Ship plate steel cable type welding wire CO2 gas shielded welding system and method

By combining the CO2 gas shielded welding system for ship plate steel with a magnetic control device, and using an alternating step magnetic field to confine the plasma and molten pool, the problems of low efficiency and poor stability of CO2 gas shielded welding in ship plate steel welding are solved, achieving efficient and stable welding results.

CN118926654APending Publication Date: 2024-11-12NANJING WAVELENGTH OPTO ELECTRONICS SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411129944.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing CO2 gas shielded welding has low welding efficiency and poor arc stability in ship plate steel welding, which affects the welding quality.

Method used

A CO2 gas shielded welding system using ship plate steel cable welding wire, combined with a magnetic control device of a specific structure, is adopted. An alternating step magnetic field is generated by a conical magnetic core with high saturation magnetic induction intensity to confine the plasma and molten pool, thereby improving the arc stiffness and stability.

Benefits of technology

It significantly improves welding efficiency and quality, enhances the tensile strength of joints, meets the high-quality and high-efficiency requirements of ship welding, simplifies the operation process, and is suitable for welding thick plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926654A_ABST
    Figure CN118926654A_ABST
Patent Text Reader

Abstract

The invention discloses a ship plate steel cable type welding wire CO2 gas shielded welding system and method, and the ship plate steel cable type welding wire CO2 gas shielded welding system comprises a CO2 gas shielded welding system and a magnetic control device; the CO2 gas shielded welding system comprises a welding gun, a positive electrode cable, a negative electrode cable, a welding power source, a wire feeder, a wire feeding hose, a wire feeding cable, a wire reel, a gas pipe, a gas cylinder and a workpiece to be welded. The magnetic control device comprises an even number of high saturation flux density conical magnetic cores and an alternating current power supply, and the high saturation flux density conical magnetic cores are connected with the alternating current power supply; the high-saturation-flux-density conical magnetic cores are distributed around a welding gun in a pairwise opposite mode, every two opposite high-saturation-flux-density conical magnetic cores form a magnetic core pair, and all the magnetic core pairs are sequentially electrified to generate an alternating stepping magnetic field. While the welding efficiency is ensured, the welding quality is remarkably improved, and the requirements for high quality and high efficiency of ship welding are better met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a ship plate steel cable type welding wire CO2 gas shielded welding system and method, belonging to the technical field of ship plate steel cable type welding wire CO2 gas shielded welding. Background Art

[0002] Ship plate steel is an important hull structural material, and the quality of its welded joints directly determines the service life and service safety of the ship. Currently, CO2 gas shielded welding is the most widely used welding method in the shipbuilding industry, but the on-site working environment of the shipyard is harsh, and the welding process is often affected by many uncontrollable factors, resulting in poor welding arc stability and seriously affecting the welding quality.

[0003] In order to solve the above problems, the present invention has developed a cable-type welding wire CO2 gas shielded welding technology, which constrains the arc through an alternating stepping magnetic field, improves arc stiffness and stability, and significantly improves welding quality; on the other hand, it takes advantage of the high melting efficiency of the cable-type welding wire to significantly improve welding efficiency and meet the requirements of high-quality and high-efficiency ship welding. The present invention is of great significance for shortening the shipbuilding period, ensuring product quality, and enhancing the core competitiveness of enterprises. Summary of the invention

[0004] The present invention provides a ship plate steel cable type welding wire CO2 gas shielded welding system and method, which solves the problems of low welding efficiency and poor welding arc stability in the existing ship plate steel CO2 gas shielded welding, and significantly improves the welding quality through the coordination of a magnetic control device with a specific structure and the ship plate steel cable type welding wire CO2 gas shielded welding.

[0005] In order to solve the above technical problems, the technical solutions adopted by the present invention are as follows:

[0006] A ship plate steel cable type welding wire CO2 gas shielded welding system, comprising a CO2 gas shielded welding system and a magnetron device;

[0007] The CO2 gas shielded welding system includes a welding gun, a positive cable, a negative cable, a welding power source, a wire feeder, a wire feeding hose, a wire feeding cable, a welding wire reel, a gas pipe, a gas cylinder and a workpiece to be welded;

[0008] The positive electrode of the welding power source is connected to the welding gun through the positive cable, and the negative electrode of the welding power source is connected to the workpiece to be welded through the negative cable; the welding wire reel is connected to the wire feeder through the wire feeding hose, the wire feeder is connected to the welding power source through the wire feeding cable, and the welding gun is connected to the wire feeder; the gas cylinder is connected to the wire feeder through the gas pipe;

[0009] The magnetron device comprises a high saturation magnetic induction intensity conical magnetic core and an AC power supply. The number of the high saturation magnetic induction intensity conical magnetic core is an even number, and the high saturation magnetic induction intensity conical magnetic core is connected to the AC power supply. The bottom of the high saturation magnetic induction intensity conical magnetic core is a pointed structure.

[0010] The high saturation magnetic induction intensity conical magnetic cores are distributed around the welding gun in pairs, and each two relatively high saturation magnetic induction intensity conical magnetic cores form a high saturation magnetic induction intensity conical magnetic core pair. Each high saturation magnetic induction intensity conical magnetic core pair is energized in turn to generate an alternating stepping magnetic field. The welding gun and the high saturation magnetic induction intensity conical magnetic core are both located above the workpiece to be welded.

[0011] The present application selects a high saturation magnetic induction intensity conical magnetic core with a bottom tip structure, which can generate a stronger magnetic field than a traditional electromagnetic induction coil and focus the magnetic field at the low end, thereby obtaining better welding quality. The high saturation magnetic induction intensity conical magnetic core includes a ferromagnetic core and a coil wound on the core.

[0012] The two high saturation magnetic induction intensity conical magnetic cores in the above-mentioned high saturation magnetic induction intensity conical magnetic core pair are opposite poles, and the magnetic field is generated between the opposite poles. By passing alternating current through each pair of opposite poles in turn, an alternating magnetic field is generated, that is, only a single magnetic field is generated at each moment. This is completely different from the prior art of generating a magnetic field inside the coil, and is also completely different from the simple superposition of magnetic fields between multiple coils. The magnetic field strength of this application is stronger, the scope of action is wider, and the control of the welding effect is more precise and effective. The gas cylinder contains carbon dioxide.

[0013] If a magnetic pad is set on the welding support platform, the magnetic pad has a groove structure at the welding position of the workpiece, a strong magnetic strip is installed in the groove structure, and a cover plate flush with the upper surface of the magnetic pad is installed on the surface of the strong magnetic strip. The strong magnetic strip and the high saturation magnetic induction intensity conical magnetic core form opposite magnetic poles, and the magnetic pad is made of magnetic conductive material. This device has the following defects: 1) The structure is complex and the processing cost is high: it is necessary to purchase a large piece of magnetic pad and open a groove. At the same time, it is also necessary to purchase a strong magnetic strip and place it in the groove, and it is also necessary to set a non-high saturation magnetic induction intensity conical magnetic core; 2) The operation is difficult: during processing, the welding position of the workpiece needs to be aligned with the groove. If there is a deviation, it will seriously affect the welding quality; 3) Only the control of the molten pool is considered; 4) This device is difficult to apply to the welding of ship plate steel. Ship plate steel is large in size, heavy in weight, and the welding position is variable. In actual operation, it is difficult to align the welding position with the groove in real time.

[0014] The present application does not require the setting of a magnetic conductive pad, nor does it require the opening of grooves, the installation of strong magnetic strips, and the like. There is no special requirement for the position of the welding workpiece, and there is no need to repeatedly adjust the position of the workpiece during operation. An alternating stepping magnetic field is generated by pairwise high saturation magnetic induction intensity conical magnetic cores, which can simultaneously control the plasma and the molten pool, and the welding flexibility and effect are significantly better than the above-mentioned structure with a magnetic conductive pad, etc.

[0015] In order to further improve the welding quality, as one of the preferred implementation schemes, the number of high saturation magnetic induction intensity conical magnetic cores is 4, and the high saturation magnetic induction intensity conical magnetic cores are axially symmetrically distributed relative to the central axis of the welding gun. The connecting line connecting the lower end points of each high saturation magnetic induction intensity conical magnetic core in sequence is a square, and the vertical distance from the lower end point of each high saturation magnetic induction intensity conical magnetic core to the surface of the workpiece to be welded is 6 to 8 mm.

[0016] Further preferably, two high saturation magnetic induction intensity conical magnetic cores distributed along the diagonal direction of the square form a high saturation magnetic induction intensity conical magnetic core pair, and alternating current is passed through the two pairs of high saturation magnetic induction intensity conical magnetic core pairs in sequence to generate an alternating stepping magnetic field.

[0017] The high saturation magnetic induction intensity conical magnetic core is made of ferromagnetic material.

[0018] In order to facilitate manufacturing and control, the shapes, structures and sizes of the high saturation magnetic flux density conical magnetic cores are the same. The two high saturation magnetic flux density conical magnetic cores in the high saturation magnetic flux density conical magnetic core pair are opposite poles.

[0019] The cable-type welding wire wound on the welding wire reel is formed by rotating and twisting 3 or 5 welding wires with a diameter of 0.8 mm. The cable-type welding wire is fed to the welding gun by a wire feeder.

[0020] A ship plate steel cable type welding wire CO2 gas shielded welding method, using the ship plate steel cable type welding wire CO2 gas shielded welding system for welding, comprises the following steps:

[0021] Step 1: Use machining method to make groove on the ship plate steel to be welded (workpiece to be welded);

[0022] Step 2: Pre-treat the grooved ship plate steel: Use a grinder to remove the scale and other impurities within 20mm on both sides of the weld and in the groove, and use absorbent cotton dipped in acetone to clean it, and then dip it in alcohol to clean it, to ensure that the surface of the welding area is clean and free of pollution;

[0023] Step 3: Clamp the pre-treated ship plate steel with a fixture to form a workpiece to be welded;

[0024] Step 4: Start the ship plate steel cable type welding wire CO2 gas shielded welding system, and perform base layer welding, filling layer welding and cover layer welding in sequence. During the welding process, each high saturation magnetic induction intensity conical magnetic core pair is energized in sequence to generate an alternating stepping magnetic field in the welding area, and at the same time, constrains and controls the plasma and the molten pool. The midpoint of the line connecting the lower end points of the two high saturation magnetic induction intensity conical magnetic cores (2-1) in each high saturation magnetic induction intensity conical magnetic core pair passes through the center of the weld. After welding is completed, stop the ship plate steel cable type welding wire CO2 gas shielded welding system to allow the workpiece to cool naturally to room temperature in a clamped state to reduce welding deformation.

[0025] The welding in the above step 4 is multi-layer and multi-pass welding. For ship plate steel with a thickness of 20 to 30 mm, preferably, 7 passes are welded, in order: weld pass 1 is the base layer, weld passes 2 to 6 are the filling layer, and weld pass 7 is the capping layer. For ship plate steel with a thickness of 30 to 40 mm, preferably, 9 passes are welded, in order: weld pass 1 is the base layer, weld passes 2 to 8 are the filling layer, and weld pass 9 is the capping layer. For ship plate steel with a thickness of 40 to 60 mm, preferably, 10 passes are welded, in order: weld pass 1 is the base layer, weld passes 2 to 9 are the filling layer, and weld pass 10 is the capping layer.

[0026] The fixture used in the above step 3 adopts an existing structure as long as it can fix the ship plate steel to be welded.

[0027] In the above step 4, the ship plate steel cable wire CO2 gas shielded welding system is started, that is, the AC power supply and welding power supply need to be turned on at the same time, and the welding gun, wire feeder and gas cylinder are started at the same time.

[0028] In the above step 4, the magnetic flux lines of the alternating stepping magnetic field pass through the plasma and the molten pool, exerting a Lorentz force pointing to the center on the moving charged particles, thereby constraining the plasma and the molten pool, increasing the arc stiffness and stability, and improving the welding quality.

[0029] In the above step 1, the groove is Y-shaped, V-shaped or X-shaped, the blunt edge height is 2mm, and the groove angle is 55±5°. When an X-shaped groove is used, double-sided welding is required. After the first side is welded, the back must be cleaned before welding the second side.

[0030] In the above step 4, the electrode backward tilt method is used for welding, and the tilt angle is 60-70°. That is, the welding wire tilt angle is 60-70°, and the electrode (welding wire) tilt is divided into two types: electrode forward tilt and electrode backward tilt. The inventor found that the backward tilt method with a specific tilt angle of the present application can better ensure the welding quality.

[0031] In order to better ensure the welding quality, in step 4,

[0032] The base layer welding parameters are: welding current 220-260A, arc voltage 25-30V, welding speed 10-18mm / s, wire extension 15mm, shielding gas is CO2, shielding gas flow 17-20L / min, alternating stepping magnetic field operating frequency range 200-400 steps / second; peak current of the magnetron device is 150-300A;

[0033] The welding parameters of the filling layer are: welding current 240-280A, arc voltage 27-30V, welding speed 12-20mm / s, wire extension 15mm, shielding gas is CO2, shielding gas flow 17-20L / min, alternating stepping magnetic field operating frequency range 200-400 steps / second; peak current of the magnetron device is 150-300A;

[0034] The welding parameters of the cover layer are: welding current 220~260A, arc voltage 25~30V, welding speed 10~18mm / s, wire dry extension 15mm, shielding gas is CO2, shielding gas flow rate 17~20L / min, the operating frequency range of the alternating stepping magnetic field is 200~400 steps / second; the peak current of the magnetron device is 150~300A; the interlayer temperature of each layer is 100~250℃.

[0035] The thickness of the ship plate steel to be welded is 20 to 60 mm.

[0036] The welding parent materials applicable to this application include various grades of steel for hull structures.

[0037] The technologies not mentioned in the present invention are all referred to the prior art.

[0038] The present invention has the following excellent effects:

[0039] 1) A magnetic control device with a specific structure is introduced into the CO2 gas shielded welding process of ship plate steel cable welding wire. On the one hand, the advantage of the high melting efficiency of the cable welding wire is used to improve the welding efficiency; on the other hand, an alternating stepping magnetic field is generated by the magnetic control device to constrain and control the plasma and the molten pool, thereby increasing the arc stiffness and stability, enhancing the tensile strength of the joint, and significantly improving the welding quality to meet the requirements of high-quality and efficient ship welding. The magnetic control device with a specific structure in this application is combined with the CO2 gas shielded welding of ship plate steel cable welding wire, which produces a significant synergistic promotion effect on ship plate steel welding.

[0040] 2) There is no need to set up a magnetic pad, nor is there any need to open grooves, install strong magnetic strips, etc. There is no special requirement for the position of the welding workpiece, and there is no need to repeatedly adjust the position of the workpiece during operation. It is simple and easy to operate, and the welding flexibility and effect are significantly better than the above-mentioned structure with a magnetic pad.

[0041] 3) The present invention is of great significance for shortening the shipbuilding period, ensuring product quality, and improving the core competitiveness of enterprises. At the same time, it has broad application prospects in the welding of large thick plates. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 It is a schematic diagram of the overall structure of the welding system of the ship plate steel cable type welding wire CO2 gas shielded welding of the present invention.

[0043] Figure 2 It is a three-dimensional diagram of the spatial orientation distribution of the high saturation magnetic induction intensity conical magnetic core of the present invention.

[0044] Figure 3 It is a top view of the spatial orientation distribution of the high saturation magnetic induction intensity conical magnetic core of the present invention.

[0045] Figure 4 This is the magnetic field assisted cable-type welding wire gas shielded welding arc of embodiment 3.

[0046] Figure 5 This is the gas shielded welding arc in Comparative Example 2.

[0047] In the figure: 1 is a CO2 gas shielded welding system, 1-1 is a welding gun, 1-2 is a positive cable, 1-3 is a negative cable, 1-4 is a welding power source, 1-5 is a wire feeder, 1-6 is a wire feeding hose, 1-7 is a wire feeding cable, 1-8 is a welding wire reel, 1-9 is a gas pipe, 1-10 is a gas cylinder, 1-11 is a workpiece to be welded, 2 is a magnetic field regulating device, 2-1 is a high saturation magnetic induction intensity conical magnetic core, and 2-2 is an AC power source. DETAILED DESCRIPTION

[0048] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0049] In this application, directional words such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc. are based on the orientation or position relationship shown in the drawings or in use, and are only for the convenience of describing the application, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the application.

[0050] Example 1

[0051] like Figure 1 As shown, a ship plate steel cable wire CO2 gas shielded welding system comprises a CO2 gas shielded welding system 1 and a magnetron device 2;

[0052] The CO2 gas shielded welding system 1 includes a welding gun 1-1, a positive cable 1-2, a negative cable 1-3, a welding power source 1-4, a wire feeder 1-5, a wire feeding hose 1-6, a wire feeding cable 1-7, a welding wire reel 1-8, a gas pipe 1-9, a gas cylinder 1-10 and a workpiece to be welded 1-11;

[0053] The positive electrode of the welding power source 1-4 is connected to the welding gun through the positive cable 1-2, and the negative electrode of the welding power source 1-4 is connected to the workpiece 1-11 to be welded through the negative cable 1-3; the welding wire reel 1-8 is connected to the wire feeder 1-5 through the wire feeding hose 1-6, the wire feeder 1-5 is connected to the welding power source 1-4 through the wire feeding cable 1-7, and the welding gun 1-1 is connected to the wire feeder 1-5; the gas cylinder 1-10 is connected to the wire feeder 1-5 through the gas pipe 1-9; the gas cylinder contains carbon dioxide;

[0054] The magnetron device 2 comprises a high saturation magnetic induction intensity conical magnetic core 2-1 and an AC power supply 2-2. The number of the high saturation magnetic induction intensity conical magnetic cores 2-1 is an even number. The shapes, structures and sizes of the high saturation magnetic induction intensity conical magnetic cores 2-1 are the same. The high saturation magnetic induction intensity conical magnetic cores 2-1 are all connected to the AC power supply 2-2. The bottoms of the high saturation magnetic induction intensity conical magnetic cores 2-1 are all pointed structures.

[0055] The high saturation magnetic induction intensity conical magnetic cores 2-1 are distributed around the welding gun 1-1 in pairs, and every two relatively high saturation magnetic induction intensity conical magnetic cores 2-1 form a high saturation magnetic induction intensity conical magnetic core pair. The two high saturation magnetic induction intensity conical magnetic cores in the high saturation magnetic induction intensity conical magnetic core pair are opposite poles. Each high saturation magnetic induction intensity conical magnetic core pair is energized in turn to generate an alternating stepping magnetic field; the welding gun 1-1 and the high saturation magnetic induction intensity conical magnetic core 2-1 are both located above the workpiece 1-11 to be welded.

[0056] Example 2

[0057] On the basis of Example 1, the following improvements are further made: the number of high saturation magnetic induction intensity conical magnetic cores is 4, the high saturation magnetic induction intensity conical magnetic cores are axially symmetrically distributed with respect to the central axis of the welding gun 1-1, the connecting line connecting the lower end points of each high saturation magnetic induction intensity conical magnetic core in sequence is a square, and the two high saturation magnetic induction intensity conical magnetic cores distributed along the diagonal direction of the square constitute a high saturation magnetic induction intensity conical magnetic core pair, the high saturation magnetic induction intensity conical magnetic core 2-1 is made of ferromagnetic material, and alternating current is passed through the two pairs of high saturation magnetic induction intensity conical magnetic core pairs in sequence to generate an alternating stepping magnetic field.

[0058] Example 3

[0059] A ship plate steel cable type welding wire CO2 gas shielded welding method, using the ship plate steel cable type welding wire CO2 gas shielded welding system in Example 2 for welding, comprising the following steps:

[0060] (1) The base material is DH36 high-strength steel for hull structure (workpiece to be welded), with dimensions of 300×150×30 mm. The filler wire is a cable-type welding wire twisted together by three ER50-6 welding wires with a diameter of 0.8 mm. The cable-type welding wire is fed to the welding gun by a wire feeder;

[0061] (2) A Y-shaped groove is made on the steel plate by machining, with a blunt edge height of 2 mm and a groove angle of 55°;

[0062] (3) Pre-treat the steel plate with grooves, remove impurities such as scale within 20 mm on both sides of the weld and in the groove with a grinder, and then use absorbent cotton dipped in acetone and alcohol to clean them to ensure that the surface of the welding area is clean and free of pollution;

[0063] (4) The pretreated steel plate is clamped and fixed with a fixture to form a workpiece to be welded;

[0064] (5) The electrode backward tilt method is used for welding, the tilt angle is 70°, the vertical distance from the lower end point of the high saturation magnetic induction intensity conical magnetic core to the weld surface is 7 mm, and the midpoint of the line connecting the lower end points of the two high saturation magnetic induction intensity conical magnetic cores 2-1 in each high saturation magnetic induction intensity conical magnetic core pair passes through the center of the weld;

[0065] (6) Start the ship plate steel cable wire CO2 gas shielded welding system and perform multi-layer and multi-pass welding. A total of 7 passes are welded, which are: pass 1 is the base layer, passes 2 to 6 are the filling layer, and pass 7 is the cover layer. The welding parameters for the base layer are: welding current 230A, arc voltage 26V, welding speed 14mm / s, welding wire dry extension length 15mm, shielding gas is CO2, shielding gas flow rate 20L / min, the operating frequency range of the alternating stepping magnetic field is 300 steps / second, and the peak current of the magnetron device is 180A; the welding parameters for the filling layer are: welding current 280A, arc voltage 30V, welding speed 20mm / s, welding wire dry extension length 15mm, shielding gas is CO2, shielding gas flow rate 20L / min, the operating frequency range of the alternating stepping magnetic field is 400 steps / second, and the peak current of the magnetron device is 180A; the welding parameters of the cap layer are: welding current 250A, arc voltage 28V, welding speed 17mm / s, wire dry extension length 15mm, shielding gas is CO2, shielding gas flow rate 20L / min, the operating frequency range of the alternating stepping magnetic field is 300 steps / second, and the peak current of the magnetron device is 180A; the interlayer temperature of each layer is 100-250℃; during the welding process, two pairs of high saturation magnetic induction intensity conical core pairs are energized in turn, and an alternating stepping magnetic field is generated in the welding area, in which magnetic flux lines pass through the welding arc and the molten pool, and at the same time, a confinement control is formed on the plasma and the molten pool; Figure 4 As shown, the arc has high stiffness and good stability during the entire welding process.

[0066] (7) After welding is completed, the ship plate steel cable wire CO2 gas shielded welding system is stopped to allow the workpiece to cool naturally to room temperature in the clamped state to reduce welding deformation. According to the tensile test, the tensile strength of the welded joint in this embodiment is 585MPa.

[0067] Embodiment 4:

[0068] This embodiment is basically the same as the embodiment 3, except that the parent material is AH36 high-strength hull structure steel, and the rest is referred to the embodiment 3. According to the tensile test, the tensile strength of the welded joint in this embodiment is 570 MPa.

[0069] Embodiment 5:

[0070] This embodiment is basically the same as the embodiment 3, except that the parent material is E-grade general strength hull structure steel, and the rest is referred to the embodiment 3. According to the tensile test, the tensile strength of the welded joint in this embodiment is 539 MPa.

[0071] Comparative Example 1

[0072] The difference between the gas shielded welding system used in this example and Example 2 is that the number of high saturation magnetic induction intensity conical magnetic cores is 1, the number of non-high saturation magnetic induction intensity conical magnetic cores is 1, and the high saturation magnetic induction intensity conical magnetic cores and the non-high saturation magnetic induction intensity conical magnetic cores are arranged relative to each other. The high saturation magnetic induction intensity conical magnetic cores and the non-high saturation magnetic induction intensity conical magnetic cores are axially symmetrically distributed relative to the central axis of the welding gun. A magnetic conductive pad is arranged on the welding support platform, and a groove structure is provided on the magnetic conductive pad at the welding position of the workpiece. A strong magnetic strip is installed in the groove structure. A cover plate flush with the upper surface of the magnetic conductive pad is installed on the surface of the strong magnetic strip. The strong magnetic strip and the high saturation magnetic induction intensity conical magnetic core form opposite magnetic poles, and the magnetic conductive pad is made of magnetic conductive material. The rest of the structure of the gas shielded welding system refers to Example 2. This gas shielded welding system is used to weld DH36 high-strength hull structure steel. The specific process and parameters are all referred to Example 3. Compared with this example, the arc stiffness and stability of Example 3 are significantly improved during the entire welding process. After the tensile test, the tensile strength of the welded joint in this embodiment is 465 MPa.

[0073] Comparative Example 2

[0074] The gas shielded welding system used in this example is different from that in Example 2 in that the magnetic control device 2 is not provided. This gas shielded welding system is used to weld DH36 high-strength hull structure steel. The specific process and parameters are all referred to Example 3. The welding arc in this example is as follows Figure 5 As shown, compared Figure 4 and Figure 5 It can be seen that, compared with this example, the arc stiffness during the entire welding process is significantly improved in Example 3. According to the tensile test, the tensile strength of the welded joint in this embodiment is 445 MPa.

[0075] Comparative Example 3

[0076] The difference from Example 3 is that the welding speed of the base layer is 8 mm / s, the welding speed of the filling layer is 10 mm / s, and the welding speed of the cover layer is 8 mm / s, that is, the welding speed is reduced relative to Example 3, and the rest is referred to Example 3. The tensile strength of the welded joint is 515 MPa, which is 12% lower than that of Example 3.

[0077] Comparative Example 4

[0078] The difference from Example 3 is that the welding speed of the base layer is 20 mm / s, the welding speed of the filling layer is 22 mm / s, and the welding speed of the cover layer is 20 mm / s, that is, the welding speed is faster than that of Example 3, and the rest is referred to Example 3. The tensile strength of the welded joint is 499 MPa, which is nearly 15% lower than that of Example 3.

Claims

1. A ship plate steel cable welding wire CO 2 Gas shielded welding system, Features: Including CO 2 Gas shielded welding system (1) and magnetron device (2); CO 2 The gas shielded welding system (1) comprises a welding gun (1-1), a positive cable (1-2), a negative cable (1-3), a welding power source (1-4), a wire feeder (1-5), a wire feeding hose (1-6), a wire feeding cable (1-7), a welding wire reel (1-8), a gas pipe (1-9), a gas cylinder (1-10) and a workpiece to be welded (1-11); The positive electrode of the welding power source (1-4) is connected to the welding gun (1-1) through the positive cable (1-2), and the negative electrode of the welding power source (1-4) is connected to the workpiece (1-11) to be welded through the negative cable (1-3); the welding wire reel (1-8) is connected to the wire feeder (1-5) through the wire feeding hose (1-6), the wire feeder (1-5) is connected to the welding power source (1-4) through the wire feeding cable (1-7), and the welding gun (1-1) is connected to the wire feeder (1-5); the gas cylinder (1-10) is connected to the wire feeder (1-5) through the gas pipe (1-9); The magnetron device (2) comprises a high saturation magnetic induction intensity conical magnetic core (2-1) and an AC power source (2-2); the number of the high saturation magnetic induction intensity conical magnetic cores (2-1) is an even number, and the high saturation magnetic induction intensity conical magnetic cores (2-1) are all connected to the AC power source (2-2); the bottoms of the high saturation magnetic induction intensity conical magnetic cores (2-1) are all pointed structures; The high saturation magnetic induction intensity conical magnetic cores (2-1) are distributed around the welding gun (1-1) in pairs, and each two of the high saturation magnetic induction intensity conical magnetic cores (2-1) are opposite to each other to form a high saturation magnetic induction intensity conical magnetic core pair. Each high saturation magnetic induction intensity conical magnetic core pair is energized in turn to generate an alternating stepping magnetic field. The welding gun (1-1) and the high saturation magnetic induction intensity conical magnetic core (2-1) are both located above a workpiece (1-11) to be welded.

2. The shipboard steel cable welding wire CO according to claim 1 2 Gas shielded welding system, Features: The number of high saturation magnetic induction intensity conical magnetic cores (2-1) is 4. The high saturation magnetic induction intensity conical magnetic cores (2-1) are axially symmetrically distributed relative to the central axis of the welding gun (1-1). The connecting line connecting the lower end points of each high saturation magnetic induction intensity conical magnetic core (2-1) in sequence is a square. The vertical distance from the lower end point of each high saturation magnetic induction intensity conical magnetic core (2-1) to the workpiece (1-11) to be welded is 6 to 8 mm.

3. The shipboard steel cable welding wire CO according to claim 2 2 Gas shielded welding system, Features: Two high saturation magnetic induction intensity conical magnetic cores (2-1) distributed along the diagonal direction of the square form a high saturation magnetic induction intensity conical magnetic core pair. Alternating current is passed through the two pairs of high saturation magnetic induction intensity conical magnetic core pairs in sequence to generate an alternating step magnetic field.

4. The ship plate steel cable welding wire CO according to any one of claims 1 to 3 2 Gas shielded welding system, Features: The high saturation magnetic induction intensity conical magnetic core (2-1) is made of ferromagnetic material.

5. The ship plate steel cable welding wire CO according to any one of claims 1 to 3 2 Gas shielded welding system, Features: The shapes, structures and sizes of the high saturation magnetic induction intensity conical magnetic cores (2-1) are all the same, and the two high saturation magnetic induction intensity conical magnetic cores in the high saturation magnetic induction intensity conical magnetic core pair are magnetic poles of opposite names.

6. The ship plate steel cable welding wire CO according to any one of claims 1 to 3 2 Gas shielded welding system, Features: The cable-type welding wire wound on the welding wire reel (1-8) is formed by rotating and twisting 3 or 5 welding wires with a diameter of 0.8 mm.

7. A shipboard steel cable welding wire CO 2 Gas shielded welding method, using the ship plate steel cable type welding wire CO according to any one of claims 1 to 6 2 Welding is performed using a gas shielded welding system. Features: The following steps are involved: Step 1: Use machining method to make groove on the ship plate steel to be welded; Step 2: Pre-treat the grooved ship plate steel: Use a grinder to remove impurities within 20mm on both sides of the weld and in the groove, and use absorbent cotton dipped in acetone to clean it, and then dip it in alcohol to clean it, to ensure that the surface of the welding area is clean and free of pollution; Step 3: Clamp the pre-treated ship plate steel with a fixture to form a workpiece to be welded; Step 4: Start the shipboard steel cable welding wire CO 2 The gas shielded welding system sequentially performs base layer welding, filling layer welding and cover layer welding. During the welding process, each high saturation magnetic induction intensity conical magnetic core pair is energized in turn to generate an alternating stepping magnetic field in the welding area, and at the same time, a constraint control is formed on the plasma and the molten pool. The midpoint of the line connecting the lower end points of the two high saturation magnetic induction intensity conical magnetic cores (2-1) in each high saturation magnetic induction intensity conical magnetic core pair passes through the center of the weld. After the welding is completed, the ship plate steel cable type welding wire CO is stopped. 2 The gas shielded welding system allows the workpiece to cool naturally to room temperature while being clamped.

8. The ship plate steel cable welding wire CO according to claim 7 2 Gas shielded welding method, Features: In step 1, the groove is Y-shaped, V-shaped or X-shaped, the blunt edge height is 2mm, and the groove angle is 55±5°. When an X-shaped groove is used, double-sided welding is required. After the first side is welded, the back side is cleaned first, and then the second side is welded.

9. The ship plate steel cable welding wire CO according to claim 7 or 8 2 Gas shielded welding method, Features: In step 4, welding is performed by using the electrode backward tilting method with a tilting angle of 60 to 70 degrees; the thickness of the ship plate steel to be welded is 20 to 60 mm.

10. The ship plate steel cable welding wire CO according to claim 7 or 8 2 Gas shielded welding method, Features: In step four, The base layer welding parameters are: welding current 220~260A, arc voltage 25~30V, welding speed 10~18mm / s, wire extension length 15mm, shielding gas is CO 2 , the protective gas flow rate is 17-20L / min, and the operating frequency range of the alternating stepping magnetic field is 200-400 steps / second; The welding parameters of the filling layer are: welding current 240-280A, arc voltage 27-30V, welding speed 12-20mm / s, wire extension 15mm, shielding gas CO 2 , the protective gas flow rate is 17-20L / min, and the operating frequency range of the alternating stepping magnetic field is 200-400 steps / second; The welding parameters of the cover layer are: welding current 220~260A, arc voltage 25~30V, welding speed 10~18mm / s, wire extension length 15mm, shielding gas is CO 2 , the protective gas flow rate is 17-20L / min, the operating frequency range of the alternating stepping magnetic field is 200-400 steps / second; the interlayer temperature of each layer is 100-250℃.