel, using an optimized roller model to increase the distance between the local high point and the edge of the strip steel, and improving the cold rolling middle Adaptability of roller negative trench position.
Effectively avoid the occurrence of rib defects during cold rolling, improve the adaptability of the negative trajectory position of the cold rolling intermediate roll, increase the distance between the local high point and the strip side, and reduce the rib defects in the cross-section of the cold rolling process. The occurrence of
Smart Images

Figure CN118926315A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hot rolling, and in particular to a working roll shifting method for improving the local high point position of a steel strip. Background Art
[0002] The thickness of the hot-rolled strip in the width direction is also called the cross-sectional profile of the hot-rolled strip, which directly affects the cross-sectional profile quality of the downstream process. For example, when there are local high points in the cross-sectional profile of the hot-rolled silicon steel product, cold rolling is very likely to produce rib defects, resulting in a decrease in the cold rolling yield, and ultimately affecting the silicon steel lamination effect and the electromagnetic properties of the product. In addition, when the hot-rolled cross-sectional profile is poor, it may also cause complex wave shapes in the downstream production process, affecting the stability of downstream production. In order to avoid the impact of poor cross-sectional profile quality of the strip on the downstream, the hot rolling line needs to be shut down and the working rolls replaced in advance if necessary, affecting the hot rolling stability and production efficiency. It can be seen that improving the cross-sectional profile quality of hot-rolled strip is of great significance to both hot rolling and downstream processes.
[0003] To improve the cross-sectional quality of hot-rolled strip, two main considerations are to reduce the local high point value and optimize the local high point position. When the width and thickness specifications of the strip remain unchanged in a single hot rolling plan, the position of the working rolls equipped with the CVC roll shape curve remains basically unchanged, which leads to local wear on the working roll surface at the corresponding sides of the strip, and then leads to local high points in the cross-sectional profile of the strip. For such local high points, by designing the downstream F5-F7 frames as concave rolls and adopting a reciprocating roll shifting strategy, and then cooperating with the optimized roll shifting model, the upstream F3-F4 frames of the finishing rolling also perform reciprocating roll shifting, which reduces the local high point value or avoids the occurrence of local high point defects to a certain extent. The cold rolling UCMW mill is equipped with a tapered intermediate roll. The shifting position of the intermediate roll affects the edge depression of the strip. In order to meet the production needs of different shifting roll positions for cold rolling, it is necessary to keep the local high points of the hot-rolled strip as far away from the edge as possible to ensure that the local high points of the strip are effectively depressed during the cold rolling process. Therefore, how to improve the position of the local high points has become another important measure to reduce rib formation in cold rolling production. Summary of the invention
[0004] The object of the present invention is to provide a working roll shifting method for improving the local high point position of the strip, by collaboratively optimizing the working roll shifting position, avoiding the working roll shifting from staying near the zero position, making the local high point of the strip cross section away from the edge of the strip, further avoiding the rib defects that may occur during negative shifting during cold rolling, and solving the technical problem of ribs in cold rolling production caused by the local high point position of the working roll.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for improving working roll shifting at a local high point position of a strip steel comprises the following steps:
[0007] Step 1: Track the intermediate roll shifting and cold rolling beading of the downstream cold rolling mill, and determine the distribution of the local high points of the cross section of the strip where beading is prone to occur during negative roll shifting of the cold rolling mill;
[0008] Step 2: clarify the position relationship between the ribbed coil and the local high point of the hot-rolled strip cross section, and determine the optimal area of the local high point of the hot-rolled strip cross section to avoid ribbed cold-rolled strip;
[0009] Step 3: clarify the relationship between the local high point of the cross section of the hot-rolled strip and the position of the hot-rolled working roll shifting, and subsequently improve the position of the local high point of the cross section of the strip by preventing the working roll from staying at the shifting position;
[0010] Step 4: Optimize the roll shifting model to avoid the work roll shifting position that easily causes local high points to appear at the edge of the strip, and modify the roll shifting model data of the work roll;
[0011] Step 5: Write the above roll shifting model data into the roll shifting model and put it into use during production. The roll shifting model data is input into the rolling model in the form of roll shifting values. During the production process, the specific stand shifts the rolls back and forth according to the set roll shifting values.
[0012] As a further solution of the present invention: determining the position distribution of local high points in the cross-section of the strip where ribs are prone to occur during negative runaway during cold rolling. The specific method is: during the cold rolling process, there is negative runaway in the intermediate rolls of the cold rolling mill. When the negative runaway of the intermediate rolls reaches the maximum Smax, the taper area of the intermediate rolls is offset to the inside of the strip, and the ability to press down the edge of the strip is weakened. The roll runaway and rib formation of the intermediate rolls of the cold rolling mill are studied, so as to determine the position distribution of local high points in the cross-section of the strip where ribs are prone to occur during negative runaway during cold rolling.
[0013] As a further solution of the present invention: a specific method for determining the optimal area of the local high point position in the cross section of the hot-rolled strip for avoiding ribbing in the cold-rolled strip is: based on the ribbing situation fed back from cold rolling, the distance between the local high point and the edge of the hot-rolled strip corresponding to the ribbed coil is checked, and the relationship between the cold-rolled ribbing and the local high point position of the strip is determined, thereby clarifying the optimal area of the local high point position in the cross section of the hot-rolled strip for avoiding ribbing in the cold-rolled strip.
[0014] As a further solution of the present invention: A specific method for improving the position of the local high point of the cross-section of the strip by avoiding the working roll to stay in the shifting position is as follows: for the position of the rib roll feedback from cold rolling, after determining the position of the local high point of the cross-section of hot rolling, check the change of the shifting position of the working roll during the hot rolling process, clarify the relationship between the shifting position of the working roll and the local high point of the cross-section, and subsequently improve the position of the local high point of the cross-section of the strip by avoiding the working roll to stay in the shifting position.
[0015] Beneficial effects of the present invention:
[0016] (1) By collaboratively optimizing the position of the working roll shifting, the working roll shifting is prevented from staying near the zero position, and the local high point of the strip cross section is kept away from the edge of the strip, thereby avoiding the rib defects that may occur during negative shifting during cold rolling.
[0017] (2) When the optimized rear-shifting roll model is used for production, the distance between the local high point of the strip and the edge of the strip increases to more than 150 mm, which improves the adaptability of the negative shifting position of the cold-rolled intermediate roll, improves the position of the local high point of the cross-sectional profile of the hot-rolled strip, increases the distance between the local high point and the edge of the strip, and improves the negative shifting adaptability of the cold-rolled intermediate roll, which is beneficial to reduce the occurrence of cross-sectional rib defects during the cold rolling process. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be further described below in conjunction with the accompanying drawings.
[0019] Figure 1 is a flow chart of the method of the present invention;
[0020] Figure 2 Schematic diagram of negative roll shifting of cold rolling working rolls of the present invention;
[0021] Figure 3 Schematic diagram of the comparison between the local high point position and the rib situation of the strip steel cross section of the present invention;
[0022] Figure 4 This is a schematic diagram of the F5-F7 roller shifting distribution before the optimization of the present invention;
[0023] Figure 5 This is a schematic diagram of the F5-F7 roller shifting distribution after optimization of the present invention;
[0024] Figure 6 It is a schematic diagram of the location of local high points in the cross section of the hot-rolled strip after optimization according to the present invention. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] See also Figure 1 As shown, the present invention is a method for improving the working roll shifting of the local high point position of the strip, comprising the following steps:
[0027] Step 1. Track the intermediate roll shifting and beading of the downstream cold rolling mill to determine the position distribution of local high points in the cross-section of the strip where beading is prone to occur during negative shifting during cold rolling. Specifically, there is negative shifting of the intermediate rolls of the cold rolling mill during the cold rolling process. When the negative shifting of the intermediate rolls reaches the maximum Smax, the taper area of the intermediate rolls shifts to the inside of the strip, and the ability to press down the edge of the strip is weakened. The shifting and beading of the intermediate rolls of the cold rolling mill are studied to determine the position distribution of local high points in the cross-section of the strip where beading is prone to occur during negative shifting during cold rolling.
[0028] Step 2. Clarify the relationship between the ribbed coil and the local high point position of the hot-rolled strip cross section, and determine the optimal area of the local high point position of the hot-rolled strip cross section to avoid ribbed cold-rolled strip; the specific method for determining the optimal area of the local high point position of the hot-rolled strip cross section to avoid ribbed cold-rolled strip is as follows: according to the ribbed situation feedback from cold rolling, check the distance between the local high point and the edge of the hot-rolled strip corresponding to the ribbed coil, determine the relationship between the cold-rolled ribbed and the local high point position of the strip, and then clarify the optimal area of the local high point position of the hot-rolled strip cross section to avoid ribbed cold-rolled strip.
[0029] Step three, clarify the relationship between the local high point of the hot-rolled strip cross section and the position of the hot-rolled working roll shifting, and subsequently improve the position of the local high point of the strip cross section by preventing the working roll from staying at the shifting position; specifically, for the position of the rib roll feedback from cold rolling, after determining the position of the local high point of the hot-rolled cross section, check the change of the working roll shifting position during the hot rolling process, clarify the relationship between the working roll shifting position and the local high point of the cross section, and subsequently improve the position of the local high point of the strip cross section by preventing the working roll from staying at the shifting position.
[0030] Step 4: Optimize the roll shifting model. Based on the relationship between the local high point of the cross section and the work roll shifting position, avoid the work roll shifting position where the local high point is likely to appear at the edge of the strip, and modify the work roll shifting model data.
[0031] Step 5. Write the above-mentioned roll shifting model data into the roll shifting model, which is put into use during production. The roll shifting model data is input into the rolling model in the form of roll shifting values. During the production process, the specific stand shifts the rolls back and forth according to the set roll shifting values. In this way, the local high point position of the cross-section of the hot-rolled strip can be improved by optimizing the roll shifting position of the working rolls, thereby reducing the occurrence of cold rolling rib defects without affecting the cold rolling roll shifting.
[0032] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and specific embodiments:
[0033] Track the intermediate roll shifting and cold rolling ribs in the downstream cold rolling mill. When the intermediate roll shifts negatively, the position of the strip and the roll system is as follows: Figure 2As shown in the figure, the upper working roll, the upper intermediate roll and the upper support roll are arranged from bottom to top above the steel strip, and the lower working roll, the lower intermediate roll and the lower support roll are arranged from top to bottom below the steel strip. The cold rolling process requires that the maximum negative shifting value Smax of the intermediate roll does not exceed 30mm. In a hot rolling plan, 3 hot-rolled steel coils have rib defects after cold rolling. The cold rolling roll shifting positions are all negative. In this case, if the cold rolling roll shifting value is adjusted, the occurrence of strip rib defects after cold rolling can be avoided, but it will affect the efficiency and rolling stability of the cold rolling unit.
[0034] Clarify the relationship between the local high point position of the cross section of the ribbed coil and the hot-rolled strip. Check the local high point of the cross section of the hot-rolled strip of the cold-rolled feedback ribbed coil, and check the cross section of the non-ribbed coil in the hot-rolled strip plan corresponding to the ribbed coil, such as Figure 3 As shown. The local high point of the hot-rolled cross-section of the ribbed steel coil is 100mm away from the edge of the strip, while the local high point of the hot-rolled cross-section of the non-ribbed steel coil is farther away from the edge of the strip, reaching 136mm. The local high point of the hot-rolled strip cross-section is far away from the edge of the strip. When there is negative runaway in the cold-rolled intermediate roll, the local high point of the strip is pressed down more, which can reduce the occurrence of cold-rolled rib defects. Analyze the local high point of the hot-rolled strip cross-section corresponding to the ribs of multiple coils cold-rolled, and the distance between the local high point of the hot-rolled strip cross-section and the edge of the strip cannot be less than 120mm.
[0035] The relationship between the local high point of the hot-rolled strip cross section and the position of the hot-rolled working roll shifting is clarified. Check the hot-rolled roll shifting of cold-rolled steel coils with ribs and non-ribbed steel coils. The corresponding hot-rolled F5-F7 stand roll shifting of the three cold-rolled steel coils with ribs is 10mm, -5mm and -20mm respectively. The corresponding hot-rolled F5-F7 stand roll shifting of the cold-rolled non-ribbed steel coils exceeds 25mm, that is, when the hot-rolled F5-F7 stand roll shifting is within 20mm, the high point of the hot-rolled cross section is close to the edge, which is prone to rib defects during cold rolling. The hot-rolled roll shifting position of the cold-rolled steel coils prone to ribs is as follows Figure 4 shown.
[0036] like Figure 5 As shown in the figure, when the roll shifting of the F5-F7 frames reaches within 20mm at the same time, the local high point of the hot rolling cross-section profile is closer to the edge, and the roll shifting model needs to be optimized. After the optimized roll shifting model, the F5-F7 working roll roll shifting avoids the 30mm roll shifting interval, and the roll shifting of different frames is changed from the synchronous roll shifting of F5 and F7 before optimization to the asynchronous roll shifting mode of three frames.
[0037] like Figure 6 As shown in the figure, the model is put into use and tracks the position of the local high point of the strip. When the optimized rear-shifting roll model is used for production, the distance between the local high point of the strip and the edge of the strip increases to more than 150mm, which improves the adaptability of the negative shifting position of the cold rolling intermediate roll.
[0038] The above-mentioned roll shifting method is adopted to improve the position of the local high point of the cross-sectional profile of the hot-rolled strip, increase the distance between the local high point and the edge of the strip, improve the negative shifting adaptability of the cold-rolled intermediate roll, and help reduce the occurrence of cross-sectional rib defects during the cold rolling process.
[0039] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for improving the working roll shifting of the local high point position of the strip, characterized in that: The following steps are involved: Step 1: Track the intermediate roll shifting and cold rolling beading of the downstream cold rolling mill, and determine the distribution of the local high points of the cross section of the strip where beading is prone to occur during negative roll shifting of the cold rolling mill; Step 2: clarify the position relationship between the ribbed coil and the local high point of the hot-rolled strip cross section, and determine the optimal area of the local high point of the hot-rolled strip cross section to avoid ribbed cold-rolled strip; Step 3: clarify the relationship between the local high point of the cross section of the hot-rolled strip and the position of the hot-rolled working roll shifting, and subsequently improve the position of the local high point of the cross section of the strip by preventing the working roll from staying at the shifting position; Step 4: Optimize the roll shifting model to avoid the work roll shifting position that easily causes local high points to appear at the edge of the strip, and modify the roll shifting model data of the work roll; Step 5: Write the above roll shifting model data into the roll shifting model and put it into use during production. The roll shifting model data is input into the rolling model in the form of roll shifting values. During the production process, the specific stand shifts the rolls back and forth according to the set roll shifting values.
2. A method for improving work roll shifting at the local high point position of a strip according to claim 1, characterized in that: The specific method for determining the distribution of the local high points in the cross-section of the strip where ribs are prone to occur during negative runaway in cold rolling is as follows: during the cold rolling process, there is negative runaway in the intermediate rolls of the cold rolling mill. When the negative runaway of the intermediate rolls reaches the maximum Smax, the taper area of the intermediate rolls shifts to the inside of the strip, and the ability to press down the edge of the strip is weakened. The roll runaway and rib formation of the intermediate rolls of the cold rolling mill are studied, so as to determine the distribution of the local high points in the cross-section of the strip where ribs are prone to occur during negative runaway in cold rolling.
3. A method for improving work roll shifting of a local high point of a strip according to claim 2, characterized in that: The specific method for determining the optimal area of the local high point position in the cross section of the hot-rolled strip to avoid ribbing in the cold-rolled strip is: based on the ribbing situation fed back from cold rolling, the distance between the local high point and the edge of the hot-rolled strip corresponding to the ribbed coil is checked, and the relationship between the cold-rolled ribbing and the local high point position of the strip is determined, thereby clarifying the optimal area of the local high point position in the cross section of the hot-rolled strip to avoid ribbing in the cold-rolled strip.
4. A method for improving the working roll shifting of the local high point position of the strip according to claim 3, characterized in that: The specific method for improving the position of the local high point of the cross section of the strip by avoiding the working roll to stay in the shifting position is as follows: for the position of the rib roll feedback from cold rolling, after determining the position of the local high point of the cross section of hot rolling, check the change of the working roll shifting position during the hot rolling process, clarify the relationship between the working roll shifting position and the local high point of the cross section, and subsequently improve the position of the local high point of the cross section of the strip by avoiding the working roll to stay in the shifting position.
Citation Information
Patent Citations
Method for controlling swelling rib in central section of color coating base material
CN102226231A
Methods to improve the rib formation defect in cold-rolled strip steel
CN102274862A
Method for eliminating local abrasion of flat work rolls
CN102755996A
Cold rolling rib forming early warning method based on strip steel section feature recognition
CN117000783A
Method for rolling strip
JP1998166020A