Rare-earth-doped high-speed steel thin strip as well as preparation method and application thereof
Through the casting of rare earth-doped high-speed steel billets and copper roller spraying belt swing method, the problem that traditional refined grain method cannot suppress re-crystallization is solved, and the grain refinement and mechanical performance of high-speed steel thin strips are improved. A new method for preparing high-speed steel materials was developed.
Patent Information
- Application Number
- CN202410870699.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-12
AI Technical Summary
The traditional method of refining grains in the prior art cannot effectively suppress re-crystallization and the degree of fine crystallization is insufficient, resulting in insufficient mechanical properties and wear resistance of high-speed steel materials.
Rare-earth-doped high-speed steel billets are prepared by traditional casting combined with copper roller jet rolling slitting method, and high-melting point oxygen/sulfur-rare earth composite inclusions are formed by using rapid cooling and affinity of rare earth elements. Inhibit grain growth and achieve grain refinement and microalloyation.
Re-crystallization is effectively suppressed, and a rare earth-doped high-speed steel thin strip with excellent comprehensive mechanical properties and wear resistance is obtained, providing new high-speed steel material design ideas and efficient and low-cost preparation technology.
Smart Images

Figure CN118926494A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel material preparation, and in particular to a rare earth-doped high-speed steel thin strip and a preparation method and application thereof. Background Art
[0002] High-speed steel, also known as wind steel or sharp steel, is a tool steel with high hardness, high wear resistance and high heat resistance. High-speed steel has the advantages of high hardness, good wear resistance, good process performance, good strength and toughness, etc. Therefore, it is mainly used to manufacture complex thin-blade and impact-resistant metal cutting tools, and can also be used to manufacture cold working dies, rollers, high-temperature bearings and high-temperature springs with high performance requirements.
[0003] Grain refinement is a common characteristic of metal materials, which can be described by the famous Hall-Petch relationship. The grain size of the material is inversely proportional to the mechanical properties of the metal. Strengthening is one of the effective methods to improve the mechanical properties of metal materials. In addition, grain refinement is also conducive to homogenizing the alloy composition and improving the corrosion resistance of the alloy material. Under the premise of a given composition, the high-speed steel material prepared by the strengthening mechanism has excellent comprehensive mechanical properties. It has important value and broad prospects both in industrial production and in the military industry.
[0004] In the prior art, high-speed steel grades are mostly processed by forging and rolling processes, both of which belong to traditional thermal deformation treatment methods. During the hot extrusion process, the network carbide is broken, its size gradually decreases, and its distribution is more uniform, thereby achieving the purpose of grain refinement and strengthening the high-speed steel alloy material. However, forging and rolling require higher temperatures, the effect of grain refinement does not meet the ideal requirements, and it is difficult to avoid the occurrence of re-crystallization during the cooling process. Based on this, the development of a high-speed steel material that can inhibit re-crystallization and achieve the purpose of fine grain strengthening has a significant driving significance for the preparation of steel materials. Summary of the invention
[0005] Aiming at the problem that the conventional grain refinement method in the prior art cannot suppress re-crystallization and the degree of grain refinement is not enough. The present invention provides a rare earth doped high-speed steel strip and its preparation method and application. The present invention uses rare earth doped high-speed steel billet as raw material and combines conventional casting and strip spinning to produce the rare earth doped high-speed steel strip. The rare earth doped high-speed steel strip obtained by the present invention has excellent comprehensive mechanical properties and provides a new material source for the application of high-speed steel materials.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] A first aspect of the present invention provides a method for preparing a rare earth-doped high-speed steel strip, comprising the following steps:
[0008] Step 1: taking a rare earth-doped high-speed steel billet as a raw material, subjecting it to primary annealing, forging, hot rolling, secondary annealing, and cutting to obtain a master alloy ingot;
[0009] Step 2, removing the surface oxide layer of the master alloy ingot to obtain a pretreated master alloy ingot;
[0010] Step 3, melting the pretreated master alloy ingot under an inert atmosphere to obtain alloy steel liquid; pressurizing and spraying the alloy steel liquid onto the surface of a copper roller with a rotation speed of 15m / s-55m / s, and cooling to obtain a rare earth-doped high-speed steel thin strip;
[0011] Among them, the rare earth doped high-speed steel billet contains the following components in percentage by mass: C: 0.70%-1.35%, Si: 0.05%-0.80%, Mn: 0.05%-0.65%, Cr: 3.50%-5.20%, Ni: 0.00%-0.25%, Cu: 0.00%-0.15%, Mo: 0.50%-10.55%, W: 0.45%-20.05%, V: 0.75%-2.55%, Co: 0.05%-9.05%, Al: 0.00%-1.25%, RE: 0.001%-0.055%, S≤0.025%, P≤0.025% and the balance Fe, and the RE is any one or more of La, Ce, Y or Nb.
[0012] Compared with the prior art, the present invention adopts the method of traditional casting combined with copper roller spraying strip to prepare rare earth doped high-speed steel thin strip. The strip-spinning method is characterized by rapid solidification, which is a non-equilibrium solidification process and can reach 10 4 K / s-10 6 The cooling rate of K / s is very fast. It is precisely because of this fast cooling rate that the disordered structure of the alloy steel liquid can be maintained, and its re-crystallization during the cooling process can be inhibited, thereby producing an alloy strip with excellent solidified structure. At the same time, the strip-spinning method is easy to operate and has a short process. It is an efficient and low-cost preparation process.
[0013] Furthermore, due to the strong affinity of rare earth elements with oxygen and sulfur, high melting point oxygen / sulfur-rare earth composite inclusions are easily formed. During the solidification of molten steel, the inclusions can serve as heterogeneous nucleation cores to avoid the formation of new grains, thereby achieving the purpose of grain refinement. On the other hand, rare earth, as a surface active element, is easily enriched at the grain boundary, which can hinder the growth of grains and inhibit the occurrence of the crystallization process. It can be seen that the interaction between rare earth elements and other elements realizes the microalloying of high-speed steel, thereby achieving the effect of purifying grain boundaries and refining grains. Furthermore, the addition of rare earth elements can improve the morphology, size and content of carbides in high-speed steel, thereby enhancing the mechanical properties and wear resistance of high-speed steel.
[0014] In summary, the rare earth doped high-speed steel strip provided by the present invention not only has a simple preparation method, but also has more uniform and fine grains, effectively improving the comprehensive performance of the strip material. The technical solution of the present invention effectively solves the problem that the traditional grain refinement method in the prior art cannot inhibit re-crystallization and the degree of grain refinement is not enough, and provides a new design idea and preparation process for high-speed steel strip.
[0015] Preferably, in step three, the pretreated master alloy ingot is melted in a quartz tube connected to a spray device.
[0016] Further preferably, the nozzle diameter of the spraying device is 0.8 mm-2 mm, and the vertical distance from the nozzle to the copper roller is 0.1 mm-0.3 mm; the spraying pressure of the spraying device is 0.01 MPa-0.5 MPa.
[0017] Preferably, the temperature of the primary annealing is 840° C.-890° C., and the holding time of the primary annealing is 6 h-8 h.
[0018] Preferably, the temperature of the secondary annealing is 840° C.-890° C., and the holding time of the secondary annealing is 6 h-8 h.
[0019] Preferably, the heating temperature of the forging is 1120° C.-1150° C., and the forging time is 11 h-13 h.
[0020] Further preferably, the initial forging temperature of the forging is 1000°C-1050°C, and the final forging temperature is 900-1100°C.
[0021] Preferably, the hot rolling temperature is 1000°C-1100°C.
[0022] Preferably, the smelting temperature is 1500°C-1650°C.
[0023] Preferably, the oxide layer on the surface of the master alloy ingot is removed by mechanical grinding or immersion pickling.
[0024] Preferably, the rare earth doped high speed steel billet is produced by induction melting.
[0025] A second aspect of the present invention provides a rare earth doped high-speed steel thin strip, which is prepared by using the preparation method of the rare earth doped high-speed steel thin strip.
[0026] Preferably, the rare earth doped high speed steel strip has a width of 2 mm to 5 mm and a thickness of 20 μm to 80 μm.
[0027] A third aspect of the present invention provides an application of a rare earth-doped high-speed steel thin strip in the preparation of a micro-cutting tool.
[0028] In summary, the present invention provides a rare earth doped high-speed steel strip and a preparation method and application thereof, wherein a high-speed steel billet containing rare earth elements is used as a raw material, and the rare earth doped high-speed steel strip is prepared by a strip-spinning method. The present invention improves the steel material and the preparation method, and obtains a high-speed steel strip with uniform and tiny grains, which effectively solves the problem that the traditional grain refinement method in the prior art cannot inhibit re-crystallization and the degree of grain refinement is not enough. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the metallographic structure diagram of the La and Ce co-doped high-speed steel strip obtained in Example 1;
[0030] Figure 2 This is the metallographic structure diagram of the La and Ce co-doped high-speed steel strip obtained in Example 2;
[0031] Figure 3 This is the metallographic structure diagram of the La and Ce co-doped high-speed steel strip obtained in Example 3;
[0032] Figure 4 This is the metallographic structure diagram of the La and Ce co-doped high-speed steel strip obtained in Comparative Example 1;
[0033] Figure 5 The metallographic structure diagram of the La and Ce co-doped high speed steel forging state obtained in Comparative Example 2;
[0034] Figure 6 This is a grain size distribution diagram of the La and Ce co-doped high-speed steel strip obtained in Example 1-3;
[0035] Figure 7 2. The Vickers hardness diagram of the La and Ce co-doped high-speed steel strips obtained in Examples 1-3 and Comparative Example 1. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] This embodiment provides a method for preparing a La and Ce co-doped high-speed steel strip, which specifically includes the following contents:
[0039] Step 1, using a La and Ce co-doped high-speed steel billet prepared by an induction melting method as a raw material, first annealing at 870°C and keeping it warm for 8 hours; after annealing, heating the billet to 1130°C for forging, and the overall forging time is 12 hours; obtaining a forged high-speed steel; hot rolling the forged high-speed steel at 1050°C to obtain a rolled steel; performing a secondary annealing on the rolled steel at 860°C, keeping it warm for 6.5 hours, and cutting to obtain a master alloy ingot;
[0040] Step 2: mechanically polishing to remove the oxide layer on the surface of the master alloy ingot, ultrasonically cleaning it in anhydrous ethanol for 15 minutes, and drying it to obtain a pretreated master alloy ingot;
[0041] Step 3: Place 3g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the liquid spraying device. The nozzle diameter of the spraying device is 1mm, and the vertical distance from the nozzle to the copper roller is 0.2mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the speed of the copper roller to 15m / s. After the speed of the copper roller remains uniform and constant, start the induction power supply, induction heat to 1600℃, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0042] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, quickly open the spray gun air valve, set the spray pressure to 0.15 MPa, and quickly spray the alloy melt onto the surface of the rolling copper wheel. Rapidly solidify to obtain a La and Ce co-doped high-speed steel strip with a width of 3 mm and a thickness of 60 μm.
[0043] Among them, the La and Ce co-doped high-speed steel billet contains the following components in percentage by mass: C: 0.93%, Si: 0.37%, Mn: 0.30%, W: 6.20%, Mo: 4.80%, Cr: 4.15%, V: 1.90%, La: 0.032%, Ce: 0.044%, Ni: 0.20%, P: 0.018%, S: 0.01% and the balance Fe.
[0044] Example 2
[0045] This embodiment provides a method for preparing a La and Ce co-doped high-speed steel strip, which specifically includes the following contents:
[0046] Step 1, using a La and Ce co-doped high-speed steel billet prepared by an induction melting method as a raw material, first annealing at 870°C and keeping it warm for 8 hours; after annealing, heating the billet to 1130°C for forging, and the overall forging time is 12 hours; obtaining a forged high-speed steel; hot rolling the forged high-speed steel at 1050°C to obtain a rolled steel; performing a secondary annealing on the rolled steel at 860°C, keeping it warm for 6.5 hours, and cutting to obtain a master alloy ingot;
[0047] Step 2: mechanically polishing to remove the oxide layer on the surface of the master alloy ingot, ultrasonically cleaning it in anhydrous ethanol for 15 minutes, and drying it to obtain a pretreated master alloy ingot;
[0048] Step 3: Place 3g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the liquid spraying device. The nozzle diameter of the spraying device is 1mm, and the vertical distance from the nozzle to the copper roller is 0.2mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the speed of the copper roller to 20m / s. After the speed of the copper roller remains uniform and constant, start the induction power supply, induction heat to 1600℃, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0049] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, quickly open the spray gun air valve, set the spray pressure to 0.15 MPa, and quickly spray the alloy melt onto the surface of the rolling copper wheel. Rapidly solidify to obtain a La and Ce co-doped high-speed steel strip with a width of 3 mm and a thickness of 60 μm.
[0050] Among them, the La and Ce co-doped high-speed steel billet contains the following components in percentage by mass: C: 0.93%, Si: 0.37%, Mn: 0.30%, W: 6.20%, Mo: 4.80%, Cr: 4.15%, V: 1.90%, La: 0.032%, Ce: 0.044%, Ni: 0.20%, P: 0.018%, S: 0.01% and the balance Fe.
[0051] Example 3
[0052] This embodiment provides a method for preparing a La and Ce co-doped high-speed steel strip, which specifically includes the following contents:
[0053] Step 1, using a La and Ce co-doped high-speed steel billet prepared by an induction melting method as a raw material, first annealing at 870°C and keeping it warm for 8 hours; after annealing, heating the billet to 1130°C for forging, and the overall forging time is 11 hours; obtaining a forged high-speed steel; hot rolling the forged high-speed steel at 1050°C to obtain a rolled steel; performing a secondary annealing on the rolled steel at 860°C, keeping it warm for 6.5 hours, and cutting to obtain a master alloy ingot;
[0054] Step 2: mechanically polishing to remove the oxide layer on the surface of the master alloy ingot, ultrasonically cleaning it in anhydrous ethanol for 15 minutes, and drying it to obtain a pretreated master alloy ingot;
[0055] Step 3: Place 3g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the liquid spraying device. The nozzle diameter of the spraying device is 1mm, and the vertical distance from the nozzle to the copper roller is 0.2mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the speed of the copper roller to 30m / s. After the speed of the copper roller remains uniform and constant, start the induction power supply, induction heat to 1600℃, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0056] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, quickly open the spray gun air valve, set the spray pressure to 0.15 MPa, and quickly spray the alloy melt onto the surface of the rolling copper wheel. Rapidly solidify to obtain a La and Ce co-doped high-speed steel strip with a width of 3 mm and a thickness of 60 μm.
[0057] Among them, the La and Ce co-doped high-speed steel billet contains the following components in percentage by mass: C: 0.93%, Si: 0.37%, Mn: 0.30%, W: 6.20%, Mo: 4.80%, Cr: 4.15%, V: 1.90%, La: 0.032%, Ce: 0.044%, Ni: 0.20%, P: 0.018%, S: 0.01% and the balance Fe.
[0058] Example 4
[0059] This embodiment provides a method for preparing a La-doped high-speed steel strip, which specifically includes the following contents:
[0060] Step 1, using a Ce-doped high-speed steel billet prepared by an induction melting method as a raw material, first annealing at 890°C and keeping it warm for 8 hours; after annealing, heating the billet to 1135°C for forging, and the overall forging time is 12.5 hours; obtaining a forged high-speed steel; hot rolling the forged high-speed steel at 1080°C to obtain a rolled steel; performing a secondary annealing on the rolled steel at 865°C, keeping it warm for 6.5 hours, and cutting to obtain a master alloy ingot;
[0061] Step 2: mechanically polishing to remove the oxide layer on the surface of the master alloy ingot, ultrasonically cleaning it in anhydrous ethanol for 10 minutes, and drying it to obtain a pretreated master alloy ingot;
[0062] Step 3: Place 2.5g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the jet device. The nozzle diameter of the jet device is 1mm, and the vertical distance from the nozzle to the copper roller is 0.3mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the speed of the copper roller to 20m / s. After the speed of the copper roller remains uniform and constant, start the induction power supply, induction heat to 1600℃, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0063] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, quickly open the spray gun air valve and set the spray pressure to 0.05 MPa to quickly spray the molten alloy onto the surface of the rolling copper wheel and quickly solidify to obtain a La-doped high-speed steel strip with a width of 2.5 mm and a thickness of 50 μm.
[0064] Among them, the La-doped high-speed steel billet contains the following components in mass percentage: C: 0.75%, Si: 0.78%, Mn: 0.65%, W: 14.83%, Mo: 0.82%, Cr: 5.01%, V: 0.79%, La: 0.044%, Ni: 0.12%, P: 0.024%, S: 0.01% and the balance Fe.
[0065] Example 5
[0066] This embodiment provides a method for preparing a Y and Nb co-doped high-speed steel strip, which specifically includes the following contents:
[0067] Step 1, using a Y and Nb co-doped high-speed steel billet prepared by an induction melting method as a raw material, first annealing at 875°C and keeping it warm for 8 hours; after annealing, heating the billet to 1125°C for forging, and the overall forging time is 13 hours; obtaining a forged high-speed steel; hot rolling the forged high-speed steel at 1050°C to obtain a rolled steel; performing a secondary annealing on the rolled steel at 845°C, keeping it warm for 7.5 hours, and cutting to obtain a master alloy ingot;
[0068] Step 2: mechanically polishing to remove the oxide layer on the surface of the master alloy ingot, ultrasonically cleaning with anhydrous ethanol for 15 minutes, and drying to obtain a pretreated master alloy ingot;
[0069] Step 3: Place 2.8g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the jet device. The nozzle diameter of the jet device is 1.2mm, and the vertical distance from the nozzle to the copper roller is 0.3mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the copper roller speed to 35m / s. After the copper roller speed remains uniform and constant, start the induction power supply, induction heat to 1590℃, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0070] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, quickly open the spray gun air valve and set the spray pressure to 0.2 MPa to quickly spray the molten alloy onto the surface of the rolling copper wheel and quickly solidify to obtain a Y and Nb co-doped high-speed steel strip with a width of 3 mm and a thickness of 54 μm.
[0071] Among them, the Y and Nb co-doped high-speed steel billet contains the following components in mass percentage: C: 0.93%, Si: 0.37%, Mn: 0.39%, W: 18.44%, Mo: 9.42%, Cr: 4.05%, V: 1.21%, Co: 7.87%, Al: 1.35%, Cu: 0.11%, Y: 0.024%, Nb: 0.024%, Ni: 0.22%, P: 0.017%, S: 0.012% and the balance Fe.
[0072] Example 6
[0073] This embodiment provides a method for preparing a La and Ce co-doped high-speed steel strip, which specifically includes the following contents:
[0074] Step 1, using a La and Ce co-doped high-speed steel billet prepared by an induction melting method as a raw material, first annealing at 880°C and keeping it warm for 8 hours; after annealing, heating the billet to 1128°C for forging, and the overall forging time is 11.5 hours; obtaining a forged high-speed steel; hot rolling the forged high-speed steel at 1050°C to obtain a rolled steel; performing a secondary annealing on the rolled steel at 855°C, keeping it warm for 7 hours, and cutting to obtain a master alloy ingot;
[0075] Step 2, immersing the master alloy ingot in a 0.5 mol / L sulfuric acid solution for 30 minutes, then ultrasonically cleaning the master alloy ingot with anhydrous ethanol for 15 minutes, and drying to obtain a pretreated master alloy ingot;
[0076] Step 3: Place 3g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the jet device. The nozzle diameter of the jet device is 1.1mm, and the vertical distance from the nozzle to the copper roller is 0.2mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the copper roller speed to 40m / s. After the copper roller speed remains uniform and constant, start the induction power supply, induction heat to 1590℃, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0077] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, quickly open the spray gun air valve and set the spray pressure to 0.15 MPa to quickly spray the molten alloy onto the surface of the rolling copper wheel and quickly solidify to obtain a La and Ce co-doped high-speed steel strip with a width of 3 mm and a thickness of 60 μm.
[0078] Among them, the La and Ce co-doped high-speed steel billet contains the following components in mass percentage: C: 0.94%, Si: 0.29%, Mn: 0.30%, W: 6.30%, Mo: 4.83%, Cr: 4.25%, V: 1.94%, Al: 1.05%, La: 0.035%, Ce: 0.016%, Ni: 0.20%, P: 0.014%, S: 0.018% and the balance Fe.
[0079] Example 7
[0080] This embodiment provides a method for preparing a La and Ce co-doped high-speed steel strip, which specifically includes the following contents:
[0081] Step 1, using La and Ce co-doped M35 high-speed steel billet prepared by induction melting as raw material, first annealing at 870°C and keeping warm for 8 hours; after annealing, heating the billet to 1130°C for forging, and the overall forging time is 12 hours; obtaining forged high-speed steel; hot rolling the forged high-speed steel at 1060°C to obtain rolled steel; performing secondary annealing on the rolled steel at 845°C, keeping warm for 8 hours, cutting, and obtaining a master alloy ingot;
[0082] Step 2: mechanically polishing to remove the oxide layer on the surface of the master alloy ingot, ultrasonically cleaning with anhydrous ethanol for 15 minutes, and drying to obtain a pretreated master alloy ingot;
[0083] Step 3: Place 3g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the jet device. The nozzle diameter of the jet device is 1mm, and the vertical distance from the nozzle to the copper roller is 0.2mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the speed of the copper roller to 55m / s. After the speed of the copper roller remains uniform and constant, start the induction power supply, induction heat to 1620℃, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0084] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, the spray gun air valve is quickly opened and the spray pressure is set to 0.1 MPa, so that the alloy steel liquid is quickly sprayed onto the surface of the rolling copper wheel and quickly solidified to obtain a La and Ce co-doped high-speed steel thin strip with a width of 3 mm and a thickness of 60 μm.
[0085] Among them, the La and Ce co-doped high-speed steel billet contains the following components in mass percentage: C: 0.91%, Si: 0.27%, Mn: 0.32%, W: 6.21%, Mo: 4.80%, Cr: 4.16%, V: 1.90%, La: 0.038%, Ce: 0.017%, Ni: 0.18%, P: 0.014%, S: 0.018% and the balance Fe.
[0086] Example 8
[0087] This embodiment provides a method for preparing a La and Ce co-doped high-speed steel strip, which specifically includes the following contents:
[0088] Step 1, using a La and Ce co-doped high-speed steel billet prepared by an induction melting method as a raw material, first annealing at 885°C and keeping it warm for 8 hours; after annealing, heating the billet to 1130°C for forging, and the overall forging time is 13 hours; obtaining a forged high-speed steel; hot rolling the forged high-speed steel at 1050°C to obtain a rolled steel; performing a secondary annealing on the rolled steel at 860°C, keeping it warm for 6.5 hours, and cutting to obtain a master alloy ingot;
[0089] Step 2: mechanically polishing to remove the oxide layer on the surface of the master alloy ingot, ultrasonically cleaning with anhydrous ethanol for 15 minutes, and drying to obtain a pretreated master alloy ingot;
[0090] Step 3: Place 3g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the jet device. The nozzle diameter of the jet device is 0.8mm, and the vertical distance from the nozzle to the copper roller is 0.3mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the copper roller speed to 45m / s. After the copper roller speed remains uniform and constant, start the induction power supply, induction heat to 1650℃, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0091] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, quickly open the spray gun air valve, set the spray pressure to 0.15 MPa, and quickly spray the alloy melt onto the surface of the rolling copper wheel. Rapidly solidify to obtain a La and Ce co-doped high-speed steel strip with a width of 3 mm and a thickness of 60 μm.
[0092] Among them, the La and Ce co-doped high-speed steel billet contains the following components in mass percentage: C: 1.15%, Si: 0.69%, Mn: 0.37%, W: 8.34%, Mo: 4.81%, Cr: 5.15%, V: 1.90%, Al: 0.98%, La: 0.032%, Ce: 0.021%, Ni: 0.20%, P: 0.014%, S: 0.018% and the balance Fe.
[0093] Example 9
[0094] This embodiment provides a method for preparing a La and Ce co-doped high-speed steel strip, which specifically includes the following contents:
[0095] Step 1, using a La and Ce co-doped high-speed steel billet prepared by an induction melting method as a raw material, first annealing at 870°C and keeping it warm for 8 hours; after annealing, heating the billet to 1130°C for forging, and the overall forging time is 12.5 hours; obtaining a forged high-speed steel; hot rolling the forged high-speed steel at 1050°C to obtain a rolled steel; performing a secondary annealing on the rolled steel at 860°C, keeping it warm for 6.5 hours, and cutting to obtain a master alloy ingot;
[0096] Step 2: mechanically polishing to remove the oxide layer on the surface of the master alloy ingot, ultrasonically cleaning with anhydrous ethanol for 15 minutes, and drying to obtain a pretreated master alloy ingot;
[0097] Step 3: Place 3g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the jet device. The nozzle diameter of the jet device is 1.4mm, and the vertical distance from the nozzle to the copper roller is 0.2mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the speed of the copper roller to 25m / s. After the speed of the copper roller remains uniform and constant, start the induction power supply, induction heat to 1640°C, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0098] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, quickly open the spray gun air valve, set the spray pressure to 0.25 MPa, and quickly spray the alloy melt onto the surface of the rolling copper wheel. Rapidly solidify to obtain a La and Ce co-doped high-speed steel strip with a width of 3 mm and a thickness of 60 μm.
[0099] Among them, the La and Ce co-doped high-speed steel billet contains the following components in mass percentage: C: 0.90%, Si: 0.30%, Mn: 0.39%, W: 16.20%, Mo: 4.80%, Cu: 0.12%, Cr: 4.14%, V: 1.92%, La: 0.036%, Ce: 0.005%, Ni: 0.04%, P: 0.014%, S: 0.018% and the balance Fe.
[0100] Comparative Example 1
[0101] This comparative example provides a method for preparing a La and Ce co-doped high-speed steel strip, which is different from Example 1 in that the rotation speed of the copper roller is controlled to be 5 m / s, and specifically includes the following contents:
[0102] Step 1, using a La and Ce co-doped high-speed steel billet prepared by an induction melting method as a raw material, first annealing at 870°C and keeping it warm for 8 hours; after annealing, heating the billet to 1130°C for forging, and the overall forging time is 12 hours; obtaining a forged high-speed steel; hot rolling the forged high-speed steel at 1050°C to obtain a rolled steel; performing a secondary annealing on the rolled steel at 860°C, keeping it warm for 6.5 hours, and cutting to obtain a master alloy ingot;
[0103] Step 2: mechanically polishing to remove the oxide layer on the surface of the master alloy ingot, ultrasonically cleaning with anhydrous ethanol for 15 minutes, and drying to obtain a pretreated master alloy ingot;
[0104] Step 3: Place 3g of the pretreated master alloy ingot in a quartz tube with a diameter of 15mm. The quartz tube is fixed in the center of the induction coil to ensure that the quartz tube is tightly connected to the liquid spraying device. The nozzle diameter of the spraying device is 1mm, and the vertical distance from the nozzle to the copper roller is 0.2mm. Close the cabin door and fill the cabin with argon to maintain a vacuum state. After the cabin reaches the vacuum condition, start the copper roller and control the speed of the copper roller to 5m / s. After the speed of the copper roller remains uniform and constant, start the induction power supply, induction heat to 1600℃, melt the pretreated master alloy ingot, and obtain alloy steel liquid.
[0105] Step 4: After the master alloy is completely melted and 1-3 drops of molten steel are dripped, quickly open the spray gun air valve, set the spray pressure to 0.15 MPa, and quickly spray the alloy melt onto the surface of the rolling copper wheel. Rapidly solidify to obtain a La and Ce co-doped high-speed steel strip with a width of 3 mm and a thickness of 60 μm.
[0106] Among them, the La and Ce co-doped high-speed steel billet contains the following components in percentage by mass: C: 0.93%, Si: 0.37%, Mn: 0.30%, W: 6.20%, Mo: 4.80%, Cr: 4.15%, V: 1.90%, La: 0.032%, Ce: 0.044%, Ni: 0.20%, P: 0.018%, S: 0.01% and the balance Fe.
[0107] Comparative Example 2
[0108] This comparative example provides a method for preparing a La and Ce co-doped high-speed steel material, which is different from Example 1 in that a forging process is used for grain refinement, and specifically includes the following contents:
[0109] The La and Ce co-doped high-speed steel billet prepared by induction melting method is used as raw material, and is first annealed at 870°C and kept warm for 8 hours. After annealing, the billet is heated to 1130°C for forging, and the overall forging time is 12 hours; thus, La and Ce co-doped high-speed steel material is obtained.
[0110] Among them, the La and Ce co-doped high-speed steel billet contains the following components in percentage by mass: C: 0.93%, Si: 0.37%, Mn: 0.30%, W: 6.20%, Mo: 4.80%, Cr: 4.15%, V: 1.90%, La: 0.032%, Ce: 0.044%, Ni: 0.20%, P: 0.018%, S: 0.01% and the balance Fe.
[0111] In order to further demonstrate the technical effect of the present invention, the present invention uses a LEICA Dmi8 metallographic microscope to characterize and test the microstructure and mechanical properties of the rare earth-doped high-speed steel strips prepared in Examples 1-3 and the high-speed steel materials prepared in Comparative Examples 1-2. The results are as follows: Figure 1-5 As shown. Figure 1-5 It can be seen that the metallographic structure of the rare earth doped high-speed steel strips obtained in Examples 1-3 is related to the rotation speed of the copper roller. The faster the rotation speed of the copper roller, the faster the cooling rate of the alloy steel liquid, the greater the degree of supercooling, the finer the strip microstructure, and the finer the grain size.
[0112] The present invention also tested the grain size of the rare earth doped high speed steel strips obtained in Examples 1-3. The results are as follows: Figure 6 As shown. Figure 6 It can be seen that the grain size of the rare earth doped high-speed steel thin strip provided by the present invention is mainly concentrated in the range of 1 μm-3 μm, and as the rotation speed of the copper roller increases, the grain size of the obtained strip becomes finer.
[0113] The present invention also uses a microhardness tester to measure the Vickers hardness of the rare earth-doped high-speed steel strip samples obtained in Examples 1-3 and Comparative Example 1. The test load is 50 gf, the holding time is 10 s, and the average value is taken from the 5 test points. Figure 7 As shown. Figure 7 It can be seen that the faster the cooling rate of the rare earth-doped high-speed steel strips obtained in Examples 1-3, the finer the grain size of the strips. Due to the synergistic effect of grain refinement and rare earth microstructure refinement, the Vickers hardness of the strip material tends to increase.
[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a rare earth-doped high-speed steel strip, characterized in that: The steps include: Step 1: taking a rare earth-doped high-speed steel billet as a raw material, subjecting it to primary annealing, forging, hot rolling, secondary annealing, and cutting to obtain a master alloy ingot; Step 2, removing the surface oxide layer of the master alloy ingot to obtain a pretreated master alloy ingot; Step 3, melting the pretreated master alloy ingot in an inert atmosphere to obtain alloy steel liquid; The alloy steel liquid is pressurized and sprayed onto the surface of a copper roller with a rotation speed of 15 m / s-55 m / s, and cooled to obtain a rare earth-doped high-speed steel thin strip; Among them, the rare earth doped high-speed steel billet contains the following components in percentage by mass: C: 0.70%-1.35%, Si: 0.05%-0.80%, Mn: 0.05%-0.65%, Cr: 3.50%-5.20%, Ni: 0.00%-0.25%, Cu: 0.00%-0.15%, Mo: 0.50%-10.55%, W: 0.45%-20.05%, V: 0.75%-2.55%, Co: 0.05%-9.05%, Al: 0.00%-1.25%, RE: 0.001%-0.055%, S≤0.025%, P≤0.025% and the balance Fe, and the RE is any one or more of La, Ce, Y or Nb.
2. The method for preparing a rare earth-doped high-speed steel strip according to claim 1, characterized in that: In step three, the pretreated master alloy ingot is melted in a quartz tube connected to a spray device.
3. The method for preparing a rare earth-doped high-speed steel strip according to claim 2, characterized in that: The nozzle diameter of the spraying device is 0.8mm-2mm, and the vertical distance from the nozzle to the copper roller is 0.1mm-0.3mm; the spraying pressure of the spraying device is 0.01MPa-0.5MPa.
4. The method for preparing a rare earth-doped high-speed steel strip according to claim 1, characterized in that: The primary annealing temperature is 840°C-890°C, and the primary annealing holding time is 6h-8h; and / or The temperature of the secondary annealing is 840° C.-890° C., and the holding time of the secondary annealing is 6 h-8 h.
5. The method for preparing a rare earth-doped high-speed steel strip according to claim 1, characterized in that: The heating temperature of the forging is 1120° C.-1150° C., and the forging time is 11 h-13 h; and / or The hot rolling temperature is 1000°C-1100°C; and / or The smelting temperature is 1500°C-1650°C.
6. The method for preparing a rare earth-doped high-speed steel strip according to claim 1, characterized in that: The oxide layer on the surface of the master alloy ingot is removed by mechanical grinding or immersion pickling.
7. The method for preparing a rare earth-doped high-speed steel strip according to claim 1, characterized in that: The rare earth doped high speed steel blank is prepared by induction melting.
8. A rare earth doped high speed steel strip, characterized in that: The high-speed steel strip is prepared by the method for preparing the rare earth-doped high-speed steel strip according to any one of claims 1 to 7.
9. The rare earth doped high speed steel strip according to claim 8, characterized in that: The rare earth doped high speed steel thin strip has a width of 2 mm to 5 mm and a thickness of 20 μm to 80 μm.
10. Use of the rare earth doped high-speed steel strip according to any one of claims 8 to 9 in preparing micro cutting tools.
Citation Information
Cited By
Lanthanum-containing silicon steel ultrathin strip and preparation method thereof
CN117701979A