Titanium-aluminum alloy in complex shape and manufacturing method of composite material component of titanium-aluminum alloy

Through the specific process processing of titanium-aluminum alloy and its composite materials, the problems of difficult forming and poor performance of complex shape parts are solved, efficient and low-cost manufacturing methods are realized, forming rate and mechanical properties are improved, and the scope of use is expanded.

CN118926531APending Publication Date: 2024-11-12DANYANG DANJIN AVIATION MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411016507.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Titanium-aluminum alloys and their composite materials face problems such as molding difficulties, coarse grains, serious segregation, serious material waste, large brittleness, low deformation capacity and low machining efficiency when manufacturing complex shape parts. The existing forging and powder metallurgy methods are difficult to Solve these problems.

Method used

A complex-shaped titanium-aluminum alloy and its composite material components are used to manufacture methods, including material preparation, plasticizer preparation, blank preparation, blank preparation, prefixed parts preparation, inspection and dressing and thermal isostatic sintering steps, through uniformity The powder and plasticizer are mixed, and processed using a vacuum furnace and a hot isostatic furnace to produce complex-shaped components with high density and excellent performance.

Benefits of technology

Achieve near-net molding of complex shapes, improve molding rate and mechanical properties, reduce casting defects and material waste, reduce cracks and coarse grain problems, improve manufacturing efficiency and material performance, reduce costs, and expand the scope of use .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965881660000051
    Figure BDA0004965881660000051
Patent Text Reader

Abstract

The invention is suitable for the technical field of composite material component manufacturing, and provides a titanium-aluminum alloy in a complex shape and a manufacturing method of a composite material component of the titanium-aluminum alloy. Preparing a plasticizer; preparing a blank; preparing a biscuit; preparing a pre-sintered part; inspecting and trimming; and performing hot isostatic pressing sintering. Complex shapes which cannot be achieved through forging and powder metallurgy are achieved; compared with precision casting near-net forming, the component manufactured through the method has the advantages that the forming rate is increased, casting defects are reduced, and the mechanical performance of the material is improved; compared with machining, materials are saved, the manufacturing efficiency is improved, and the manufacturing cost is reduced; and compared with additive manufacturing, the problems of cracks, coarse grains and the like are solved, the material performance is improved, the cost is reduced, and the application range is expanded. According to the method, the performance of the component can be accurately controlled by adjusting technological parameters, and the density can reach 95-100% of the theoretical density; the whole process is simple to control and easy to realize industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material component manufacturing, and in particular relates to a method for manufacturing a complex-shaped titanium-aluminum alloy and a composite material component thereof. Background Art

[0002] Titanium aluminum alloys and their composite materials have important application value in aerospace, automobile, electronics, target materials and other fields due to their excellent properties such as high strength, low density and high temperature resistance. However, due to their poor fluidity in liquid state and severe solidification segregation, the use of precision casting methods to manufacture complex-shaped parts is difficult to form, with coarse grains, severe segregation, poor performance, and serious material waste. At room temperature, they are brittle, have low deformation capacity, are difficult to machine, have low efficiency, and waste materials. It is difficult to manufacture parts of complex shapes using forging and powder metallurgy methods.

[0003] Additive manufacturing can break through the constraints of shape, but it still faces problems such as cracks and coarse grains. Therefore, developing a new manufacturing technology for complex-shaped parts of titanium-aluminum alloys and their composite materials is of great significance to give full play to the performance of titanium-aluminum alloys and their composite materials and improve the manufacturing efficiency of complex-shaped parts of titanium-aluminum alloys and their composite materials. Summary of the invention

[0004] The purpose of the present invention is to provide a method for manufacturing a complex-shaped titanium-aluminum alloy and a composite material component thereof, aiming to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for manufacturing a complex-shaped titanium-aluminum alloy and a composite material component thereof, comprising the following steps:

[0007] Step 1: Material preparation: Select dry and pure titanium-aluminum alloy and its composite material powders, screen and grade them according to their shape and particle size distribution, and mix them evenly;

[0008] Step 2, plasticizer preparation: prepare according to the plasticizer formula;

[0009] Step 3, blank preparation: the powder and the plasticizer are mixed evenly in proportion to form a blank;

[0010] Step 4, blank preparation: adding the blank into the injection molding machine with the mold installed, and injecting according to the preset process parameters to form the blank;

[0011] Step 5, preparation of pre-sintered parts: put the green blank into a high temperature resistant container, fill it with non-oxidizing material powder and compact it, then put the container into a vacuum furnace, open the furnace according to a specific heating and vacuuming procedure, and take out the pre-sintered parts after cooling in the furnace;

[0012] Step 6: Inspection and finishing: surface treatment of the pre-burned parts;

[0013] Step 7, hot isostatic pressing sintering: Place the pre-burned parts in the partition layer of the hot isostatic pressing furnace tooling, perform hot isostatic pressing sintering according to the established process parameters, and take out the parts after cooling in the furnace.

[0014] Furthermore, in step 1, select d 50 The spherical Ti45Al2Cr2Nb powder has a particle size of 10 to 20 μm and a maximum particle size of no more than 40 μm.

[0015] Furthermore, in step 2, the plasticizer is prepared according to the proportion of paraffin, beeswax and other materials.

[0016] Furthermore, in step 3, the ratio of plasticizer to powder is 1:4 to 1:20.

[0017] Furthermore, in step 4, the mold temperature is maintained at 30-40° C., the blank is added, and the preform is produced according to the process parameters of injection temperature 100-150° C., injection pressure 100-2000 bar, and holding time 90-180 seconds.

[0018] Furthermore, in step 5, after placing the container in a vacuum furnace, the vacuum furnace is heated to 400-500°C at a heating rate of 3-5°C / min, maintained for 1.5-2h, and then vacuumized to 1.3x10 -1 ~13x10 -1 Pa, continue to heat up to 680-780℃, maintain for 4-6h, increase to 890-950℃ at a heating rate of 5-10℃ / min, maintain for 30-60min, cool with the furnace to below 250℃, take out the heat-resistant container and pre-burned parts.

[0019] Furthermore, in step 7, the pre-sintered component is placed in a partition layer in a hot isostatic pressing furnace, and the argon pressure is 110-130 MPa, the furnace temperature is 920±20° C., and the temperature is kept for 90-180 min. The component is taken out after cooling to room temperature.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The complex-shaped titanium-aluminum alloy and composite material component manufacturing method are provided by setting

[0022] 1. The present invention realizes the near-net forming of complex-shaped titanium-aluminum alloy and composite material components, and realizes complex shapes that cannot be achieved by forging and powder metallurgy;

[0023] 2. Compared with near-net-shape forming by precision casting, the complex-shaped titanium-aluminum alloy and composite material components produced by the present invention have improved forming rate, reduced casting defects, and improved mechanical properties of materials; compared with mechanical processing, they save materials, improve manufacturing efficiency, and reduce manufacturing costs; compared with additive manufacturing, they reduce problems such as cracks and coarse grains, improve material properties, reduce costs, and expand the scope of use.

[0024] 3. The present invention can achieve precise control of component performance by adjusting process parameters, and the density can reach 95-100% of the theoretical density; the whole process is simple to control and easy to realize industrial production. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0026] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0027] Embodiment 1: A method for manufacturing a complex-shaped titanium-aluminum alloy and a composite material component thereof provided in one embodiment of the present invention comprises the following steps:

[0028] Step 1, material preparation: select dry, pure titanium-aluminum alloy and its composite material powder, screen and grade its shape and particle size distribution, and mix them evenly;

[0029] Step 2, plasticizer preparation: prepare according to the plasticizer formula;

[0030] Step 3, blank preparation: the powder and the plasticizer are mixed evenly in proportion to form a blank;

[0031] Step 4, blank preparation: adding the blank into the injection molding machine with the mold installed, and injecting according to the preset process parameters to form the blank;

[0032] Step 5, preparation of pre-sintered parts: put the green blank into a high temperature resistant container, fill it with high temperature resistant non-oxidizing material powder and compact it, then put the container into a vacuum furnace, open the furnace according to a specific heating and vacuuming procedure, and take out the pre-sintered parts after cooling in the furnace;

[0033] Step 6: Inspection and finishing: Perform surface treatment on the pre-burned parts; check the size, surface finish, etc., and perform finishing if necessary;

[0034] Step 7, hot isostatic pressing sintering: Place the pre-burned parts in the partition layer of the hot isostatic pressing furnace tooling (overlapping is not allowed), perform hot isostatic pressing sintering according to the established process parameters, and take out the parts after cooling in the furnace.

[0035] Embodiment 2: A method for manufacturing a complex-shaped titanium-aluminum alloy and a composite material component thereof provided by an embodiment of the present invention comprises the following steps:

[0036] Step 1: Select pure and dry materials with a particle size of less than 40 μm. 50 The particle shape and distribution of Ti45Al2Cr2Nb spherical powder with a particle size of 10 to 20 μm can be adjusted by ball milling or other methods if it does not meet the requirements;

[0037] Step 2, preparing plasticizer according to the proportion of paraffin wax, beeswax and other materials;

[0038] Step 3, melt the plasticizer, add 4 to 20 times of metal powder, stir evenly, and make a crushed blank;

[0039] Step 4: Place the compressor low-pressure turbine middle piece mold on an injection molding machine, maintain the mold temperature at 30-40° C., add the crushed blank, and prepare a preform according to the process parameters of injection temperature of 100-150° C., injection pressure of 100-2000 bar, and hold for 90-180 seconds;

[0040] Step 5: Place the preform in a high temperature resistant container, fill it with graphite powder or Y2O3 powder, compact it appropriately, and then place the container in a vacuum furnace. Raise the temperature of the vacuum furnace to 400-500°C at a rate of 3-5°C / min, keep it for 1.5-2h, and then start to evacuate to 1.3x10 -1 ~13x10 -1 Pa, continue to heat up to 680-780℃, maintain for 4-6h, increase to 890-950℃ at a heating rate of 5-10℃ / min, maintain for 30-60min, cool with the furnace to below 250℃, take out the heat-resistant container and pre-burned parts.

[0041] Step 6: Inspection and finishing: Perform surface treatment such as sandblasting on the pre-burned parts, check the size and surface finish, and finish those that do not meet the requirements;

[0042] Step 7, put the qualified pre-burned parts into a hot isostatic pressing furnace (placed in a separate layer, no overlapping is allowed), keep the temperature at 920±20℃ and argon pressure of 110-130Mpa for 90-180min, and take out the components after cooling to room temperature;

[0043] Step 8. Final inspection: Conduct a comprehensive inspection of the components as required to ensure that they meet the requirements.

[0044] The manufacturing technology of complex-shaped titanium-aluminum alloy and composite material components obtained by the above manufacturing method is compared with other technologies, as shown in Table 1;

[0045] Table 1

[0046]

[0047] It can be seen from Table 1 that the components manufactured by this method, compared with the near-net-shape molding of precision casting, have improved the molding rate, reduced casting defects, and improved the mechanical properties of the material; compared with mechanical processing, it saves materials, improves manufacturing efficiency, and reduces manufacturing costs; compared with additive manufacturing, it reduces problems such as cracks and coarse grains, improves material properties, reduces costs, and expands the scope of use.

[0048] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.

Claims

1. A method for manufacturing a complex-shaped titanium-aluminum alloy and a composite material component thereof, characterized in that: The following steps are involved: Step 1, material preparation: select dry, pure titanium aluminum alloy and its composite material powder, screen and grade the shape and particle size distribution, and mix them evenly; Step 2, plasticizer preparation: prepare according to the plasticizer formula; Step 3, blank preparation: the powder and the plasticizer are mixed evenly in proportion to form a blank; Step 4, blank preparation: adding the blank into the injection molding machine with the mold installed, and injecting according to the preset process parameters to form the blank; Step 5, preparation of pre-sintered parts: put the green blank into a high temperature resistant container, fill it with non-oxidizing material powder and compact it, then put the container into a vacuum furnace, open the furnace according to a specific heating and vacuuming procedure, and take out the pre-sintered parts after cooling in the furnace; Step 6: Inspection and finishing: surface treatment of the pre-burned parts; Step 7, hot isostatic pressing sintering: Place the pre-burned parts in the partition layer of the hot isostatic pressing furnace tooling, perform hot isostatic pressing sintering according to the established process parameters, and take out the parts after cooling in the furnace.

2. The method for manufacturing complex-shaped titanium-aluminum alloy and composite material components thereof according to claim 1, characterized in that: In step 1, select d 50 The spherical Ti45Al2Cr2Nb powder has a particle size of 10 to 20 μm and a maximum particle size of no more than 40 μm.

3. The method for manufacturing complex-shaped titanium-aluminum alloy and composite material components according to claim 1, characterized in that: In the step 2, a plasticizer is prepared according to the proportion of paraffin wax, beeswax and other materials.

4. The method for manufacturing complex-shaped titanium-aluminum alloy and composite material components according to claim 1, characterized in that: In the step 3, the ratio of plasticizer to powder is 1:4 to 1:

20.

5. The method for manufacturing complex-shaped titanium-aluminum alloy and composite material components thereof according to claim 1, characterized in that: In step 4, the mold temperature is maintained at 30-40° C., the blank is added, and the preform is produced according to the process parameters of injection temperature 100-150° C., injection pressure 100-2000 bar, and holding time 90-180 seconds.

6. The method for manufacturing complex-shaped titanium-aluminum alloy and composite material components thereof according to claim 1, characterized in that: In step 5, after placing the container in a vacuum furnace, the vacuum furnace is heated to 400-500°C at a heating rate of 3-5°C / min, maintained for 1.5-2h, and then vacuumized to 1.3x10 -1 ~13x10 -1 Pa, continue to heat up to 680-780℃, maintain for 4-6h, increase to 890-950℃ at a heating rate of 5-10℃ / min, maintain for 30-60min, cool with the furnace to below 250℃, take out the heat-resistant container and pre-burned parts.

7. The method for manufacturing complex-shaped titanium-aluminum alloy and composite material components thereof according to claim 1, characterized in that: In step 7, the pre-sintered parts are placed in a partition layer in a hot isostatic pressing furnace, and the argon pressure is 110-130 MPa, the furnace temperature is 920±20° C., and the temperature is kept for 90-180 minutes. The parts are then taken out after cooling to room temperature.