Glass and metal laser brazing method and aircraft optical window

By preparing a quadrangular array beam shaping microtexture on the glass surface and combining ultrasonic welding, the problem of poor interface bonding in glass and metal laser brazing is solved, the connection strength and service life are improved, the assembly accuracy requirements are reduced, and the assembly accuracy requirements are improved. Processing quality and accuracy.

CN118926643AInactive Publication Date: 2024-11-12ZHEJIANG UNIV OF TECH

Patent Information

Application Number
CN202411430022.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing glass-metal connection technology aged under mechanical stress, temperature, radiation and other conditions, and the laser brazing process is complex and requires high quality of microlens arrays, making it difficult to solve the problems of interface wetting and spreading and residual stress, resulting in connection strength Low.

Method used

The microtextured quadrilateral array beam shaping is prepared on the glass surface by ultrafast laser, and the welding area is irradiated by non-focused parallel laser, combined with ultrasonic wavewelding to act on the upper surface of the glass to complete the pre-embedding and welding of the solder, improving the The bonding strength of solder and glass and the mechanical structure of interface.

Benefits of technology

It significantly improves the laser brazing connection strength and service life of glass and metal, reduces assembly accuracy requirements, improves the wetting and spreading ability of solder, and improves processing quality and accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926643A_ABST
    Figure CN118926643A_ABST
Patent Text Reader

Abstract

The invention discloses a laser brazing method for glass and metal and an aircraft optical window. The method comprises the steps that 1, ultrafast laser is used for preparing a rectangular pyramid type array beam shaping micro-texture on the surface of the glass; 2, the glass with the texture on the surface, a strip-shaped welding material and a metal base body are sequentially stacked and clamped, an ultrasonic amplitude-change pole is adopted to act on the upper surface of the glass, and pre-embedding of brazing filler metal is completed; and 3, the whole laser spot capable of covering the welding area is adopted for irradiation, the laser focus is located on the strip-shaped brazing filler metal, the irradiation power is changed according to a power curve, and after vertical irradiation is finished, the connector is naturally cooled. According to the method, the rectangular pyramid-shaped array beam shaping micro-texture is manufactured on the surface of the glass through ultrafast laser, the laser penetrates through the glass micro-texture and irradiates the connected metal for heating, the molten metal material is immersed into the glass micro-texture, the brazing filler metal wettability in the brazing process can be improved, and the mechanical structure of an interface can be enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of welding of dissimilar materials, and in particular to a laser brazing method for glass and metal and an aircraft optical window. Background Art

[0002] With the development of industrial fields such as aerospace, metallurgy, materials and mechanical engineering, the application of a single material can no longer meet the needs of our actual lives. Welding between dissimilar materials can give full play to the advantages of different materials. Glass has good high compressive strength, corrosion resistance and optical properties. However, its application is limited due to its fragility and low impact. Metal has good mechanical properties and ductility. The combination of glass and metal can expand the application of glass in many industrial fields, such as space plane reflectors, aircraft optical windows, solar thermal receivers, vacuum feedthrough connectors and pacemakers. Therefore, the connection technology between glass and metal is very important.

[0003] At present, methods such as gluing, mechanical riveting, brazing, anodic bonding and laser welding are used to connect dissimilar materials between glass and metal. For example, adhesives have aging problems under mechanical stress, temperature, radiation and other conditions. Anodic bonding is difficult to connect micro-welds and materials with large differences in thermal expansion coefficients, and it is difficult to select welding areas. Ultrafast lasers use the nonlinear light absorption characteristics of laser radiation to connect glass and metal, but the assembly process during welding is relatively harsh. Brazing takes a long time and requires a vacuum environment. In the existing connection technology, optical windows used in aviation generally use gluing. This connection method ages under mechanical stress, temperature, radiation and other conditions, resulting in failure during service. Lasers achieve selective welding between glass and metal in a relatively short time. A Chinese patent (CN114131188B) discloses a laser welding method for glass and metal. The microlens array is made on the glass surface by ultrafast laser. The radius of curvature of the microlens sphere is R, the radius of the microlens is r, and the distance between the centers of two adjacent microlenses on the same horizontal line or the same vertical line is D; among them, 0.04 mm≤r≤R, 3 r≤D≤1 mm. After laser irradiation, the molten metal material is immersed in the microlens array of glass to form a self-locking structure, thereby achieving connection. However, its disadvantage is that it is difficult for the microlens array to solve the problems of interface wetting and spreading, reaction and residual stress between glass and metal, and it only plays a mechanical structure role. At the same time, the quality requirements of the microlens array are high, otherwise it will affect the assembly accuracy. Summary of the invention

[0004] The present invention aims to overcome the problems existing in the prior art and provides a laser brazing method for glass and metal and an aircraft optical window.

[0005] The first aspect of the present invention relates to a method for laser brazing of glass and metal, comprising the following steps:

[0006] Step 1: Use ultrafast laser to prepare a tetrahedral array beam shaping micro-texture on the glass surface;

[0007] Step 2: stack and clamp the textured glass, strip solder and metal substrate in sequence, and use ultrasonic variable amplitude welding to act on the upper surface of the glass to complete the pre-embedding of the solder;

[0008] Step 3: Use non-focused parallel laser to irradiate the welding area, change the irradiation power according to the power curve, and allow the joint to cool naturally after the vertical irradiation is completed.

[0009] As a further solution of the present invention, in step one, ultrafast laser "well" scanning is used to prepare a quadrangular prism array beam shaping microtexture. The ultrafast laser "well" scanning has a scanning interval of 100 microns. After the scanning is completed, it is offset by 20 microns and scanned again. The above process is a one-time processing. The ultrafast laser process parameters are: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 400-600 mm / s, and processing times 5 times.

[0010] As a further solution of the present invention, in step one, the optimal process parameters of the ultrafast laser process are: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s, and processing times 5 times.

[0011] As a further solution of the present invention, in step one, the quadrangular prism array beam shaping micro-texture is an oblique quadrangular prism, the bottom surface is a square with an edge length of 100 microns, the top surface is a square with an edge length of 45 microns, and the angle between the side edge and the bottom surface is 48°.

[0012] As a further solution of the present invention, in step 1, the glass includes but is not limited to sapphire, quartz glass, silicate glass, and soda-lime glass.

[0013] As a further solution of the present invention, in step 2, the metal includes but is not limited to aluminum alloy, stainless steel, titanium alloy, and Kovar alloy.

[0014] As a further solution of the present invention: in step 2, the solder is in strip shape with a thickness of 0.2 mm, and the solder includes but is not limited to Al-Zn, Al-Si, Ag-Cu-Ti, Sn-Ag-Ti.

[0015] As a further scheme of the present invention, in step three, the laser welding uses an unfocused parallel 1.15 mm circular spot, the welding area is larger than the glass preparation texture area, and the welding laser process parameters are: increased to 20 W at a rate of 5 W / s, kept warm for 5 s, then increased to 45-55 W at the same rate, kept warm for 5 s, decreased to 0 W at a rate of 2 W / s, and then cooled to room temperature to obtain a laser brazed joint.

[0016] Furthermore, in step three, the preferred process for laser welding is: increase the power to 20 W at a rate of 5 W / s, keep warm for 5 s, then increase the power to 50 W at the same rate, keep warm for 5 s, decrease the power to 0 W at a rate of 2 W / s, and then cool to room temperature to obtain a laser brazed joint.

[0017] As a further solution of the present invention: in step three, the laser brazing is carried out in air, vacuum, nitrogen, hydrogen or inert gas atmosphere.

[0018] The second aspect of the present invention relates to an aircraft optical window made by a laser brazing method of glass and metal of the present invention, comprising a metal base, a strip solder, and a quadrangular prism array beam shaping micro-textured optical glass. The strip solder is placed in a groove of the metal base, the quadrangular prism array beam shaping micro-textured optical glass is pressed against the metal base and the solder, and the solder of the strip solder is embedded in the texture of the upper surface of the glass.

[0019] The present invention is used for the optical window of an aircraft, and the laser brazing method used for the metal base and the glass can effectively enhance the connection strength and service life of the optical window of the aircraft. The use of ultrafast laser on the glass surface to prepare a tetrahedral array beam shaping micro-texture and pre-embed the brazing material on the glass surface can not only change the mechanical connection state of the interface between the brazing material and the glass, but also further control the shape and distribution of the laser heat source, provide a more controllable heating effect, and reduce thermal stress concentration. At the same time, the brazing between glass and metal can reduce the assembly accuracy requirements, and the micro-texture can enhance the wetting and spreading ability of the brazing material. This laser brazing method for glass and metal is extremely beneficial to improving processing quality and accuracy.

[0020] The present invention utilizes ultrafast laser to produce tetrahedral array beam shaping micro-texture on the glass surface. The laser irradiates the connected metal through the glass micro-texture to heat it, so that the molten metal material is immersed in the glass micro-texture, which can improve the wettability of the solder during the brazing process and strengthen the mechanical structure of the interface, thereby solving the problem of poor bonding between glass and solder in existing glass-metal laser brazing resulting in low joint strength.

[0021] Beneficial effects of the present invention: Compared with the traditional glass and metal connection method, the present invention uses ultrafast laser to make a tetrahedral array beam shaping micro-texture on the glass surface, and the non-focused parallel laser irradiates the brazing material through the glass micro-texture to heat it, so that the liquid metal brazing material is immersed in the glass micro-texture, which can improve the wettability of the brazing material during the brazing process and enhance the mechanical structure of the interface. The aircraft optical window made by the laser brazing method of glass and metal of the present invention can effectively enhance the connection strength and service life of the optical window connector. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a flow chart of a method for laser brazing of glass and metal.

[0023] Figure 2 The present invention is a schematic diagram of an aircraft optical window using a laser brazing method for glass and metal.

[0024] Figure 3 It is a schematic diagram of the metal-solder-glass position relationship of the present invention.

[0025] Figure 4 This is a scanning electron microscope image of the preferred textured glass of the present invention.

[0026] Figure 5 It is a scanning electron microscope image of the welded joint of Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0028] Example 1

[0029] This embodiment relates to a laser brazing method for glass and metal, comprising the following steps:

[0030] Step 1: Use ultrafast laser to prepare tetrahedral array beam shaping microtexture on the surface of quartz glass. Use pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s, ultrafast laser "well" scanning, scanning spacing 100 microns, after scanning, offset 20 microns and scan again; ultrafast laser process parameters: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s; the above process is one-time processing, the number of processing times is 5 times;

[0031] Step 2: The quartz glass with a textured surface, the Sn-Ag-Ti strip welding material with a thickness of 0.2 mm, and the TC4 titanium alloy substrate are stacked and clamped in sequence, and an ultrasonic horn is used to act on the upper surface of the glass to complete the pre-embedding of the solder;

[0032] Step 3: The laser welding uses an unfocused parallel 1.15 mm circular spot. The welding area is larger than the texture area of ​​the glass preparation. The welding laser process parameters are: increased to 20 W at a rate of 5 W / s, kept at a temperature for 5 s, then increased to 50 W at the same rate, kept at a temperature for 5 s, decreased to 0 W at a rate of 2 W / s, and then cooled to room temperature to obtain a laser brazed joint. Laser brazing is carried out in air.

[0033] After shear test, the shear strength of the joint reached 18.6 MPa.

[0034] Example 2

[0035] This embodiment relates to a laser brazing method for glass and metal, comprising the following steps:

[0036] Step 1: Use ultrafast laser to prepare tetrahedral array beam shaping microtexture on the surface of quartz glass. Use pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s, ultrafast laser "well" scanning, scanning spacing 100 microns, after scanning, offset 20 microns and scan again; ultrafast laser process parameters: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s; the above process is one-time processing, the number of processing times is 5 times;

[0037] Step 2: The quartz glass with a textured surface, the Sn-Ag-Ti strip welding material with a thickness of 0.2 mm, and the TC4 titanium alloy substrate are stacked and clamped in sequence, and an ultrasonic horn is used to act on the upper surface of the glass to complete the pre-embedding of the solder;

[0038] Step 3: The laser welding uses an unfocused parallel 1.15 mm circular spot. The welding area is larger than the texture area of ​​the glass preparation. The welding laser process parameters are as follows: increase the power to 20 W at a rate of 5 W / s, keep warm for 5 s, then increase the power to 45 W at the same rate, keep warm for 5 s, decrease the power to 0 W at a rate of 2 W / s, and then cool to room temperature to obtain a laser brazed joint. The laser brazing is carried out in air.

[0039] After shear test, the shear strength of the joint reached 12.3 MPa.

[0040] Example 3

[0041] This embodiment relates to a laser brazing method for glass and metal, comprising the following steps:

[0042] Step 1: Use ultrafast laser to prepare tetrahedral array beam shaping microtexture on the surface of quartz glass. Use pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s, ultrafast laser "well" scanning, scanning spacing 100 microns, after scanning, offset 20 microns and scan again; ultrafast laser process parameters: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s; the above process is one-time processing, the number of processing times is 5 times;

[0043] Step 2: The quartz glass with a textured surface, the Sn-Ag-Ti strip welding material with a thickness of 0.2 mm, and the TC4 titanium alloy substrate are stacked and clamped in sequence, and an ultrasonic horn is used to act on the upper surface of the glass to complete the pre-embedding of the solder;

[0044] Step 3: The laser welding uses an unfocused parallel 1.15 mm circular spot. The welding area is larger than the texture area of ​​the glass preparation. The welding laser process parameters are as follows: increase the power to 20 W at a rate of 5 W / s, keep warm for 5 s, then increase the power to 55 W at the same rate, keep warm for 5 s, decrease the power to 0 W at a rate of 2 W / s, and then cool to room temperature to obtain a laser brazed joint. The laser brazing is carried out in air.

[0045] After shear test, the shear strength of the joint reached 15.1 MPa.

[0046] Example 4

[0047] This embodiment relates to a laser brazing method for glass and metal, comprising the following steps:

[0048] Step 1: Use ultrafast laser to prepare tetrahedral array beam shaping microtexture on the surface of quartz glass. Use pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 400 mm / s, ultrafast laser "well" scanning, scanning spacing 100 microns, after scanning, offset 20 microns and scan again; ultrafast laser process parameters: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s; the above process is one-time processing, the number of processing times is 5 times;

[0049] Step 2: The quartz glass with a textured surface, the Sn-Ag-Ti strip welding material with a thickness of 0.2 mm, and the TC4 titanium alloy substrate are stacked and clamped in sequence, and an ultrasonic horn is used to act on the upper surface of the glass to complete the pre-embedding of the solder;

[0050] Step 3: The laser welding uses an unfocused parallel 1.15 mm circular spot. The welding area is larger than the texture area of ​​the glass preparation. The welding laser process parameters are: increased to 20 W at a rate of 5 W / s, kept at a temperature for 5 s, then increased to 50 W at the same rate, kept at a temperature for 5 s, decreased to 0 W at a rate of 2 W / s, and then cooled to room temperature to obtain a laser brazed joint. Laser brazing is carried out in air.

[0051] After shear test, the shear strength of the joint reached 17.4 MPa.

[0052] Example 5

[0053] This embodiment relates to a laser brazing method for glass and metal, comprising the following steps:

[0054] Step 1: Use ultrafast laser to prepare tetrahedral array beam shaping microtexture on the surface of quartz glass. Use pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 600 mm / s, ultrafast laser "well" scanning, scanning spacing 100 microns, after scanning, offset 20 microns and scan again; ultrafast laser process parameters: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s; the above process is one-time processing, the number of processing times is 5 times;

[0055] Step 2: The quartz glass with a textured surface, the Sn-Ag-Ti strip welding material with a thickness of 0.2 mm, and the TC4 titanium alloy substrate are stacked and clamped in sequence, and an ultrasonic horn is used to act on the upper surface of the glass to complete the pre-embedding of the solder;

[0056] Step 3: The laser welding uses an unfocused parallel 1.15 mm circular spot. The welding area is larger than the texture area of ​​the glass preparation. The welding laser process parameters are as follows: increase the power to 20 W at a rate of 5 W / s, keep warm for 5 s, then increase the power to 45 W at the same rate, keep warm for 5 s, decrease the power to 0 W at a rate of 2 W / s, and then cool to room temperature to obtain a laser brazed joint. The laser brazing is carried out in air.

[0057] After shear test, the shear strength of the joint reached 16.8 MPa.

[0058] Example 6

[0059] This embodiment relates to a laser brazing method for glass and metal, comprising the following steps:

[0060] Step 1: Use ultrafast laser to prepare tetrahedral array beam shaping microtexture on the surface of quartz glass. Use pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s, ultrafast laser "well" scanning, scanning spacing 100 microns, after scanning, offset 20 microns and scan again; ultrafast laser process parameters: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s; the above process is one-time processing, the number of processing times is 5 times;

[0061] Step 2: The quartz glass with a textured surface, the Ag-Cu-Ti strip welding material with a thickness of 0.2 mm, and the TC4 titanium alloy substrate are stacked and clamped in sequence, and an ultrasonic horn is used to act on the upper surface of the glass to complete the pre-embedding of the solder;

[0062] Step 3: The laser welding uses an unfocused parallel 1.15 mm circular spot. The welding area is larger than the texture area of ​​the glass preparation. The welding laser process parameters are: increased to 20 W at a rate of 5 W / s, kept at a temperature for 5 s, then increased to 50 W at the same rate, kept at a temperature for 5 s, decreased to 0 W at a rate of 2 W / s, and then cooled to room temperature to obtain a laser brazed joint. Laser brazing is carried out in air.

[0063] After shear test, the shear strength of the joint reaches 20 MPa.

[0064] Example 7

[0065] This embodiment relates to a laser brazing method for glass and metal, comprising the following steps:

[0066] Step 1: Use ultrafast laser to prepare tetrahedral array beam shaping microtexture on the surface of quartz glass. Use pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s, ultrafast laser "well" scanning, scanning spacing 100 microns, after scanning, offset 20 microns and scan again; ultrafast laser process parameters: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s; the above process is one-time processing, the number of processing times is 5 times;

[0067] Step 2: The quartz glass with a textured surface, the Al-Si strip welding material with a thickness of 0.2 mm, and the 6061 aluminum alloy substrate are stacked and clamped in sequence, and an ultrasonic horn is used to act on the upper surface of the glass to complete the pre-embedding of the solder;

[0068] Step 3: The laser welding uses an unfocused parallel 1.15 mm circular spot. The welding area is larger than the texture area of ​​the glass preparation. The welding laser process parameters are: increased to 20 W at a rate of 5 W / s, kept at a temperature for 5 s, then increased to 50 W at the same rate, kept at a temperature for 5 s, decreased to 0 W at a rate of 2 W / s, and then cooled to room temperature to obtain a laser brazed joint. Laser brazing is carried out in air.

[0069] After shear test, the shear strength of the joint reached 16.7 MPa.

[0070] Example 8

[0071] This embodiment relates to a laser brazing method for glass and metal, comprising the following steps:

[0072] Step 1: Use ultrafast laser to prepare tetrahedral array beam shaping microtexture on the surface of quartz glass. Use pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s, ultrafast laser "well" scanning, scanning spacing 100 microns, after scanning, offset 20 microns and scan again; ultrafast laser process parameters: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 500 mm / s; the above process is one-time processing, the number of processing times is 5 times;

[0073] Step 2: The quartz glass with a textured surface, the Ni-Cr strip welding material with a thickness of 0.2 mm, and the 304 stainless steel substrate are stacked and clamped in sequence, and an ultrasonic horn is used to act on the upper surface of the glass to complete the pre-embedding of the solder;

[0074] Step 3: The laser welding uses an unfocused parallel 1.15 mm circular spot. The welding area is larger than the texture area of ​​the glass preparation. The welding laser process parameters are: increased to 20 W at a rate of 5 W / s, kept at a temperature for 5 s, then increased to 50 W at the same rate, kept at a temperature for 5 s, decreased to 0 W at a rate of 2 W / s, and then cooled to room temperature to obtain a laser brazed joint. Laser brazing is carried out in air.

[0075] After shear test, the shear strength of the joint reached 22 MPa.

[0076] Example 9

[0077] This embodiment relates to an aircraft optical window made by a laser brazing method of glass and metal of the present invention, comprising a metal base, a strip brazing material, and a quadrangular prism array beam shaping micro-textured optical glass. The strip brazing material is placed in a groove of the metal base, the quadrangular prism array beam shaping micro-textured optical glass is pressed tightly on the metal base and the brazing material, and the brazing material of the strip brazing material is embedded in the texture of the upper surface of the glass. The present invention is used for an optical window of an aircraft, and the laser brazing method used for the metal base and the glass can effectively enhance the connection strength and service life of the optical window.

[0078] Comparative Example 1

[0079] This comparative example relates to a laser brazing method for glass and metal, comprising the following steps:

[0080] Step 1: stack and clamp the quartz glass, the Sn-Ag-Ti strip welding material with a thickness of 0.2 mm, and the TC4 titanium alloy substrate in sequence;

[0081] Step 2: The laser welding adopts an unfocused parallel 1.15 mm circular spot. The welding laser process parameters are as follows: increase to 20 W at a rate of 5 W / s, keep warm for 5 s, then increase to 50 W at the same rate, keep warm for 5 s, decrease to 0 W at a rate of 2 W / s, and then cool to room temperature to obtain a laser brazed joint. Laser brazing is carried out in air.

[0082] Figure 5 This is a scanning electron microscope image of the welding joint of comparative example 1 of the present invention. It can be seen from the figure that the interface between the quartz glass and the Sn-Ag-Ti solder is relatively flat. After the shear resistance test, the shear strength of the joint reaches 8 MPa.

[0083] Comparative Example 2

[0084] This comparative example relates to a laser brazing method for glass and metal, comprising the following steps:

[0085] Step 1: stack and clamp the quartz glass, the Ag-Cu-Ti strip welding material with a thickness of 0.2 mm, and the TC4 titanium alloy substrate in sequence;

[0086] Step 2: The laser welding adopts an unfocused parallel 1.15 mm circular spot. The welding laser process parameters are as follows: increase to 20 W at a rate of 5 W / s, keep warm for 5 s, then increase to 50 W at the same rate, keep warm for 5 s, decrease to 0 W at a rate of 2 W / s, and then cool to room temperature to obtain a laser brazed joint. Laser brazing is carried out in air.

[0087] It can be seen that the interface between quartz glass and Ag-Cu-Ti solder is relatively flat. After the shear test, the shear strength of the joint reaches 9.8 MPa.

[0088] Comparative Example 3

[0089] This comparative example relates to a laser brazing method for glass and metal, comprising the following steps:

[0090] Step 1: stack and clamp the quartz glass, the Al-Si strip welding material with a thickness of 0.2 mm, and the 6061 aluminum alloy substrate in sequence;

[0091] Step 2: The laser welding adopts an unfocused parallel 1.15 mm circular spot. The welding laser process parameters are as follows: increase to 20 W at a rate of 5 W / s, keep warm for 5 s, then increase to 50 W at the same rate, keep warm for 5 s, decrease to 0 W at a rate of 2 W / s, and then cool to room temperature to obtain a laser brazed joint. Laser brazing is carried out in air.

[0092] It can be seen that the interface between quartz glass and Ag-Cu-Ti solder is relatively flat. After the shear test, the shear strength of the joint reaches 9.8 MPa.

[0093] Comparative Example 4

[0094] This comparative example relates to a laser brazing method for glass and metal, comprising the following steps:

[0095] Step 1: stack and clamp the quartz glass, the Ni-Cr strip welding material with a thickness of 0.2 mm, and the 304 stainless steel substrate in sequence;

[0096] Step 2: The laser welding adopts an unfocused parallel 1.15 mm circular spot. The welding laser process parameters are as follows: increase to 20 W at a rate of 5 W / s, keep warm for 5 s, then increase to 50 W at the same rate, keep warm for 5 s, decrease to 0 W at a rate of 2 W / s, and then cool to room temperature to obtain a laser brazed joint. Laser brazing is carried out in air.

[0097] It can be seen from the observation that the interface between the quartz glass and the Ni-Cr solder is relatively flat. After the shear test, the shear strength of the joint reaches 12.3 MPa.

[0098] The contents described in the embodiments of this specification are merely an enumeration of the implementation forms of the inventive concept. The protection scope of the present invention should not be regarded as limited to the specific forms described in the embodiments. The protection scope of the present invention also extends to equivalent technical means that can be conceived by those skilled in the art based on the inventive concept.

Claims

1. A laser brazing method for glass and metal, characterized in that: The following steps are involved: Step 1: Use ultrafast laser to prepare a tetrahedral array beam shaping micro-texture on the glass surface; Step 2: stack and clamp the textured glass, strip solder, and metal substrate in sequence, and use an ultrasonic horn to act on the upper surface of the glass to complete the pre-embedding of the solder; Step 3: Use non-focused parallel laser to irradiate the welding area, change the irradiation power according to a certain power curve, and allow the joint to cool naturally after the vertical irradiation is completed.

2. A method for laser brazing of glass and metal according to claim 1, characterized in that: Ultrafast laser "well" scanning was used to prepare quadrangular prism array beam shaping microtexture with a scanning interval of 100 μm. After the scanning was completed, it was scanned again after an offset of 20 μm. The above process was one-time processing. The ultrafast laser process parameters were: pulse width 0.8 ps, average power 20 W, pulse repetition frequency 100 kHz, scanning speed 400-600 mm / s, and processing times 5 times.

3. A laser brazing method for glass and metal according to claim 2, characterized in that: Scanning speed: 500 mm / s.

4. The laser brazing method for glass and metal according to claim 1, characterized in that: The quadrangular prism array beam shaping micro-texture is an oblique quadrangular prism, the bottom surface is a square with an edge length of 100 microns, the top surface is a square with an edge length of 45 microns, and the angle between the side edge and the bottom surface is 48°.

5. The laser brazing method for glass and metal according to claim 1, characterized in that: The glass includes sapphire, fused quartz glass, silicate glass and soda-lime glass.

6. The laser brazing method for glass and metal according to claim 1, characterized in that: The metals include aluminum alloy, stainless steel, titanium alloy, and Kovar alloy.

7. The laser brazing method for glass and metal according to claim 1, characterized in that: The solder is in a strip shape with a thickness of 0.2 mm, and the solder includes Al-Zn, Al-Si, Ag-Cu-Ti, and Sn-Ag-Ti.

8. The laser brazing method for glass and metal according to claim 1, characterized in that: In step three, the laser welding uses an unfocused parallel 1.15 mm circular spot, the welding area is larger than the glass preparation texture area, and the welding laser process parameters are: increased to 20 W at a rate of 5 W / s, kept warm for 5 s, then increased to 45-55 W at the same rate, kept warm for 5 s, reduced to 0 W at a rate of 2 W / s, and then cooled to room temperature to obtain a laser brazed joint.

9. The laser brazing method for glass and metal according to claim 1, characterized in that: The laser brazing is performed in air, vacuum, nitrogen, hydrogen or inert gas atmosphere.

10. An aircraft optical window made by the laser brazing method of glass and metal as described in claim 1, comprising a metal base, a strip solder, and a quadrangular prism array beam shaping micro-textured optical glass; the strip solder is placed in a groove of the metal base, the quadrangular prism array beam shaping micro-textured optical glass is pressed against the metal base and the solder, and the solder of the strip solder is embedded in the texture of the upper surface of the glass.

Citation Information

Patent Citations

  • Laser welding method for glass and metal

    CN114131188B

  • Laser welding method for glass and metal

    CN114131188A

  • Method for realizing laser sealing of glass and stainless steel by adding titanium as transition layer

    CN115213561A

  • Brazing filler metal distribution control method used in metal-glass laser brazing process

    CN115922010A

  • Large-gap metal-glass laser hybrid welding device

    CN116079175A

Cited By

  • Ceramic / metal heterogeneous material connection method based on thermal-shape cooperative regulation and control

    CN121798076A