Device and method for spiral stirring friction additive forming of dissimilar metal composite pipe
Through spiral friction stir additive technology, the metal plate is formed into a spiral shape and friction stir additive on the surface, solving the problems of low production efficiency and low interface strength of different metal composite tubes, achieving efficient preparation of different metal composite tubes, improving the Production efficiency and material properties.
Patent Information
- Application Number
- CN202411305481.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-12
AI Technical Summary
The existing methods for preparing heterogeneous metal composite tubes have problems of low production efficiency and low composite interface strength, especially when using extrusion and drawing composite methods.
Using spiral friction stir additive technology, the metal plate is formed into a spiral structure and friction stir additive is performed on its surface to form a different metal composite tube, and the metal is realized by lifting stirring needles, plasticized screws and shoulders. Deposition and plasticization.
It improves the production efficiency of different metal composite pipes, enhances the bonding strength of metal interfaces, reduces production costs, and fills the gap in the formation of pipe fittings by Friction Stir Additive Manufacturing.
Smart Images

Figure CN118926674A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of additive manufacturing of metal materials, and in particular relates to a device and method for spiral stir friction additive forming of a dissimilar metal composite pipe. Background Art
[0002] Friction stir additive manufacturing technology uses friction heat generation and plastic deformation to soften metal materials, allowing them to be formed in the designed position and shape without melting. After the components to be processed are cut in the appropriate direction, this technology can be used to form them layer by layer. This technology is a new type of solid-phase additive method for metal materials developed based on friction stir welding. Compared with metal molten additive, it is like friction stir welding compared to traditional welding. It has the advantages of not producing thermal stress defects such as cracks and pores. Stirring friction causes the material to undergo fine grain strengthening and improves the comprehensive mechanical properties of the material.
[0003] In production practice, in order to cope with the working conditions brought about by different working conditions, dissimilar metal composite pipes are usually used to solve the problem, that is, pipes prepared by stacking two or more metals layer by layer to utilize the advantages of each metal to meet the production needs in production practice; for example, since aluminum has excellent thermal conductivity, electrical conductivity, corrosion resistance and oxidation resistance, good plasticity, low density and other characteristics, and steel has high strength and good cold processing properties, aluminum-steel composite pipes have the advantages of corrosion resistance, high strength, small weight and low cost. Therefore, aluminum / steel bimetallic materials have been widely used in electrolytic cells, light industry, shipbuilding, metallurgy, atomic energy and other fields.
[0004] Nowadays, metal composite pipes are mostly produced by extrusion and drawing, which uses the high temperature generated by pressure and extrusion or friction to produce metallurgical bonding between metal pipes of different materials; however, similar production methods have complex procedures and low yields. There are also more advanced methods for preparing dissimilar metal composite pipes, such as explosive welding, cold / hot spraying, solid-liquid casting and rolling, but they all have problems such as low production efficiency or low composite interface strength. Summary of the invention
[0005] In view of the above-mentioned existing technical problems and shortcomings, the present invention provides a forming device and method for a dissimilar metal composite tube based on spiral stir friction additive. The method first forms a plate into a spiral structure, and stirs friction additively a layer of dissimilar metal on the outer surface of the formed spiral structure to finally obtain a dissimilar metal composite tube.
[0006] To achieve the above-mentioned object of the invention, the technical solution of the present invention is as follows:
[0007] A device for spiral friction stir additive forming of dissimilar metal composite pipes comprises a roller group and a friction stir additive spindle, wherein the roller group is used to form a plate into a spiral structure; the friction stir additive spindle is used to stir friction add a layer of dissimilar metal on the outer surface of the formed spiral structure, and finally obtain the dissimilar metal composite pipe.
[0008] The friction stir additive spindle includes a lifting and pulling stirring needle 203, a plasticizing screw 201 and a shoulder 202. The shoulder 202 is nested outside the plasticizing screw so that the highest point of its lower surface is aligned with the lower surface of the plasticizing screw. The lifting and pulling stirring needle 203 is fixed on the plasticizing screw 201, and the plasticizing screw 201 is connected to the machine tool spindle. The shoulder 202 is fixed so that the shoulder 202 does not rotate when the plasticizing screw 201 rotates; the lifting and pulling stirring needle 203 includes a support disc 403, a stirring needle 402 and a shaft rod 401, which are an integrated structure; the friction stir additive spindle can be loaded by CNC machine tools, robotic arms and other equipment. During processing, the lifting and pulling stirring needle provides support and most of the heat for the welding additive area of the spindle, and the plasticizing screw cooperates with the shoulder to cut and plasticize the metal; finally, the metal sheet is formed into a tube and heterogeneous metals are deposited on its surface to achieve the preparation of heterogeneous metal composite tubes.
[0009] Preferably, the upper surface of the support disc 403 in the pulling stirring needle 203 and the surface of the stirring needle 402 have threads in the same direction.
[0010] Preferably, the curvature of the upper surface of the support disc 403 should be consistent with the curvature of the inner surface of the processed pipe, so that the support disc and the inner surface of the processed pipe can be fitted together during the friction stir additive process.
[0011] Preferably, the threads on the upper surface of the support disc 403 can gather the plates to facilitate the stir-friction welding of the plates; at the same time, the flash and burrs on the inner surface of the pipe caused by the stir-friction welding can be milled off.
[0012] Preferably, the pulling and stirring needle 203 rotates in a direction such that the thread direction points to the outside of the tube wall, thereby providing support for the plate in the welding area and allowing the plasticized metal to flow toward the outside of the tube wall to ensure the forming accuracy of the inner wall of the tube.
[0013] Preferably, the length of the stirring needle 402 should be greater than the thickness of the processed plate, so that when the supporting disc 403 is in contact with the inner surface of the processed plate, the distance between the lower surface of the shoulder and the outer surface of the processed pipe is 1 to 2 mm for depositing dissimilar metals.
[0014] Preferably, the lifting and stirring needle 203 is fixed in the plasticizing screw 201 by a thread and a set screw.
[0015] Preferably, the plasticizing screw 201 has a thread groove on the outside with a rotation direction opposite to that of the thread on the pulling and stirring needle 203, which is used to cut the metal wire to be deposited on the surface of the pipe. At the same time, the friction heat and axial downward pressure generated by the rotation cause the metal to be plasticized and deposited on the surface of the pipe.
[0016] Preferably, the inner wall of the plasticizing screw 201 has an internal thread for fixing the lifting and stirring needle.
[0017] Preferably, the curvature of the lower surface of the shoulder should be consistent with the curvature of the outer surface of the processed pipe to ensure the forming quality of the outer wall of the pipe.
[0018] Preferably, the shaft shoulder is provided with a through hole for wire feeding, which should be located in the upper middle part of the shaft shoulder to prevent the high temperature generated in the processing area from causing the wire to soften too much and thus causing poor wire feeding.
[0019] Preferably, the wire feeding hole should be radially connected to the inside of the shaft shoulder at a certain angle, which can increase the area of the wire feeding hole and reduce the time the wire feeding hole is closed by the plasticizing screw, thereby reducing the probability of blockage and facilitating wire feeding.
[0020] To achieve the above-mentioned purpose of the invention, the present invention provides a method for preparing a dissimilar metal composite tube based on spiral stir friction additive, using the above-mentioned device, and the steps are as follows:
[0021] Step 1: Feed the metal sheet into a roller group to roll it into a spiral structure.
[0022] Step 2: Stir friction welding along the spiral gap of the spiral structure.
[0023] Step 3: When the shoulder is completely placed on the plate, wire feeding begins, friction stir additive is performed, and the deposition of dissimilar metals begins.
[0024] Step 4: Cut the ends of the formed pipe.
[0025] Preferred: In order to form the plate into a spiral structure, the plate should be fed in at a certain angle for rolling. The angle should be determined by the plate to be processed and the required forming tube diameter. The calculation formula is: Where α is the angle between the feeding direction of the sheet and the axial direction of the formed tube, d is the width of the processed sheet, t is the thickness of the processed sheet, and R is the required diameter of the formed tube.
[0026] Preferably: when processing composite tubes of different sizes, the stir friction additive spindle needs to be replaced according to the inner and outer diameters of the processed tube and the pitch of the plate bending during processing, so as to avoid interference between the spindle and the plate during processing while ensuring the welding of the plate and ensuring that the deposited layer of metal can completely cover the surface of the tube.
[0027] Further: The calculation formula for the plate bending pitch is:
[0028] Furthermore: to ensure that the deposited metal completely covers the tube, the diameter of the plasticizing screw and the inner diameter of the shoulder of the stir friction additive spindle should be larger than the pitch of the plate when it is bent, so that there is overlap between the deposited layers.
[0029] Optimum: To ensure the tube forming effect, welding and additive processing are performed when the plate is screwed in 1.5 turns. Taking the stirring needle as the reference, the axial distance between the stir friction additive spindle and the plate feeding point is l, and the radial distance is 2r.
[0030] Preferably: the roller group consists of a pair of bending rollers and two retaining rollers to bend the plate, and the roller width is the plate width; the bending rollers are installed at the plate input in the axial direction, and the retaining rollers are axially close to the bending rollers to ensure the roundness of the bent pipe.
[0031] Optimum: The rollers should be evenly distributed inside and outside the pipe, and the angle between the rollers should be 30° or 60° to ensure the roundness of the plate bending.
[0032] Preferably, the roller in contact with the outer side of the tube after the material addition should reserve a thickness of the material addition layer with the surface of the tube compared with the roller in contact with the outer side of the tube before the material addition, so as to ensure the roundness of the plate bending.
[0033] Preferably, the outer edge of the roller should have rounded corners to ensure the surface quality of the formed pipe.
[0034] The technical effects of the device and method for preparing a heterogeneous metal composite tube based on spiral stir friction additive are as follows:
[0035] 1. The spiral stir friction additive manufacturing method for dissimilar metal composite pipes provided by the present invention can realize the stir friction additive manufacturing of dissimilar metal composite pipes, fill the gap of stir friction additive manufacturing for pipe forming, and solve the problem of low metal interface bonding strength of dissimilar metal composite pipes.
[0036] 2. The method provided by the present invention can flexibly form heterogeneous metal composite pipes of different materials, pipe diameters, wall thicknesses and lengths according to production needs, thereby improving production efficiency and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 Schematic diagram of preparing dissimilar metal composite tubes by spiral stir friction additive manufacturing;
[0038] Figure 2 Schematic diagram of the friction stir additive spindle;
[0039] Figure 3 Cross-sectional view of the friction stir additive manufacturing spindle;
[0040] Figure 4 Schematic diagram of the pulling stirring needle.
[0041] Figure 5 Schematic diagram of the plate roll bending forming angle;
[0042] Figure 6 Schematic diagram of steel-aluminum bimetallic composite pipe.
[0043] Figure 7 Schematic diagram of roller group structure
[0044] Description of reference numerals:
[0045] 1- Friction stir additive spindle; 2- Roller bending roller; 3- Holding roller; 4- Feeding roller; 5- Metal sheet; 6- Metal wire; Vz- Spindle forward direction.
[0046] 201- plasticizing screw; 202- shaft shoulder; 203- lifting stirring needle;
[0047] 301-wire feeding hole; 302-threaded hole;
[0048] 401-shaft rod; 402-stirring needle; 403-support disc; 404-tightening surface;
[0049] 501-welding starting point; α-sheet forming angle; L-pitch; d-sheet width; R-tube inner diameter; Vs-sheet input direction; Vc-tube forming direction;
[0050] 601-6061 aluminum alloy; 602-304 stainless steel. DETAILED DESCRIPTION
[0051] The present invention is described in detail below in conjunction with specific embodiments.
[0052] Example 1
[0053] As shown in the figure, this embodiment provides a friction stir additive spindle for processing heterogeneous metal composite pipes, including a pulling stirring needle 203, a shoulder 202 and a plasticizing screw 201.
[0054] The pulling stirring needle 203 includes an axial rod 401, a stirring needle 402, and a supporting disc 403, which is connected to the plasticizing screw 201 by the thread on the screw 401, and is fixed by a set screw through a threaded hole 302 and a fixing surface 404. The upper surface of the supporting disc 403 is a spherical surface with a diameter of 80 mm and a thickness of 3.5 mm, the stirring needle 402 has a diameter of 8 mm and a height of 6.5 mm, and the axial rod has a height of 28.5 mm.
[0055] The shoulder 202 is nested outside the plasticizing screw so that the highest point of its lower surface is aligned with the lower surface of the plasticizing screw. Its lower surface is an arc surface with a diameter of 86 mm. The inner diameter of the shoulder 202 is 22 mm, the outer diameter is 28 mm, and the distance from the upper surface to the highest point of the lower surface is 35 mm.
[0056] The diameter of the plasticizing screw 201 is 22 mm, and on its outer surface 30 mm above the lower surface, there is a spiral groove with a width of 5 mm, a depth of 2.5 mm, and a pitch of 10 mm.
[0057] When the friction stir additive spindle is loaded onto a CNC machine tool, the lifting stirring needle 203 is fixed on the plasticizing screw 201, and the plasticizing screw 201 is connected to the spindle of the machine tool, and the shoulder 202 is fixed so that the shoulder 202 does not rotate when the plasticizing screw 201 rotates, so that the friction stir additive spindle can cut and frictionally extrude the metal wire fed from the wire feeding hole 301. At the same time, according to the above installation method, the stirring needle 402 protrudes 5mm from the highest point of the lower surface of the shoulder.
[0058] Example 2
[0059] The present embodiment provides a method for preparing a spiral stir friction additive dissimilar metal composite tube, which includes using the stir friction additive spindle described in Example 1 to weld and add materials to the plates; using 18 mm wide and 3 mm thick 304 stainless steel plates and 2 mm diameter 6061 aluminum alloy wires as materials to achieve the preparation of a steel-aluminum bimetallic composite tube with an inner diameter of 80 mm and an outer diameter of 90 mm.
[0060] Specifically, the method for preparing a spiral stir friction additive heterogeneous metal composite tube provided in this embodiment comprises the following steps:
[0061] Step 1: Fix the above-mentioned friction stir additive spindle 1 on the CNC machine tool, and feed the plate 5 into the roller group from the feeding roller 4 for roller bending to a specified arc, wherein the plate forming angle α=85.9° and the pitch L=18.05 mm.
[0062] Step 2: Continue to feed the plate 5, and stop rolling after the plate 5 is rotated 1.75 turns, so that the plate is placed in the two retaining rollers 3; the friction stir additive spindle 1 starts to rotate, and the stirring needle 402 is inserted into the plate along the main shaft forward direction Vz to the welding starting point 501 when the plate 5 is rotated 1.5 turns (the stirring needle is inserted into the gap between the plate 5 and the plate 5 to stir and mix for welding), wherein the main shaft forward direction is parallel to the tube forming direction Vc, and the support disk 403 is 1mm away from the inner wall of the tube, and the lower surface of the shoulder 202 is 1mm away from the outer wall of the tube.
[0063] Step 3: The wire 6 is fed into the stir friction additive spindle 1 through the wire feeding hole 301. The wire 6 is cut into particles due to the rotation of the plasticizing screw 201 and filled into the gap between the plasticizing screw 201 and the lower surface of the shoulder 202 and the outer surface of the pipe. The wire 6 is gradually plasticized and deposited on the surface of the pipe under the action of rotation, extrusion, friction and the high temperature generated during the process.
[0064] Step 4: gradually pull up the friction stir additive spindle 1 according to the filling and plasticization of the wire 6. While ensuring that the gap is fully filled, lift the spindle 1 until the support disc 403 is close to the pipe, and the lower surface of the shoulder 202 is 2 mm away from the outer wall of the pipe.
[0065] Step 5: Start feeding the plate 5 again. As the plate continues to be screwed in, the friction stir additive spindle 1 welds the adjacent plates together and deposits an aluminum alloy deposition layer with a width of 22 mm and a thickness of 2 mm on the weld.
[0066] Step 6: After the tube is formed to a specified length, the feeding of the wire 6 and the plate 5 is stopped, and the friction stir additive spindle 1 continues to move along the spindle forward direction Vz to exit the tube.
[0067] Step 7: Cut off the parts with poor forming quality at the beginning and end of the formed pipe (for example, 1.75-1.5=0.25 circles at the starting position), cut the beginning and end of the formed pipe flat, sandblast and polish the metal burrs produced on the inner and outer surfaces of the pipe, and complete the preparation of the steel-aluminum bimetallic composite pipe with an inner diameter of 80mm and an outer diameter of 90mm.
[0068] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
Claims
1. A device for spiral stir friction additive forming of heterogeneous metal composite pipes, characterized in that: The invention comprises a roller set and a friction stirring additive spindle. The roller set is used to form a plate into a spiral structure. The friction stirring additive spindle is used to perform friction stirring additive on the outer surface of the formed spiral structure to form a layer of heterogeneous metal, and finally obtain a heterogeneous metal composite tube.
2. The device according to claim 1, characterized in that The friction stir additive spindle comprises a lifting and pulling stirring needle (203), a plasticizing screw (201) and a shoulder (202); the shoulder (202) is nested outside the plasticizing screw so that the highest point of its lower surface is aligned with the lower surface of the plasticizing screw, the lifting and pulling stirring needle (203) is fixed on the plasticizing screw (201), and the plasticizing screw (201) is further connected to the main shaft of the machine tool, and the shoulder (202) is fixed so that the shoulder (202) does not rotate when the plasticizing screw (201) rotates; the lifting and pulling stirring needle (203) comprises a supporting disc (403), a stirring needle (402) and a shaft rod (401), and the three are an integrated structure.
3. The device according to claim 1, characterized in that The upper surface of the support disc (403) in the lifting stirring needle (203) and the surface of the stirring needle (402) have threads in the same direction.
4. The device according to claim 1, characterized in that The curvature of the upper surface of the support disc (403) should be consistent with the curvature of the inner surface of the processed pipe.
5. The device according to claim 1, characterized in that The plasticizing screw (201) has a thread groove on the outside with a rotation direction opposite to that of the thread on the pulling and stirring needle (203), which is used to cut the metal wire to be deposited on the surface of the pipe. At the same time, the friction heat and axial downward pressure generated by the rotation cause the metal to be plasticized and deposited on the surface of the pipe.
6. A method for preparing a heterogeneous metal composite tube based on spiral stir friction additive, characterized in that: Using the device described in claims 1-5, the steps are as follows: Step 1: Feed the metal sheet into a roller group to roll it into a spiral structure; Step 2: Stir friction welding along the spiral gap of the spiral structure; Step 3: When the shoulder is completely placed on the plate, wire feeding is started, friction stir additive is performed, and deposition of dissimilar metals begins; Step 4: Cut the ends of the formed pipe.
7. The preparation method according to claim 6, characterized in that: In order to form the plate into a spiral structure, the plate should be fed in at a certain angle for rolling. The angle should be determined by the plate being processed and the required forming tube diameter. The calculation formula is: Where α is the angle between the feeding direction of the sheet and the axial direction of the formed tube, d is the width of the processed sheet, t is the thickness of the processed sheet, and R is the required diameter of the formed tube.
8. The preparation method according to claim 6, characterized in that: When processing composite pipes of different sizes, the stir friction additive spindle needs to be replaced according to the inner and outer diameters of the processed pipe and the pitch of the plate bending during processing, so as to avoid interference between the spindle and the plate during processing while ensuring the welding of the plate and ensuring that the deposited layer of metal can completely cover the surface of the pipe.
9. The preparation method according to claim 6, characterized in that: To ensure that the deposited metal completely covers the tube, the diameter of the plasticizing screw and the inner diameter of the shoulder of the stir friction additive spindle should be larger than the pitch of the plate when it is bent, so that there is overlap between the deposited layers.
10. The preparation method according to claim 6, characterized in that: In order to ensure the tube forming effect, welding and additive processing are carried out when the plate is screwed in 1.5 turns. Taking the stirring needle as the reference, the axial distance between the stir friction additive spindle and the plate feeding point is l, and the radial distance is 2r.