Shape memory alloy in-situ alloying method with low phase change lag
By improving the microstructure of NiTiCu alloy through ultra-high frequency pulsed TIG welding and heat treatment, the problems of non-uniform structure and poor mechanical properties in dual-wire arc additive manufacturing were solved, and efficient preparation of NiTiCu alloy with low phase transformation hysteresis was achieved, significantly improving its mechanical properties.
Patent Information
- Application Number
- CN202410979056.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Existing dual-wire arc additive manufacturing methods for NiTiCu alloys suffer from structural inhomogeneity and poor mechanical properties, especially with significant phase transformation hysteresis, which limits their application areas.
In-situ alloying of NiTiCu alloy was carried out using ultra-high frequency pulsed TIG welding, and the microstructure was improved by solution treatment and aging heat treatment, including preheating, solution treatment and aging treatment steps, with specific parameters including heating rate, holding time and gas protection.
It significantly improves the microstructure of NiTiCu alloy, reduces the size of precipitated phases, increases tensile strength and fracture strain, achieves more uniform microhardness distribution, maintains low phase transformation hysteresis, and enhances mechanical properties.
Smart Images

Figure CN118926541A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of arc additive manufacturing, and more specifically, to a NiTiCu alloy heat treatment process for arc fuse additive manufacturing. Background Art
[0002] Shape memory alloys have the special property of restoring a preset shape when heated to a critical transition temperature. Among them, near-equiatomic NiTi alloys have shape memory properties, superelastic properties, as well as biocompatibility, corrosion resistance, and fatigue resistance. They are widely used in many fields such as medical, automotive, aerospace, and intelligent manufacturing.
[0003] The addition of a third element such as Cu, Pd, Pt, Au, and Hf can improve the properties of NiTi alloys. The addition of Cu can enable the alloy to obtain good properties such as high damping performance, strong corrosion resistance, high biocompatibility, low phase change hysteresis, and stable phase change temperature.
[0004] However, NiTi-based alloys are easily doped with impurities during the traditional smelting process to form TiC and Ti4Ni2O x Ti-rich phases such as NiTi and Cu will form, resulting in changes in phase transition temperature, as well as decreased strength and ductility. In addition, the work hardening and shape memory effect of NiTi-based alloys during processing will cause severe wear of the tool, and the heat generated during processing can easily lead to phase changes in the alloy. Therefore, traditional manufacturing and processing methods limit the expansion of the application field of NiTi-based alloys. The double-wire arc fuse additive technology uses an arc as a heat source to melt two metal wires to complete layer-by-layer deposition, which can realize the in-situ alloying of NiTi and Cu and efficiently obtain NiTiCu alloy. Compared with other additive manufacturing methods, it has the characteristics of low cost, high efficiency, and fewer defects, avoiding the difficulties of traditional NiTiCu alloy processing.
[0005] On the other hand, alloys prepared by double-wire arc-fuse additive technology usually have the problem of uneven structure, and the microstructure morphology and mechanical properties between different layers are different, which affects the mechanical properties of NiTiCu alloy. Therefore, the current problem to be solved is to propose a method for manufacturing and post-processing a low phase transformation hysteresis NiTiCu alloy with excellent mechanical properties. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide an in-situ alloying and heat treatment method of a NiTiCu shape memory alloy with low phase transformation hysteresis, which is used to solve the problems of unevenness and poor mechanical properties existing in the existing twin-wire arc additively manufactured NiTiCu alloy structure.
[0007] The present invention solves the above technical problems by the following technical means:
[0008] An in-situ alloying method for a shape memory alloy with low phase transformation hysteresis comprises the following steps:
[0009] Step 1: Fix the NiTi substrate and load the NiTi alloy wire and Cu wire into the wire feeder respectively;
[0010] Step 2: Preheat the substrate with direct current TIG, TIG stands for tungsten inert gas shielded welding, and use ultra-high frequency pulse TIG to in-situ alloy the NiTi wire and the Cu wire to realize double-wire arc additive manufacturing of the NiTiCu alloy. Multiple continuous stacking is performed to obtain a deposited NiTiCu alloy sample, and the sample is cut to obtain a deposited NiTiCu alloy sample;
[0011] Step 3: Place the deposited NiTiCu alloy sample in a heat treatment furnace, raise the temperature to 900°C at a heating rate of 10-20°C / min, keep it in the furnace for 30-90 minutes, then take it out, quickly quench it in water, and complete the solution treatment;
[0012] Step 4: The NiTiCu alloy sample after the solution treatment is placed in the heat treatment furnace again, and the temperature is increased to the target aging temperature at a heating rate of 10-20°C / min. After keeping the temperature for 30-90 minutes, it is taken out and quickly quenched in water to complete the aging treatment to obtain the aged NiTiCu alloy sample.
[0013] Furthermore, the diameters of the NiTi alloy wire and the Cu wire are both 1.0 mm.
[0014] Furthermore, in step 1, the NiTi substrate is pretreated by polishing the surface of the NiTi substrate to make it smooth, then soaking it in acetone and alcohol solvents successively, ultrasonically cleaning it for 10 minutes, and drying it for later use.
[0015] Furthermore, during the preheating process of step 2, the base current of the TIG welding power supply is 100A.
[0016] Furthermore, in the additive process of step 2, the base current of the TIG welding power supply is 100A, the ultra-high frequency pulse current is 60A, the ultra-high frequency current duty cycle is 50%, and the ultra-high frequency current pulse frequency is 20kHz.
[0017] Furthermore, in the additive process of step 2, the angle between the double wire feeding nozzles of the wire feeder and the base plate is 20°, and the horizontal angle between the two wire feeding nozzles is 60°.
[0018] Furthermore, in the additive process of step 2, the welding gun travel speed is 300 mm / min, the NiTi wire feeding speed is 2200 mm / min, and the Cu wire feeding speed is 240 mm / min.
[0019] Furthermore, during the additive process of step 2, 15 L / min of high-purity argon gas is continuously introduced into the TIG welding gun and the local gas protection device to reduce oxidation.
[0020] Furthermore, during the heat treatment process of step 3 and step 4, high-purity argon gas with a flow rate of 15 L / min was continuously introduced for protection.
[0021] The present invention has the following beneficial effects:
[0022] (1) The present invention provides a heat treatment process for arc fuse additive manufacturing of NiTiCu alloy, which improves the microstructure morphology of NiTiCu and reduces the size and area of precipitated phase through solid solution and aging heat treatment.
[0023] (2) The NiTiCu alloy manufactured by arc fuse additive manufacturing after solid solution aging treatment in the present invention has greatly improved tensile strength and fracture strain compared with the deposited NiTiCu alloy while maintaining low phase transformation hysteresis, and the microhardness distribution is more uniform. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a flow chart of the present invention.
[0025] Figure 2 It is a schematic structural diagram of the double-wire arc material adding device of the present invention;
[0026] Figure 3 The chemical composition analysis results of the aged NiTiCu alloy phases of Examples 1-3 of the present invention are shown in Figures 1-3, where (a) is Example 1, (b) is Example 2, and (c) is Example 3.
[0027] Figure 4 It is a comparison diagram of the phase change behavior curves of the aged NiTiCu alloys of Examples 1-3 of the present invention and the deposited NiTiCu alloy of Comparative Example 1.
[0028] Figure 5 The statistical results of phase transformation hysteresis of the aged NiTiCu alloys of Examples 1-3 of the present invention and the deposited NiTiCu alloy of Comparative Example 1 are shown.
[0029] Figure 6 The microhardness distribution cloud diagrams of the aged NiTiCu alloys of Examples 1-3 of the present invention and the deposited NiTiCu alloy of Comparative Example 1 are shown in FIG. 1 , wherein (a) is Comparative Example 1, (b) is Example 1, (c) is Example 2, and (d) is Example 3.
[0030] Figure 7 The tensile strength and fracture strain statistics of the aged NiTiCu alloys of Examples 1-3 of the present invention and the deposited NiTiCu alloy of Comparative Example 1 are shown. DETAILED DESCRIPTION
[0031] The present invention is further described clearly and completely below in conjunction with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only used to explain the present invention, but not to limit the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] The experimental materials used in the embodiments of the present invention are NiTi substrate, NiTi alloy wire, and Cu metal wire.
[0033] Please refer to Figure 2 The double-wire arc additive device in the following embodiments includes but is not limited to an ultra-high frequency TIG welding gun, a double-wire wire feed nozzle, a local argon shielding cover and a substrate. The welding gun and the wire feed nozzle are connected by a fixing ring, and an adjustment device is provided on the fixing ring to achieve angle adjustment and distance adjustment between the two wire feed nozzles. The local argon shielding cover is fixed to the welding gun by bolts.
[0034] The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis of the present invention uses ultra-high frequency pulse TIG to in-situ alloy NiTi wire and Cu wire, realizes double-wire arc additive manufacturing of NiTiCu alloy, and uses a heat treatment furnace to perform two heat treatments of aging and solid solution on NiTiCu alloy. Specifically, it includes the following steps:
[0035] S1: Fix the NiTi substrate with a clamp, load the NiTi alloy wire and the Cu wire into the wire feeder respectively, and adjust the position and angle of the wire feeder nozzle;
[0036] The angle between the wire feeding nozzle and the substrate is 20°, the horizontal angle between the two wire feeding nozzles is 60°, and the NiTi wire is placed above the Cu wire to ensure sufficient melting of the double-wire droplets and liquid bridge transition.
[0037] S2: Set the ultra-high frequency pulse TIG welding power supply parameters, preheat the substrate with DC TIG, and use ultra-high frequency pulse TIG to in-situ alloy the NiTi wire and the Cu wire to realize the double-wire arc additive manufacturing of the NiTiCu alloy. The deposited NiTiCu alloy specimens are obtained by multiple continuous stacking, and the specimens are cut to obtain the deposited NiTiCu alloy samples.
[0038] Specifically, the substrate was pretreated before adding materials, the surface of the NiTi substrate was polished smooth, then immersed in acetone and alcohol solvents successively, ultrasonically cleaned for 10 minutes, and dried for use.
[0039] Furthermore, during the preheating process, the base current of the TIG welding power supply is 100A.
[0040] Furthermore, in the additive process, the base current of the TIG welding power source is 100A, the ultra-high frequency pulse current is 60A, the ultra-high frequency current duty cycle is 50%, and the ultra-high frequency current pulse frequency is 20kHz. The ultra-high frequency pulse TIG can ensure that the NiTi wire and the Cu wire can be fully and evenly melted, and the microstructure morphology of the obtained NiTiCu shape memory alloy is fine grains.
[0041] Furthermore, in the double-wire arc material addition step, the diameters of the NiTi alloy wire and the Cu wire are both 1.0 mm.
[0042] Furthermore, in the double-wire arc additive step, the welding gun travel speed is 300 mm / min, the NiTi wire feeding speed is 2200 mm / min, the Cu wire feeding speed is 240 mm / min, the time interval between each stacking layer is 60 s, and the layer height is 2 mm.
[0043] Furthermore, in the twin-wire arc material addition step, 15 L / min of high-purity argon gas is continuously introduced into the TIG welding gun and the local gas protection device to reduce oxidation.
[0044] S3: The cut NiTiCu alloy sample is placed in a heat treatment furnace, and the temperature is increased to 900°C at a heating rate of 10°C / min. After being kept in the furnace for 60 minutes, the sample is taken out and quickly quenched in water to complete the solution treatment.
[0045] S4: The NiTiCu alloy sample after solution treatment was put into the heat treatment furnace again, and the temperature was raised to 450℃~650℃ at a heating rate of 10℃ / min. After being kept in the furnace for 60min, it was taken out and quickly quenched in water to complete the aging treatment to obtain the aged NiTiCu alloy sample. In order to prevent oxidation of the sample during the heat treatment process, high-purity argon gas with a flow rate of 15L / min was continuously introduced for protection.
[0046] The in-situ alloying method of the shape memory alloy with low phase transformation hysteresis is described below through Examples 1-3:
[0047] Example 1
[0048] In this embodiment, a method for in-situ alloying of a shape memory alloy with low phase transition hysteresis comprises the following steps:
[0049] Step 1: Polish the surface of the NiTi substrate until it is smooth, then soak it in acetone and alcohol solvents successively, clean it ultrasonically for 10 minutes, and dry it for later use.
[0050] Step 2: Fix the substrate, load the NiTi alloy wire and Cu wire with a diameter of 1.0 mm into the wire feeder respectively, adjust the angle of the wire feeding nozzle relative to the substrate to 20°, the horizontal angle between the two wire feeding nozzles to 60°, and place the NiTi wire above the Cu wire to ensure sufficient melting of the double wire droplets and liquid bridge transition.
[0051] Step 3: Continue to introduce 15L / min of high-purity argon gas into the TIG welding gun and the local gas protection device to reduce oxidation, use DC TIG for preheating, the preheating base current is 100A, and the preheating welding gun speed is 100mm / min. Then use ultra-high frequency pulse TIG to in-situ alloy the NiTi wire and the Cu wire, the additive base current is 100A, the additive ultra-high frequency pulse current is 60A, the ultra-high frequency current duty cycle is 50%, the ultra-high frequency current pulse frequency is 20kHz, the welding gun stroke speed is set to 300mm / min, the NiTi wire feeding speed is 2200mm / min, and the Cu wire feeding speed is 240mm / min. The time interval between each stacking layer is 60s, the layer height is 2mm, and the NiTiCu alloy sample is obtained by multiple continuous stacking.
[0052] Step 4: After forming is completed, turn off the ultra-high frequency pulse TIG welding machine and wire feeder, turn off the high-purity argon gas, wait for the sample and substrate to cool to room temperature, and then cut the sample to obtain the required sample.
[0053] Step 5: Place the cut NiTiCu alloy sample into a heat treatment furnace, continuously introduce high-purity argon gas at a flow rate of 15 L / min for protection, increase the temperature to 900°C at a heating rate of 10°C / min, keep it in the furnace for 60 minutes, then take it out and quickly quench it in water to obtain a solid solution NiTiCu alloy sample.
[0054] Step 6: The NiTiCu alloy sample after solution treatment is placed in the heat treatment furnace again, and high-purity argon gas with a flow rate of 15L / min is continuously introduced for protection. The temperature is increased to the target aging temperature of 450°C at a heating rate of 10°C / min. After keeping the temperature for 60 minutes, it is taken out and quickly quenched in water to complete the aging treatment to obtain the aged NiTiCu alloy sample.
[0055] Example 2
[0056] The preparation method of Example 2 is substantially the same as that of Example 1, except that the target aging temperature in step 6 is set to 550°C.
[0057] Example 3
[0058] The preparation method of Example 3 is substantially the same as that of Example 1, except that the target aging temperature in step 6 is set to 650°C.
[0059] Comparative Example 1
[0060] The preparation method of Comparative Example 1 is substantially the same as that of Example 1, except that only the twin-wire arc additive manufacturing part is performed, and the heat treatment in steps 5 and 6 is not performed.
[0061] The following tests were performed on the NiTiCu shape memory alloys prepared in the above examples and comparative examples.
[0062] 1. Phase chemical composition analysis
[0063] Figure 3 The results of phase chemical composition analysis of the aged NiTiCu alloys of Examples 1-3 of the present invention were performed using a scanning electron microscope equipped with an energy dispersive spectrometer, wherein (a) is Example 1, (b) is Example 2, and (c) is Example 3.
[0064] Depend on Figure 3 It can be known that: in the NiTiCu alloy obtained by the three embodiments, the Ni element is evenly distributed, the Ti element is mainly distributed inside the matrix, and the Cu element is mainly distributed on the precipitated phase formed along the grain boundary, indicating that different aging temperatures have no significant effect on the element distribution law. The copper-containing precipitated phase in embodiment 1 is mainly spherical particles, and the size is finer and more evenly distributed. The copper-containing precipitated phase of embodiment 2 is mainly mesh-shaped, and the size is larger. Embodiment 3 observed that the obvious mesh-shaped precipitated phase grew up and coarsened. It is shown that different aging temperatures can cause the morphology of the precipitated phase to change. The coarsened precipitated phase can cause the mechanical properties to deteriorate, and therefore, the precipitated phase morphology of embodiment 1 is more conducive to the improvement of mechanical properties.
[0065] 2. Differential scanning calorimetry
[0066] Figure 4 The following is a comparison diagram of the phase change behavior curves of the aged NiTiCu alloys of Examples 1-3 of the present invention and the deposited NiTiCu alloy of Comparative Example 1. Figure 4 It can be seen that the deposited sample and the three example samples only undergo one phase transition from B2 to B19 during the heating and cooling process.
[0067] Figure 5 The phase transition temperature and phase transition hysteresis of the aged NiTiCu alloys of Examples 1-3 of the present invention and the deposited NiTiCu alloy of Comparative Example 1 are statistical results. Wherein, As, Ap, Af, Ms, Mp, Mf, Ap-Mp are respectively the austenite phase transition start temperature, austenite phase transition peak temperature, austenite phase transition end temperature, martensite phase transition start temperature, martensite phase transition peak temperature, martensite phase transition end temperature and phase transition hysteresis.
[0068] Depend on Figure 5It can be seen that the phase transition temperatures of the samples of the embodiments are lower than those of the comparative samples, and as the aging temperature increases, the sharpness of the phase transition peaks in the heating and cooling processes gradually decreases, and the corresponding phase transition temperature range (Af-As, Ms-Mf) increases significantly, which indicates that the heat treatment method of the present invention will change the phase transition temperature of the NiTiCu alloy. The phase transition hysteresis of Example 1, Example 2, and Example 3 are 11.7°C, 14.6°C, and 13.8°C, respectively, all of which maintain low phase transition hysteresis, among which the phase transition hysteresis of Example 1 is the lowest, indicating that the heat treatment method of the present invention can effectively maintain the low phase transition hysteresis of the NiTiCu alloy.
[0069] 3. Microhardness test
[0070] Figure 6 The microhardness distribution cloud diagrams of the aged NiTiCu alloys of Examples 1-3 of the present invention and the deposited NiTiCu alloy of Comparative Example 1 are shown in FIG. 1 , wherein (a) is Comparative Example 1, (b) is Example 1, (c) is Example 2, and (d) is Example 3.
[0071] like Figure 6 As shown in a, the microhardness distribution of Comparative Example 1 is obviously uneven, and the overall microhardness shows a trend of gradually increasing from the bottom to the top. Figure 6 It can be seen from b, c, and d that the microhardness distribution of Examples 1-3 is significantly more uniform than that of Comparative Example 1. The overall average microhardness of Comparative Example 1, Example 1, Example 2, and Example 3 are 346.4 HV, 326.3 HV, 243.5 HV, and 272.5 HV, respectively, indicating that the heat treatment method of the present invention can reduce the average microhardness of the NiTiCu sample and make the microhardness distribution more uniform.
[0072] 4. Tensile performance test
[0073] Figure 7 The tensile strength and fracture strain statistics of the aged NiTiCu alloys of Examples 1-3 of the present invention and the deposited NiTiCu alloy of Comparative Example 1 are shown in the figure. The tensile strength and fracture strain values indicated in the figure are the average values calculated after three parallel tensile tests of the corresponding samples.
[0074] like Figure 7 As shown, it can be clearly seen that the tensile strength and fracture strain of Example 1, Example 2, and Example 3 are significantly higher than those of Comparative Example 1. The sample of Example 1 has the best tensile properties, with a maximum tensile strength of 468 MPa and a maximum fracture strain of 5.8%. Compared with Comparative Example 1, the average tensile strength and fracture strain of the sample of Example 1 are increased by 81% and 43%, respectively.
[0075] The above tensile properties test results show that the tensile properties of the NiTiCu sample are significantly improved while maintaining low phase transformation hysteresis, indicating that the heat treatment method of the low phase transformation hysteresis NiTiCu shape memory alloy prepared by the double-wire arc fuse additive technology of the present invention can effectively improve the mechanical properties of the deposited NiTiCu sample, and the mechanical properties obtained at a lower aging temperature are better.
[0076] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that it should be understood by those of ordinary skill in the art that several modifications and substitutions made without departing from the concept of the present invention all belong to the protection scope of the present invention. The technology, shape, and structural parts not described in detail in the present invention are all well-known technologies.
Claims
1. A method for in-situ alloying of a shape memory alloy with low phase transition hysteresis, comprising the following steps: Step 1: Fix the NiTi substrate and load the NiTi alloy wire and Cu wire into the wire feeder respectively; Step 2: Preheat the substrate with direct current TIG, TIG stands for tungsten inert gas shielded welding, and use ultra-high frequency pulse TIG to in-situ alloy the NiTi wire and the Cu wire to realize double-wire arc additive manufacturing of the NiTiCu alloy. Multiple continuous stacking is performed to obtain a deposited NiTiCu alloy sample, and the sample is cut to obtain a deposited NiTiCu alloy sample; Step 3: Place the deposited NiTiCu alloy sample in a heat treatment furnace, raise the temperature to 900°C at a heating rate of 10-20°C / min, keep it in the furnace for 30-90 minutes, then take it out, quickly quench it in water, and complete the solution treatment; Step 4: The NiTiCu alloy sample after the solution treatment is placed in the heat treatment furnace again, and the temperature is increased to the target aging temperature at a heating rate of 10-20°C / min. After keeping the temperature for 30-90 minutes, it is taken out and quickly quenched in water to complete the aging treatment to obtain the aged NiTiCu alloy sample.
2. The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis as claimed in claim 1, It is characterized in that The diameters of the NiTi alloy wire and the Cu wire are both 1.0 mm.
3. The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis as claimed in claim 1, It is characterized in that In the step 1, the NiTi substrate is pretreated by polishing the surface of the NiTi substrate to make it smooth, then soaking it in acetone and alcohol solvents successively, ultrasonically cleaning it for 10 minutes, and drying it for later use.
4. The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis as claimed in claim 1, It is characterized in that During the preheating process of step 2, the base current of the TIG welding power source is 100A.
5. The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis as claimed in claim 1, It is characterized in that During the additive process of step 2, the base current of the TIG welding power source is 100A, the ultra-high frequency pulse current is 60A, the ultra-high frequency current duty cycle is 50%, and the ultra-high frequency current pulse frequency is 20kHz.
6. The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis as claimed in claim 1, It is characterized in that During the additive process of step 2, the angle between the double wire feeding nozzles of the wire feeder and the substrate is 20°, and the horizontal angle between the two wire feeding nozzles is 60°.
7. The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis as claimed in claim 1, It is characterized in that During the additive process of step 2, the welding gun travel speed is 300 mm / min, the NiTi wire feeding speed is 2200 mm / min, and the Cu wire feeding speed is 240 mm / min.
8. The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis as claimed in claim 1, It is characterized in that During the additive process of step 2, 15 L / min of high-purity argon gas is continuously introduced into the TIG welding gun and the local gas protection device to reduce oxidation.
9. The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis as claimed in claim 1, It is characterized in that During the heat treatment process of step 3 and step 4, high-purity argon gas with a flow rate of 15 L / min was continuously introduced for protection.
10. The in-situ alloying method of a shape memory alloy with low phase transformation hysteresis as claimed in claim 1, It is characterized in that The target aging temperature in step 4 is 450-650°C.
Citation Information
Cited By
Shape memory alloy spring based on NiTiCu ternary alloy and preparation method thereof
CN120311120A