Composite aluminum alloy and short-wavelength laser additive manufacturing method and application thereof

By adding ceramic powder to the aluminum alloy and using green light selected laser melting technology, the problem of cracks and uneven forming in laser additive manufacturing of composite aluminum alloys is solved, and its mechanical properties and molding quality are significantly improved.

CN118926546APending Publication Date: 2024-11-12GUANGDONG INST OF NEW MATERIALS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410996607.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing composite aluminum alloys are prone to cracks and pores in the laser additive manufacturing process, resulting in uneven forming and insufficient comprehensive performance.

Method used

Add two ceramic powders to the aluminum alloy, and use green light selection laser melting technology to refine grains, reduce columnar crystal growth, promote the formation of equiaxed crystal structure, and use low reflectance short-wavelength laser to improve energy absorption and solve the interface Defect problems: uniform molding and reducing burning of elements such as Zn and Mg.

Benefits of technology

It significantly reduces the generation of cracks and improves the mechanical properties of composite aluminum alloys, especially the tensile strength and hardness, achieving uniform molding of aluminum alloys and comprehensive performance improvements in materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926546A_ABST
    Figure CN118926546A_ABST
Patent Text Reader

Abstract

The invention provides a composite aluminum alloy and a short-wavelength laser additive manufacturing method and application thereof, and the short-wavelength laser additive manufacturing method of the composite aluminum alloy comprises the following steps: S1, preparing composite aluminum alloy powder which comprises the following element components in percentage by mass: 1.00-2.00% of SiC, 1.00-2.00% of TiC and the balance of aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises 90.8 + / -0.05% of Al, 5.0 + / -0.07% of Zn, 2.5 + / -0.05% of Mg and 1.7 + / -0.08% of Cu; ball-milling and mixing for later use; s2, performing three-dimensional digital modeling by using three-dimensional modeling software; and S3, green laser selective melting is used for preparing the composite aluminum alloy powder to obtain a modeling target, and the composite aluminum alloy is obtained. Two kinds of ceramic powder are added into the aluminum alloy, the composite aluminum alloy is prepared through the green light selective laser melting technology, grains can be refined, cracks are obviously reduced, short-wavelength laser is used for preparation, burning loss of elements such as Zn and Mg is reduced, and the mechanical property of the composite aluminum alloy is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal additive manufacturing, and in particular to a composite aluminum alloy and a short-wavelength laser additive manufacturing method and application thereof. Background Art

[0002] Aluminum alloy has a series of advantages, such as low density, high specific strength, good plasticity, strong corrosion resistance, strong electrical and thermal conductivity, and has been increasingly widely used in aerospace, transportation, shipbuilding, chemical industry, electronic devices, etc. However, with the development of related technical fields, traditional manufacturing methods and single materials are gradually unable to meet technical standards, which puts forward higher requirements for aluminum alloy lightweight and high strength.

[0003] Particle-reinforced aluminum matrix composites (PRAMCs) are based on pure aluminum or aluminum alloys. By introducing TiB2, TiC, SiC, Al2O3, SiO2 or related metal particles or in-situ generation of particle reinforcement phases, new materials with different properties from the matrix are obtained. Compared with traditional aluminum alloys, they have performance advantages such as high specific strength, high stiffness, and low thermal expansion coefficient. However, in some application scenarios, due to the requirements of the geometric structure of complex aluminum alloy components, it is difficult to achieve good forming by traditional methods. Laser additive manufacturing technology, as a rapid prototyping technology, has printing flexibility that traditional manufacturing technologies cannot match. At the same time, it has the characteristics of short printing cycle and high material utilization, which can effectively solve the problem of forming complex, high-performance precision aluminum alloy components.

[0004] However, due to the high laser reflection, high thermal conductivity and high thermal expansion of aluminum metal, aluminum alloys are prone to cracks and other defects during laser additive manufacturing. In addition, although the addition of alloying elements such as Cu, Mg, and Zn to aluminum alloys can effectively improve the mechanical properties of the material, it also increases the solidification temperature range of the material, thereby increasing the thermal cracking sensitivity of such materials, causing cracks to form in the aluminum alloy during the solidification process, which poses a great challenge to the additive manufacturing technology preparation method.

[0005] Chinese patent CN117920990A "A 7075 aluminum alloy composite powder and laser selective melting forming method" discloses a composite aluminum alloy material with added titanium particles and tantalum particles, but the powder in the composite aluminum alloy is not fully melted, there are many internal cracks and pores, and the forming is uneven, and its comprehensive performance still needs to be further improved.

[0006] Therefore, it is of great significance to develop a composite aluminum alloy that is uniformly formed and can improve the comprehensive performance of the composite aluminum alloy, as well as a preparation method and application thereof. Summary of the invention

[0007] In view of the fact that the existing short-wavelength laser additive manufacturing method for composite aluminum alloys has the problems of insufficient powder melting, many porosities, and average forming quality, and its comprehensive performance still needs to be further improved, the present invention provides a composite aluminum alloy and its short-wavelength laser additive manufacturing method and application, with uniform ceramic phase distribution and excellent mechanical properties.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0010] S1. Prepare a composite aluminum alloy powder, comprising the following elemental components by mass percentage: SiC: 1.00-2.00%, TiC: 1.00-2.00%, and the balance is aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8±0.05%, Zn: 5.0±0.07%, Mg: 2.5±0.05%, and Cu: 1.7±0.08%; ball milling and mixing, and set aside;

[0011] S2. Perform three-dimensional digital modeling using three-dimensional modeling software;

[0012] S3. Use green laser selective melting to prepare the composite aluminum alloy powder to obtain a modeling target, thereby obtaining the composite aluminum alloy.

[0013] The present invention aims at the defects that the high laser reflection characteristics of aluminum metal in particle-reinforced aluminum-based composite materials lead to easy formation of cracks, the addition of alloy elements increases the sensitivity to thermal cracking, the difficulty in controlling the size of the particle-reinforced phase, the difficulty in uniformly dispersing ceramic or metal particles, and the poor interface bonding with the matrix, which leads to insufficient melting of the particle-reinforced aluminum-based composite material powder, more internal pores, and uneven forming. By adding two kinds of ceramic powders to the aluminum alloy, the grains are refined, the growth of columnar crystals is reduced, and the formation of equiaxed crystal structure is promoted to inhibit cracks. The generation of cracks can be significantly reduced or even inhibited, and the strength of the aluminum alloy is improved. degree, thereby improving the mechanical properties of the composite aluminum alloy; at the same time, the green light selective laser melting technology is creatively used to prepare a composite aluminum alloy containing two ceramic particles. The energy absorption rate of the composite aluminum alloy is improved during the forming process through a short-wavelength laser with low reflectivity, so that the composite aluminum alloy powder is fully melted, and the interface defect problem caused by poor wettability between the reinforcement phase and the metal matrix is ​​solved, and uniform forming is achieved. At the same time, the burn-in loss of elements such as Zn and Mg is reduced, which can ensure the MgZn2 content in the aluminum alloy with a significant strengthening effect and improve the comprehensive strength of the composite aluminum alloy, especially the tensile strength and hardness.

[0014] Furthermore, the green laser selective melting laser power in S3 is 200-300W.

[0015] Furthermore, the diameter of the green laser selective area melting spot in S3 is set to 100 μm.

[0016] Furthermore, the green light laser selective melting scanning speed in S3 is set to 600-1500 mm / s.

[0017] Furthermore, the green light laser selective melting powder thickness in S3 is 0.03-0.05 mm, and the green light laser selective melting scanning interval in S3 is set to 0.04-0.07 mm.

[0018] Furthermore, the particle size of the aluminum alloy powder in S1 is 15-60 μm, the particle size of the SiC powder is 1-5 μm, and the particle size of the TiC powder is 1-10 μm.

[0019] The present invention preferably mixes two ceramic particles, 1-5 μm SiC powder and 1-10 μm TiC powder, with 15-60 μm aluminum alloy powder to obtain composite aluminum alloy powder, thereby achieving uniform distribution of multi-scale ceramic phases regulated from submicron to micron level, and further improving the comprehensive performance of the composite aluminum alloy, especially the hardness.

[0020] Furthermore, the ball milling mixing speed in S1 is 180 rpm and the time is 4-5 h.

[0021] Furthermore, in the ball milling mixture described in S1, the grinding balls are made of zirconia, the weight ratio of the grinding balls to the composite aluminum alloy powder is 5:1, and the grinding balls are selected in two specifications of 5mm and 2mm at the same time, and the weight ratio of the large-diameter grinding balls to the small-diameter grinding balls is 4:1.

[0022] The present invention preferably uses two specifications of zirconia grinding balls with a weight ratio of 4:1 and composite aluminum alloy powder in a ratio of 5:1 and mixes them at 180rpm for 4-5 hours. By optimizing the ball milling parameters, the micron ceramic particles and aluminum alloy powder are fully crushed and evenly mixed, which promotes the uniform distribution of the ceramic phase in the aluminum alloy matrix and further improves the forming quality.

[0023] Furthermore, the 3D modeling software in S2 is one or more of Magic, UG, Pro / e, and SolidWorks.

[0024] Another object of the present invention is to provide a composite aluminum alloy.

[0025] A composite aluminum alloy is produced by any of the composite aluminum alloy short-wavelength laser additive manufacturing methods described above.

[0026] Another object of the present invention is to provide an application of the composite aluminum alloy.

[0027] The composite aluminum alloy is used in the manufacture of aviation industry structural parts, high-strength, corrosion-resistant, high-stress structural parts, and molds.

[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0029] The composite aluminum alloy of the present invention refines the grains, reduces the growth of columnar crystals, promotes the formation of equiaxed crystal structure to inhibit cracks, and can significantly reduce or even inhibit the generation of cracks, improve the strength of the aluminum alloy, and improve the mechanical properties of the composite aluminum alloy; the composite aluminum alloy of the present invention is prepared by green light selective laser melting technology, and the aluminum alloy has a high reflectivity to infrared lasers. When the aluminum alloy block is prepared by conventional selective laser melting technology, the absorption rate of laser energy is low, which leads to insufficient melting of the powder and the generation of defects such as cracks and pores. Green light belongs to short-wavelength lasers, and aluminum The alloy has low reflectivity to short-wavelength lasers, which can increase the energy absorption rate of the aluminum alloy during the forming process, fully melt the composite aluminum alloy powder, solve the interface defect problem caused by poor wettability between the reinforcement phase and the metal matrix, and form it evenly. At the same time, it reduces the burn-in loss of elements such as Zn and Mg, and can ensure the MgZn2 content in the aluminum alloy that has a significant strengthening effect, improve the strength, especially the tensile strength and hardness. The preparation method is efficient, easy to operate, and low in cost. It has important economic value and promotion significance, and has good application prospects in marine engineering equipment, rail transit, metallurgy and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0031] Figure 1 This is a SEM image of the powder morphology of the composite aluminum alloy powder of Example 1 of the present application.

[0032] Figure 2 It is the absorption rate of the composite aluminum alloy powder of Example 1 and Comparative Example 1 of the present application to red and green lasers.

[0033] Figure 3 This is a diagram showing the OM and hardness of the composite aluminum alloys of Example 1, Example 2 and Comparative Example 1 of the present application.

[0034] Figure 4 It is a diagram of the mechanical properties of the composite aluminum alloy of Example 2 and Comparative Example 1 of the present application.

[0035] Figure 5 It is a grain size diagram of the composite aluminum alloy of Example 1 and Comparative Example 1 of the present application.

[0036] Figure 61 is the XRD diagram of Example 1, Example 2 and Comparative Example 1. DETAILED DESCRIPTION

[0037] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention is further described by the following examples. Obviously, the following examples are only part of the embodiments of the present invention, rather than all the embodiments; it should be understood that the embodiments of the present invention are only used to illustrate the technical effects of the present invention, rather than to limit the scope of protection of the present invention.

[0038] The raw materials in the examples can all be obtained commercially; unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0039] Example 1

[0040] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0041] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 1.00%, TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0042] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0043] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0044] Example 2

[0045] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0046] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 2.00%, TiC: 2.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0047] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0048] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0049] Example 3

[0050] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0051] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 1.00%, TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0052] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0053] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 200 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning interval is set to 0.06 mm to obtain the composite aluminum alloy.

[0054] Example 4

[0055] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0056] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 1.00%, TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0057] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0058] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1500 mm / s, the powder thickness is 0.05 mm, and the scanning interval is set to 0.06 mm to obtain the composite aluminum alloy.

[0059] Example 5

[0060] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0061] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 1.00%, TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0062] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0063] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 600 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0064] Comparative Example 1

[0065] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0066] S1. Prepare a composite aluminum alloy powder, comprising the following elemental components: aluminum alloy powder and inevitable impurities; the aluminum alloy powder contains Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0067] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0068] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0069] Compared with Example 1, the composite aluminum alloy of this comparative example contains only aluminum alloy powder and inevitable impurities, that is, does not contain SiC and TiC.

[0070] Comparative Example 2

[0071] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0072] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0073] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0074] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0075] Compared with Example 1, the composite aluminum alloy of this comparative example contains TiC: 1.00%, and the balance is aluminum alloy powder and inevitable impurities, that is, it does not contain SiC.

[0076] Comparative Example 3

[0077] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0078] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 3.00%, TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0079] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0080] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0081] Compared with Example 1, the composite aluminum alloy of this comparative example contains SiC: 3.00%, TiC: 1.00%, and the remainder is aluminum alloy powder and inevitable impurities, that is, SiC is excessive.

[0082] Comparative Example 4

[0083] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0084] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 1.00%, TiC: 3.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0085] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0086] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0087] Compared with Example 1, the composite aluminum alloy of this comparative example contains SiC: 1.00%, TiC: 3.00%, and the remainder is aluminum alloy powder and inevitable impurities, that is, TiC is excessive.

[0088] Comparative Example 5

[0089] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0090] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: TiB2: 1.00%, SiO2: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0091] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0092] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0093] Compared with Example 1, the composite aluminum alloy of this comparative example contains TiB2: 1.00%, SiO2: 1.00%, and the remainder is aluminum alloy powder and inevitable impurities, that is, other ceramic particles are used instead.

[0094] Comparative Example 6

[0095] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0096] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 1.00%, TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0097] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0098] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using red light laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0099] Compared with Example 1, step S3 of this comparative example adopts red light laser selective melting.

[0100] Comparative Example 7

[0101] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0102] S1. Prepare a composite aluminum alloy powder, comprising the following elemental components: aluminum alloy powder and inevitable impurities; the aluminum alloy powder contains Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0103] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0104] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using red light laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0105] Compared with Example 1, the composite aluminum alloy in this comparative example contains only aluminum alloy powder and inevitable impurities, that is, does not contain SiC and TiC, and step S3 of this comparative example adopts red light laser selective melting.

[0106] Comparative Example 8

[0107] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0108] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 1.00%, TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0109] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0110] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 150 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning spacing is set to 0.06 mm, thereby obtaining the composite aluminum alloy.

[0111] Compared with Example 1, the parameters of green laser selective melting in step S3 of this comparative example are: laser power 150W.

[0112] Comparative Example 9

[0113] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0114] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 1.00%, TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0115] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0116] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 400 W, the spot diameter is set to 100 μm, the scanning speed is set to 1000 mm / s, the powder thickness is 0.05 mm, and the scanning interval is set to 0.06 mm to obtain the composite aluminum alloy.

[0117] Compared with Example 1, the parameters of green laser selective melting in step S3 of this comparative example are: laser power 400W.

[0118] Comparative Example 10

[0119] A short-wavelength laser additive manufacturing method for a composite aluminum alloy comprises the following steps:

[0120] S1. Prepare a composite aluminum alloy powder, comprising the following elements by mass percentage: SiC: 1.00%, TiC: 1.00%, the balance being aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8%, Zn: 5.0%, Mg: 2.5%, Cu: 1.7%; ball milling at 180rpm for 5h and set aside;

[0121] S2. Use SolidWorks 3D modeling software to perform 3D digital modeling;

[0122] S3. The composite aluminum alloy powder is prepared to obtain a modeling target using green laser selective melting, the laser power is 300 W, the spot diameter is set to 100 μm, the scanning speed is set to 1800 mm / s, the powder thickness is 0.05 mm, and the scanning interval is set to 0.06 mm to obtain the composite aluminum alloy.

[0123] Compared with Example 1, the parameters of green laser selective melting in step S3 of this comparative example are: scanning speed 1800 mm / s.

[0124] Figure 1 This is an SEM image of the powder morphology of the composite aluminum alloy powder of Example 1 of the present application. It can be seen from the image that the ceramic particles of the composite aluminum alloy powder of the present invention are fully mixed with the matrix aluminum alloy powder, and the components are evenly distributed, thereby achieving multi-scale ceramic particle size regulation ranging from submicron to micron.

[0125] Figure 2 It is the absorption rate of the composite aluminum alloy powder of Example 1 and Comparative Example 1 of the present application to red and green lasers. It can be seen from the figure that the absorption rate of laser energy by Comparative Example 1 is low, while the absorption rate of the composite aluminum alloy powder of the present application to red and green lasers is higher than that of the aluminum alloy powder, and the absorption rate of green light is as high as 53%.

[0126] Figure 3 It is a graph of OM and hardness of the composite aluminum alloys of Example 1, Example 2 and Comparative Example 1. It can be seen from the graph that the composite aluminum alloy with two kinds of ceramic particles added prepared by green light laser selective melting in the present invention effectively reduces the generation of cracks and effectively improves the hardness of the aluminum alloy.

[0127] Figure 4 It is a diagram of the mechanical properties of the composite aluminum alloy of Example 2 and Comparative Example 1 of the present application. It can be seen from the diagram that the tensile strength and elongation of the composite aluminum alloy to which two types of ceramic particles are added are significantly improved.

[0128] Figure 5 It is a grain size diagram of the composite aluminum alloy of Example 1 and Comparative Example 1 of the present application. It can be seen from the figure that the composite aluminum alloy of the present invention with two kinds of ceramic particles added has significantly finer grains than the composite aluminum alloy without adding ceramic particles.

[0129] Figure 6 It is the XRD diagram of Example 1, Example 2 and Comparative Example 1. It can be seen from the figure that MgZn2 exists in the examples of the present application.

[0130] The composite aluminum alloys of Example 1, Example 2 and Comparative Example 1 were subjected to EDS element analysis test, and the data are shown in the following table:

[0131] Table 1 EDS element analysis data of composite aluminum alloys of Examples 1, 2 and Comparative Examples 1, 6, 7

[0132]

[0133]

[0134] It can be seen from the above table that compared with the untreated aluminum alloy powder, the composite aluminum alloys such as Zn and Mg prepared by the green light selective laser melting technology in Examples 1 and 2 of the present application and Comparative Example 1 have less burn-out of elements such as Zn and Mg; while the composite aluminum alloys such as Zn and Mg prepared by the red light selective laser melting technology in Comparative Examples 6 and 7 have high burn-out of elements such as Zn and Mg.

[0135] The characterization test results of the remaining embodiments are basically consistent with the results of the above embodiment.

[0136] The above samples were subjected to performance tests, and the experimental test methods were as follows:

[0137] The tensile strength is tested by a universal tensile testing machine. The higher the tensile strength, the better the material strength. The elongation is calculated by tensile testing. The higher the elongation, the better the material plasticity. The microhardness is measured in accordance with the national standard "GB / T4340.1-2009". The microhardness indicates the strength of the coating. The larger the value, the higher the coating strength.

[0138] The results are shown in the following table:

[0139] Table 2 Performance test results of composite aluminum alloys of Examples 1-5 and Comparative Examples 1-10

[0140]

[0141]

[0142] As can be seen from the above table, each embodiment of the present invention has excellent mechanical properties, good tensile strength, elongation and hardness. However, Comparative Example 1 does not contain ceramic particles, has low tensile strength, elongation of only 0.6%, low microhardness, and poor comprehensive performance; Comparative Example 2 contains only one ceramic particle, and the comprehensive performance is lower than that of each embodiment, especially the elongation, which is poor; Comparative Example 3 and Comparative Example 4 have excessive ceramic particles, and the elongation is reduced; Comparative Example 5 uses TiB2 and SiO2 to replace TiC and SiC. Due to the large difference in melting points, the melting is not sufficient, resulting in more internal defects, low tensile strength, and poor elongation; Comparative Example 6 is prepared by red light laser selective melting, and the microhardness is reduced due to the influence of internal cracks and pores; Comparative Example 7 does not contain ceramic particles and is prepared by red light laser selective melting, with low tensile strength, greatly reduced elongation and microhardness, and the worst comprehensive performance; Comparative Examples 8-10 adjust the parameters of green light laser selective melting beyond the range, and the elongation and hardness of the resulting composite aluminum alloy are reduced, and the comprehensive performance cannot be compared with the embodiments.

[0143] In summary, the present invention adds two kinds of ceramic powders to the aluminum alloy and prepares the composite aluminum alloy by the green light selective laser melting technology, which can refine the grains, reduce the growth of columnar crystals, promote the formation of equiaxed crystal structure to inhibit cracks, and significantly reduce or even inhibit the generation of cracks. The green light selective laser melting using a short-wavelength laser can improve the energy absorption rate of the aluminum alloy during the forming process, so that the composite aluminum alloy powder is fully melted, and the interface defect problem caused by poor wettability between the reinforcing phase and the metal matrix is ​​solved, and the composite aluminum alloy powder is uniformly formed. At the same time, the burn loss of elements such as Zn and Mg is reduced, and the MgZn2 content with a significant strengthening effect in the aluminum alloy can be guaranteed, and the strength, especially the tensile strength and hardness, can be improved. The preparation method is efficient, easy to operate, and low in cost. It has important economic value and promotion significance, and has good application prospects in the fields of marine engineering equipment, rail transit, metallurgy, etc.

[0144] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A short-wavelength laser additive manufacturing method for composite aluminum alloys, It is characterized in that The following steps are involved: S1. Prepare a composite aluminum alloy powder, comprising the following elemental components by mass percentage: SiC: 1.00-2.00%, TiC: 1.00-2.00%, and the balance is aluminum alloy powder and inevitable impurities; the aluminum alloy powder comprises Al: 90.8±0.05%, Zn: 5.0±0.07%, Mg: 2.5±0.05%, and Cu: 1.7±0.08%; ball milling and mixing, and set aside; S2. Perform three-dimensional digital modeling using three-dimensional modeling software; S3. Use green laser selective melting to prepare the composite aluminum alloy powder to obtain a modeling target, thereby obtaining the composite aluminum alloy.

2. A composite aluminum alloy short-wavelength laser additive manufacturing method according to claim 1, It is characterized in that S3 The green laser selective melting laser power is 200-300W.

3. A composite aluminum alloy short-wavelength laser additive manufacturing method according to claim 1, It is characterized in that The diameter of the green laser selective area melting spot in S3 is set to 100 μm.

4. A composite aluminum alloy short-wavelength laser additive manufacturing method according to claim 1, It is characterized in that The scanning speed of the green laser selective melting in S3 is set to 600-1500 mm / s.

5. A composite aluminum alloy short-wavelength laser additive manufacturing method according to claim 1, It is characterized in that The green light laser selective melting powder thickness in S3 is 0.03-0.05 mm; the green light laser selective melting scanning spacing in S3 is set to 0.04-0.07 mm.

6. A composite aluminum alloy short-wavelength laser additive manufacturing method according to claim 1, It is characterized in that The particle size of the aluminum alloy powder in S1 is 15-60 μm, the particle size of the SiC powder is 1-5 μm, and the particle size of the TiC powder is 1-10 μm.

7. A composite aluminum alloy short-wavelength laser additive manufacturing method according to claim 1, It is characterized in that S1 The ball milling mixing speed is 180 rpm and the time is 4-5 h.

8. A composite aluminum alloy short-wavelength laser additive manufacturing method according to claim 1, It is characterized in that S2 The three-dimensional modeling software is one or more of Magic, UG, Pro / e, and SolidWorks.

9. A composite aluminum alloy, It is characterized in that The composite aluminum alloy is produced by the short-wavelength laser additive manufacturing method described in any one of the above.

10. Use of the composite aluminum alloy according to claim 9 in the manufacture of aviation industry structural parts, high-strength, corrosion-resistant, high-stress structural parts, and molds.

Citation Information

Patent Citations

  • Method for preparing high-strength aluminum alloy through selective laser melting

    CN110052615A

  • SiC and TiB2 dual-phase reinforced aluminum-based composite material and preparation method thereof

    CN115369276A

  • Preparation method of dual-scale ceramic particle co-reinforced aluminum-based composite material

    CN117187611A

  • Copper-based high-entropy alloy powder for blue laser cladding additive manufacturing and application of copper-based high-entropy alloy powder

    CN117551998A

  • Aluminum alloy molded body and production method therefor

    US20230158570A1